Preparation method of high-purity rare earth carbonate and oxide

By using citric acid and its salt as purification agent in the rare earth carbonate precipitation method, the precipitation pH value of aluminum ferrous ions is reduced, and the problem of co-precipitation of rare earths and impurities in the prior art is solved, and high-purity rare earth carbonate is achieved and preparation of oxides.

CN118978177AActive Publication Date: 2024-11-19NANCHANG UNIV

Patent Information

Application Number
CN202411026690.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-19
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

The existing rare earth carbonate precipitation method has poor selectivity when removing iron and aluminum impurities, resulting in co-precipitation of rare earths and impurities, affecting the purity and quality of the product. Especially under the impurity content of a wide concentration range, it is difficult to effectively remove aluminum and iron. Impurities and reduce co-precipitation losses of rare earths.

Method used

Using citric acid and its salt as organic acid or organic acid salt purification agent, the separation effect between rare earth and impurities is strengthened through coordination method, and the pH value of aluminum ferro ion precipitation is reduced, so that it precipitates under lower pH conditions and reduces rare earths. The co-precipitation loss is made of rare earths with carbonate precipitation agent, and high-purity oxidation rare earths are obtained after calcination.

Benefits of technology

Effectively remove aluminum-ferrous impurities, reduce the co-precipitation loss of rare earths, improve the purity of rare earth carbonates and oxides, and ensure the acquisition of high-purity products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978177A_ABST
    Figure CN118978177A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of high-purity rare earth carbonate and oxide, and relates to the technical field of rare earth wet separation. The method provided by the invention comprises the following steps: adding an organic acid or an organic acid salt as a purifying agent into a rare earth feed liquid, stirring and mixing, adding a precipitator, and filtering to obtain a purified feed liquid; continuously adding a carbonate precipitant into the purified feed liquid while stirring to precipitate the rare earth in the form of carbonate, aging and crystallizing at 20-80 DEG C, carrying out suction filtration, washing, and drying to obtain a rare earth-containing carbonate precipitate; and calcining the rare earth-containing carbonate precipitate at 900-1000 DEG C to obtain the high-purity rare earth oxide. According to the method, the rare earth and the ferro-aluminum are precipitated and separated from the rare earth feed liquid by utilizing the coordination effect of the organic acid or the organic acid salt, the separation efficiency is improved by utilizing the stability difference between the rare earth and the ferro-aluminum impurities, the rare earth loss caused by coprecipitation is reduced, and a high-purity rare earth oxide product can be obtained at a high yield.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of rare earth hydrometallurgy and separation, and in particular to a method for preparing high-purity rare earth carbonate and oxide. Background Art

[0002] As a typical metal element, rare earth is widely used in traditional markets such as metallurgy, petrochemicals, glass ceramics, and agriculture due to its special physical properties such as light and electricity and other chemical properties. With the rapid development of technology, high-purity and ultra-high-purity rare earths have been increasingly used due to their unique properties, and high-purity rare earth metals are the basis for the application of high-performance rare earths in magnetic, optical, and electrical functional materials.

[0003] Rare earth elements are difficult to separate due to their similar chemical properties, so it is difficult to prepare high-purity rare earths. my country's advanced extraction and separation technology has solved the problem of separation between rare earth elements. However, it is also difficult to precipitate and separate rare earths from some non-rare earth elements with similar properties, because the precipitation conditions of these impurity ions are similar to those of rare earths, such as iron, aluminum, calcium, and magnesium. When removing impurities by the permanent precipitation method, a large amount of rare earth will be lost due to the generation of co-precipitation. Therefore, how to pre-precipitate and remove impurity ions before precipitating rare earths is a method commonly used in laboratories and industrial production. For example: when recovering rare earths from ionic rare earth leachate by precipitation, the 1986 patent proposed to use ammonium bicarbonate or ammonia water to adjust the pH to between 5.0-5.6, so that iron and aluminum impurities are first precipitated as hydroxides, and the filtered purified liquid is further precipitated with ammonium bicarbonate to obtain oxidized rare earth products that meet the requirements.

[0004] Rare earth carbonate precipitation and crystallization is a classic method for precipitating rare earth from a solution and separating a large number of associated ions. Chinese invention patent CN113830817A discloses a method for preparing a cerium-based oxide material and its precursor in the prior art, comprising the following steps: preparing a rare earth feed solution mainly composed of cerium, mixing a precipitant solution with the rare earth feed solution to form a rare earth precipitate, aging and crystallizing the rare earth precipitate to obtain a rare earth precursor compound, and calcining the precursor compound to obtain a cerium-based oxide, wherein the precipitant solution is any one of ammonium bicarbonate and ammonium carbonate.

[0005] The prior art of Chinese invention patent CN112126977A also discloses a method for preparing high-purity flaky single crystals and flaky dense aggregated cerium carbonate, in which ammonium citrate is added in advance to regulate the crystallization process when cerium is precipitated with ammonium carbonate / ammonium bicarbonate. This invention uses triammonium citrate to regulate the crystallization process in the existing carbonate precipitation system, mainly by reducing the crystallization rate of rare earth carbonate to reduce the chloride content and reduce the entrainment and co-precipitation of impurities during the precipitation process.

[0006] Precipitation is the most widely used technology in scientific research and industrial production. It has the advantages of low raw material cost, low equipment requirements and simple process operation. Ammonium bicarbonate precipitant is cheap, but ammonium bicarbonate precipitation method has problems such as poor selectivity. Taking advantage of the fact that iron and aluminum ions are easier to hydrolyze to produce hydroxide precipitation than rare earth ions, iron and aluminum are preferentially precipitated and removed in advance by controlling the pH value of the solution. This method has been used in industry for decades and can remove most of the iron and aluminum. However, due to co-precipitation with rare earths, rare earths are precipitated together with iron and aluminum hydroxides and lost. Moreover, to achieve good removal of iron and aluminum, it is best to remove iron and aluminum separately in two steps. That is, first hydrolyze to remove iron, filter or liquid-solid separation, and then add alkali to increase the pH to precipitate aluminum. If you want to remove iron and aluminum at the same time by directly adjusting the pH to the pH required for aluminum hydrolysis in one step, it is theoretically feasible, but the actual effect is not good. If the aluminum concentration is reduced to the expected value, the loss of rare earth will be greater, proving that the co-hydrolysis and precipitation of iron and aluminum will increase the co-precipitation trend of rare earth, resulting in an increase in the loss of rare earth. 3+ , Fe 3+ Impurity ions such as ions are easily precipitated with rare earths, which will greatly affect the purity and quality of the final rare earth products. Therefore, it is urgent to provide a solution to improve the above problems and obtain a method that can be used in Al 3+ , Fe 3+ The invention discloses a new method for precipitating rare earth in rare earth liquid with a wide range of impurity contents and separating it from the impurities.

[0007] The coordination precipitation method is used to purify and remove impurities from rare earth liquid. It often uses the stability difference of the complex formed by the coordination agent, impurity ions and rare earth ions to delay the precipitation of ions with stronger stability and play a purification role. For example, the invention patent CN112126977A mentioned above is a method for preparing flaky rare earth carbonate crystals with good crystallinity and high purity by adding citrate to reduce the precipitation and crystallization speed of rare earth carbonate. The present invention proposes a new method for adding organic acids and salts thereof to effectively improve the removal rate of aluminum and iron impurities and reduce the loss of rare earth co-precipitation. The method utilizes the strong coordination ability of a small amount of coordination agents with iron and aluminum, so that iron and aluminum can precipitate and reduce the co-precipitation of rare earth under lower pH conditions, and can hydrolyze and remove iron and aluminum in one step, and reduce the co-precipitation loss of rare earth. Then ensure that when the rare earth carbonate is finally precipitated, the amount of impurity ions entering the product can be greatly reduced, and high-purity rare earth carbonate and oxide products thereof are obtained. Summary of the invention

[0008] The purpose of the present invention is to provide a method for preparing high-purity rare earth carbonates and oxides, which can remove aluminum and iron in advance in rare earth liquid with impurity content in a wide concentration range, and reduce the co-precipitation loss of rare earths. It is ensured that the combination and adsorption of impurity ions are reduced during the rare earth precipitation and crystallization process, so as to obtain high-purity rare earth carbonate and oxide products.

[0009] The present invention provides a method for preparing high-purity rare earth carbonates and oxides by purifying rare earth liquid by citric acid-assisted iron-aluminum coprecipitation, comprising the following steps:

[0010] Add organic acid or organic acid salt to the rare earth liquid, and use the coordination method to enhance the separation effect of rare earth and impurities. Add precipitant under stirring, pre-clean the liquid containing aluminum and iron impurities, filter, add precipitant to the filtrate and continue stirring, and the precipitated rare earth carbonate is aged and crystallized within a certain temperature range to obtain high-purity rare earth carbonate, which is calcined to obtain the corresponding rare earth oxide; the purifying agent is an organic acid or organic acid salt represented by citric acid and its salts, and their iron and aluminum complexes are more stable than their rare earth complexes; the precipitant includes at least one of carbonates;

[0011] The purified liquid is continuously added with carbonate precipitant under stirring to precipitate the rare earth in the form of carbonate, and is placed at 20-80°C for aging and crystallization, filtered, washed, and dried to obtain a rare earth-containing carbonate precipitate;

[0012] The rare earth carbonate precipitate is calcined at 900-1000°C to obtain high-purity rare earth oxide.

[0013] The beneficial effect of the preparation method of a high-purity rare earth carbonate and oxide provided by the present invention is that by adding an organic acid or an organic acid salt as a purifying agent, the organic acid or an organic acid salt is first coordinated with aluminum and iron ions, thereby reducing the pH required for precipitation of aluminum and iron ions, and reducing the co-precipitation loss of rare earth while removing aluminum and iron. The rare earth solution after filtration or liquid-solid separation is further precipitated with carbonate, and aged and crystallized to obtain a high-purity rare earth carbonate with a low impurity content. The rare earth carbonate is calcined to obtain a high-purity rare earth oxide.

[0014] Optionally, when the precipitant is carbonate, the pH adjusted in the pre-impurity removal process is 3.3-4.6, which is lower than the pH required for general pre-treatment and impurity removal, and the amount of rare earth co-precipitation is greatly reduced.

[0015] Optionally, when the precipitant is a carbonate, the pH of the rare earth carbonate prepared by adding the precipitant and stirring the reaction is controlled between 5.6 and 7.3, and the rare earth carbonate is obtained by aging and crystallization to obtain high-purity rare earth carbonate.

[0016] Optionally, an organic acid or an organic acid salt is added to the rare earth liquid, impurities are removed by coordination method, a precipitant is added after stirring and mixing, and the rare earth liquid containing aluminum and iron in a wide concentration range is pre-removed from impurities, filtered, and the precipitant is added to the filtrate and stirred continuously to prepare rare earth carbonate crystals, including:

[0017] Adding an organic acid or an organic acid salt as a purifying agent into a rare earth liquid containing iron and aluminum impurities, stirring, mixing and dissolving to obtain a mixed liquid;

[0018] Optionally, in the process of adding an organic acid or an organic acid salt as a purifying agent into the rare earth solution, the molar ratio of the purifying agent to the aluminum and iron in the rare earth solution is 0%-2.8%.

[0019] Optionally, in the process of adding an organic acid or an organic acid salt as a purifying agent into the rare earth solution, the rare earth solution includes at least one of a rare earth chloride solution and a rare earth nitrate solution.

[0020] The mixed liquid is stirred and reacted with the precipitant, the pH value of the solution is controlled between 3.6 and 4.6, and filtered. The filtrate is stirred and mixed with the precipitant again, the pH value of the solution is controlled between 5.6 and 7.3, and rare earth carbonate is prepared.

[0021] Optionally, the rare earth carbonate produced by the reaction is placed at 20-80° C. for aging and crystallization, and the aging and crystallization time is 0.5-8 hours. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 A flow chart of high-purity rare earth carbonates and oxides provided in an embodiment of the present invention;

[0023] Figure 2 Content of various ions in the supernatant after pre-removal of impurities and iron;

[0024] Figure 3 Precipitation rate of each ion in the supernatant of pre-impurity and iron removal;

[0025] Figure 4 Content of various ions in the supernatant liquid after pre-removal of impurities and aluminum;

[0026] Figure 5 Precipitation rate of each ion in the supernatant of pre-removed impurities and aluminum;

[0027] Figure 6 The proportion of each ion in the precipitate of ammonium bicarbonate at different aging times;

[0028] Figure 7 After pre-removal of impurities, the precipitation rate of the supernatant was precipitated by adding triammonium citrate and ammonium bicarbonate;

[0029] Figure 8 After pre-removal of impurities, add triammonium citrate and ammonium bicarbonate for precipitation;

[0030] Fig. 9 Effects of different amounts of ammonium citrate trihydrate added on the aluminum ion concentration of the supernatant during the pre-removal process;

[0031] Fig.10 Effects of different amounts of triammonium citrate added on the removal rate of aluminum in pre-removal;

[0032] Fig.11 The effect of different amounts of triammonium citrate added on the loss rate of pre-removed rare earth;

[0033] Fig.12 Effects of different amounts of triammonium citrate added on the removal rate of pre-removal of impurities iron;

[0034] Fig.13 The proportion of each ion in the precipitate at different aging times after adding the optimal amount of triammonium citrate in the pre-removal process;

[0035] Fig.14 The effects of different additives and different addition amounts on the aluminum ion concentration of the supernatant during the pre-removal process;

[0036] Fig.15 The effects of different additives and different addition amounts on the rare earth ion concentration of the supernatant in the pre-removal process;

[0037] Fig.16 The influence of different additives and different addition amounts on the removal rate of aluminum in pre-removal;

[0038] Fig.17 The influence of different additives and different addition amounts on the loss rate of pre-removed rare earth;

[0039] Fig.18 The effect of different amounts of ammonium citrate trihydrate added on the removal rate of aluminum in pre-removal at 0.07 mol / LAl;

[0040] Fig.19 The effect of different amounts of triammonium citrate added on the removal rate of pre-iron removal at 0.07mol / LAl;

[0041] Fig. 20 The effect of different amounts of triammonium citrate added on the loss rate of pre-removal of rare earth at 0.07 mol / LAl;

[0042] Fig.21 The effect of different amounts of ammonium citrate trihydrate added on the removal rate of aluminum in pre-removal at 0.105 mol / LAl;

[0043] Fig. 22 The effect of different amounts of triammonium citrate added on the removal rate of pre-iron removal at 0.105mol / LAl;

[0044] Fig.23 The effect of different amounts of triammonium citrate added on the loss rate of pre-removal of rare earth at 0.105mol / LAl;

[0045] Fig.24 The effect of different amounts of triammonium citrate added on the removal rate of aluminum in pre-removal at 0.14 mol / LAl;

[0046] Fig.25 The effect of different amounts of triammonium citrate added on the removal rate of pre-iron removal at 0.14 mol / LAl;

[0047] Fig.26 The effect of different amounts of triammonium citrate added on the loss rate of pre-removal of rare earth at 0.14 mol / LAl;

[0048] Fig. 27 The effect of different amounts of ammonium citrate trihydrate added on the removal rate of aluminum in pre-removal at 0.035 mol / LAl;

[0049] Fig.28 The effect of different amounts of triammonium citrate added on the removal rate of pre-iron removal at 0.035mol / LAl;

[0050] Fig.29 The effect of different amounts of triammonium citrate added on the loss rate of pre-removal of rare earth at 0.035mol / LAl;

[0051] Fig.30 The effect of different amounts of ammonium citrate trihydrate added on the removal rate of aluminum in pre-removal at 0.0175 mol / LAl;

[0052] Fig.31 The effect of different amounts of triammonium citrate added on the removal rate of pre-iron removal at 0.0175mol / LAl;

[0053] Fig.32 The effect of different amounts of triammonium citrate added on the loss rate of pre-removal of rare earth at 0.0175mol / LAl;

[0054] Fig.33 Relationship between different aluminum-iron molar ratios and the optimal amount of triammonium citrate added. DETAILED DESCRIPTION

[0055] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Unless otherwise defined, the technical terms or scientific terms used herein should be understood by people with general skills in the field to which the present invention belongs. "Including" and similar words used in this article mean that the elements or objects appearing before the word include the elements or objects listed after the word and their equivalents, without excluding other elements or objects.

[0056] See also Figure 1 The present invention provides a method for preparing high-purity rare earth carbonates and oxides, comprising the following steps:

[0057] S1. Add an organic acid or an organic acid salt as a purifying agent to a rare earth feed solution, add a precipitant after stirring and mixing, pre-remove impurities from the rare earth feed solution containing a wide range of aluminum and iron concentrations, and filter; continue to stir the filtrate and add a precipitant to obtain a rare earth carbonate precipitate;

[0058] S2, placing the rare earth carbonate precipitate at 20-80° C. for aging and crystallization, filtering, washing and drying to obtain high-purity rare earth carbonate;

[0059] S3. Calcine high-purity rare earth carbonate at 900-1000° C. to obtain high-purity rare earth oxide.

[0060] In fact, in the process of adding organic acid or organic acid salt as a purifying agent to the rare earth liquid and stirring and mixing, the purifying agent used includes at least one of triammonium citrate, citric acid, ammonium salicylate, tartaric acid, malic acid, and ammonium tartrate.

[0061] In some embodiments, during the stirring and mixing process of adding an organic acid or an organic acid salt as a purifying agent to a rare earth liquid, the rare earth liquid used may be at least one of rare earth chloride and rare earth nitrate, which may be purchased from a rare earth separation enterprise, or purchased from a high-purity rare earth chloride or rare earth nitrate, dissolved in high-purity water, and then prepared. Specifically, the molar concentration of rare earth in the rare earth liquid may be 0.1-1.5 mol / L. In fact, there is no special restriction on the molar concentration of rare earth in the rare earth liquid, and the relative purity of rare earth in the rare earth liquid may be 30%-99.9%.

[0062] In some embodiments, an organic acid or an organic acid salt is added to a rare earth feed liquid as a purifying agent, a precipitant is added after stirring and mixing, and the rare earth feed liquid containing a wide range of aluminum and iron concentrations is pre-cleaned and filtered, and the precipitant is added to the filtrate and stirred continuously to prepare a rare earth carbonate, which includes:

[0063] Adding an organic acid or an organic acid salt as a purifying agent into a rare earth liquid, stirring, mixing and dissolving to obtain a mixed liquid;

[0064] The mixed liquid is stirred and mixed with the precipitant, and the purified rare earth liquid is obtained after filtering or solid-liquid separation.

[0065] In fact, in the process of stirring and mixing the mixed liquid and the precipitant, the precipitant used includes at least one of carbonates. Specifically, the precipitant used can be at least one of ammonium bicarbonate and ammonium carbonate.

[0066] In fact, during the process of stirring and mixing the mixed liquid and the precipitant, the mixed liquid and the precipitant can be mixed by adding them simultaneously or by adding them one after another, and the mixing of the mixed liquid and the precipitant is carried out under continuous stirring. Specifically, during the process of stirring and mixing the mixed liquid and the precipitant, the precipitant is slowly added into the mixed liquid for stirring and mixing.

[0067] In some embodiments, when ammonium bicarbonate is used as the precipitant, the rare earth in the mixed liquid can be precipitated when the pH of the purified liquid and the precipitant are stirred to produce rare earth carbonate is 5.6-7.3; in fact, when the mixed liquid and the precipitant are stirred, the pH value for complete precipitation of the rare earth in the mixed liquid needs to be adaptively adjusted according to the content of rare earth in the supernatant of the reaction liquid. Specifically, complete precipitation of the rare earth means that the precipitant is added completely and no obvious reaction bubbles are generated.

[0068] In some embodiments, in the process of adding an organic acid or an organic acid salt as a purifying agent into the rare earth solution, the molar ratio of the purifying agent to the aluminum and iron in the rare earth solution is 0%-2.8%.

[0069] In some embodiments, the reaction liquid is placed in a process of aging and crystallization at 20-80° C., and the duration of aging and crystallization is controlled at 0.5-8 h.

[0070] In some embodiments, in the process of filtration, washing and drying to obtain a rare earth-containing precipitate, the filtration and washing method can adopt one of the existing conventional processes such as belt continuous vacuum filtration washing, vacuum box filtration, etc., and the washing liquid can be tested during the washing process of the precipitate after filtration. When it is detected that there are no chloride ions and ammonium ions in the washing liquid, the washing process is completed.

[0071] In fact, in the process of filtration, washing and drying to obtain rare earth-containing precipitates, it is best not to completely drain the filter cake layer before detecting that there are no chloride ions and ammonium ions in the washing liquid. It is also necessary to ensure that there are sufficient gaps in the filter cake layer to ensure washing efficiency.

[0072] Research Example 1

[0073] Take 100mL of rare earth solution with a rare earth concentration of 0.5mol / L, a Fe concentration of 0.0039mol / L, and an Al concentration of 0.085mol (the proportion of each impurity is shown in Table 1) in a beaker, slowly add 2% ammonium bicarbonate solution to the beaker, adjust the pH, and stir continuously during the addition of ammonium bicarbonate solution. Take a small amount of supernatant at different pH values, use ICP-MS to determine the concentration of each ion in the supernatant, and draw a graph as shown below: Figure 2 , calculate the precipitation rate of each ion as Figure 3 ;

[0074] Take 100 ml of the filtrate with a pH of 4.12 in a beaker, and continue to slowly add 2% ammonium bicarbonate solution to the beaker to adjust the pH. Stir continuously during the addition of ammonium bicarbonate solution. Collect a small amount of supernatant at different pH values, and use ICP-MS to determine the concentration of each ion in the supernatant. Figure 4 , calculate the precipitation rate of each ion as Figure 5 .

[0075] Research and analysis: From Figure 2 , 3 It can be seen from Figures 4 and 5 that the precipitation rate of iron and aluminum increases significantly with the increase of pH. At a pH of 4.12, iron has been completely precipitated and more than 60% of aluminum has been precipitated. If the pH is further increased, the removal effect of aluminum is not good, and a large amount of rare earth is lost. This shows that in the pre-impurity removal process, the presence of iron hydroxide will hinder the hydrolysis of aluminum, and the co-precipitation of aluminum and iron will lead to more rare earth losses. Therefore, for the purification of rare earth liquid containing aluminum and iron impurities, it is planned to remove iron first (i.e., pH is 4.12), adjust the pH of the filtered filtrate, and further remove aluminum. When the pH is 4.6, the aluminum content of the supernatant is 0.18g / L, the aluminum precipitation rate reaches 84%, and the rare earth loss rate is about 6%.

[0076] Table 1: Proportion of each ion in the initial feed solution

[0077] Na Mg Al Ca Rare Earth Fe other 1.53% 1.61% 2.87% 2.51% 90.28% 0.28% 0.90%

[0078] Research Example 2

[0079] This research example 2 investigates the effect of using ammonium bicarbonate as a precipitant on the content of rare earth and impurity ions in the final rare earth oxide product, including the following steps:

[0080] Y1. Take 150 mL of the filtered solution with a pH of 4.6 after the stepwise removal of aluminum and iron in Example 1 and place it in a beaker. Slowly add a 10% ammonium bicarbonate solution by mass to the beaker until the pH of the mixed solution in the beaker is 6.43. Stir continuously during the addition of the ammonium bicarbonate solution. A white precipitate and bubbles are generated in the beaker. Stir continuously to complete the precipitation reaction.

[0081] Y2. After stopping stirring, the precipitate in the beaker is evenly placed in five beakers, and the five beakers are sealed and placed in a room temperature environment for aging for 0.5h, 2h, 4h, 6h, and 8h respectively, and then the precipitate is filtered and washed until the washing liquid contains no chloride ions (the silver nitrate solution acidified by nitric acid cannot become turbid), and the precipitate is dried at 80° C. to obtain a rare earth carbonate precipitate;

[0082] Y3. Five groups of rare earth carbonate precipitates were placed in a muffle furnace respectively, and rare earth oxide products were obtained after being burned at 950°C. The rare earth oxide products were dissolved in a mixed solution of nitric acid and hydrogen peroxide, and the contents of rare earth and impurities such as sodium, magnesium, and aluminum in the dissolved solution were determined by ICP-MS. Three parallel tests were performed on each group of samples and the average value was taken. The results are as follows: Figure 6 shown.

[0083] Research and analysis: From Figure 6 It can be seen that if the aging time is too long, more impurities will enter the precipitation, while relatively less impurities will be precipitated after 6 hours, and the rare earth content will be relatively high. The purity of the product 6h rare earth oxide is 98.09%, of which Al accounts for 1.12%. Appropriate aging is beneficial for Na and Mg to remain in the supernatant and improve product purity. However, after pre-impurity removal, 0.18g / L of the feed liquid will all enter the precipitation, affecting the product purity.

[0084] Exploration Example 3

[0085] This research example 3 investigates the effect of adding triammonium citrate in the precipitation process using ammonium bicarbonate as a precipitant on the rare earth and impurity ion content in the rare earth oxide product, including the following steps:

[0086] Y1. Take 30 mL of the filtered solution with a pH of 4.6 after the stepwise removal of aluminum and iron in Example 1 and place it in 6 beakers, add ammonium citrate with a molar ratio of 0, 0.6, 0.8, 1, 1.2, and 1.4 to the beakers respectively, stir to dissolve, and then slowly add a 10% ammonium bicarbonate solution by mass until the pH of the mixed solution in the beaker is 6.43, and stir continuously during the addition of the ammonium bicarbonate solution. A white precipitate appears in the beaker and bubbles are generated. Stir continuously to complete the precipitation reaction;

[0087] Y2. After stopping stirring, the precipitate in the beaker is evenly placed in five beakers, and the five beakers are sealed and placed in a room temperature environment for aging for 0.5h, 2h, 4h, 6h, and 8h respectively, and then the precipitate is filtered and washed until the washing liquid contains no chloride ions (the silver nitrate solution acidified by nitric acid cannot become turbid), and the precipitate is dried at 80° C. to obtain a rare earth carbonate precipitate;

[0088] Y3. Five groups of rare earth carbonate precipitates were placed in a muffle furnace respectively, and rare earth oxide products were obtained after being burned at 950°C. The rare earth oxide products were dissolved in a mixed solution of nitric acid and hydrogen peroxide, and the contents of rare earth and impurities such as sodium, magnesium, and aluminum in the dissolved solution were determined by ICP-MS. Three parallel tests were performed on each group of samples and the average value was taken. The results are as follows: Figure 7 , 8 shown.

[0089] Research and analysis: From Figure 7 , 8 It can be seen that adding an appropriate amount of triammonium citrate can reduce the precipitation rate of aluminum, and the precipitation rate of sodium and magnesium can also be slightly reduced. When the molar ratio of citric acid is 1, the precipitation purity is the highest, which is 98.60%. Aluminum accounts for 0.8%. After pre-removal of impurities, adding triammonium citrate and precipitating with ammonium bicarbonate can complex part of the aluminum and improve the purity of the product. However, the stability constants of aluminum citrate and rare earth citrate are close, and adding triammonium citrate cannot completely complex aluminum, resulting in the aluminum content of the product being too high, affecting the purity of the product.

[0090] Exploration Example 4

[0091] 100 mL of the rare earth solution in Example 1 was added to eight beakers, and ammonium citrate was added at a molar ratio of 0, 0.6, 1, 1.4, 1.87, 2.2, 2.6, and 3 to iron, respectively. After stirring to dissolve, 2% ammonium bicarbonate solution was added to the beaker, and the pH was adjusted. During the addition of the ammonium bicarbonate solution, stirring was continued. A small amount of supernatant at different pH values ​​was collected, and the aluminum ion concentration of the supernatant was determined by ICP-MS. Fig. 9 , aluminum ion precipitation rate Fig.10 , the rare earth ion loss rate is as follows Fig.11 , the iron ion precipitation rate is Fig.12 .

[0092] Research and analysis: From Fig. 9 , 10, 11, 12 It can be seen that during the pre-removal of impurities with ammonium bicarbonate, adding triammonium citrate with a molar ratio of 1.8 to aluminum and iron can remove more aluminum at the same pH without excessive loss of rare earth. When the pH is 4.15, the aluminum removal rate can reach more than 93%, and the aluminum ion content is reduced to 0.05g / L. The complexing ability of triammonium citrate with iron is stronger than that of rare earth and aluminum. Adding a small amount of triammonium citrate to complex iron can make aluminum precipitate in advance, precipitate at a lower pH, and reduce the co-precipitation loss of rare earth.

[0093] Exploration Example 5

[0094] This research example 5 investigates the effect of adding triammonium citrate in the pre-impurity removal process using ammonium bicarbonate as a precipitant on the rare earth and impurity ion content in the rare earth oxide product, including the following steps:

[0095] Y1. Take 150 mL of the initial feed solution in Example 1 and place it in a beaker. Add ammonium citrate triammonium citrate with a molar ratio of 1.8 to iron. After stirring to dissolve, add 2% ammonium bicarbonate solution to the beaker to adjust the pH to 4.15. The filtered feed solution is placed in a beaker. Slowly add 10% ammonium bicarbonate solution by mass to the beaker until the pH of the mixed solution in the beaker is 6.43. Stir continuously during the addition of the ammonium bicarbonate solution. A white precipitate appears in the beaker and bubbles are generated. Stir continuously to complete the precipitation reaction.

[0096] Y2. After stopping stirring, the precipitate in the beaker is evenly placed in five beakers, and the five beakers are sealed and placed in a room temperature environment for aging for 0.5h, 2h, 4h, 6h, and 8h respectively, and then the precipitate is filtered and washed until the washing liquid contains no chloride ions (the silver nitrate solution acidified by nitric acid cannot become turbid), and the precipitate is dried at 80° C. to obtain a rare earth carbonate precipitate;

[0097] Y3. Five groups of rare earth carbonate precipitates were placed in a muffle furnace respectively, and rare earth oxide products were obtained after being burned at 950°C. The rare earth oxide products were dissolved in a mixed solution of nitric acid and hydrogen peroxide, and the contents of rare earth and impurities such as sodium, magnesium, and aluminum in the dissolved solution were determined by ICP-MS. Three parallel tests were performed on each group of samples and the average value was taken. The results are as follows: Fig.13 shown.

[0098] Research and analysis: From Fig.13 It can be seen that the length of aging time will affect the purity of the final rare earth oxide product, and a shorter aging time is conducive to the separation of rare earth and other impurity ions. When the aging time is 0.5h, the purity of the cerium oxide product reaches 99.55%. Among them, Al accounts for 0.35%. For the liquid with high iron and aluminum impurities, adding an appropriate amount of triammonium citrate in the pre-impurity removal process can better remove iron and aluminum and improve the purity of the final product.

[0099] Exploration Example 6

[0100] Take 100 mL of the rare earth solution in Example 1 and add it to ten beakers respectively. Add triammonium citrate with a molar ratio of 0, 0.12, 0.6, 1.2, and 1.8 to the first five beakers respectively, and add ammonium salicylate with a molar ratio of 0, 0.12, 0.6, 1.2, and 1.8 to the last five beakers respectively. After stirring and dissolving, add 2% ammonium bicarbonate solution to the beaker to adjust the pH, and stir continuously during the addition of ammonium bicarbonate solution. Filter at pH 4.15, and use ICP-MS to determine the aluminum ion concentration of the supernatant as shown in Fig.14 , the rare earth ion concentration is Fig.15 , calculate the aluminum ion precipitation rate as Fig.16 , the rare earth ion precipitation rate is as follows Fig.17 ;

[0101] Research and analysis: From Fig.14 , 15 , 16, and 17 show that the appropriate addition of triammonium citrate or ammonium salicylate during the pre-removal of impurities with ammonium bicarbonate can achieve better aluminum removal effects at the same pH without excessive loss of rare earths. When the pH is 4.15, the aluminum removal rate can reach more than 90%, among which triammonium citrate has a better aluminum removal effect.

[0102] Exploration Example 7

[0103] Take 100mL of rare earth solution with a rare earth concentration of 0.5mol / L, Fe concentration of 0.0035mol / L, and Al concentration of 0.07mol and add them to six beakers respectively, with an Al:Fe molar ratio of 20:1, and add ammonium citrate trihydrate with an aluminum-iron molar ratio of 0, 1, 1.4, 1.8, 2.2, and 2.6 respectively. After stirring and dissolving, add 2% ammonium bicarbonate solution to the beaker to adjust the pH, and stir continuously during the addition of ammonium bicarbonate solution. Collect a small amount of supernatant at different pH values, and use ICP-MS to determine the aluminum ions in the supernatant. Calculate the precipitation rate as follows: Fig.18 , the iron ion precipitation rate is Fig.19 , the rare earth ion precipitation rate is as follows Fig. 20 .

[0104] Take 100mL of rare earth solution with a rare earth concentration of 0.5mol / L, a Fe concentration of 0.0035mol / L, and an Al concentration of 0.105mol and add them to six beakers respectively, with an Al:Fe molar ratio of 30:1. Add ammonium citrate trihydrate with a molar ratio of 0, 1, 1.4, 1.8, 2.2, and 2.6 to iron respectively. After stirring and dissolving, add 2% ammonium bicarbonate solution to the beaker, adjust the pH, and stir continuously during the addition of ammonium bicarbonate solution. Collect a small amount of supernatant at different pH values, and use ICP-MS to determine the ion concentration of the supernatant. The calculated aluminum ion precipitation rate is as follows: Fig.21 , the iron ion precipitation rate is Fig. 22, the rare earth ion precipitation rate is as follows Fig.23 .

[0105] Take 100mL of rare earth solution with a rare earth concentration of 0.5mol / L, a Fe concentration of 0.0035mol / L, and an Al concentration of 0.14mol and add them to six beakers respectively, with an Al:Fe molar ratio of 40:1. Add ammonium citrate trihydrate with a molar ratio of 0, 1, 1.4, 1.8, 2.2, and 2.6 to iron respectively. After stirring and dissolving, add 2% ammonium bicarbonate solution to the beaker, adjust the pH, and stir continuously during the addition of ammonium bicarbonate solution. Collect a small amount of supernatant at different pH values, and use ICP-MS to determine the ion concentration of the supernatant. The calculated aluminum ion precipitation rate is as follows: Fig.24 , the iron ion precipitation rate is Fig.25 , the rare earth ion precipitation rate is as follows Fig.26 .

[0106] Take 100mL of rare earth solution with a rare earth concentration of 0.5mol / L, a Fe concentration of 0.0035mol / L, and an Al concentration of 0.035mol and add them to six beakers respectively, with an Al:Fe molar ratio of 10:1. Add ammonium citrate trihydrate with a molar ratio of 0, 1, 1.4, 1.8, 2.2, and 2.6 to iron respectively. After stirring and dissolving, add 2% ammonium bicarbonate solution to the beaker, adjust the pH, and stir continuously during the addition of ammonium bicarbonate solution. Collect a small amount of supernatant at different pH values, and use ICP-MS to determine the ion concentration in the supernatant. The calculated aluminum ion precipitation rate is as follows: Fig. 27 , the iron ion precipitation rate is Fig.28 , the rare earth ion precipitation rate is as follows Fig.29 .

[0107] Take 100mL of rare earth solution with a rare earth concentration of 0.5mol / L, a Fe concentration of 0.0035mol / L, and an Al concentration of 0.0175mol and add them to six beakers respectively, with an Al:Fe molar ratio of 5:1. Add ammonium citrate trihydrate with a molar ratio of 0, 1, 1.4, 1.8, 2.2, and 2.6 to iron respectively. After stirring and dissolving, add 2% ammonium bicarbonate solution to the beaker, adjust the pH, and stir continuously during the addition of ammonium bicarbonate solution. Collect a small amount of supernatant at different pH values, and use ICP-MS to determine the ion concentration in the supernatant. The calculated aluminum ion precipitation rate is as follows: Fig.30 , the iron ion precipitation rate is Fig.31 , the rare earth ion precipitation rate is as follows Fig.32 .

[0108] Research and analysis: From Figure 18-32It can be seen that adding an appropriate amount of ammonium citrate can increase the aluminum removal rate at the same pH, while iron can be completely removed without excessive loss of rare earth. By changing the iron-aluminum molar ratio of the slurry, the optimal ammonium citrate dosage with the highest aluminum precipitation rate under different ammonium citrate dosages at the same pH is obtained, which has a linear relationship with the iron-aluminum molar ratio. Fig.33 .

[0109] Although the embodiments of the present invention are described in detail above, it is obvious to those skilled in the art that various modifications and variations can be made to these embodiments. However, it should be understood that such modifications and variations are within the scope and spirit of the present invention as described in the claims. Moreover, the present invention described herein may have other embodiments and may be implemented or realized in a variety of ways.

Claims

1. A method for preparing high-purity rare earth carbonates and oxides, characterized in that: The following steps are involved: Adding an organic acid or an organic acid salt as a purifying agent to a rare earth feed liquid, stirring and mixing, adding a precipitating agent, filtering, and obtaining a purified feed liquid; the purifying agent includes citric acid or a citrate; the precipitating agent includes a carbonate; The purified liquid is continuously added with carbonate precipitant under stirring to precipitate the rare earth in the form of carbonate, and is placed at 20-80°C for aging and crystallization, filtered, washed, and dried to obtain a rare earth-containing carbonate precipitate; The rare earth carbonate precipitate is calcined at 900-1000°C to obtain high-purity rare earth oxide.

2. The method for preparing high-purity rare earth carbonates and oxides according to claim 1, characterized in that: When the precipitant is carbonate, the pH value is adjusted to 3.3-4.6 during the pre-impurity removal process.

3. The method for preparing high-purity rare earth carbonates and oxides according to claim 1, characterized in that: When the precipitant is carbonate, the pH of the reaction liquid prepared by adding the precipitant and stirring the reaction is 5.6-7.

3.

4. The method for preparing high-purity rare earth carbonates and oxides according to claim 1, characterized in that: The rare earth solution includes at least one of a rare earth chloride solution and a rare earth nitrate solution.

5. The method for preparing high-purity rare earth carbonates and oxides according to claim 1, characterized in that: In the process of adding organic acid or organic acid salt as a purifying agent into the rare earth liquid, the molar ratio of the purifying agent to the aluminum and iron in the rare earth liquid is 0%-2.8%.

6. The method for preparing high-purity rare earth carbonates and oxides according to claim 1, characterized in that: The reaction liquid is placed in a process of aging and crystallization at 20-80°C, and the duration of the aging and crystallization is 05-8h.

Citation Information

Patent Citations

  • Cerium oxide crystal preparation method and applications of cerium oxide crystal in chemical mechanical polishing liquid

    CN108249468A

Cited By

  • Method for improving filter pressing sintering yield of rare earth carbonate

    CN122406002A

  • Method for improving the filtration and calcination yield of rare earth carbonates

    CN122406002B