Porous manganese lithium ion sieve precursor as well as preparation method and application thereof

Through spray thermal decomposition and low-temperature sintering process, a porous manganese lithium ion sieve precursor was prepared, which solved the problem of poor lithium ion sieve performance, achieved efficient adsorption and good circulation performance, simplified the process flow and reduced costs .

CN118978182AActive Publication Date: 2024-11-19江西云威新材料股份有限公司 +1

Patent Information

Application Number
CN202410990518.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-19
Estimated Expiration
2044-07-23

Smart Images

  • Figure CN118978182A_ABST
    Figure CN118978182A_ABST
Patent Text Reader

Abstract

The invention provides a porous manganese lithium ion sieve precursor as well as a preparation method and application thereof, and belongs to the technical field of preparation of lithium ion sieves. The method comprises the following steps: pyrolyzing a manganese salt solution into a manganese-oxygen mixture by a spray pyrolysis method; carrying out low-temperature sintering on the manganese-oxygen mixture in an air atmosphere to form a nano-porous precursor Mn2O3; mixing and grinding the nano-porous precursor Mn2O3 and a lithium salt according to a set proportion, and performing solid-phase calcination to obtain the porous manganese-series lithium ion sieve precursor Li4Mn5O12. And carrying out lithium removal on the Li4Mn5O12 in acid, and drying to obtain the lithium ion sieve H4Mn5O12. The nano porous precursor Mn2O3 is synthesized by using a spray pyrolysis method, and low-temperature sintering of two solid phase processes is combined, so that the Li4Mn5O12 ion sieve precursor keeps the porous morphology and has the characteristics of large specific surface area and uniform particle size, the processes of acid pickling lithium removal and ion sieve lithium adsorption are facilitated, and the adsorption rate is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lithium ion sieve preparation, and particularly relates to a porous manganese-based lithium ion sieve precursor and a preparation method and application thereof. Background Art

[0002] Lithium has unique and excellent physical and chemical properties. It is widely used in energy, aerospace, metallurgy, medical treatment and other fields. It is known as "white oil". The raw materials for industrial preparation of lithium mainly come from salt lake brine and lithium ore. The lithium reserves of salt lake brine are much greater than those of lithium ore. However, compared with lithium ore, lithium extraction from salt lake brine is more difficult and more expensive. Lithium ion sieve adsorption method is a green and environmentally friendly method for lithium extraction with relatively low cost. Lithium ion sieve has good selectivity for lithium and can improve the extraction efficiency of lithium from salt lake brine.

[0003] Since the lithium ion sieve is composed of H + Replace Li in lithium ion sieve precursor + Therefore, the quality of the precursor is directly related to the quality of the lithium ion sieve. Its synthesis is the key to the entire lithium ion sieve preparation process, and there are many methods. 12 It is one of the common manganese-based lithium ion sieve precursors. Due to its high Mn valence, the Mn dissolution loss is low in adsorption practice and has good stability. 12 The main methods for preparing ion sieve precursors include hydrothermal method, molten salt method, solid phase method, etc. The prepared particles have the shapes of rods, spheres, flakes, etc. Among them, the flake and rod-shaped Li4Mn5O 12 The particles have a small specific surface area and a low adsorption rate; spherical particles have a large specific surface area and good lithium adsorption performance, but the current synthesis method is complicated, and the formed particles are easy to agglomerate, the particle size is too large and uneven, and the subsequent lithium ion sieve performance is poor. Summary of the invention

[0004] In view of this, the object of the present invention is to provide a porous manganese-based lithium ion sieve precursor and a preparation method and application thereof, aiming to solve at least one technical problem in the background technology.

[0005] The present invention is achieved in that:

[0006] The first aspect of the present invention provides a method for preparing a porous manganese-based lithium ion sieve precursor, comprising the following steps:

[0007] The manganese salt solution is pyrolyzed into a manganese-oxygen mixture by a spray pyrolysis method;

[0008] The manganese-oxygen mixture is sintered at low temperature in an air atmosphere to form a nanoporous precursor Mn2O3;

[0009] The nanoporous precursor Mn2O3 and lithium salt are mixed and ground according to a set ratio, and the porous lithium-rich manganese oxide Li4Mn5O is obtained after solid phase calcination. 12 , which is a porous manganese-based lithium ion sieve precursor;

[0010] Wherein, oxygen is used as the carrier gas in the spray thermal decomposition method; the amount of the lithium salt exceeds the theoretical amount;

[0011] Furthermore, the spray pyrolysis method has a temperature of 650°C to 950°C, a pyrolysis time of 5h to 10h, and a gas flow rate of 2L / min to 8L / min.

[0012] Furthermore, the low-temperature sintering temperature is 200° C. to 500° C., and the sintering time is 2 h to 5 h.

[0013] Furthermore, the solid phase calcination temperature is 300° C. to 700° C., the calcination time is 10 h to 24 h, and the solid phase calcination atmosphere is oxygen or air.

[0014] Furthermore, the manganese salt solution adopts at least one of manganese chloride, manganese sulfate, manganese acetate and manganese nitrate solution.

[0015] Furthermore, the lithium salt is selected from at least one of lithium chloride, lithium hydroxide, lithium nitrate and lithium carbonate; in terms of molar ratio, the nanoporous precursor Mn2O3 and the lithium salt have a Mn:Li ratio of 5:4 to 4.1.

[0016] The second invention of the present invention provides a porous manganese-based lithium ion sieve precursor, which is prepared by the above preparation method.

[0017] The third aspect of the present invention provides an application of a porous manganese-based lithium ion sieve precursor for preparing a porous manganese-based lithium ion sieve, specifically: the porous lithium-rich manganese oxide Li4Mn5O 12 Lithium is removed in acid and dried to obtain lithium ion sieve H4Mn5O 12 .

[0018] Furthermore, the acid is formic acid, nitric acid, hydrochloric acid, sulfuric acid, phosphoric acid or sulfurous acid, the acid concentration is 0.1 mol / L to 1 mol / L, and the acid elution lithium time is 0.5h to 3h.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] 1. The present invention uses spray pyrolysis to synthesize nanoporous precursor Mn2O3, combined with two solid-phase processes of low-temperature sintering to make Li4Mn5O 12 The ion sieve precursor maintains a porous morphology, has the characteristics of large specific surface area and uniform particle size, which is beneficial to the process of acid elution of lithium and ion sieve adsorption of lithium, and improves the adsorption rate.

[0021] 2. Li4Mn5O synthesized by the present invention 12 Ion sieve precursor, in which the high-valent Mn reduces the Mn dissolution loss during the pickling process and has good cycle performance.

[0022] 3. The synthesis method provided by the present invention has the advantages of short process, simple operation, low cost, and green environmental protection, and has considerable industrial application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 A flow chart for preparing a lithium ion sieve according to the present invention;

[0024] Figure 2 XRD diagram of the precursor Mn2O3 prepared in Examples 1 to 5 of the present invention;

[0025] Figure 3 This is a SEM image of Mn2O3 prepared in Example 2 of the present invention;

[0026] Figure 4 The porous lithium-rich manganese oxide Li4Mn5O prepared in Examples 1 to 5 of the present invention 12 XRD pattern of . DETAILED DESCRIPTION

[0027] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific implementation cases described herein are only used to explain the present invention and are not used to limit the present invention.

[0028] A method for preparing a porous manganese-based lithium ion sieve precursor comprises the following steps:

[0029] S1. Pyrolyzing a manganese salt solution into a manganese-oxygen mixture by a spray pyrolysis method;

[0030] Dissolve manganese salts such as manganese chloride, manganese sulfate, manganese acetate, and manganese nitrate in water to form a manganese salt solution;

[0031] The manganese salt solution is placed in a spray pyrolysis furnace, and oxygen is introduced at a gas flow rate of 2 to 8 L / min, heated to 650 to 950° C., and kept warm for 5 to 10 hours to pyrolyze the manganese salt into a manganese-oxygen mixture;

[0032] The pyrolysis temperature is selected to be 650-950°C. On the one hand, a larger proportion of Mn2O3 can be formed; on the other hand, Mn2O3 can remain stable within this temperature range; the specific temperature selection in the following embodiments can be adjusted according to the type of manganese salt.

[0033] S2, sintering the manganese-oxygen mixture at 200-500° C. for 2-5 h in an air atmosphere to form a nanoporous precursor Mn2O3;

[0034] S3, the nanoporous precursor Mn2O3 and lithium salt are mixed and ground according to a set ratio, and the porous lithium-rich manganese oxide Li4Mn5O is obtained after solid phase calcination. 12 ,

[0035] The lithium salt is selected from at least one of lithium chloride, lithium hydroxide, lithium nitrate and lithium carbonate, and since the lithium salt is easily volatile during high-temperature calcination, the amount of lithium salt used exceeds the theoretical amount. Specifically, according to the molar ratio, the nanoporous precursor Mn2O3 and the lithium salt have a Mn:Li ratio of 5:4 to 4.1;

[0036] The solid phase calcination temperature is 300-700° C., the calcination time is 10-24 hours, the solid phase calcination atmosphere is oxygen or air, and the product obtained after calcination is a porous manganese-based lithium ion sieve precursor.

[0037] The manganese-based lithium ion sieve precursor prepared by the above method maintains a porous morphology and has the characteristics of large specific surface area and uniform particle size. These morphological characteristics are conducive to the process of acid elution of lithium and ion sieve adsorption of lithium, and improve the adsorption rate.

[0038] The porous manganese-based lithium ion sieve precursor was used to prepare the lithium ion sieve. 12 Lithium is removed in acid and dried to obtain lithium ion sieve H4Mn5O 12 The acid used is formic acid, nitric acid, hydrochloric acid, sulfuric acid, phosphoric acid or sulfurous acid, the acid concentration is 0.1-1 mol / L, and the acid elution lithium time is 0.5-3h.

[0039] Example 1

[0040] A method for preparing a porous manganese-based lithium ion sieve, the process of which is as follows Figure 1 As shown, the steps are as follows:

[0041] (1) preparing 500 mL of a 0.6 mol / L MnCl2 solution, placing the MnCl2 solution in a three-head atomizer for pyrolysis at an oxygen flow rate of 2 L / min, the pyrolysis temperature being 800° C., the pyrolysis time being 6 h, and obtaining manganese oxide;

[0042] (2) The manganese oxide was placed in a tube furnace and heated to 450°C at a heating rate of 5°C / min under air atmosphere and kept at this temperature for 4 hours. After natural cooling, the precursor Mn2O3 was obtained. The XRD characterization results are shown in FIG. Figure 2 , the physical phase conforms to the characteristic spectrum of Mn2O3. The precursor particles are loose and porous;

[0043] (3) Mn2O3 and LiOH·H2O were mixed and ground, and the stoichiometric ratio was maintained at Mn:Li=5:4.05 according to the molar ratio. The temperature was raised to 500°C and kept for 18 h under an oxygen atmosphere to obtain Li4Mn5O 12 As a porous manganese-based lithium ion sieve precursor, the XRD characterization results are as follows Figure 4 ;

[0044] (4) Li4Mn5O 12 The ion sieve precursor was washed with 0.15 mol / L hydrochloric acid for 1 h to obtain H4Mn5O 12 After washing and drying, a porous manganese-based lithium ion sieve is obtained.

[0045] Example 2

[0046] A method for preparing a porous manganese-based lithium ion sieve, the process of which is as follows Figure 1 As shown, the steps are as follows:

[0047] (1) preparing 500 mL of a 0.6 mol / L MnCl2 solution, placing the MnCl2 solution in a three-head atomizer for pyrolysis at an oxygen flow rate of 4 L / min, the pyrolysis temperature of which was 800° C., and the pyrolysis time of which was 6 h, to obtain manganese oxide;

[0048] (2) The manganese oxide was placed in a tube furnace and heated to 450°C at a heating rate of 5°C / min under air atmosphere and kept at this temperature for 4 hours. After natural cooling, the precursor Mn2O3 was obtained. The XRD characterization results are shown in FIG. Figure 2 The physical phase conforms to the characteristic spectrum of Mn2O3, and its SEM image is as follows Figure 3 As shown, Figure 3 The scale bars in A and B are 1 μm and 10 μm, respectively, and the precursor particles are loose and porous;

[0049] (3) Mn2O3 and LiCl were mixed and ground, and the stoichiometric ratio was maintained at Mn:Li=5:4.1 according to the molar ratio. The temperature was raised to 500°C and kept for 18 h under an oxygen atmosphere to obtain Li4Mn5O 12 As the XRD characterization results of porous manganese lithium ion sieve precursor are as follows Figure 4 ;

[0050] (4) Li4Mn5O 12 The ion sieve precursor was washed with 0.15 mol / L hydrochloric acid for 1 h to obtain H4Mn5O 12 After washing and drying, a porous manganese-based lithium ion sieve is obtained.

[0051] Example 3

[0052] A method for preparing a porous manganese-based lithium ion sieve, the process of which is as follows Figure 1 As shown, the steps are as follows:

[0053] (1) preparing 500 mL of a 0.6 mol / L MnCl2 solution, placing the MnCl2 solution in a three-head atomizer for pyrolysis at an oxygen flow rate of 6 L / min, the pyrolysis temperature being 800° C., the pyrolysis time being 6 h, and obtaining manganese oxide;

[0054] (2) The manganese oxide was placed in a tube furnace and heated to 450°C at a heating rate of 5°C / min under air atmosphere and kept at this temperature for 4 hours. After natural cooling, Mn2O3 was obtained. The XRD characterization results are shown in FIG. Figure 2 , the phase conforms to the characteristic spectrum of Mn2O3, and the precursor particles are loose and porous;

[0055] (3) Mn2O3 and Li2NO3 were mixed and ground, and the stoichiometric ratio was maintained at Mn:Li=5:4.07 according to the molar ratio, and the temperature was raised to 500°C in an oxygen atmosphere and kept for 18 h to obtain Li4Mn5O 12 As a porous manganese-based lithium ion sieve precursor, the XRD characterization results are as follows Figure 4 ;

[0056] (4) Li4Mn5O 12 The ion sieve precursor was washed with 0.15 mol / L nitric acid for 1 h to obtain H4Mn5O 12 After washing and drying, a porous manganese-based lithium ion sieve is obtained.

[0057] Example 4

[0058] A method for preparing a porous manganese-based lithium ion sieve, the process of which is as follows Figure 1 As shown, the steps are as follows:

[0059] (1) preparing 500 mL of a 0.6 mol / L MnSO4 solution, placing the MnSO4 solution in a three-head atomizer for pyrolysis at an oxygen flow rate of 4 L / min, the pyrolysis temperature being 950° C., the pyrolysis time being 8 h, and obtaining manganese oxide;

[0060] (2) The manganese oxide was placed in a tube furnace and heated to 400°C at a heating rate of 5°C / min under air atmosphere and kept at a constant temperature for 3 h. After natural cooling, loose and porous precursor Mn2O3 particles were obtained. The XRD characterization results are shown in Figure 2 ;

[0061] (3) Mn2O3 and Li2CO3 were mixed and ground, and the stoichiometric ratio was maintained at Mn:Li=5:4.1 according to the molar ratio, and the temperature was raised to 500°C in an oxygen atmosphere and kept for 20 h to obtain Li4Mn5O 12 As a porous manganese-based lithium ion sieve precursor, the XRD characterization results are as follows Figure 4 ;

[0062] (4) Li4Mn5O 12 The ion sieve precursor was washed with 1 mol / L formic acid for 3 h to obtain H4Mn5O 12 After washing and drying, a porous manganese-based lithium ion sieve is obtained.

[0063] Example 5

[0064] A method for preparing a porous manganese-based lithium ion sieve, the process of which is as follows Figure 1 As shown, the steps are as follows:

[0065] (1) preparing 500 mL of a 0.6 mol / L Mn(Ac)2 solution, placing the Mn(Ac)2 solution in a three-head atomizer for pyrolysis at an oxygen flow rate of 4 L / min, the pyrolysis temperature being 650° C., the pyrolysis time being 5 h, and obtaining manganese oxide;

[0066] (2) The manganese oxide was placed in a tube furnace and heated to 450°C at a heating rate of 5°C / min under air atmosphere and kept at this temperature for 3 h. After natural cooling, loose and porous precursor Mn2O3 particles were obtained. The XRD characterization results are shown in FIG. Figure 2 ;

[0067] (3) Mn2O3 and LiOH·H2O were mixed and ground, and the stoichiometric ratio was maintained at Mn:Li=5:4 according to the molar ratio. The temperature was raised to 300°C and kept for 15 h under an oxygen atmosphere to obtain Li4Mn5O 12 As a porous manganese-based lithium ion sieve precursor, the XRD characterization results are as follows Figure 4 ;

[0068] (4) Li4Mn5O 12 The ion sieve precursor was washed with 0.5 mol / L phosphoric acid for 3 h to obtain H4Mn5O 12 After washing and drying, a porous manganese-based lithium ion sieve is obtained.

[0069] Comparative Example 1

[0070] This comparative example prepares a manganese-based lithium ion sieve, and the difference between its steps and those of Example 2 is only in step (1);

[0071] Step (1) of this comparative example is: placing MnCl2 solid in a pyrolysis furnace for pyrolysis at a temperature of 800°C for 6 hours. The remaining steps and parameters are the same as those of Example 2.

[0072] The performance tests of the lithium ion sieve precursor and the ion sieve obtained in Examples 1 to 5 and Comparative Example 1 were performed, including:

[0073] 1. Characterization analysis

[0074] The specific surface area and pore structure of the material were analyzed by a fully automatic specific surface and porosity analyzer (BET). The adsorbed gas was nitrogen. The surface area and pore structure of the material were measured. The specific surface area, average pore size and pore volume of the lithium ion sieve material were calculated based on the test results. The results are shown in Table 1 below.

[0075] Table 1

[0076]

[0077]

[0078] The precursor in Table 1 refers to a manganese-based lithium ion sieve precursor. As can be seen from Table 1 above, the specific surface area and pore volume of the ion sieve precursor prepared in the embodiment of the present invention are significantly larger than those of the comparative example, while the average pore size is significantly smaller than that of the comparative example.

[0079] 2. Determination of adsorption capacity

[0080] 0.25g lithium ion sieve was added into 0.5L lithium solution (Li concentration was 50mg / L), and mechanically stirred at 500r / min at room temperature. Samples were taken at different adsorption times, once every 10min, and the Li in the liquid phase was measured by inductively coupled plasma emission spectrometry. + The concentration was measured and the adsorption amount q can be calculated using the following formula:

[0081] q=V(C0-C) / m

[0082] C0 is Li + Initial concentration mg / L; C is Li at the time of measurement + Concentration mg / L, V is the volume of lithium-containing solution L, and m is the amount of lithium ion sieve used in g.

[0083] As time goes by, + When the concentration does not change or the change is not obvious, the adsorption amount reaches saturation. The adsorption amount results of the lithium ion sieves prepared in various embodiments and comparative examples are shown in Table 2 below.

[0084] Table 2

[0085]

[0086] It can be seen from Table 2 that the adsorption capacity of lithium ions by the lithium ion sieves prepared in the embodiments of the present invention is above 35.7 mg / g, which is much higher than the adsorption capacity of Comparative Example 1, and the time to reach the saturated adsorption capacity is not much different. It can be seen that the adsorption efficiency of the lithium ion sieves in the embodiments of the present invention is better than that in Comparative Example 1.

[0087] 3. Cycle performance

[0088] (1) 0.25 g of lithium ion sieve was added to 0.5 L of lithium-containing solution (Li concentration was 50 mg / L), mechanically stirred at 500 r / min for 4 h at room temperature, and samples were taken to measure the adsorption capacity;

[0089] (2) solid-liquid separation after standing to obtain the adsorbed lithium ion sieve;

[0090] (3) washing the lithium ion sieve with 1.5 mol / L hydrochloric acid for 2 h to obtain a lithium ion sieve;

[0091] (4) The above steps (1) to (3) are repeated about 20 times, the amount of lithium adsorbed by the lithium ion sieve is calculated each time, and the recycling performance of the lithium ion sieve is analyzed.

[0092] Table 3

[0093]

[0094] According to calculation, when the lithium ion sieves prepared in Examples 1 to 5 were cycled for less than 5 times, the adsorption amount decreased by less than 10%; when the number of cycles increased to 20 times, the adsorption amount decreased by about 25%;

[0095] The lithium ion sieve prepared in Comparative Example 1 has a similar reduction ratio in adsorption capacity as that in Example 2 when the number of cycles is small (less than 5 times). However, as the number of cycles increases (more than 10 times), the adsorption capacity decreases significantly, and the reduction ratio is basically more than 30%. After 15 cycles, the adsorption capacity decreases very rapidly, and the adsorption effect decreases significantly.

[0096] 4. Mn dissolution test

[0097] The lithium ion sieve before adsorption and extraction of lithium is digested and the Mn ion concentration is measured, and then the Mn dissolution rate is calculated. The specific operation is as follows;

[0098] (1) Determination of the Mn ion concentration in the ion sieve: 0.050 g of the ion sieve was weighed and dissolved in 20 mL of HCl solution (6 mol / L) containing a few drops of 30% H2O2, and the Mn was dissolved by stirring. The volume was fixed to form a digestion solution, and the Mn ion concentration was determined by inductively coupled plasma emission spectrometry;

[0099] (2) 0.050 g of lithium ion sieve was added to 0.1 L of lithium-containing solution (Li concentration was 50 mg / L) and mechanically stirred at 500 r / min for 3 h at room temperature. During the stirring process, the lithium ion sieve + After the adsorption is completed, the MnMn ion concentration in the adsorption residual liquid is measured;

[0100] The dissolution loss of Mn D is calculated by the following formula: Mn :

[0101] D Mn (%) = V 吸 *C 吸 / (V 消 *C 消 )

[0102] C 吸 is the Mn ion concentration in the adsorption residual solution mg / L, V 吸 is the adsorption residual liquid volume L; C 消 is the Mn ion concentration in the digestion solution mg / L, V 消 is the volume of digestion solution L; the calculation results are shown in Table 4 below.

[0103] Table 4

[0104]

[0105] It can be seen from Table 4 that the Mn dissolution rate of the manganese-based ion sieve prepared in the embodiment of the present invention is relatively small, all lower than 3.1%, which is lower than that of Comparative Example 1.

[0106] 5. Selective adsorption experiment

[0107] Add interfering metal ions, such as Na, to 0.5L of lithium-containing solution. + , Ca 2+ Mg 2+ , K + etc., interfering ions and Li + The initial concentration was 50 mg / L. 0.25 g of lithium ion sieve was added for selective adsorption experiments. The mechanical stirring speed was 500 r / min, the stirring time was 3 h, and adsorption was carried out at room temperature. Then the concentration of each ion was measured and the adsorption amount of each ion was calculated. The results are shown in Table 5 below.

[0108] Table 5

[0109]

[0110] It can be seen from Table 5 that Na + , Ca 2+ Mg 2+ , K + Plasma adsorption of Li by the lithium ion sieve of the embodiment of the present invention + The degree of process interference is low, and the degree of interference to comparative example 1 is higher than that to example 2; the lithium ion sieve prepared by the embodiment of the present invention has a high + Has excellent selection performance.

[0111] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing a porous manganese-based lithium ion sieve precursor, characterized in that: The preparation method comprises the following steps: The manganese salt solution is pyrolyzed into a manganese-oxygen mixture by a spray pyrolysis method; The manganese-oxygen mixture is sintered at low temperature in an air atmosphere to form a nanoporous precursor Mn2O3; The nanoporous precursor Mn2O3 and lithium salt are mixed and ground according to a set ratio, and the porous lithium-rich manganese oxide Li4Mn5O is obtained after solid phase calcination. 12 , which is a porous manganese-based lithium ion sieve precursor; Wherein, oxygen is used as the carrier gas in the spray thermal decomposition method; and the amount of the lithium salt used exceeds the theoretical amount.

2. The method for preparing a porous manganese-based lithium ion sieve precursor according to claim 1, characterized in that: The spray pyrolysis method has a temperature of 650° C. to 950° C., a pyrolysis time of 5 h to 10 h, and a gas flow rate of 2 L / min to 8 L / min.

3. The method for preparing a porous manganese-based lithium ion sieve precursor according to claim 1, characterized in that: The low-temperature sintering temperature is 200° C. to 500° C. and the sintering time is 2 h to 5 h.

4. The method for preparing a porous manganese-based lithium ion sieve precursor according to claim 1, characterized in that: The solid phase calcination temperature is 300° C. to 700° C., the calcination time is 10 h to 24 h, and the solid phase calcination atmosphere is oxygen or air.

5. The method for preparing a porous manganese-based lithium ion sieve precursor according to claim 1, characterized in that: The manganese salt solution is at least one of manganese chloride, manganese sulfate, manganese acetate and manganese nitrate solution.

6. The method for preparing a porous manganese-based lithium ion sieve precursor according to claim 1 or 5, characterized in that: The lithium salt is selected from at least one of lithium chloride, lithium hydroxide, lithium nitrate and lithium carbonate; According to the molar ratio, the nanoporous precursor Mn2O3 and the Mn:Li in the lithium salt are 5:4-4.

1.

7. A porous manganese-based lithium ion sieve precursor, characterized in that: The porous manganese-based lithium ion sieve precursor is prepared by the preparation method described in any one of claims 1 to 6.

8. An application of a porous manganese-based lithium ion sieve precursor, characterized in that: The porous manganese-based lithium ion sieve precursor obtained by the preparation method according to any one of claims 1 to 6 is used to prepare a porous manganese-based lithium ion sieve.

9. The use according to claim 8, characterized in that: The porous lithium-rich manganese oxide Li4Mn5O 12 Lithium is removed in acid and dried to obtain lithium ion sieve H4Mn5O 12 .

10. The use according to claim 8, characterized in that: The acid is formic acid, nitric acid, hydrochloric acid, sulfuric acid, phosphoric acid or sulfurous acid, the acid concentration is 0.1 mol / L to 1 mol / L, and the acid elution lithium time is 0.5h to 3h.

Citation Information

Patent Citations

  • Manganese bioxide ionic sieve

    CN101157480A

  • Method for preparing cubic phase Li4Mn5O12

    CN103204545A

  • Method for preparing flaky Li4Mn5Ol2 ionic sieve precursor and ionic sieve

    CN109384262A

  • Spherical manganese-based lithium ionic sieve and preparation method thereof

    CN110451570A

  • Preparation method of lithium ion battery cathode Li4Mn5O12 nanoparticles

    CN110790315A

Cited By

  • Multilayer pre-alkalization nanofiber-based photo-thermal lithium ion sieve as well as preparation method and application thereof

    CN121133232A