Halogenated nitrobenzene hydrogenation catalyst and preparation method and application thereof
By acidizing the H-Beta zeolite molecular sieve and wet impregnation to support the metal active center, an efficient halogenated nitrobenzene hydrogenation catalyst was prepared, which solved the environmental and economic problems in the existing chlorinated aniline production method and achieved Highly efficient and low-cost catalytic effect.
Patent Information
- Application Number
- CN202411065269.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-19
AI Technical Summary
The existing industrial production methods of chlorinated aniline have problems such as potential environmental hazards, many by-products, high energy consumption, high production costs and limited resources of precious metal catalysts. In the preparation of non-precious metal catalysts, there are reduced product selectivity and great environmental impact. The problem.
By acidizing the H-Beta zeolite molecular sieve, loading the metal active center by wet impregnation method, a halogenated nitrobenzene hydrogenation catalyst with high dispersion and stability was prepared, using acetate, acetylacetone salt or isopropyl The metal organic salts in the alkoxide combine with H-Beta zeolite molecular sieve to form a catalyst with high catalytic activity and low cost.
The reaction efficiency and product selectivity are significantly improved, production costs and environmental impacts are reduced, and the catalyst has good cycle stability and economic benefits.
Smart Images

Figure BDA0004979170040000101 
Figure BDA0004979170040000102 
Figure BDA0004979170040000111
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of catalysts, and in particular to a halogenated nitrobenzene hydrogenation catalyst and a preparation method and application thereof. Background Art
[0002] As an important basic chemical raw material and organic synthesis intermediate, chloroaniline compounds play an important role in the synthesis of fine chemical products such as rigid polyurethane foam, dyes, pesticides, and medicines. At present, the main method for industrial production of chloroaniline is through the reduction of chloronitro compounds, including iron powder reduction, alkali sulfide reduction, electrolytic reduction, catalytic hydrogenation reduction, etc. The iron powder reduction method is one of the most commonly used methods in industry. Its advantages are that there are few by-products and it can co-produce iron oxide pigments. For example, Bayer AG in Germany still uses this method for production. However, this method has great potential harm to the environment and is accompanied by high costs for the treatment of three wastes, and there are certain technical limitations. The alkali sulfide reduction method has attracted attention for its simple process and wide sources of reducing agents. The literature reports, for example, a method of reducing halogenated nitrobenzenes using sodium persulfide. Although this method has mild reaction conditions and products that are easier to separate, its high production cost, low recovery rate, and environmental pollution problems limit its widespread application in industry. Although the electrolytic reduction method is theoretically feasible, it is limited in actual industrial applications due to its high energy consumption. Catalytic hydrogenation reduction is considered to be an effective process for synthesizing chloroaniline due to its advantages such as simple process flow, high product yield, good quality, and low environmental impact. Noble metal catalysts have strong adsorption capacity for hydrogen and thus exhibit excellent catalytic activity in catalytic hydrogenation reactions, so relevant research on precious metal catalysts is extensive.
[0003] For example, a nitrobenzene hydrogenation catalyst and a preparation method thereof are disclosed in the prior art. The method synthesizes a catalyst comprising precious metal platinum (Pt), a metal promoter, and a silica carrier. The catalyst has a high reaction rate, high aniline selectivity, and good hydrothermal stability, but the content of precious metal Pt is high (4.0-10.0wt%), and the preparation process requires the use of a dispersant to promote the dispersion of the precious metal and a transition metal as an assistant, which has a high preparation cost, and the catalytic system and process flow are complicated. A 2,4-dinitroaniline hydrogenation catalyst and a preparation method and application thereof are disclosed, wherein the catalyst has Ru-Al alloy and RuO2 as active centers and contains a metal promoter. The catalyst has a small amount of precious metal loading, low cost, and mild hydrogenation conditions, but most of the precious metals need to use a dispersant during the preparation process, and there is a problem of decreased product selectivity, which is only about 87%. The disadvantage of precious metal catalysts is that they are prone to sintering under high temperature conditions, resulting in the loss of active components, thereby reducing catalytic activity. At the same time, precious metal resources are limited and expensive, and the cost in industrial applications increases, reducing economic benefits. Non-precious metal catalysts are favored by researchers because of their hydrogenation activity comparable to that of precious metals and their low price. In recent years, the research on non-precious metals has gradually increased, and catalysts using Fe, Co, Ni, and Cu as raw materials have been widely studied in the selective hydrogenation reaction of chloronitrobenzene. The prior art also provides a method for preparing a nickel-based catalyst and a method for hydrogenating m-chloronitrobenzene, which have high catalytic activity and selectivity, but the use of acid in the process will result in waste acid discharge, which does not meet the requirements of green environmental protection. A catalyst for preparing aniline by gas phase hydrogenation of nitrobenzene, a preparation method, and an application thereof are provided. The catalyst uses an ionic liquid containing cyanide to impregnate the active component metal Cu and a carrier and perform high temperature treatment. The catalyst uses cheap non-precious metal Cu and is used for gas phase hydrogenation of nitrobenzene to prepare aniline, which can quickly reduce the content of light component phenol in the crude aniline product in the initial stage of catalyst operation. However, the use of ionic liquid containing cyanide in the preparation process has a large impact on the production cost and the environment, which is not conducive to the requirements of green environmental protection. Using non-precious metal Cu-Fe / TiO2 as a catalyst and hydrazine hydrate as a reducing agent, nitroaromatic compounds are selectively hydrogenated at 80-130°C to obtain highly selective aminoaromatic compounds. This method is simple to prepare, low in cost, and has a high product yield. However, it also involves the use of a strong reducing agent and a large amount of Fe, and there is a problem of unclear catalytic center. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a halogenated nitrobenzene hydrogenation catalyst and a preparation method and application thereof, which not only significantly improves the reaction efficiency and product selectivity, but also has lower production cost and less environmental impact in industrial applications.
[0005] To this end, the present invention provides the following technical solutions:
[0006] In a first aspect, the present invention provides a method for preparing a halogenated nitrobenzene hydrogenation catalyst in an optional embodiment, comprising the following steps:
[0007] S1: After acidification treatment of H-Beta zeolite molecular sieve, cooling, washing to neutrality, and drying to obtain a carrier;
[0008] S2: dissolving the metal organic salt in water, then adding the carrier, stirring, heating, drying and calcining to obtain a halogenated nitrobenzene hydrogenation catalyst;
[0009] Wherein, in step S2, the metal organic salt is selected from one or more of acetate, acetylacetonate or isopropoxide, and the metal in the metal organic salt is selected from one or more of iron, cobalt, nickel, copper or zinc.
[0010] In the present invention, through a specific acid treatment step, not only the impurities in the raw material are removed, but also a large number of silanol groups are provided for the subsequent introduction of metal active components. Further, a wet impregnation method is used to uniformly load the metal active center onto the acid-treated H-Beta zeolite molecular sieve, and the metal source interacts with the silanol groups of the molecular sieve in the form of an organic salt to form a highly dispersed and stable active center.
[0011] Preferably, in step S1, the temperature of the acidification treatment is 60-120°C and the time is 4-24 hours; and / or, the acid solution used in the acidification treatment is 8-16 mol / L nitric acid; and / or, the mass volume ratio of the H-Beta zeolite molecular sieve and the acid solution is 1-2:20-40; and / or, the molar ratio of SiO2 to Al2O3 in the H-Beta molecular sieve is 28. The drying temperature is 80-120°C; and / or, the drying time is 12-24 hours.
[0012] Preferably, in step S2, the stirring time is 2-6 hours; and / or the heating temperature is 60-90°C. The drying temperature is 80-120°C; and / or the drying time is 12 hours. The calcining temperature is 500-600°C; and / or the calcining time is 3-6 hours.
[0013] In a second aspect, the present invention provides, in an optional embodiment, a halogenated nitrobenzene hydrogenation catalyst prepared by the above-mentioned preparation method.
[0014] Preferably, based on the mass of the halonitrobenzene hydrogenation catalyst, the mass proportion of the metal in the metal organic salt is 1-10%, that is, the metal loading in the halonitrobenzene hydrogenation catalyst is 1-10% of the mass of the catalyst.
[0015] In a third aspect, the present invention provides, in an optional embodiment, a halogenated nitrobenzene hydrogenation catalyst obtained by the above preparation method or the use of the above halogenated nitrobenzene hydrogenation catalyst in the preparation of halogenated aniline by hydrogenation conversion of halogenated nitrobenzene.
[0016] Furthermore, the halogenated nitrobenzene hydrogenation catalyst is reduced with hydrogen, and then the halogenated nitrobenzene, the reduced catalyst, the solvent and the internal standard are reacted in a hydrogen environment at a temperature of 60-160° C. for 1-14 hours to prepare the halogenated aniline.
[0017] Specifically:
[0018] The method for using the halogenated nitrobenzene hydrogenation catalyst is:
[0019] Step 1: Pretreatment: Use hydrogen as carrier gas to reduce the catalyst in a tubular reduction furnace, with a carrier gas flow rate of 30-80 ml / min, a reduction temperature of 250-550°C, and a treatment time of 2-4 hours;
[0020] Step 2: Add a certain amount of halogenated nitrobenzene, catalyst, solvent, and internal standard into a 30 ml stainless steel high-pressure reactor, inject 0.5-4 MPa of high-purity hydrogen, and place it in a 60-160° C. heating and stirring insulation jacket for reaction for 1-14 hours; after the reaction, cool the reactor, and after the gas in the reactor is slowly and safely released, centrifuge the solid-liquid mixture, and analyze the supernatant product online by gas chromatography, using tetradecane as the internal standard.
[0021] Preferably, the solvent is selected from one of methanol, ethanol, isopropanol, ethyl acetate, 1,4-dioxane, tetrahydrofuran, toluene and xylene.
[0022] Preferably, the halogenated nitrobenzene is selected from one of o-chloronitrobenzene, m-chloronitrobenzene, p-chloronitrobenzene, o-fluoronitrobenzene, m-fluoronitrobenzene, p-fluoronitrobenzene, o-bromonitrobenzene, m-bromonitrobenzene, p-bromonitrobenzene, o-iodonitrobenzene, m-iodonitrobenzene and p-iodonitrobenzene.
[0023] Compared with the prior art, the present invention has one of the following beneficial effects:
[0024] 1. The halogenated nitrobenzene hydrogenation catalyst provided by the present invention not only removes impurities in the raw material through a specific acid treatment step, but also provides a large number of silanol groups for the subsequent introduction of metal active components. Further, the metal active center is uniformly loaded onto the acid-treated H-Beta zeolite molecular sieve by a wet impregnation method, which not only significantly improves the reaction efficiency and product selectivity, but also has lower production costs and less environmental impact in industrial applications.
[0025] 2. The preparation method provided by the present invention has the characteristics of simple process and high sample stability.
[0026] 3. The preparation method provided by the present invention can prepare a stable metal catalyst with mixed oxidation valence states.
[0027] 4. The preparation method provided by the present invention can significantly improve the catalytic ability of the catalyst for the hydrogenation reaction of o-chloronitrobenzene and the selectivity of the product.
[0028] 5. The catalyst provided by the present invention exhibits excellent cyclic stability in hydrogenation reactions, providing important technical support for industrial applications. DETAILED DESCRIPTION
[0029] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0030] In a specific embodiment of the present invention, the metal organic salt is selected from one or more of acetate, acetylacetonate or isopropoxide, and the metal in the metal organic salt is selected from one or more of iron, cobalt, nickel, copper or zinc. The metal organic salt can be selected from acetate, acetylacetonate or isopropoxide, and any combination of iron, cobalt, nickel, copper or zinc, but the present invention is not limited thereto. For example, it can be cupric acetate.
[0031] The following is a detailed description of the solutions of the present invention.
[0032] Example 1
[0033] This embodiment provides a method for preparing a halogenated nitrobenzene hydrogenation catalyst, comprising the following steps:
[0034] Step 1: First, use H-Beta zeolite molecular sieve (SiO2 / Al2O3 molar ratio is 28) as raw powder and treat it with concentrated nitric acid, wherein the acid treatment conditions are: H-Beta molecular sieve and concentrated nitric acid (concentration is 10 mol / L) are mixed in a mass volume ratio of 1:20 (g / mL), and heated and stirred in a 90°C oil bath under condensation reflux conditions for 15 hours;
[0035] Step 2: Cool the mixture in step 1) to room temperature and then wash it. After washing with water until it is neutral, place it in a 90° C. forced air drying oven for 12 hours;
[0036] Step 3: Place copper acetate (based on the mass of the halogenated nitrobenzene hydrogenation catalyst, the mass proportion of copper in copper acetate is 5%) in a beaker containing 40 ml of water, stir thoroughly, then add 1 g of the Beta sample in step 2) above, stir for 3 hours, and then heat and stir at 80°C until evaporated to dryness;
[0037] Step 4: Place the sample impregnated and evaporated in the above step 3) in a forced air drying oven at a constant temperature of 90° C. for 12 hours, and then place it in a muffle furnace and calcine it at 550° C. for 6 hours to obtain the halogenated nitrobenzene hydrogenation catalyst.
[0038] Embodiment 2-5
[0039] Examples 2-5 all provide a method for preparing a halogenated nitrobenzene hydrogenation catalyst, comprising the following steps:
[0040] The difference between Example 2 and Example 1 is that in step 3, the mass proportion of copper in copper acetate is 1%; the difference between Example 3 and Example 1 is that in step 3, the mass proportion of copper in copper acetate is 3%; the difference between Example 4 and Example 1 is that in step 3, the mass proportion of copper in copper acetate is 7%; the difference between Example 5 and Example 1 is that in step 3, the mass proportion of copper in copper acetate is 10%. The remaining steps are the same as those in Example 1.
[0041] Embodiment 6-9
[0042] Examples 6-9 all provide a method for preparing a halogenated nitrobenzene hydrogenation catalyst, comprising the following steps:
[0043] The difference between Example 6 and Example 1 is that: in step S3, the metal organic salt adopts ferric acetate (based on the mass of the halogenated nitrobenzene hydrogenation catalyst, the mass proportion of iron in ferric acetate is 5%); the difference between Example 7 and Example 1 is that: in step S3, the metal organic salt adopts cobalt acetate (based on the mass of the halogenated nitrobenzene hydrogenation catalyst, the mass proportion of cobalt in cobalt acetate is 5%); the difference between Example 8 and Example 1 is that: in step S3, the metal organic salt adopts nickel acetate (based on the mass of the halogenated nitrobenzene hydrogenation catalyst, the mass proportion of nickel in nickel acetate is 5%); the difference between Example 9 and Example 1 is that: in step S3, the metal organic salt adopts zinc acetate (based on the mass of the halogenated nitrobenzene hydrogenation catalyst, the mass proportion of zinc in zinc acetate is 5%). The remaining steps are the same as those in Example 1.
[0044] Comparative Example 1
[0045] This comparative example provides a method for preparing a halogenated nitrobenzene hydrogenation catalyst, comprising the following steps:
[0046] Step 1: put copper acetate (based on the mass of halonitrobenzene hydrogenation catalyst, the mass proportion of copper in copper acetate is 5%) into a beaker containing 40 ml of water, stir well, then add 1 g of H-Beta zeolite molecular sieve, stir for 3 hours, and then heat and stir at 80° C. until evaporated to dryness;
[0047] Step 2: The sample impregnated and evaporated in the above step is placed in a forced air drying oven at a constant temperature of 90° C. for 12 hours, and then placed in a muffle furnace for calcination at 550° C. for 6 hours to obtain the halogenated nitrobenzene hydrogenation catalyst.
[0048] Comparative Examples 2-8
[0049] Comparative Example 2-8 provides a method for preparing a halogenated nitrobenzene hydrogenation catalyst, comprising the following steps:
[0050] The difference between Comparative Example 2 and Comparative Example 1 is that in step 1, the H-Beta zeolite molecular sieve is replaced by α-Al2O3 (purchased from Shanghai Aladdin, analytical grade); the difference between Comparative Example 3 and Comparative Example 1 is that in step 1, the H-Beta zeolite molecular sieve is replaced by SnO2 (purchased from Shanghai Aladdin, analytical grade); the difference between Comparative Example 4 and Comparative Example 1 is that in step 1, the H-Beta zeolite molecular sieve is replaced by TiO2 (purchased from Shanghai Aladdin, analytical grade, rutile type, nanometer grade 10-20nm); the difference between Comparative Example 5 and Comparative Example 1 is that in step 1, the H-Beta zeolite molecular sieve is replaced by The sieve is replaced by HZSM-5 molecular sieve (purchased from the catalyst plant of Nankai University, SiO2 / Al2O3=28); the difference between Comparative Example 6 and Comparative Example 1 is that in step 1, the H-Beta zeolite molecular sieve is replaced by S-1 molecular sieve (purchased from the catalyst plant of Nankai University); the difference between Comparative Example 7 and Comparative Example 1 is that in step 1, the H-Beta zeolite molecular sieve is replaced by MCM-41 molecular sieve (purchased from the catalyst plant of Nankai University); the difference between Comparative Example 8 and Comparative Example 1 is that in step 1, the H-Beta zeolite molecular sieve is replaced by SiO2 (purchased from Shanghai Aladdin, with a specific surface area of 200cm 2 The remaining steps are the same as those in Example 1.
[0051] Comparative Examples 9-11
[0052] This comparative example provides a method for preparing a halogenated nitrobenzene hydrogenation catalyst, comprising the following steps:
[0053] The difference between Comparative Example 9 and Example 1 is that, in step 3, cupric acetate is replaced by copper nitrate; the difference between Comparative Example 10 and Example 1 is that, in step 3, cupric acetate is replaced by cupric chloride; the difference between Comparative Example 11 and Example 1 is that, in step 3, cupric acetate is replaced by copper sulfate; the remaining steps are the same as those in Example 1.
[0054] Test Example 1
[0055] The performance of the halogenated nitrobenzene hydrogenation catalyst prepared in Example 1 was evaluated by the following method:
[0056] Step 1: Pretreatment: Hydrogen is used as a carrier gas to perform reduction treatment on the halogenated nitrobenzene hydrogenation catalyst prepared in Example 1 in a tubular reduction furnace, the carrier gas flow rate is 50 ml / min, and the treatment time is 2 hours;
[0057] Step 2: Reaction: add 1 mmol of halogenated nitrobenzene, 0.1 g of the catalyst reduced in step 1), 3 mL of solvent and internal standard into a 30 ml stainless steel high-pressure reactor, inject high-purity hydrogen, and place in a 90° C. heating and stirring insulation jacket for reaction;
[0058] Step 3: After the reaction, the reactor is cooled to room temperature, and the gas in the reactor is slowly and safely released, the solid-liquid mixture is centrifuged, and the supernatant product is analyzed online by gas chromatography, with tetradecane as the internal standard.
[0059] When the halogenated nitrobenzene in step 2 is o-chloronitrobenzene, the solvent is 1,4-dioxane, the hydrogen pressure is 1 MPa, and the reaction time is 8 hours, the conversion rate of the catalyst and the selectivity of the halogenated aniline at different reduction temperatures (250°C, 350°C, and 450°C) are tested. The results are shown in Table 1.
[0060] Table 1 Catalyst conversion and selectivity of halogenated aniline at different reduction temperatures
[0061]
[0062] It can be seen from Table 1 that when the reduction temperature is 450°C, the conversion rate and the selectivity of halogenated aniline of the catalyst are the highest.
[0063] The conversion rate of the catalyst and the selectivity of the halogenated aniline were tested under different hydrogen pressures (1 MPa, 2 MPa and 3 MPa) when the reduction temperature in step 1 was 450°C, the halogenated nitrobenzene in step 2 was o-chloronitrobenzene, the solvent was 1,4-dioxane, and the reaction time was 8 hours. The results are shown in Table 2.
[0064] Table 2 Catalyst conversion and selectivity of halogenated aniline at different reduction temperatures
[0065]
[0066] It can be seen from Table 2 that the hydrogen pressure has little effect on the conversion rate and selectivity of the catalyst. Considering energy consumption, the best hydrogen pressure is 1MPa.
[0067] The conversion rate of the catalyst and the selectivity of the halogenated aniline were tested at different reaction times (1h, 2h, 4h, 6h and 8h) when the reduction temperature in step 1 was 450°C, the halogenated nitrobenzene in step 2 was o-chloronitrobenzene, the solvent was 1,4-dioxane, and the hydrogen pressure was 1MPa. The results are shown in Table 3
[0068] Table 3 Catalyst conversion and selectivity of halogenated aniline at different reaction times
[0069]
[0070] It can be seen from Table 3 that when the reaction time is 8 h, the conversion rate and selectivity of the catalyst are the highest.
[0071] The conversion rate of the catalyst and the selectivity of the halogenated aniline were tested in different solvents (methanol, ethanol, isopropanol, ethyl acetate, 1,4-dioxane, tetrahydrofuran, toluene and xylene) when the reduction temperature in step 1 was 450°C, the halogenated nitrobenzene in step 2 was o-chloronitrobenzene, the hydrogen pressure was 1 MPa, and the reaction time was 6 hours. The results are shown in Table 4.
[0072] Table 4 Catalyst conversion and selectivity of halogenated aniline under different solvents
[0073]
[0074]
[0075] It can be seen from Table 4 that the conversion rate of the catalyst is different under different solvents, but the selectivity of the halogenated aniline is not affected.
[0076] The conversion rate of the catalyst and the selectivity of halogenated aniline were tested under different halogenated nitrobenzenes (o-chloronitrobenzene, m-chloronitrobenzene, p-chloronitrobenzene, o-fluoronitrobenzene, m-fluoronitrobenzene, p-fluoronitrobenzene, o-bromonitrobenzene, m-bromonitrobenzene, p-bromonitrobenzene, o-iodonitrobenzene, m-iodonitrobenzene and p-iodonitrobenzene) when the reduction temperature in step 1 was 450°C, the solvent in step 2 was 1,4-dioxane, the hydrogen pressure was 1 MPa, and the reaction time was 8 hours. The results are shown in Table 5.
[0077] Table 5 Catalyst conversion and selectivity of halogenated aniline under different halogenated nitrobenzenes
[0078]
[0079]
[0080] It can be seen from Table 5 that the halogenated nitrobenzene hydrogenation catalyst prepared in Example 1 has a good catalytic effect on halogenated nitrobenzene.
[0081] Test Example 2
[0082] The catalytic effects of the halogenated nitrobenzene hydrogenation catalysts prepared in Example 1 and Comparative Examples 1-8 were tested by the following method:
[0083] Step 1: Pretreatment: Using hydrogen as carrier gas, the halogenated nitrobenzene hydrogenation catalysts prepared in Example 1 and Comparative Examples 1-8 were subjected to reduction treatment in a tubular reduction furnace, respectively, with a carrier gas flow rate of 50 ml / min, a reduction temperature of 450° C., and a treatment time of 2 hours;
[0084] Step 2: Reaction: 1 mmol of o-chloronitrobenzene, 0.1 g of the catalyst reduced in step 1), 3 mL of dioxane and an internal standard were added to a 30 ml stainless steel high-pressure reactor, 1 MPa of high-purity hydrogen was injected, and the reactor was placed in a 90° C. heating and stirring insulation jacket for reaction for 8 hours;
[0085] Step 3: After the reaction, the reactor is cooled to room temperature, and the gas in the reactor is slowly and safely released, the solid-liquid mixture is centrifuged, and the supernatant product is analyzed online by gas chromatography, with tetradecane as the internal standard.
[0086] The conversion rates of the catalysts in Example 1 and Comparative Examples 1-8 and the selectivity results of halogenated aniline are shown in Table 6.
[0087] Table 6 Conversion rate of catalysts in Example 1 and Comparative Examples 1-8 and selectivity of halogenated aniline
[0088]
[0089]
[0090] It can be seen from Table 3 that the conversion rate of the catalyst can be improved by acidifying the H-Beta molecular sieve as a catalyst carrier.
[0091] Test Example 3
[0092] The catalytic effect of the halogenated nitrobenzene hydrogenation catalyst prepared in Examples 1-5 was tested, and the specific method was the same as that in Test Example 2.
[0093] The conversion rates of the catalysts of Examples 1-5 and the selectivity results of halogenated aniline are shown in Table 7.
[0094] Table 7 Conversion rate of catalysts of Examples 1-5 and selectivity of halogenated aniline
[0095] catalyst Conversion rate (%) Selectivity of halogenated aniline (%) Example 1 3.5 100 Example 2 51 100 Example 3 100 100 Example 4 100 100 Example 5 100 100
[0096] It can be seen from Table 4 that: based on the mass of the halogenated nitrobenzene hydrogenation catalyst, when the mass proportion of copper in copper acetate exceeds 5%, that is, when the mass of the metal loaded on the halogenated nitrobenzene hydrogenation catalyst exceeds 5%, the performance of the catalyst reaches the best.
[0097] Test Example 4
[0098] The catalytic effects of the halogenated nitrobenzene hydrogenation catalysts prepared in Example 1 and Examples 6-9 were tested, and the specific method was the same as that in Test Example 2.
[0099] See Table 8 for the conversion rates of the catalysts in Example 1 and Examples 6-9 and the selectivity results of the halogenated aniline.
[0100] Table 8 Conversion rate of catalysts in Example 1 and Examples 6-9 and selectivity of halogenated aniline
[0101] catalyst Conversion rate (%) Selectivity of halogenated aniline (%) Example 1 100 100 Example 6 50.2 98.7 Example 7 34.4 100 Example 8 89.3 100 Example 9 0.2 100
[0102] It can be seen from Table 8 that when the metal in the metal organic salt is copper, the catalytic effect of the catalyst is the best, and the catalytic effects from best to worst are copper, nickel, iron, cobalt, and zinc.
[0103] Test Example 5
[0104] The catalytic effect of the halogenated nitrobenzene hydrogenation catalyst prepared in Example 1 for recycling was evaluated by the following specific method:
[0105] The halogenated nitrobenzene hydrogenation catalyst prepared in Example 1 was used according to the method in Test Example 2, which was used once. The catalyst used once was washed, dried, calcined, reduced, activated, and regenerated, and then used again, which was used twice. The catalyst used twice was washed, dried, calcined, reduced, activated, and regenerated, and then used again, which was used three times. The catalyst used three times was washed, dried, calcined, reduced, activated, and regenerated, and then used again, which was used four times. See Table 9 for specific results.
[0106] Table 9 Conversion rate after using the catalyst once, twice, three times and four times
[0107] Use times Conversion rate (%) once 100 twice 96.5 three times 95.7 Four times 94
[0108] It can be seen from Table 9 that the halogenated nitrobenzene hydrogenation catalyst prepared in Example 1 has a good recycling effect.
[0109] Test Example 6
[0110] The catalytic effects of the halogenated nitrobenzene hydrogenation catalysts prepared in Example 1 and Comparative Examples 9-11 were evaluated using the same specific methods as in Test Example 2.
[0111] The conversion rates of the catalysts in Example 1 and Comparative Examples 9-11 and the selectivity results of halogenated aniline are shown in Table 10.
[0112] Table 10 Conversion rate of catalysts and selectivity of halogenated aniline of Example 1 and Comparative Examples 9-11
[0113] catalyst Conversion rate (%) Selectivity of halogenated aniline (%) Example 1 100 100 Comparative Example 9 10.8 100 Comparative Example 10 5.3 100 Comparative Example 11 1.6 100
[0114] It can be seen from Table 10 that organic metal salts significantly improve the activity of the catalyst for the hydrogenation of halonitrobenzene compared to inorganic metal salts.
[0115] Although the principles of the present invention are described in detail above in conjunction with the preferred embodiments of the present invention, those skilled in the art should understand that the above embodiments are merely explanations of the exemplary implementations of the present invention, and are not intended to limit the scope of the present invention. The details in the embodiments do not constitute limitations on the scope of the present invention, and any obvious changes such as equivalent transformations, simple replacements, etc. based on the technical solution of the present invention, without departing from the spirit and scope of the present invention, fall within the protection scope of the present invention.
Claims
1. A method for preparing a halogenated nitrobenzene hydrogenation catalyst, characterized in that: The following steps are involved: S1: After acidification treatment of H-Beta zeolite molecular sieve, cooling, washing to neutrality, and drying to obtain a carrier; S2: dissolving the metal organic salt in water, then adding the carrier, stirring, heating, drying and calcining to obtain a halogenated nitrobenzene hydrogenation catalyst; Wherein, in step S2, the metal organic salt is selected from one or more of acetate, acetylacetonate or isopropoxide, and the metal in the metal organic salt is selected from one or more of iron, cobalt, nickel, copper or zinc.
2. The method for preparing a halogenated nitrobenzene hydrogenation catalyst according to claim 1, characterized in that: In step S1, the acidification treatment is performed at a temperature of 60-120° C. for a time of 4-24 hours; and / or, The acid solution used in the acidification treatment is 8-16 mol / L nitric acid; and / or, The mass volume ratio of the H-Beta zeolite molecular sieve to the acid solution is 1-2:20-40; and / or, The molar ratio of SiO2 to Al2O3 in the H-Beta molecular sieve is 28.
3. The method for preparing a halogenated nitrobenzene hydrogenation catalyst according to claim 1, characterized in that: In step S1, the drying temperature is 80-120°C; and / or, The drying time is 12-24 hours.
4. The method for preparing a halogenated nitrobenzene hydrogenation catalyst according to claim 1, characterized in that: In step S2, the stirring time is 2-6 hours; and / or, The heating temperature is 60-90°C.
5. The method for preparing a halogenated nitrobenzene hydrogenation catalyst according to claim 1, characterized in that: In step S2, the drying temperature is 80-120°C; and / or, The drying time is 12 hours.
6. The method for preparing a halogenated nitrobenzene hydrogenation catalyst according to claim 1, characterized in that: In step S2, the calcination temperature is 500-600°C; and / or, The calcination time is 3-6 hours.
7. A halogenated nitrobenzene hydrogenation catalyst, characterized in that: The preparation method is adopted according to any one of claims 1 to 7.
8. The halogenated nitrobenzene hydrogenation catalyst according to claim 7, characterized in that: Based on the mass of the halogenated nitrobenzene hydrogenation catalyst, the mass proportion of the metal in the metal organic salt is 1-10%.
9. Use of the halogenated nitrobenzene hydrogenation catalyst obtained by the preparation method according to any one of claims 1 to 6 or the halogenated nitrobenzene hydrogenation catalyst according to claim 7 or 8 in the preparation of halogenated aniline by hydrogenation conversion of halogenated nitrobenzene.
10. The use according to claim 9, characterized in that: The halogenated nitrobenzene hydrogenation catalyst is subjected to reduction treatment with hydrogen, and then the halogenated nitrobenzene, the reduced catalyst, the solvent and the internal standard are reacted in a hydrogen environment at a temperature of 60-160° C. for 1-14 hours to prepare the halogenated aniline.
Citation Information
Patent Citations
Catalyst for preparing halogeno anilin through catalytic hydrogenation of halogeno nitrobenzene and preparation method
CN101049562A
Method for preparing p-chloroaniline through catalytic hydrogenation of p-chloronitrobenzene
CN102351714A
Non-alloyed metal complex and its preparation and application
CN106914255A
Copper-based supported catalyst for synthesizing aniline through nitrobenzene hydrogenation and preparation method of copper-based supported catalyst
CN112958097A
Catalyst for fluidized bed gaseous hydrogenation of nitrobenzene to produce aniline, and process therefor
CN1861254A