Graphite fluoride and preparation method thereof
By forming porous graphite through alkaline etching and vapor deposition on a graphite matrix, and then reacting it with a fluorine source under ultraviolet irradiation, the problems of low efficiency and impurity introduction in existing fluorinated graphite preparation methods have been solved, achieving efficient and safe fluorinated graphite production.
Patent Information
- Application Number
- CN202410962695.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-19
AI Technical Summary
Existing methods for preparing fluorinated graphite suffer from problems such as low preparation efficiency, complex production process, and insufficient fluorine content in the product. Furthermore, existing methods are prone to introducing impurities at lower temperatures, affecting product quality, and have long production cycles and low production efficiency.
A porous graphite matrix was formed by treating the graphite matrix with alkaline etching and vapor deposition. Then, a fluorination reaction was carried out under ultraviolet irradiation using a composite gas of fluorine source and inert gas. The ultraviolet irradiation caused the ground-state molecules in the fluorinating agent to jump to the excited state to generate fluorine free radicals, which promoted the rapid reaction with graphite and reduced the reaction temperature and time.
It improves fluorination efficiency, shortens reaction time, lowers the required reaction temperature, enhances process safety and product quality, simplifies process steps, and increases production efficiency.
Smart Images

Figure CN118978154A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of fluorinated graphite, and in particular to fluorinated graphite and a preparation method thereof. Background Art
[0002] Graphite fluoride, with the molecular formula CFx, where X is an indefinite value ranging from 0 to 1.25, is a new type of high-tech, high-performance, and high-efficiency carbon / graphite material in the world today. Graphite fluoride has a structure similar to that of graphene. Compared with general graphite materials, it has the characteristics of low surface energy and interlayer energy, and can easily achieve the dual characteristics of superoleophobicity and superhydrophobicity. Moreover, using graphite fluoride as the active material of battery electrodes, the batteries produced have high energy density, wide operating temperature range, high safety, and a capacity that is 5-10 times that of general batteries. In addition, graphite fluoride also has the advantages of stable chemical properties, non-corrosiveness, acid and alkali resistance, solvent resistance, and long service life. Therefore, graphite fluoride is also widely used in aerospace, metallurgy, chemical industry, machinery, electrical and other industries.
[0003] Graphite fluoride is a fine chemical product, and only a few countries in the world have the capacity for industrial production. At present, the production processes of graphite fluoride mainly include direct synthesis, catalytic synthesis, electrolytic synthesis and solid phase synthesis.
[0004] (1) Direct synthesis is the earliest synthesis method, which involves heating graphite and gaseous fluorine at a certain temperature.
[0005] (2) The catalytic synthesis method is to add a trace amount of metal fluoride as a catalyst to the reaction system of graphite and fluorine. The synthesis can be carried out below 300°C.
[0006] (3) The solid phase synthesis method is to mix a fluorinated solid polymer with graphite, heat it to a certain temperature under an inert atmosphere, and produce fluorinated graphite.
[0007] (4) The electrolytic synthesis method is to use electrolysis to electrolyze graphite in anhydrous hydrofluoric acid to generate new graphite fluoride.
[0008] At present, the main method for preparing fluorinated graphite can solve the problem of uneven contact between fluorine gas and graphite and large heat release in the traditional graphite preparation process, but the reaction requires high temperature, long insulation time, long process cycle, complicated steps, and is not conducive to industrial production. There are also some methods that can reduce the heat required for the reaction and cause fluorination reaction at a lower temperature, but at the same time, they are easy to introduce impurities, affect product quality, have a long production cycle, and have low production efficiency. Summary of the invention
[0009] Based on this, the present invention proposes a fluorinated graphite and a preparation method thereof, which solves the technical problems of low preparation efficiency, complex production process, insufficient fluorine content in the product and the like in the prior art.
[0010] According to a first aspect of the present invention, there is provided a method for preparing fluorinated graphite, comprising the following steps:
[0011] Porous graphite is obtained by alkaline etching and vapor deposition of a graphite substrate;
[0012] Pickling the porous graphite;
[0013] Under ultraviolet irradiation conditions, subjecting the acid-washed porous graphite to a fluorination reaction to obtain the fluorinated graphite;
[0014] The fluorinating agent used in the fluorination reaction is a composite gas of a fluorine source and an inert gas, and the fluorine source is F 2 , CIF, CIF 3 NF 3 One or more of;
[0015] The irradiation intensity of the ultraviolet irradiation condition is 5lx-25lx, and the irradiation reaction temperature is 150°C-400°C.
[0016] According to an embodiment of the present invention, the step of obtaining porous graphite by alkali etching and vapor deposition on a graphite substrate comprises:
[0017] When the graphite substrate is alkali-etched, CO 2 The alkali vapor formed during the alkali etching process is deposited onto the graphite substrate to obtain the porous graphite.
[0018] According to an embodiment of the present invention, the alkali used in the alkali etching is a strong alkali;
[0019] The etching temperature in the alkaline etching is 500° C. to 600° C.;
[0020] The molar ratio of the graphite substrate to the alkali in the alkali etching is 1:1.15 to 1:1.5.
[0021] According to an embodiment of the present invention, the CO introduced during the alkaline etching 2 The pressure is 100kPa~500kPa.
[0022] According to an embodiment of the present invention, pickling the porous graphite comprises:
[0023] The porous graphite is immersed in acid, left to stand, and then taken out;
[0024] The porous graphite after pickling is cleaned, dried and dried.
[0025] According to an embodiment of the present invention, the acid is carbonic acid or hydrofluoric acid;
[0026] The porous graphite is immersed in the acid for 15 to 35 hours;
[0027] The concentration of the acid is 30% to 60%.
[0028] According to an embodiment of the present invention, the graphite substrate adopts a high-purity graphite substrate, including flake graphite and expanded graphite;
[0029] The graphite matrix may be in a powdery, spherical, blocky, stripy, flake or irregular shape.
[0030] According to an embodiment of the present invention, the inert gas is one of nitrogen and argon;
[0031] The volume ratio of the fluorine source to the inert gas is 0.05:1 to 0.5:1.
[0032] According to an embodiment of the present invention, the reaction time of the fluorination reaction is 2h to 6h.
[0033] According to a second aspect of the present invention, there is provided a fluorinated graphite obtained by the above-mentioned preparation method.
[0034] It can be seen from the above technical scheme that the preparation method of graphite fluoride provided by the present invention has the following beneficial effects:
[0035] The present invention uses a fluorination reaction under ultraviolet irradiation conditions to make the stable ground state molecules in the fluorinating agent transition to an unstable excited state, thereby generating fluorine free radicals. Accompanied by heating, more fluorine free radicals are generated to react rapidly with graphite. Since the reaction of fluorine free radicals with graphite is an exothermic process, the reaction can be promoted and the external heat required for the reaction can be reduced, so that the graphite and fluorine gas can undergo a fluorination reaction at a relatively low temperature. This method can effectively shorten the reaction time and improve the fluorination efficiency. On the other hand, it can effectively reduce the temperature required for the reaction, thereby reducing the heating power load of the reaction device and improving the intrinsic safety of the process.
[0036] The preparation method adopted by the invention has simple steps, easy process control, fast reaction rate, good finished product quality and the like. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 It is a schematic flow chart of the method for preparing fluorinated graphite in Example 1 of the present invention. DETAILED DESCRIPTION
[0038] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments and with reference to the accompanying drawings.
[0039] At present, the main method for preparing fluorinated graphite can solve the problem of uneven contact between fluorine gas and graphite and large heat release in the traditional graphite preparation process, but the reaction requires high temperature, long insulation time, long process cycle, complicated steps, and is not conducive to industrial production. There are also some methods that can reduce the heat required for the reaction and cause fluorination reaction at a lower temperature, but at the same time, they are easy to introduce impurities, affect product quality, have a long production cycle, and have low production efficiency.
[0040] For example, there are several methods for preparing fluorinated graphite under high temperature conditions, mainly by mixing fluoride molten salt and graphite pretreated with hydrofluoric acid, removing air and water in the reaction system with inert gas; then heating and melting the fluoride molten salt, introducing a mixed gas of fluorine gas and argon gas, and reacting to obtain fluorinated graphite. This method can solve the problem of uneven contact between fluorine gas and graphite and large heat release in the traditional graphite preparation process, but the temperature required for the reaction is 500°C, the insulation time is 3h to 8h, the process cycle is long, and the steps are relatively cumbersome.
[0041] Or, fluorinated graphite can be obtained by heating an inorganic fluorinating agent and graphite in the presence of high-purity nitrogen. The final fluorinated graphite obtained by this method has a content of up to 59% and does not require external fluorine gas. However, this method uses nitrogen pressure between 0.5Mpa and 5Mpa, and the reaction temperature is relatively high. In addition, the product needs to be soaked in a mixture of hydrochloric acid and sulfuric acid, which poses certain safety risks.
[0042] Or by reacting graphite with antimony pentachloride to obtain antimony pentachloride graphite intercalation compound, and finally introducing fluorine and nitrogen mixed gas for reaction to obtain fluorinated graphite. Although this method can be formed in ordinary fluorination equipment and has a wide reaction temperature range, the reaction temperature is high, and the required reaction time is long. The production process is relatively cumbersome and is not conducive to industrial production.
[0043] There are also several methods for preparing fluorinated graphite under low temperature conditions, for example, by soaking graphite in hydrochloric acid and hydrogen peroxide to obtain expanded graphite, then reacting a certain concentration of fluorine gas and antimony powder in a closed container to obtain antimony pentafluoride, and then placing the expanded graphite and antimony pentafluoride in a closed container to react to obtain intercalated graphite; then placing the intercalated graphite in a closed reactor, passing fluorine gas, and reacting to obtain fluorinated graphite. This method has a low reaction temperature and can be mass-produced, but the reaction time for preparing intercalated graphite is 9h to 11h, and the reaction time for preparing fluorinated graphite is more than 7 hours, the production cycle is long, and the production efficiency is not high.
[0044] Or graphite fluoride can be obtained by uniformly mixing graphite, citrate and metal fluoride, introducing a mixed gas containing fluorine into the mixture and performing a fluorination reaction at 150°C to 250°C. This method can reduce the heat required for the reaction, and the fluorination reaction can occur at a lower temperature, thereby increasing the reaction rate and selectivity, but it is easy to introduce impurities, which affects the product quality.
[0045] Therefore, it is necessary to provide a method with high preparation efficiency, simple production process, low preparation temperature and high fluorine content in the product.
[0046] According to a first aspect of the present invention, there is provided a method for preparing fluorinated graphite, comprising the following steps:
[0047] S1: porous graphite is obtained by alkaline etching and vapor deposition of a graphite substrate;
[0048] S2: pickling the porous graphite;
[0049] S3: Under ultraviolet irradiation conditions, subjecting the acid-washed porous graphite to a fluorination reaction to obtain fluorinated graphite;
[0050] The fluorination agent used in the fluorination reaction is a composite gas of a fluorine source and an inert gas, and the fluorine source is F 2 , CIF, CIF 3 NF 3 One or more of;
[0051] The irradiation intensity of the ultraviolet irradiation condition is 5lx-25lx, and the irradiation reaction temperature is 150°C-400°C.
[0052] The fluorine source has strong reactivity.
[0053] The present invention adopts a fluorination reaction under ultraviolet irradiation conditions, which can make the stable ground state molecules in the fluorinating agent transition to an unstable excited state, thereby generating fluorine free radicals, and accompanied by heating, more fluorine free radicals are generated to react quickly with graphite. Because the reaction of fluorine free radicals with graphite is an exothermic process, the reaction can be promoted and the external heat required for the reaction can be reduced, so that the graphite and fluorine gas can undergo fluorination reaction at a relatively low temperature. The method can effectively shorten the reaction time and improve the fluorination efficiency. On the other hand, it can effectively reduce the temperature required for the reaction, thereby reducing the heating power load of the reaction device and improving the intrinsic safety of the process. The preparation method adopted by the present invention has simple steps, is easy to control the process, has the advantages of fast reaction rate, good finished product quality, and the like.
[0054] According to an embodiment of the present invention, in S1, obtaining porous graphite by etching and vapor deposition on a graphite substrate comprises:
[0055] In the case of alkaline etching of the graphite substrate, CO2 The alkali vapor formed during the alkali etching process is deposited onto the graphite substrate to obtain porous graphite.
[0056] According to an embodiment of the present invention, in S1, the processing device used in the alkaline etching process is a rotary furnace.
[0057] During the reaction, CO was continuously introduced 2 Gas, in addition to depositing excess alkali vapor, can also maintain an inert atmosphere. The present invention uses an alkali etching method to treat the graphite substrate. The alkali is in a molten state, and KOH or NaOH is extremely corrosive to graphite, so that the alkali fully etches the graphite to form porous graphite; CO is introduced 2 Excess alkali can be deposited on the graphite substrate and simultaneously act as a protective gas, making the reaction safer and more reliable.
[0058] According to an embodiment of the present invention, in S1, the alkali used in the alkali etching is a strong alkali, and the alkali may be KOH, NaOH, etc., preferably KOH.
[0059] According to an embodiment of the present invention, in S1, the etching temperature in the alkaline etching is 500°C to 600°C, for example, it can be 500°C, 520°C, 540°C, 560°C, 580°C, 600°C, etc.
[0060] According to an embodiment of the present invention, in S1, the molar ratio of the graphite substrate to the alkali in the alkali etching is 1:1.15 to 1:1.5, for example, it can be 1:1.15, 1:1.25, 1:1.3, 1:1.4, 1:1.45, 1:1.5, etc.
[0061] According to an embodiment of the present invention, in S1, CO introduced during the alkaline etching 2 The pressure is 100 kPa to 500 kPa, for example, 100 kPa, 200 kPa, 300 kPa, 400 kPa, 500 kPa, etc., preferably 300 kPa to 500 kPa.
[0062] According to an embodiment of the present invention, in S1, the graphite substrate adopts a high-purity graphite substrate, including one of flake graphite and expanded graphite, preferably flake graphite.
[0063] According to an embodiment of the present invention, in S1, the shape of the graphite matrix includes one of powder, spherical, block, strip, sheet, and irregular shape.
[0064] According to an embodiment of the present invention, in S1, the etching time in the alkaline etching is 4 hours to 6 hours, for example, it can be 4 hours, 5 hours, 6 hours, etc.
[0065] According to an embodiment of the present invention, S1 specifically comprises: placing the graphite substrate in the feed hopper of the rotary kiln and uniformly adding solid alkali; setting the vacuum degree of the rotary kiln, evacuating the kiln, and then introducing CO 2 After the leak test is qualified, the temperature begins to rise. When the temperature reaches 500℃~600℃, it is kept warm for 4h~6h to obtain porous graphite.
[0066] According to an embodiment of the present invention, in S2, pickling the porous graphite comprises:
[0067] Soak the porous graphite in acid and let it stand before taking it out;
[0068] The porous graphite after pickling is cleaned, dried and dried.
[0069] Acid washing can clean the residual alkali on the graphite matrix and also increase the porous structure.
[0070] According to an embodiment of the present invention, in S2, the acid is carbonic acid or hydrofluoric acid, preferably hydrofluoric acid.
[0071] According to an embodiment of the present invention, in S2, when the acid is hydrofluoric acid, the concentration of the hydrofluoric acid is 30% to 60%, preferably 40%.
[0072] According to an embodiment of the present invention, in S2, the porous graphite is immersed in hydrofluoric acid for 15 hours to 35 hours, for example, 15 hours, 20 hours, 25 hours, 30 hours, 35 hours, etc., preferably 20 hours to 30 hours.
[0073] According to an embodiment of the present invention, in S2, when the acid is carbonic acid, saturated carbonic acid is used with a concentration of about 16%.
[0074] According to an embodiment of the present invention, in S2, the porous graphite is immersed in hydrofluoric acid for 35 hours to 40 hours.
[0075] According to an embodiment of the present invention, S2 is specifically: soaking the porous graphite after alkaline etching in an acid with a concentration of 30% to 60%, letting it stand for 15h to 35h, pouring out the acid, adding deionized water for stirring, letting it stand for 1h after stirring, pouring out the deionized water, and then repeatedly washing the porous graphite with water until the pH value of the water after washing is neutral; placing the porous graphite in a box-type drying oven at 60°C for drying, and then placing it in a vacuum drying oven at 80°C for drying for 8h to obtain the treated porous graphite, which is temporarily stored.
[0076] According to an embodiment of the present invention, in S3, the type of reaction device used for the fluorination reaction can be various static reactors or fluidized bed reactors such as flat plate, fixed bed, fluidized bed, vertical reactor, etc., and preferably a fluidized bed is used as the reactor.
[0077] According to an embodiment of the present invention, in S3, the inert gas is one of nitrogen and argon;
[0078] According to an embodiment of the present invention, in S3, the volume ratio of the fluorine source to the inert gas is 0.05:1 to 0.5:1, for example, it can be 0.05:1, 0.1:1, 0.2:1, 0.3:1, 0.4:1, 0.5:1, etc., and is preferably 0.1:1 to 0.2:1.
[0079] Since the fluorination reaction is an exothermic reaction with a huge amount of heat released, the use of pure fluorine gas as a fluorination agent is unsafe, and therefore it is preferred to use an inert gas to dilute the pure fluorine.
[0080] According to an embodiment of the present invention, in S3, the reaction time of the fluorination reaction is 2 h to 6 h, for example, 2 h, 3 h, 4 h, 5 h, 6 h, etc., and the reaction time is preferably 4 h to 6 h.
[0081] According to an embodiment of the present invention, in S3, the irradiation intensity during the fluorination reaction can be 5lx, 10lx, 15lx, 20lx, 25lx, etc., preferably 101x to 201x.
[0082] According to an embodiment of the present invention, in S3, the reaction temperature may be 150°C, 200°C, 250°C, 300°C, 350°C, 400°C, etc., and the reaction temperature is preferably 200°C to 300°C.
[0083] According to an embodiment of the present invention, S3 specifically comprises: adding porous graphite into a fluidized bed reactor and allowing it to stand; introducing an inert gas into the fluidized bed reactor to remove water and oxygen until the water and oxygen contents in the fluidized bed reactor are respectively lower than 10 ppm and 100 ppm; then, setting the temperature of the fluidized bed reactor to 150° C. to 400° C. for heating;
[0084] When the temperature of the fluidized bed reactor reaches a predetermined temperature, a fluorinating agent is introduced into the fluidized bed reactor, and an ultraviolet irradiation lamp source is turned on to make the porous graphite react with the fluorine source, and the ultraviolet irradiation intensity is 5lx to 25lx;
[0085] After 2 to 6 hours of reaction, the fluorinating agent is stopped, and an inert gas is introduced into the fluidized bed for replacement to remove the residual fluorinating agent in the fluidized bed. When the fluorine source content in the tail gas is detected to be below 3 ppm, the inert gas is stopped, the fluorination reaction is terminated, and fluorinated graphite is obtained.
[0086] Under the action of ultraviolet radiation, the stable ground state molecules in the fluorinating agent are transitioned to an unstable excited state, thereby inducing defluorination to produce free radical centers (generating fluorine free radicals) and reacting rapidly with graphite. The use of ultraviolet radiation can effectively increase the reaction rate of the fluorination reaction and improve the fluorination effect.
[0087] According to a second aspect of the present invention, there is provided a fluorinated graphite obtained by the above-mentioned preparation method.
[0088] The technical solution of the present invention is described in detail below through preferred embodiments. It should be noted that the specific embodiments below are only used for illustration and are not used to limit the present invention.
[0089] Example 1
[0090] like Figure 1 As shown in the figure, 5 kg of flake graphite was placed in the feed hopper of the rotary kiln, and 11 kg of KOH was added; the vacuum degree of the rotary kiln was set, and 500 kPa CO was introduced. 2 After the leak test is qualified, start heating up. When the temperature reaches 500℃, keep it warm for 5h.
[0091] Soak the porous graphite after alkaline etching in 40% hydrofluoric acid, let it stand for 20 hours, pour out the hydrofluoric acid, add deionized water and stir, let it stand for 1 hour after stirring, and pour out the deionized water. Then use water to repeatedly wash the graphite until the pH value of the water after washing is neutral; put the porous graphite in a box-type drying oven at 60°C for drying, and then put it in a vacuum drying oven at 80°C for drying for 8 hours to obtain the treated porous graphite, which is temporarily stored;
[0092] The treated porous graphite is added into a fluidized bed reactor and allowed to stand; high-purity nitrogen is introduced into the fluidized bed reactor to remove water and oxygen until the water and oxygen contents in the fluidized bed reactor are lower than 10 ppm and 100 ppm, respectively;
[0093] Subsequently, the temperature of the fluidized bed reactor was set to 200° C. for heating. When the temperature of the fluidized bed reactor reached a predetermined temperature, a 10% (volume ratio) fluorine-nitrogen mixed gas (i.e., the volume ratio of the fluorine source to the inert gas was 0.1:1) was introduced into the fluidized bed reactor, and an ultraviolet irradiation lamp was turned on to react the porous graphite with the fluorine gas. The ultraviolet irradiation intensity was 51x.
[0094] After 5 hours of reaction, the introduction of fluorine-nitrogen mixed gas was stopped, and nitrogen was introduced into the fluidized bed for replacement to remove the residual fluorine gas in the fluidized bed. When the fluorine content in the tail gas was detected to be below 3 ppm, nitrogen blowing was stopped, and the fluorination reaction was completed to obtain the final sample, and its fluorine content was detected to be F:C=0.73.
[0095] Example 2
[0096] like Figure 1 As shown in the figure, 5 kg of flake graphite was placed in the feed hopper of the rotary kiln, and 11 kg of KOH was added; the vacuum degree of the rotary kiln was set, and 500 kPa CO was introduced. 2After the leak test is qualified, start heating up. When the temperature reaches 500℃, keep it warm for 5h.
[0097] Soak the porous graphite after alkaline etching in 40% hydrofluoric acid, let it stand for 20 hours, pour out the hydrofluoric acid, add deionized water and stir, let it stand for 1 hour after stirring, and pour out the deionized water. Then use water to repeatedly wash the graphite until the pH value of the water after washing is neutral; put the porous graphite in a box-type drying oven at 60°C for drying, and then put it in a vacuum drying oven at 80°C for drying for 8 hours to obtain the treated porous graphite, which is temporarily stored;
[0098] The treated porous graphite is added into a fluidized bed reactor and allowed to stand; high-purity nitrogen is introduced into the fluidized bed reactor to remove water and oxygen until the water and oxygen contents in the fluidized bed reactor are lower than 10 ppm and 100 ppm, respectively;
[0099] Subsequently, the temperature of the fluidized bed reactor was set to 200° C. for heating. When the temperature of the fluidized bed reactor reached a predetermined temperature, a 15% (volume ratio) fluorine-nitrogen mixed gas (i.e., the volume ratio of the fluorine source to the inert gas was 0.15:1) was introduced into the fluidized bed reactor, and an ultraviolet irradiation lamp was turned on to react the porous graphite with the fluorine gas. The ultraviolet irradiation intensity was 51x.
[0100] After 5 hours of reaction, the introduction of fluorine-nitrogen mixed gas was stopped, and nitrogen was introduced into the fluidized bed for replacement to remove the residual fluorine gas in the fluidized bed. When the fluorine content in the tail gas was detected to be below 3 ppm, nitrogen blowing was stopped, and the fluorination reaction was completed to obtain the final sample, and its fluorine content was detected to be F:C=0.79.
[0101] Example 3
[0102] like Figure 1 As shown in the figure, 5 kg of flake graphite was placed in the feed hopper of the rotary kiln, and 11 kg of KOH was added; the vacuum degree of the rotary kiln was set, and 500 kPa CO was introduced. 2 After the leak test is qualified, start heating up. When the temperature reaches 500℃, keep it warm for 5h.
[0103] Soak the porous graphite after alkaline etching in 40% hydrofluoric acid, let it stand for 20 hours, pour out the hydrofluoric acid, add deionized water and stir, let it stand for 1 hour after stirring, and pour out the deionized water. Then use water to repeatedly wash the graphite until the pH value of the water after washing is neutral; put the porous graphite in a box-type drying oven at 60°C for drying, and then put it in a vacuum drying oven at 80°C for drying for 8 hours to obtain the treated porous graphite, which is temporarily stored;
[0104] The treated porous graphite is added into a fluidized bed reactor and allowed to stand; high-purity nitrogen is introduced into the fluidized bed reactor to remove water and oxygen until the water and oxygen contents in the fluidized bed reactor are lower than 10 ppm and 100 ppm, respectively;
[0105] Subsequently, the temperature of the fluidized bed reactor was set to 250° C. for heating. When the temperature of the fluidized bed reactor reached a predetermined temperature, a 15% (volume ratio) fluorine-nitrogen mixed gas (i.e., the volume ratio of the fluorine source to the inert gas was 0.15:1) was introduced into the fluidized bed reactor, and an ultraviolet irradiation lamp was turned on to react the porous graphite with the fluorine gas. The ultraviolet irradiation intensity was 51x.
[0106] After 5 hours of reaction, the introduction of fluorine-nitrogen mixed gas was stopped, and nitrogen was introduced into the fluidized bed for replacement to remove the residual fluorine gas in the fluidized bed. When the fluorine content in the tail gas was detected to be below 3 ppm, nitrogen blowing was stopped, and the fluorination reaction was completed to obtain the final sample, and its fluorine content was detected to be F:C=0.85.
[0107] Example 4
[0108] like Figure 1 As shown in the figure, 5 kg of flake graphite was placed in the feed hopper of the rotary kiln, and 11 kg of KOH was added; the vacuum degree of the rotary kiln was set, and 500 kPa CO was introduced. 2 After the leak test is qualified, start heating up. When the temperature reaches 500℃, keep it warm for 5h.
[0109] Soak the porous graphite after alkaline etching in 40% hydrofluoric acid, let it stand for 20 hours, pour out the hydrofluoric acid, add deionized water and stir, let it stand for 1 hour after stirring, and pour out the deionized water. Then use water to repeatedly wash the graphite until the pH value of the water after washing is neutral; put the porous graphite in a box-type drying oven at 60°C for drying, and then put it in a vacuum drying oven at 80°C for drying for 8 hours to obtain the treated porous graphite, which is temporarily stored;
[0110] The treated porous graphite is added into a fluidized bed reactor and allowed to stand; high-purity nitrogen is introduced into the fluidized bed reactor to remove water and oxygen until the water and oxygen contents in the fluidized bed reactor are lower than 10 ppm and 100 ppm, respectively;
[0111] Subsequently, the temperature of the fluidized bed reactor was set to 300° C. for heating. When the temperature of the fluidized bed reactor reached a predetermined temperature, a 15% (volume ratio) fluorine-nitrogen mixed gas (i.e., the volume ratio of the fluorine source to the inert gas was 0.15:1) was introduced into the fluidized bed reactor, and an ultraviolet irradiation lamp was turned on to react the porous graphite with the fluorine gas. The ultraviolet irradiation intensity was 51x.
[0112] After 5 hours of reaction, the introduction of fluorine-nitrogen mixed gas was stopped, and nitrogen was introduced into the fluidized bed for replacement to remove the residual fluorine gas in the fluidized bed. When the fluorine content in the tail gas was detected to be below 3 ppm, nitrogen blowing was stopped, and the fluorination reaction was completed to obtain the final sample, and its fluorine content was detected to be F:C=0.91.
[0113] Example 5
[0114] like Figure 1 As shown in the figure, 5 kg of flake graphite was placed in the feed hopper of the rotary kiln, and 11 kg of KOH was added; the vacuum degree of the rotary kiln was set, and 500 kPa CO was introduced. 2 After the leak test is qualified, start heating up. When the temperature reaches 500℃, keep it warm for 5h.
[0115] Soak the porous graphite after alkaline etching in 40% hydrofluoric acid, let it stand for 20 hours, pour out the hydrofluoric acid, add deionized water and stir, let it stand for 1 hour after stirring, and pour out the deionized water. Then use water to repeatedly wash the graphite until the pH value of the water after washing is neutral; put the porous graphite in a box-type drying oven at 60°C for drying, and then put it in a vacuum drying oven at 80°C for drying for 8 hours to obtain the treated porous graphite, which is temporarily stored;
[0116] The treated porous graphite is added into a fluidized bed reactor and allowed to stand; high-purity nitrogen is introduced into the fluidized bed reactor to remove water and oxygen until the water and oxygen contents in the fluidized bed reactor are lower than 10 ppm and 100 ppm, respectively;
[0117] Subsequently, the temperature of the fluidized bed reactor was set to 350° C. for heating. When the temperature of the fluidized bed reactor reached a predetermined temperature, a 15% (volume ratio) fluorine-nitrogen mixed gas (i.e., the volume ratio of the fluorine source to the inert gas was 0.15:1) was introduced into the fluidized bed reactor, and an ultraviolet irradiation lamp was turned on to react the porous graphite with the fluorine gas. The ultraviolet irradiation intensity was 51x.
[0118] After 5 hours of reaction, the introduction of fluorine-nitrogen mixed gas was stopped, and nitrogen was introduced into the fluidized bed for replacement to remove the residual fluorine gas in the fluidized bed. When the fluorine content in the tail gas was detected to be below 3 ppm, nitrogen blowing was stopped, and the fluorination reaction was completed to obtain the final sample, and its fluorine content was detected to be F:C=0.98.
[0119] Example 6
[0120] like Figure 1 As shown in the figure, 5 kg of flake graphite was placed in the feed hopper of the rotary kiln, and 11 kg of KOH was added; the vacuum degree of the rotary kiln was set, and 500 kPa CO was introduced. 2 After the leak test is qualified, start heating up. When the temperature reaches 500℃, keep it warm for 5h.
[0121] Soak the porous graphite after alkaline etching in 40% hydrofluoric acid, let it stand for 20 hours, pour out the hydrofluoric acid, add deionized water and stir, let it stand for 1 hour after stirring, and pour out the deionized water. Then use water to repeatedly wash the graphite until the pH value of the water after washing is neutral; put the porous graphite in a box-type drying oven at 60°C for drying, and then put it in a vacuum drying oven at 80°C for drying for 8 hours to obtain the treated porous graphite, which is temporarily stored;
[0122] The treated porous graphite is added into a fluidized bed reactor and allowed to stand; high-purity nitrogen is introduced into the fluidized bed reactor to remove water and oxygen until the water and oxygen contents in the fluidized bed reactor are lower than 10 ppm and 100 ppm, respectively;
[0123] Subsequently, the temperature of the fluidized bed reactor was set to 200° C. for heating. When the temperature of the fluidized bed reactor reached a predetermined temperature, a 15% (volume ratio) fluorine-nitrogen mixed gas (i.e., the volume ratio of the fluorine source to the inert gas was 0.15:1) was introduced into the fluidized bed reactor, and an ultraviolet irradiation lamp was turned on to react the porous graphite with the fluorine gas. The ultraviolet irradiation intensity was 101x.
[0124] After 5 hours of reaction, the introduction of fluorine-nitrogen mixed gas was stopped, and nitrogen was introduced into the fluidized bed for replacement to remove the residual fluorine gas in the fluidized bed. When the fluorine content in the tail gas was detected to be below 3 ppm, nitrogen blowing was stopped, the fluorination reaction was terminated, and the final sample was obtained, and its fluorine content was detected to be F:C=0.82.
[0125] Example 7
[0126] like Figure 1 As shown in the figure, 5 kg of flake graphite was placed in the feed hopper of the rotary kiln, and 11 kg of KOH was added; the vacuum degree of the rotary kiln was set, and 500 kPa CO was introduced. 2 After the leak test is qualified, start heating up. When the temperature reaches 500℃, keep it warm for 5h.
[0127] Soak the porous graphite after alkaline etching in 40% hydrofluoric acid, let it stand for 20 hours, pour out the hydrofluoric acid, add deionized water and stir, let it stand for 1 hour after stirring, and pour out the deionized water. Then use water to repeatedly wash the graphite until the pH value of the water after washing is neutral; put the porous graphite in a box-type drying oven at 60°C for drying, and then put it in a vacuum drying oven at 80°C for drying for 8 hours to obtain the treated porous graphite, which is temporarily stored;
[0128] The treated porous graphite is added into a fluidized bed reactor and allowed to stand; high-purity nitrogen is introduced into the fluidized bed reactor to remove water and oxygen until the water and oxygen contents in the fluidized bed reactor are lower than 10 ppm and 100 ppm, respectively;
[0129] Subsequently, the temperature of the fluidized bed reactor was set to 200° C. for heating. When the temperature of the fluidized bed reactor reached a predetermined temperature, a 15% (volume ratio) fluorine-nitrogen mixed gas (i.e., the volume ratio of the fluorine source to the inert gas was 0.15:1) was introduced into the fluidized bed reactor, and an ultraviolet irradiation lamp was turned on to react the porous graphite with the fluorine gas. The ultraviolet irradiation intensity was 151x.
[0130] After 5 hours of reaction, the introduction of fluorine-nitrogen mixed gas was stopped, and nitrogen was introduced into the fluidized bed for replacement to remove the residual fluorine gas in the fluidized bed. When the fluorine content in the tail gas was detected to be below 3 ppm, nitrogen blowing was stopped, and the fluorination reaction was completed to obtain the final sample, and its fluorine content was detected to be F:C=0.86.
[0131] Example 8
[0132] like Figure 1 As shown in the figure, 5 kg of flake graphite was placed in the feed hopper of the rotary kiln, and 11 kg of KOH was added; the vacuum degree of the rotary kiln was set, and 500 kPa CO was introduced. 2 After the leak test is qualified, start heating up. When the temperature reaches 500℃, keep it warm for 5h.
[0133] Soak the porous graphite after alkaline etching in 40% hydrofluoric acid, let it stand for 20 hours, pour out the hydrofluoric acid, add deionized water and stir, let it stand for 1 hour after stirring, and pour out the deionized water. Then use water to repeatedly wash the graphite until the pH value of the water after washing is neutral; put the porous graphite in a box-type drying oven at 60°C for drying, and then put it in a vacuum drying oven at 80°C for drying for 8 hours to obtain the treated porous graphite, which is temporarily stored;
[0134] The treated porous graphite is added into a fluidized bed reactor and allowed to stand; high-purity nitrogen is introduced into the fluidized bed reactor to remove water and oxygen until the water and oxygen contents in the fluidized bed reactor are lower than 10 ppm and 100 ppm, respectively;
[0135] Subsequently, the temperature of the fluidized bed reactor was set to 200° C. for heating. When the temperature of the fluidized bed reactor reached a predetermined temperature, a 15% (volume ratio) fluorine-nitrogen mixed gas (i.e., the volume ratio of the fluorine source to the inert gas was 0.15:1) was introduced into the fluidized bed reactor, and an ultraviolet irradiation lamp was turned on to react the porous graphite with the fluorine gas. The ultraviolet irradiation intensity was 201x.
[0136] After 5 hours of reaction, the introduction of fluorine-nitrogen mixed gas was stopped, and nitrogen was introduced into the fluidized bed for replacement to remove the residual fluorine gas in the fluidized bed. When the fluorine content in the tail gas was detected to be below 3 ppm, nitrogen blowing was stopped, and the fluorination reaction was completed to obtain the final sample, and its fluorine content was detected to be F:C=0.88.
[0137] Comparative Example 1:
[0138] Place flake graphite in 50% hydrofluoric acid and let it stand for 24 hours to separate into layers, then pour off the upper layer of hydrofluoric acid, add water, stir, let it stand to separate into layers, and pour off the upper layer of water. Use water to wash the graphite repeatedly until the pH value of the washed water is neutral. Dry the graphite in a 150°C forced air drying oven for 12 hours, and then dry it in a 150°C vacuum drying oven for 8 hours. Add the pretreated graphite to a fluidized bed reactor and let it stand; pass high-purity nitrogen into the fluidized bed reactor to remove water and oxygen until the water and oxygen contents in the fluidized bed reactor are less than 10ppm and 100ppm, respectively;
[0139] Subsequently, the temperature of the reactor was set to 200°C for heating and insulation for 2 hours; at the end of insulation, the atmosphere in the reactor was replaced with pure argon; the reactor was heated again to increase the temperature from 200°C to 400°C and then insulation for 2 hours; at the end of insulation, the atmosphere in the reactor was replaced with pure argon again to remove water generated during the heating process.
[0140] Continue to heat the reactor to 500°C, start to introduce 15% (volume ratio) fluorine-nitrogen mixed gas (i.e., the volume ratio of fluorine source to inert gas is 0.15:1), and after 5 hours of reaction, stop introducing the fluorine-nitrogen mixed gas, introduce nitrogen into the fluidized bed for replacement, and remove the residual fluorine gas in the fluidized bed. When the fluorine content in the tail gas is detected to be below 3ppm, stop blowing nitrogen, the fluorination reaction is completed, and the final sample is obtained, and its fluorine content is detected to be F:C=0.62.
[0141] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A method for preparing graphite fluoride, characterized in that: The steps include: Porous graphite is obtained by alkaline etching and vapor deposition of a graphite substrate; Pickling the porous graphite; Under ultraviolet irradiation conditions, subjecting the acid-washed porous graphite to a fluorination reaction to obtain the fluorinated graphite; Wherein, the fluorinating agent used in the fluorination reaction is a composite gas of a fluorine source and an inert gas, and the fluorine source is one or more of F2, CIF, CIF3, and NF3; The irradiation intensity of the ultraviolet irradiation condition is 5lx-25lx, and the irradiation reaction temperature is 150°C-400°C.
2. The preparation method according to claim 1, characterized in that: The method of obtaining porous graphite by alkali etching and vapor deposition on a graphite substrate comprises: When the graphite substrate is subjected to alkali etching, CO2 is introduced to deposit the alkali vapor formed during the alkali etching process onto the graphite substrate to obtain the porous graphite.
3. The preparation method according to claim 2, characterized in that: The alkali used in the alkali etching is a strong alkali; The etching temperature in the alkaline etching is 500° C. to 600° C.; The molar ratio of the graphite substrate to the alkali in the alkali etching is 1:1.15 to 1:1.
5.
4. The preparation method according to claim 2, characterized in that: The pressure of CO2 introduced during the alkaline etching is 100 kPa to 500 kPa.
5. The preparation method according to claim 1, characterized in that: The step of pickling the porous graphite comprises: The porous graphite is immersed in acid, allowed to stand, and then taken out; The porous graphite after pickling is cleaned, dried and dried.
6. The preparation method according to claim 5, characterized in that: The acid is carbonic acid or hydrofluoric acid; The porous graphite is immersed in the acid for 15 to 35 hours; The concentration of the acid is 30% to 60%.
7. The preparation method according to claim 1, characterized in that: The graphite matrix adopts a high-purity graphite matrix, including flake graphite and expanded graphite; The graphite matrix may be in a powdery, spherical, blocky, stripy, flake or irregular shape.
8. The preparation method according to claim 1, characterized in that: The inert gas is one of nitrogen and argon; The volume ratio of the fluorine source to the inert gas is 0.05:1 to 0.5:
1.
9. The preparation method according to claim 1, characterized in that: The reaction time of the fluorination reaction is 2h to 6h.
10. Graphite fluoride obtained by the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
High specific surface area graphene with well-developed mesopores, and preparation method thereof
CN102992313A
Method for preparing carbon monofluoride or fluorocarbon through inner circulation of fluorine
CN103332669A
Method for preparing fluorine-doped graphene quantum dots
CN108706579A
Porous fluorinated graphene as well as preparation method and application thereof
CN109319772A
Functionalized reduced graphene oxide and methods of producing the same
US20160376154A1