Preparation method of ultra-small particle precursor with high sphericity degree
Through the wet process and control of precipitation conditions, high spherical and high consistency ternary precursor particles with D50=1.5-2.1um were prepared, which solved the problem of poor particle density and dispersion in the existing technology and improved ternary lithium Performance of the positive electrode material of ion battery.
Patent Information
- Application Number
- CN202410330644.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-22
- Publication Date
- 2024-11-19
AI Technical Summary
In the prior art, the precursor particle tap density of the positive electrode material of the ternary lithium-ion battery has low density, poor dispersion, and poor spherical shape, which affects product performance, and it is difficult to achieve high consistency and high spherical shape in small particles.
Using the wet process, a mixed metal salt solution is prepared by soluble nickel salt, cobalt salt and manganese salt, combined with sodium hydroxide and ammonia water for coprecipitation, and the particle growth conditions such as pH and temperature are controlled to achieve a high spherical shape of D50=1.5-2.1um Preparation of high consistency particles.
It improves the dispersion and density of particles, enhances spherical degree and consistency, solves the problems of tap density and proportional table, and improves product performance.
Smart Images

Figure CN118978189A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of new energy lithium battery cathode material technology, specifically a method for preparing a precursor with high sphericity and ultra-small particle size. Background Technology
[0002] In recent years, the new energy lithium battery industry has developed rapidly, especially ternary materials, which have received unprecedented development and attention. This is mainly attributed to their advantages such as high capacity, good cycle performance, and good rate performance. As the core material at the upper end of ternary cathode materials, the ternary precursor has a significant impact on the performance of cathode materials. Currently, high capacity, good cycle performance, high safety, and high rate performance are the development trends of ternary materials.
[0003] The publication number "CN108946827B" discloses an ultra-small particle size nickel-cobalt-manganese hydroxide and its preparation method. Although this method produces a precursor with D50 < 2.0 μm, the tap density of the product is low, generally less than 1.20 g / cm³. 3 Compared with this patent, the particle dispersibility and sphericity are poor, and there are problems such as serious secondary particle agglomeration, uneven particle size, and poor consistency of primary particles.
[0004] In actual production, to improve the energy density and cycle performance of ternary lithium-ion batteries, the precursor needs to have higher tap density, higher strength, and higher nickel content. Currently, a mainstream process is to use a bimodal particle size distribution by mixing particles of different sizes. However, even small particles typically achieve a D50 > 2.5µm. Smaller particles lead to problems such as poor sphericity, poor dispersibility, and low tap density, which in turn affect product performance.
[0005] To overcome the shortcomings of the aforementioned patents, this patent provides a wet process with a short process flow and simple operation. It allows for control of ultra-small particle sizes within the range of 1.5-2.1 μm, high primary particle uniformity, high secondary particle dispersibility and sphericity, and low tap density (1.00-1.80 g / cm³) and specific surface area (8-45 μm). 2 / g) A method for preparing ternary precursors with controllable operation. Summary of the Invention
[0006] The purpose of this invention is to provide a method for preparing a precursor with high sphericity and ultra-small particles, so as to solve the problems mentioned in the background art.
[0007] To achieve the above objectives, the present invention provides the following technical solution:
[0008] A method for preparing a precursor with high sphericity and ultra-small particles involves using soluble nickel salt, cobalt salt, and manganese salt as raw materials. A mixed metal salt solution is prepared according to the desired molar ratio of nickel, cobalt, and manganese in the nickel-cobalt-manganese hydroxide, wherein the molar ratio of nickel, cobalt, and manganese is 0.70≤x≤0.90, 0.05≤y≤0.20, and 0.01≤z≤0.10. Sodium hydroxide solution is used as a precipitant, and ammonia water is used as a complexing agent to achieve the co-precipitation of nickel, cobalt, and manganese elements.
[0009] Includes the following steps,
[0010] S1. Solution preparation: Prepare nickel cobalt manganese salt solution, sodium hydroxide solution and ammonia solution;
[0011] S2. Pretreatment: Introduce submerged nitrogen protective gas into the sealed main reactor, and at the same time add pure water to the main reactor to cover the upper edge of the upper stirring blades, and start stirring;
[0012] S3. Preparation of the base solution: Add complexing agent ammonia water and sodium hydroxide solution to the main reactor in sequence to adjust the ammonia value and pH of the system, which serve as the base solution and starting conditions for the reaction.
[0013] S4. Adjust the atmosphere of the reactor: to prevent the oxidation of particles;
[0014] S5. Precipitation Mixing: Add nickel cobalt manganese salt solution, sodium hydroxide solution, and ammonia solution to the reaction vessel simultaneously while maintaining the flow of inert gas to induce precipitation.
[0015] S6. Seed crystal generation and growth in slurry: Lowering the pH of the reaction system while increasing the temperature facilitates the development and growth of particles; low pH is conducive to particle growth, while high temperature is conducive to the perfect stacking of particle crystals.
[0016] S7. Cleaning and Concentration: After the main vessel is full, the overflow valve is opened to overflow into the secondary vessel. After the secondary vessel is submerged by the built-in filter element, the cleaning valve is opened to concentrate the contents.
[0017] S8. Slurry aging and washing: The slurry is placed in an aging tank for aging, and then the slurry in the aging tank is pumped into a washing device for washing.
[0018] S9. Drying and Shaping: The washed ternary precursor filter cake is placed in an oven and dried to obtain the ternary precursor. Then, the dried material is sieved and demagnetized to obtain the corresponding precursor finished product.
[0019] Preferably, the solution preparation includes: preparing a nickel-cobalt-manganese salt solution, a sodium hydroxide solution, and an ammonia solution, specifically including:
[0020] Prepare a nickel-cobalt-manganese salt solution with a metal ion concentration of 1-2.5 mol / L, a sodium hydroxide solution with a concentration of 8-15 mol / L, and an ammonia solution with a concentration of 100-150 g / L.
[0021] Preferably, the pretreatment involves: introducing submerged nitrogen protective gas into the sealed main reactor, simultaneously adding pure water to the main reactor to cover the upper edge of the upper stirring blades, and starting the stirring process, specifically including:
[0022] Introduce submerged nitrogen protective gas into the sealed main reactor for 1-3 hours at a flow rate of 300-600 L / h. During the process, add pure water to the main reactor to cover the upper edge of the upper stirring blades, start stirring at 500-650 rpm, and control the temperature at 35-45℃.
[0023] Preferably, the base solution is prepared by successively adding ammonia water and sodium hydroxide solution as complexing agents to the main reactor to adjust the ammonia value and pH of the system, serving as the base solution and starting condition for the reaction. Specifically, this includes:
[0024] Add ammonia water as a complexing agent to the main reactor sequentially, controlling the ammonia value at 1.0-3.0 g / L. Add sodium hydroxide solution to adjust the pH of the system to 12.0-13.0, which serves as the base liquid and starting condition for the reaction.
[0025] Preferably, the atmosphere of the reaction vessel is adjusted to prevent particle oxidation, specifically including:
[0026] After the above S1 and S3 conditions are prepared, adjust the atmosphere of the reactor to 300-600 L / h of lower nitrogen and 100-300 L / h of upper nitrogen, and avoid particle oxidation throughout the process.
[0027] Preferably, precipitation mixing involves simultaneously adding a nickel-cobalt-manganese salt solution, a sodium hydroxide solution, and an ammonia solution to the reaction vessel while maintaining the flow of an inert gas to induce precipitation. Specifically, this includes:
[0028] Nickel-cobalt-manganese salt solution, sodium hydroxide solution, and ammonia solution were simultaneously added to the reactor while maintaining the flow of inert gas. During this process, the pH of the system was maintained at 12.0-13.0, and the ammonia value at 1.0-3.0 g / L. The co-precipitation synthesis was then started.
[0029] Preferably, the generation and growth of slurry seed crystals involves lowering the pH of the reaction system while simultaneously increasing the temperature to improve the efficiency of particle development and growth, specifically including:
[0030] After maintaining the above S4 conditions for 60-240 minutes, the desired seed crystals are generated. To further promote the growth of this seed crystal slurry, the pH of the reaction system is lowered. The process involves a gradual decrease in pH to between 10.40 and 11.60, taking 4-10 hours. This is because directly shutting off the alkali solution would cause a rapid pH drop, leading to excessively fast growth and particle agglomeration. Once the pH is reached, the temperature is raised to 45-60℃ to improve the efficiency of particle development and growth.
[0031] Preferably, the clarification and concentration process is as follows: After the main vessel is full, the overflow valve is opened to overflow into the secondary vessel. Once the secondary vessel has submerged its built-in filter element, the clarification process is initiated for concentration, specifically including:
[0032] Two hours before the main reactor is full, start the secondary reactor with nitrogen at a flow rate of 300-600 L / h to replace the air inside. After the main reactor is full, open the overflow valve to overflow into the secondary reactor. Once the secondary reactor has submerged the built-in filter, start the discharge valve for concentration. During this process, adjust the discharge rate according to the liquid levels in the main and secondary reactors to maintain the stability of the system.
[0033] Preferably, the pulp aging and washing process involves: placing the pulp in an aging tank for aging, and then pumping the pulp from the aging tank into a washing device for washing, specifically including:
[0034] When the reaction particle size D50 = 1.5-2.1 μm, the reaction ends and the machine is stopped. Nitrogen gas is retained. After the machine is stopped for 30-150 minutes, the particle size is retested and no abnormality is found. The slurry is then placed in an aging tank for aging, to be used for washing. After that, the slurry in the aging tank is pumped into the washing equipment and washed with a sodium hydroxide solution with a concentration of 30-80 g / L.
[0035] Preferably, the drying and shaping process involves placing the washed ternary precursor filter cake in an oven to dry it, obtaining the ternary precursor. The dried material is then sieved and demagnetized to obtain the corresponding finished precursor product, specifically including:
[0036] The washed ternary precursor filter cake was placed in an oven for static drying. Once the moisture content was within acceptable limits, the drying process was complete, yielding a filter cake with high primary particle uniformity, high secondary particle dispersibility and sphericity, and a tap density (1.00-1.80 g / cm³) and specific surface area (8-45 μm). 2 / g) The ternary precursor is controlled by operation. Finally, the dried material is sieved and demagnetized to obtain the corresponding precursor product for use in cathode sintering.
[0037] Compared with the prior art, the beneficial effects of the present invention are:
[0038] This invention improves particle uniformity by employing a low-temperature granulation process to enhance particle dispersibility and a higher growth pH. Extending the reaction time increases the granulation pH or time. Furthermore, by controlling the thickness of the primary particle morphology, and while maintaining a constant ammonia value, the thickness in the 001 direction and whisker uniformity are adjusted by increasing the pH during the growth process. As the growth pH increases, sphericity gradually improves, particle density, whisker uniformity, and thickness gradually increase, resulting in a corresponding increase in tap density and a decrease in specific surface area, thereby solving the problems mentioned in the background art. Attached Figure Description
[0039] Figure 1This is a SEM image of the ternary precursor obtained in Example 1 of the present invention;
[0040] Figure 2 This is a particle size distribution diagram of the ternary precursor obtained in Example 1 of the present invention;
[0041] Figure 3 This is a SEM image of the ternary precursor obtained in Example 2 of the present invention;
[0042] Figure 4 This is a particle size distribution diagram of the ternary precursor obtained in Example 2 of the present invention;
[0043] Figure 5 This is a SEM image of the ternary precursor obtained in Example 3 of the present invention;
[0044] Figure 6 This is a particle size distribution diagram of the ternary precursor obtained in Example 3 of the present invention;
[0045] Figure 7 This is a SEM image of the ternary precursor obtained in Example 4 of the present invention;
[0046] Figure 8 This is a particle size distribution diagram of the ternary precursor obtained in Example 4 of the present invention;
[0047] Figure 9 This is a SEM image of the ternary precursor obtained in Comparative Example 1 of the present invention;
[0048] Figure 10 This is a particle size distribution diagram of the ternary precursor obtained in Comparative Example 1 of the present invention;
[0049] Figure 11 This is a SEM image of the ternary precursor obtained in Example 2 according to the present invention;
[0050] Figure 12 This is a particle size distribution diagram of the ternary precursor obtained in Example 2 of the present invention. Detailed Implementation
[0051] The following will clearly and completely describe the technical solutions in the embodiments of the present invention in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of the present invention.
[0052] Example 1:
[0053] A method for preparing a precursor with high sphericity and ultra-small particles includes the following steps:
[0054] S1. Solution preparation: Prepare nickel cobalt manganese salt solution, sodium hydroxide solution and ammonia solution;
[0055] S2. Pretreatment: Introduce submerged nitrogen protective gas into the sealed main reactor, and at the same time add pure water to the main reactor to cover the upper edge of the upper stirring blades, and start stirring;
[0056] S3. Preparation of the base solution: Add complexing agent ammonia water and sodium hydroxide solution to the main reactor in sequence to adjust the ammonia value and pH of the system, which serve as the base solution and starting conditions for the reaction.
[0057] S4. Adjust the atmosphere of the reactor: to prevent the oxidation of particles;
[0058] S5. Precipitation Mixing: Add nickel cobalt manganese salt solution, sodium hydroxide solution, and ammonia solution to the reaction vessel simultaneously while maintaining the flow of inert gas to induce precipitation.
[0059] S6. Seed crystal generation and growth in slurry: Lowering the pH of the reaction system while increasing the temperature facilitates the development and growth of particles; low pH is conducive to particle growth, while high temperature is conducive to the perfect stacking of particle crystals.
[0060] S7. Cleaning and Concentration: After the main vessel is full, the overflow valve is opened to overflow into the secondary vessel. After the secondary vessel is submerged by the built-in filter element, the cleaning valve is opened to concentrate the contents.
[0061] S8. Slurry aging and washing: The slurry is placed in an aging tank for aging, and then the slurry in the aging tank is pumped into a washing device for washing.
[0062] S9. Drying and Shaping: The washed ternary precursor filter cake is placed in an oven and dried to obtain the ternary precursor. Then, the dried material is sieved and demagnetized to obtain the corresponding precursor finished product.
[0063] Preferably, the solution preparation includes: preparing a nickel-cobalt-manganese salt solution, a sodium hydroxide solution, and an ammonia solution, specifically including:
[0064] Prepare a nickel-cobalt-manganese salt solution with a metal ion concentration of 2 mol / L, wherein the molar ratio of nickel, cobalt, and manganese is Ni:Co:Mn = 83:12:5. Prepare a sodium hydroxide solution with a concentration of 10.50 mol / L and an ammonia solution with a concentration of 125 g / L.
[0065] Preferably, the pretreatment involves: introducing submerged nitrogen protective gas into the sealed main reactor, simultaneously adding pure water to the main reactor to cover the upper edge of the upper stirring blades, and starting the stirring process, specifically including:
[0066] Submerged nitrogen protective gas was introduced into the sealed main reactor for 3 hours at a flow rate of 400 L / h. During the process, pure water was added to the main reactor to cover the upper edge of the upper stirring blades. Stirring was started at 600 rpm, and the temperature was controlled at 38℃.
[0067] Preferably, the base solution is prepared by sequentially adding ammonia water and sodium hydroxide solution as complexing agents to the main reactor to adjust the system, which serves as the base solution and starting condition for the reaction. Specifically, this includes:
[0068] Ammonia water, a complexing agent, was added sequentially to the main reactor to control the ammonia value at 1.5 g / L. Sodium hydroxide solution was added to adjust the pH of the system to 12.2 and the ammonia value to 1.50 g / L, which served as the base liquid and starting conditions for the reaction.
[0069] Preferably, the atmosphere of the reaction vessel is adjusted to prevent particle oxidation, specifically including:
[0070] After the above S1 and S3 conditions are prepared, adjust the atmosphere of the reactor to 400 L / h for lower nitrogen and 100 L / h for upper nitrogen, and avoid particle oxidation throughout the process.
[0071] Preferably, precipitation mixing involves simultaneously adding a nickel-cobalt-manganese salt solution, a sodium hydroxide solution, and an ammonia solution to the reaction vessel while maintaining the flow of an inert gas to induce precipitation. Specifically, this includes:
[0072] Nickel-cobalt-manganese salt solution, sodium hydroxide solution, and ammonia solution were simultaneously added to the reactor while maintaining the flow of inert gas. During this process, the pH of the system was maintained at 12.2 and the ammonia value at 1.50 g / L, and the co-precipitation synthesis was started.
[0073] Preferably, the generation and growth of slurry seed crystals involves lowering the pH of the reaction system while simultaneously increasing the temperature to improve the efficiency of particle development and growth, specifically including:
[0074] After maintaining the above S4 conditions for 90 minutes, the desired seed crystals were generated. To further promote the growth of the seed crystal slurry, the pH of the reaction system was lowered. The process involved a gradual decrease in pH to 10.60 over 4 hours. This was primarily because directly shutting off the alkali solution would cause a rapid pH drop, leading to excessively fast growth and particle agglomeration. Once the pH was reached, the temperature was raised to 50°C to improve the efficiency of particle development and growth.
[0075] Preferably, the clarification and concentration process is as follows: After the main vessel is full, the overflow valve is opened to overflow into the secondary vessel. Once the secondary vessel has submerged its built-in filter element, the clarification process is initiated for concentration, specifically including:
[0076] Two hours before the main reactor is full, start the secondary reactor with nitrogen at a flow rate of 400L / h to replace the air inside. After the main reactor is full, open the overflow valve to overflow into the secondary reactor. Once the secondary reactor has submerged the built-in filter, start the discharge valve for concentration. During this process, adjust the discharge rate according to the liquid levels in the main and secondary reactors to maintain the stability of the system.
[0077] Preferably, the pulp aging and washing process involves: placing the pulp in an aging tank for aging, and then pumping the pulp from the aging tank into a washing device for washing, specifically including:
[0078] When the reaction particle size D50 = 1.60 μm, the reaction ends and the machine is stopped. Nitrogen gas is retained. After 60 minutes of shutdown, the particle size is retested and no abnormalities are found. The slurry is then placed in an aging tank for aging, to be used for washing. After that, the slurry in the aging tank is pumped into the washing equipment and washed with a sodium hydroxide solution with a concentration of 40 g / L.
[0079] Preferably, the drying and shaping process involves placing the washed ternary precursor filter cake in an oven to dry it, obtaining the ternary precursor. The dried material is then sieved and demagnetized to obtain the corresponding finished precursor product, specifically including:
[0080] The washed ternary precursor filter cake was placed in an oven for static drying. Once the moisture content was within acceptable limits, the drying process was complete, yielding a filter cake with high primary particle uniformity, high secondary particle dispersibility and sphericity, and a tap density of 1.00 g / cm³. 3 ) and ratio (38.07m) 2 The ternary precursor ( / g) is then processed by sieving and demagnetizing the dried material to obtain the corresponding precursor product, which is then used for cathode sintering.
[0081] The key physicochemical properties of the ternary precursor obtained in Example 1 are shown in Table 1 below:
[0082] Table 1 Key physicochemical properties of the ternary precursor obtained in Example 1
[0083] project D50(um) <![CDATA[BET(m 2 / g)]]> Tap density (g / m3) index 1.604 38.07 1.00
[0084] The SEM images and particle size distributions of the obtained ternary precursors are as follows: Figure 1 and Figure 2 As shown:
[0085] Example 2:
[0086] Includes the following steps,
[0087] S1. Solution preparation: Prepare nickel cobalt manganese salt solution, sodium hydroxide solution and ammonia solution;
[0088] S2. Pretreatment: Introduce submerged nitrogen protective gas into the sealed main reactor, and at the same time add pure water to the main reactor to cover the upper edge of the upper stirring blades, and start stirring;
[0089] S3. Preparation of the base solution: Add complexing agent ammonia water and sodium hydroxide solution to the main reactor in sequence to adjust the ammonia value and pH of the system, which serve as the base solution and starting conditions for the reaction.
[0090] S4. Adjust the atmosphere of the reactor: to prevent the oxidation of particles;
[0091] S5. Precipitation Mixing: Add nickel cobalt manganese salt solution, sodium hydroxide solution, and ammonia solution to the reaction vessel simultaneously while maintaining the flow of inert gas to induce precipitation.
[0092] S6. Seed crystal generation and growth in slurry: Lowering the pH of the reaction system while increasing the temperature facilitates the development and growth of particles; low pH is conducive to particle growth, while high temperature is conducive to the perfect stacking of particle crystals.
[0093] S7. Cleaning and Concentration: After the main vessel is full, the overflow valve is opened to overflow into the secondary vessel. After the secondary vessel is submerged by the built-in filter element, the cleaning valve is opened to concentrate the contents.
[0094] S8. Slurry aging and washing: The slurry is placed in an aging tank for aging, and then the slurry in the aging tank is pumped into a washing device for washing.
[0095] S9. Drying and Shaping: The washed ternary precursor filter cake is placed in an oven and dried to obtain the ternary precursor. Then, the dried material is sieved and demagnetized to obtain the corresponding precursor finished product.
[0096] Preferably, the solution preparation includes: preparing a nickel-cobalt-manganese salt solution, a sodium hydroxide solution, and an ammonia solution, specifically including:
[0097] Prepare a nickel-cobalt-manganese salt solution with a metal ion concentration of 2 mol / L, wherein the molar ratio of nickel, cobalt, and manganese is Ni:Co:Mn = 83:12:5. Prepare a sodium hydroxide solution with a concentration of 10.50 mol / L and an ammonia solution with a concentration of 125 g / L.
[0098] Preferably, the pretreatment involves: introducing submerged nitrogen protective gas into the sealed main reactor, simultaneously adding pure water to the main reactor to cover the upper edge of the upper stirring blades, and starting the stirring process, specifically including:
[0099] Submerged nitrogen protective gas was introduced into the sealed main reactor for 3 hours at a flow rate of 400 L / h. During the process, pure water was added to the main reactor to cover the upper edge of the upper stirring blades. Stirring was started at 600 rpm, and the temperature was controlled at 38℃.
[0100] Preferably, the base solution is prepared by sequentially adding ammonia water and sodium hydroxide solution as complexing agents to the main reactor to adjust the system, which serves as the base solution and starting condition for the reaction. Specifically, this includes:
[0101] Ammonia water, a complexing agent, was added sequentially to the main reactor to control the ammonia value at 1.50 g / L. Sodium hydroxide solution was added to adjust the pH of the system to 12.10, which served as the base liquid and starting condition for the reaction.
[0102] Preferably, the atmosphere of the reaction vessel is adjusted to prevent particle oxidation, specifically including:
[0103] After the above S1 and S3 conditions are prepared, adjust the atmosphere of the reactor to 400 L / h for lower nitrogen and 100 L / h for upper nitrogen, and avoid particle oxidation throughout the process.
[0104] Preferably, precipitation mixing involves simultaneously adding a nickel-cobalt-manganese salt solution, a sodium hydroxide solution, and an ammonia solution to the reaction vessel while maintaining the flow of an inert gas to induce precipitation. Specifically, this includes:
[0105] Nickel-cobalt-manganese salt solution, sodium hydroxide solution, and ammonia solution were simultaneously added to the reactor while maintaining the flow of inert gas. During this process, the pH of the system was maintained at 12.1 and the ammonia value at 1.50 g / L, and the co-precipitation synthesis was started.
[0106] Preferably, the generation and growth of slurry seed crystals involves lowering the pH of the reaction system while simultaneously increasing the temperature to improve the efficiency of particle development and growth, specifically including:
[0107] After maintaining the above S4 conditions for 120 minutes, the desired seed crystals were generated. To further promote the growth of the seed crystal slurry, the pH of the reaction system was lowered. The process involved a gradual decrease in pH to 10.50 over 6 hours. This was primarily because directly shutting off the alkali solution would cause a rapid pH drop, leading to excessively fast growth and particle agglomeration. Once the pH was reached, the temperature was raised to 50°C to improve the efficiency of particle development and growth.
[0108] Preferably, the clarification and concentration process is as follows: After the main vessel is full, the overflow valve is opened to overflow into the secondary vessel. Once the secondary vessel has submerged its built-in filter element, the clarification process is initiated for concentration, specifically including:
[0109] Two hours before the main reactor is full, start the secondary reactor with nitrogen at a flow rate of 400L / h to replace the air inside. After the main reactor is full, open the overflow valve to overflow into the secondary reactor. Once the secondary reactor has submerged the built-in filter, start the discharge valve for concentration. During this process, adjust the discharge rate according to the liquid levels in the main and secondary reactors to maintain the stability of the system.
[0110] Preferably, the pulp aging and washing process involves: placing the pulp in an aging tank for aging, and then pumping the pulp from the aging tank into a washing device for washing, specifically including:
[0111] When the reaction particle size D50 = 2 μm, the reaction ends and the machine is stopped. Nitrogen gas is retained. After 60 minutes of shutdown, the particle size is retested and no abnormalities are found. The slurry is then placed in an aging tank for aging, to be used for washing. After that, the slurry in the aging tank is pumped into the washing equipment and washed with a sodium hydroxide solution with a concentration of 40 g / L.
[0112] Preferably, the drying and shaping process involves placing the washed ternary precursor filter cake in an oven to dry it, obtaining the ternary precursor. The dried material is then sieved and demagnetized to obtain the corresponding finished precursor product, specifically including:
[0113] The washed ternary precursor filter cake was placed in an oven for static drying. Once the moisture content was within acceptable limits, the drying process was complete, yielding a filter cake with high primary particle uniformity, high secondary particle dispersibility and sphericity, and a tap density of 1.24 g / cm³ and a specific surface area of 28.17 μm³. 2 / g) The ternary precursor is controlled by operation. Finally, the dried material is sieved and demagnetized to obtain the corresponding precursor product for use in cathode sintering.
[0114] The key physicochemical properties of the ternary precursor obtained in Example 2 are shown in Table 2 below:
[0115] Table 2 Key Physicochemical Indicators of the Ternary Precursor Obtained in Example 2
[0116] project D50(um) <![CDATA[BET(m 2 / g)]]> <![CDATA[Tap density (g / m 3 )]]> index 2.05 28.17 1.24
[0117] The SEM images and particle size distributions of the obtained ternary precursors are as follows: Figure 3 and Figure 4 As shown
[0118] Example 3:
[0119] Includes the following steps,
[0120] S1. Solution preparation: Prepare nickel cobalt manganese salt solution, sodium hydroxide solution and ammonia solution;
[0121] S2. Pretreatment: Introduce submerged nitrogen protective gas into the sealed main reactor, and at the same time add pure water to the main reactor to cover the upper edge of the upper stirring blades, and start stirring;
[0122] S3. Preparation of the base solution: Add complexing agent ammonia water and sodium hydroxide solution to the main reactor in sequence to adjust the ammonia value and pH of the system, which serve as the base solution and starting conditions for the reaction.
[0123] S4. Adjust the atmosphere of the reactor: to prevent the oxidation of particles;
[0124] S5. Precipitation Mixing: Add nickel cobalt manganese salt solution, sodium hydroxide solution, and ammonia solution to the reaction vessel simultaneously while maintaining the flow of inert gas to induce precipitation.
[0125] S6. Seed crystal generation and growth in slurry: Lowering the pH of the reaction system while increasing the temperature facilitates the development and growth of particles; low pH is conducive to particle growth, while high temperature is conducive to the perfect stacking of particle crystals.
[0126] S7. Cleaning and Concentration: After the main vessel is full, the overflow valve is opened to overflow into the secondary vessel. After the secondary vessel is submerged by the built-in filter element, the cleaning valve is opened to concentrate the contents.
[0127] S8. Slurry aging and washing: The slurry is placed in an aging tank for aging, and then the slurry in the aging tank is pumped into a washing device for washing.
[0128] S9. Drying and Shaping: The washed ternary precursor filter cake is placed in an oven and dried to obtain the ternary precursor. Then, the dried material is sieved and demagnetized to obtain the corresponding precursor finished product.
[0129] Preferably, the solution preparation includes: preparing a nickel-cobalt-manganese salt solution, a sodium hydroxide solution, and an ammonia solution, specifically including:
[0130] Prepare a nickel-cobalt-manganese salt solution with a metal ion concentration of 2 mol / L, wherein the molar ratio of nickel, cobalt, and manganese is Ni:Co:Mn = 80:12:8; prepare a sodium hydroxide solution with a concentration of 10.50 mol / L; and prepare an ammonia solution with a concentration of 125 g / L.
[0131] Preferably, the pretreatment involves: introducing submerged nitrogen protective gas into the sealed main reactor, simultaneously adding pure water to the main reactor to cover the upper edge of the upper stirring blades, and starting the stirring process, specifically including:
[0132] Submerged nitrogen protective gas was introduced into the sealed main reactor for 3 hours at a flow rate of 400 L / h. During the process, pure water was added to the main reactor to cover the upper edge of the upper stirring blades. Stirring was started at 600 rpm, and the temperature was controlled at 38℃.
[0133] Preferably, the base solution is prepared by sequentially adding ammonia water and sodium hydroxide solution as complexing agents to the main reactor to adjust the system, which serves as the base solution and starting condition for the reaction. Specifically, this includes:
[0134] Ammonia water, a complexing agent, was added sequentially to the main reactor to control the ammonia value at 1.50 g / L. Sodium hydroxide solution was added to adjust the pH of the system to 12.30, which served as the base liquid and starting condition for the reaction.
[0135] Preferably, the atmosphere of the reaction vessel is adjusted to prevent particle oxidation, specifically including:
[0136] After the above S1 and S3 conditions are prepared, adjust the atmosphere of the reactor to 400 L / h for lower nitrogen and 400 L / h for upper nitrogen, and avoid particle oxidation throughout the process.
[0137] Preferably, precipitation mixing involves simultaneously adding a nickel-cobalt-manganese salt solution, a sodium hydroxide solution, and an ammonia solution to the reaction vessel while maintaining the flow of an inert gas to induce precipitation. Specifically, this includes:
[0138] Nickel-cobalt-manganese salt solution, sodium hydroxide solution, and ammonia solution were simultaneously added to the reactor while maintaining the flow of inert gas. During this process, the pH of the system was maintained at 12.3 and the ammonia value at 1.50 g / L, and the co-precipitation synthesis was started.
[0139] Preferably, the generation and growth of slurry seed crystals involves lowering the pH of the reaction system while simultaneously increasing the temperature to improve the efficiency of particle development and growth, specifically including:
[0140] After maintaining the above S4 conditions for 120 minutes, the desired seed crystals were generated. To further promote the growth of the seed crystal slurry, the pH of the reaction system was lowered. The process involved a gradual decrease in pH to 10.90 over 6 hours. This was primarily because directly shutting off the alkali solution would cause a rapid pH drop, leading to excessively fast growth and particle agglomeration. Once the pH was reached, the temperature was raised to 50°C to improve the efficiency of particle development and growth.
[0141] Preferably, the clarification and concentration process is as follows: After the main vessel is full, the overflow valve is opened to overflow into the secondary vessel. Once the secondary vessel has submerged its built-in filter element, the clarification process is initiated for concentration, specifically including:
[0142] Two hours before the main reactor is full, start the secondary reactor with nitrogen at a flow rate of 400L / h to replace the air inside. After the main reactor is full, open the overflow valve to overflow into the secondary reactor. Once the secondary reactor has submerged the built-in filter, start the discharge valve for concentration. During this process, adjust the discharge rate according to the liquid levels in the main and secondary reactors to maintain the stability of the system.
[0143] Preferably, the pulp aging and washing process involves: placing the pulp in an aging tank for aging, and then pumping the pulp from the aging tank into a washing device for washing, specifically including:
[0144] When the reaction particle size D50 = 2 μm, the reaction ends and the machine is stopped. Nitrogen gas is retained. After 60 minutes of shutdown, the particle size is retested and no abnormalities are found. The slurry is then placed in an aging tank for aging, to be used for washing. After that, the slurry in the aging tank is pumped into the washing equipment and washed with a sodium hydroxide solution with a concentration of 40 g / L.
[0145] Preferably, the drying and shaping process involves placing the washed ternary precursor filter cake in an oven to dry it, obtaining the ternary precursor. The dried material is then sieved and demagnetized to obtain the corresponding finished precursor product, specifically including:
[0146] The washed ternary precursor filter cake was placed in an oven for static drying. Once the moisture content was within acceptable limits, the drying process was complete, yielding a filter cake with high primary particle uniformity, high secondary particle dispersibility and sphericity, and a tap density (1.52 g / cm³) and specific surface area (17.17 μm³). 2 The ternary precursor ( / g) is then processed by sieving and demagnetizing the dried material to obtain the corresponding precursor product, which is then used for cathode sintering.
[0147] The key physicochemical properties of the ternary precursor obtained in Example 3 are shown in Table 3 below:
[0148] Table 3 Key physicochemical properties of the ternary precursor obtained in Example 3
[0149] project D50(um) <![CDATA[BET(m 2 / g)]]> <![CDATA[Tap density (g / m 3 )]]> index 1.99 17.17 1.52
[0150] The SEM images and particle size distributions of the obtained ternary precursors are as follows: Figure 5 and Figure 6 As shown:
[0151] Example 4:
[0152] Includes the following steps,
[0153] S1. Solution preparation: Prepare nickel cobalt manganese salt solution, sodium hydroxide solution and ammonia solution;
[0154] S2. Pretreatment: Introduce submerged nitrogen protective gas into the sealed main reactor, and at the same time add pure water to the main reactor to cover the upper edge of the upper stirring blades, and start stirring;
[0155] S3. Preparation of the base solution: Add complexing agent ammonia water and sodium hydroxide solution to the main reactor in sequence to adjust the ammonia value and pH of the system, which serve as the base solution and starting conditions for the reaction.
[0156] S4. Adjust the atmosphere of the reactor: to prevent the oxidation of particles;
[0157] S5. Precipitation Mixing: Add nickel cobalt manganese salt solution, sodium hydroxide solution, and ammonia solution to the reaction vessel simultaneously while maintaining the flow of inert gas to induce precipitation.
[0158] S6. Seed crystal generation and growth in slurry: Lowering the pH of the reaction system while increasing the temperature facilitates the development and growth of particles; low pH is conducive to particle growth, while high temperature is conducive to the perfect stacking of particle crystals.
[0159] S7. Cleaning and Concentration: After the main vessel is full, the overflow valve is opened to overflow into the secondary vessel. After the secondary vessel is submerged by the built-in filter element, the cleaning valve is opened to concentrate the contents.
[0160] S8. Slurry aging and washing: The slurry is placed in an aging tank for aging, and then the slurry in the aging tank is pumped into a washing device for washing.
[0161] S9. Drying and Shaping: The washed ternary precursor filter cake is placed in an oven and dried to obtain the ternary precursor. Then, the dried material is sieved and demagnetized to obtain the corresponding precursor finished product.
[0162] Preferably, the solution preparation includes: preparing a nickel-cobalt-manganese salt solution, a sodium hydroxide solution, and an ammonia solution, specifically including:
[0163] Prepare a nickel-cobalt-manganese salt solution with a metal ion concentration of 2 mol / L, wherein the molar ratio of nickel, cobalt, and manganese is Ni:Co:Mn = 88:9.5:2.5; prepare a sodium hydroxide solution with a concentration of 10.50 mol / L; and prepare an ammonia solution with a concentration of 125 g / L.
[0164] Preferably, the pretreatment involves: introducing submerged nitrogen protective gas into the sealed main reactor, simultaneously adding pure water to the main reactor to cover the upper edge of the upper stirring blades, and starting the stirring process, specifically including:
[0165] Submerged nitrogen protective gas was introduced into the sealed main reactor for 3 hours at a flow rate of 400 L / h. During the process, pure water was added to the main reactor to cover the upper edge of the upper stirring blades. Stirring was started at 600 rpm, and the temperature was controlled at 38℃.
[0166] Preferably, the base solution is prepared by sequentially adding ammonia water and sodium hydroxide solution as complexing agents to the main reactor to adjust the system, which serves as the base solution and starting condition for the reaction. Specifically, this includes:
[0167] Ammonia water, a complexing agent, was added sequentially to the main reactor to control the ammonia value at 1.50 g / L. Sodium hydroxide solution was added to adjust the pH of the system to 12.50, which served as the base liquid and starting condition for the reaction.
[0168] Preferably, the atmosphere of the reaction vessel is adjusted to prevent particle oxidation, specifically including:
[0169] After the above S1 and S3 conditions are prepared, adjust the atmosphere of the reactor to 400 L / h for lower nitrogen and 100 L / h for upper nitrogen, and avoid particle oxidation throughout the process.
[0170] Preferably, precipitation mixing involves simultaneously adding a nickel-cobalt-manganese salt solution, a sodium hydroxide solution, and an ammonia solution to the reaction vessel while maintaining the flow of an inert gas to induce precipitation. Specifically, this includes:
[0171] Nickel-cobalt-manganese salt solution, sodium hydroxide solution, and ammonia solution were simultaneously added to the reactor while maintaining the flow of inert gas. During this process, the pH of the system was maintained at 12.5 and the ammonia value at 1.50 g / L, and the co-precipitation synthesis was started.
[0172] Preferably, the generation and growth of slurry seed crystals involves lowering the pH of the reaction system while simultaneously increasing the temperature to improve the efficiency of particle development and growth, specifically including:
[0173] After maintaining the above S4 conditions for 120 minutes, the desired seed crystals were generated. To further promote the growth of the seed crystal slurry, the pH of the reaction system was lowered. The process involved a gradual decrease in pH to 11.20 over 6 hours. This was primarily because directly shutting off the alkali solution would cause a rapid pH drop, leading to excessively fast growth and particle agglomeration. Once the pH was reached, the temperature was raised to 50°C to improve the efficiency of particle development and growth.
[0174] Preferably, the clarification and concentration process is as follows: After the main vessel is full, the overflow valve is opened to overflow into the secondary vessel. Once the secondary vessel has submerged its built-in filter element, the clarification process is initiated for concentration, specifically including:
[0175] Two hours before the main reactor is full, start the secondary reactor with nitrogen at a flow rate of 400L / h to replace the air inside. After the main reactor is full, open the overflow valve to overflow into the secondary reactor. Once the secondary reactor has submerged the built-in filter, start the discharge valve for concentration. During this process, adjust the discharge rate according to the liquid levels in the main and secondary reactors to maintain the stability of the system.
[0176] Preferably, the pulp aging and washing process involves: placing the pulp in an aging tank for aging, and then pumping the pulp from the aging tank into a washing device for washing, specifically including:
[0177] When the reaction particle size D50 = 2 μm, the reaction ends and the machine is stopped. Nitrogen gas is retained. After 60 minutes of shutdown, the particle size is retested and no abnormalities are found. The slurry is then placed in an aging tank for aging, to be used for washing. After that, the slurry in the aging tank is pumped into the washing equipment and washed with a sodium hydroxide solution with a concentration of 40 g / L.
[0178] Preferably, the drying and shaping process involves placing the washed ternary precursor filter cake in an oven to dry it, obtaining the ternary precursor. The dried material is then sieved and demagnetized to obtain the corresponding finished precursor product, specifically including:
[0179] The washed ternary precursor filter cake was placed in an oven for static drying. Once the moisture content was within acceptable limits, the drying process was complete, yielding a filter cake with high primary particle uniformity, high secondary particle dispersibility and sphericity, and a tap density of 1.71 g / cm³. 3 ) and ratio (8.98m 2 The ternary precursor ( / g) is then processed by sieving and demagnetizing the dried material to obtain the corresponding precursor product, which is then used for cathode sintering.
[0180] The key physicochemical properties of the ternary precursor obtained in Example 4 are shown in Table 4 below:
[0181] Table 4 Key physicochemical properties of the ternary precursor obtained in Example 4
[0182] project D50(um) <![CDATA[BET(m 2 / g)]]> Tap density (g / m3) index 2.09 8.98 1.71
[0183] The SEM images and particle size distributions of the obtained ternary precursors are as follows: Figure 7 and Figure 8 As shown:
[0184] Through the above embodiments, it was found that to further improve particle sphericity and density, the reaction time can be extended, i.e., the granulation pH or time can be increased. Additionally, by controlling the thickness of the primary particle morphology, while keeping the ammonia value constant, the thickness in the 001 direction and whisker uniformity can be adjusted by increasing the pH during the growth process. As the growth pH increases, sphericity gradually improves, particle density, whisker uniformity, and thickness gradually increase, and the corresponding tap density gradually increases while the specific surface area gradually decreases.
[0185] Comparative Example 1:
[0186] Includes the following steps,
[0187] S1. Solution preparation: Prepare nickel cobalt manganese salt solution, sodium hydroxide solution and ammonia solution;
[0188] S2. Pretreatment: Introduce submerged nitrogen protective gas into the sealed main reactor, and at the same time add pure water to the main reactor to cover the upper edge of the upper stirring blades, and start stirring;
[0189] S3. Preparation of the base solution: Add complexing agent ammonia water and sodium hydroxide solution to the main reactor in sequence to adjust the ammonia value and pH of the system, which serve as the base solution and starting conditions for the reaction.
[0190] S4. Adjust the atmosphere of the reactor: to prevent the oxidation of particles;
[0191] S5. Precipitation Mixing: Add nickel cobalt manganese salt solution, sodium hydroxide solution, and ammonia solution to the reaction vessel simultaneously while maintaining the flow of inert gas to induce precipitation.
[0192] S6. Seed crystal generation and growth in slurry: Lowering the pH of the reaction system while increasing the temperature facilitates the development and growth of particles; low pH is conducive to particle growth, while high temperature is conducive to the perfect stacking of particle crystals.
[0193] S7. Cleaning and Concentration: After the main vessel is full, the overflow valve is opened to overflow into the secondary vessel. After the secondary vessel is submerged by the built-in filter element, the cleaning valve is opened to concentrate the contents.
[0194] S8. Slurry aging and washing: The slurry is placed in an aging tank for aging, and then the slurry in the aging tank is pumped into a washing device for washing.
[0195] S9. Drying and Shaping: The washed ternary precursor filter cake is placed in an oven and dried to obtain the ternary precursor. Then, the dried material is sieved and demagnetized to obtain the corresponding precursor finished product.
[0196] Preferably, the solution preparation includes: preparing a nickel-cobalt-manganese salt solution, a nickel-cobalt-manganese salt solution, and an ammonia solution, specifically including:
[0197] Prepare a nickel-cobalt-manganese salt solution with a metal ion concentration of 2 mol / L, wherein the molar ratio of nickel, cobalt, and manganese is Ni:Co:Mn = 83:11:6. Prepare a sodium hydroxide solution with a concentration of 10.50 mol / L and an ammonia solution with a concentration of 125 g / L.
[0198] Preferably, the pretreatment involves: introducing submerged nitrogen protective gas into the sealed main reactor, simultaneously adding pure water to the main reactor to cover the upper edge of the upper stirring blades, and starting the stirring process, specifically including:
[0199] Submerged nitrogen protective gas was introduced into the sealed main reactor for 3 hours at a flow rate of 400 L / h. During the process, pure water was added to the main reactor to cover the upper edge of the upper stirring blades. Stirring was started at 600 rpm, and the temperature was controlled at 38℃.
[0200] Preferably, the base solution is prepared by sequentially adding ammonia water and sodium hydroxide solution as complexing agents to the main reactor to adjust the system, which serves as the base solution and starting condition for the reaction. Specifically, this includes:
[0201] Ammonia water, a complexing agent, was added sequentially to the main reactor to control the ammonia value at 1.50 g / L. Sodium hydroxide solution was added to adjust the pH of the system to 13.20, which served as the base liquid and starting condition for the reaction.
[0202] Preferably, the atmosphere of the reaction vessel is adjusted to prevent particle oxidation, specifically including:
[0203] After the above S1 and S3 conditions are prepared, adjust the atmosphere of the reactor to 400 L / h for lower nitrogen and 100 L / h for upper nitrogen, and avoid particle oxidation throughout the process.
[0204] Preferably, precipitation mixing involves simultaneously adding a nickel-cobalt-manganese salt solution, a sodium hydroxide solution, and an ammonia solution to the reaction vessel while maintaining the flow of an inert gas to induce precipitation. Specifically, this includes:
[0205] Nickel-cobalt-manganese salt solution, sodium hydroxide solution, and ammonia solution were simultaneously added to the reactor while maintaining the flow of inert gas. During this process, the pH of the system was maintained at 13.2 and the ammonia value at 1.50 g / L, and the co-precipitation synthesis was started.
[0206] Preferably, the generation and growth of slurry seed crystals involves lowering the pH of the reaction system while simultaneously increasing the temperature to improve the efficiency of particle development and growth, specifically including:
[0207] After maintaining the above S4 conditions for 120 minutes, the desired seed crystals were generated. To further promote the growth of the seed crystal slurry, the pH of the reaction system was lowered. The process involved a gradual decrease in pH to 11.20 over 6 hours. This was primarily because directly shutting off the alkali solution would cause a rapid pH drop, leading to excessively fast growth and particle agglomeration. Once the pH was reached, the temperature was raised to 50°C to improve the efficiency of particle development and growth.
[0208] Preferably, the clarification and concentration process is as follows: After the main vessel is full, the overflow valve is opened to overflow into the secondary vessel. Once the secondary vessel has submerged its built-in filter element, the clarification process is initiated for concentration, specifically including:
[0209] Two hours before the main reactor is full, start the secondary reactor with nitrogen at a flow rate of 400L / h to replace the air inside. After the main reactor is full, open the overflow valve to overflow into the secondary reactor. Once the secondary reactor has submerged the built-in filter, start the discharge valve for concentration. During this process, adjust the discharge rate according to the liquid levels in the main and secondary reactors to maintain the stability of the system.
[0210] Preferably, the pulp aging and washing process involves: placing the pulp in an aging tank for aging, and then pumping the pulp from the aging tank into a washing device for washing, specifically including:
[0211] When the reaction particle size D50 < 1.50 μm, the reaction ends and the machine is stopped. Nitrogen gas is retained. After 60 minutes of shutdown, the particle size is retested and no abnormality is found. The slurry is then placed in an aging tank for aging, to be used for washing. After that, the slurry in the aging tank is pumped into the washing equipment and washed with a sodium hydroxide solution with a concentration of 40 g / L.
[0212] Preferably, the drying and shaping process involves placing the washed ternary precursor filter cake in an oven to dry it, obtaining the ternary precursor. The dried material is then sieved and demagnetized to obtain the corresponding finished precursor product, specifically including:
[0213] The washed ternary precursor filter cake was placed in an oven for static drying. Once the moisture content was within acceptable limits, drying was completed, and the resulting precursor was amorphous with a tap density of 0.74 g / cm³. 3 The specific gravity is 55.99m. 2 / g of ternary precursor is obtained. Finally, the dried material is sieved and demagnetized to obtain the corresponding precursor product for use in cathode sintering.
[0214] The key physicochemical properties of the ternary precursor obtained in Comparative Example 1 are shown in Table 5 below:
[0215] Table 5 Key physicochemical properties of the ternary precursors obtained in Comparative Example 1
[0216] project D50(um) <![CDATA[BET(m 2 / g)]]> Tap density (g / m3) index 1.14 55.99 0.74
[0217] The SEM images and particle size distributions of the obtained ternary precursors are as follows: Figure 9 and Figure 10 As shown:
[0218] Comparative Example 2:
[0219] Includes the following steps,
[0220] S1. Solution preparation: Prepare nickel cobalt manganese salt solution, sodium hydroxide solution and ammonia solution;
[0221] S2. Pretreatment: Introduce submerged nitrogen protective gas into the sealed main reactor, and at the same time add pure water to the main reactor to cover the upper edge of the upper stirring blades, and start stirring;
[0222] S3. Preparation of the base solution: Add complexing agent ammonia water and sodium hydroxide solution to the main reactor in sequence to adjust the ammonia value and pH of the system, which serve as the base solution and starting conditions for the reaction.
[0223] S4. Adjust the atmosphere of the reactor: to prevent the oxidation of particles;
[0224] S5. Precipitation Mixing: Add nickel cobalt manganese salt solution, sodium hydroxide solution, and ammonia solution to the reaction vessel simultaneously while maintaining the flow of inert gas to induce precipitation.
[0225] S6. Seed crystal generation and growth in slurry: Lowering the pH of the reaction system while increasing the temperature facilitates the development and growth of particles; low pH is conducive to particle growth, while high temperature is conducive to the perfect stacking of particle crystals.
[0226] S7. Cleaning and Concentration: After the main vessel is full, the overflow valve is opened to overflow into the secondary vessel. After the secondary vessel is submerged by the built-in filter element, the cleaning valve is opened to concentrate the contents.
[0227] S8. Slurry aging and washing: The slurry is placed in an aging tank for aging, and then the slurry in the aging tank is pumped into a washing device for washing.
[0228] S9. Drying and Shaping: The washed ternary precursor filter cake is placed in an oven and dried to obtain the ternary precursor. Then, the dried material is sieved and demagnetized to obtain the corresponding precursor finished product.
[0229] Preferably, the solution preparation includes: preparing a nickel-cobalt-manganese salt solution, a sodium hydroxide solution, and an ammonia solution, specifically including:
[0230] Prepare a nickel-cobalt-manganese salt solution with a metal ion concentration of 2.0 mol / L, wherein the molar ratio of nickel, cobalt, and manganese is Ni:Co:Mn = 88:9.5:2.5; prepare a sodium hydroxide solution with a concentration of 10.50 mol / L; and prepare an ammonia solution with a concentration of 125 g / L.
[0231] Preferably, the pretreatment involves: introducing submerged nitrogen protective gas into the sealed main reactor, simultaneously adding pure water to the main reactor to cover the upper edge of the upper stirring blades, and starting the stirring process, specifically including:
[0232] Submerged nitrogen protective gas was introduced into the sealed main reactor for 3 hours at a flow rate of 400 L / h. During the process, pure water was added to the main reactor to cover the upper edge of the upper stirring blades. Stirring was started at 600 rpm, and the temperature was controlled at 38℃.
[0233] Preferably, the base solution is prepared by sequentially adding ammonia water and sodium hydroxide solution as complexing agents to the main reactor to adjust the system, which serves as the base solution and starting condition for the reaction. Specifically, this includes:
[0234] Ammonia water, a complexing agent, was added sequentially to the main reactor to control the ammonia value at 1.50 g / L. Sodium hydroxide solution was added to adjust the pH of the system to 12.10, which served as the base liquid and starting condition for the reaction.
[0235] Preferably, adjusting the atmosphere of the reactor to prevent particle oxidation specifically includes:
[0236] After the above S1 and S3 conditions are prepared, adjust the atmosphere of the reactor to 400 L / h for lower nitrogen and 100 L / h for upper nitrogen, and avoid particle oxidation throughout the process.
[0237] Preferably, precipitation mixing involves simultaneously adding a nickel-cobalt-manganese salt solution, a sodium hydroxide solution, and an ammonia solution to the reaction vessel while maintaining the flow of an inert gas to induce precipitation. Specifically, this includes:
[0238] Nickel-cobalt-manganese salt solution, sodium hydroxide solution, and ammonia solution were simultaneously added to the reactor while maintaining the flow of inert gas. During this process, the pH of the system was maintained at 12.1 and the ammonia value at 1.50 g / L, and the co-precipitation synthesis was started.
[0239] Preferably, the generation and growth of slurry seed crystals involves lowering the pH of the reaction system while simultaneously increasing the temperature to improve the efficiency of particle development and growth, specifically including:
[0240] After maintaining the above S4 conditions for 120 minutes, the desired seed crystals were generated. To further promote the growth of the seed crystal slurry, the pH of the reaction system was lowered. The process involved a gradual decrease in pH to 11.65 over 6 hours. This was primarily because directly shutting off the alkali solution would cause a rapid pH drop, leading to excessively fast growth and particle agglomeration. Once the pH was reached, the temperature was raised to 50°C to improve the efficiency of particle development and growth.
[0241] Preferably, the clarification and concentration process is as follows: After the main vessel is full, the overflow valve is opened to overflow into the secondary vessel. Once the secondary vessel has submerged its built-in filter element, the clarification process is initiated for concentration, specifically including:
[0242] Two hours before the main reactor is full, start the secondary reactor with nitrogen at a flow rate of 400L / h to replace the air inside. After the main reactor is full, open the overflow valve to overflow into the secondary reactor. Once the secondary reactor has submerged the built-in filter, start the discharge valve for concentration. During this process, adjust the discharge rate according to the liquid levels in the main and secondary reactors to maintain the stability of the system.
[0243] Preferably, the pulp aging and washing process involves: placing the pulp in an aging tank for aging, and then pumping the pulp from the aging tank into a washing device for washing, specifically including:
[0244] When the reaction particle size D50 = 2.0 μm, the reaction ends and the machine is stopped. Nitrogen gas is retained. After 60 minutes of shutdown, the particle size is retested and no abnormalities are found. The slurry is then placed in an aging tank for aging, to be used for washing. After that, the slurry in the aging tank is pumped into the washing equipment and washed with a sodium hydroxide solution with a concentration of 40 g / L.
[0245] Preferably, the drying and shaping process involves placing the washed ternary precursor filter cake in an oven to dry it, obtaining the ternary precursor. The dried material is then sieved and demagnetized to obtain the corresponding finished precursor product, specifically including:
[0246] The washed ternary precursor filter cake was placed in an oven for static drying. Once the moisture content was within acceptable limits, the drying process was complete, yielding a filter cake with high primary particle uniformity, high secondary particle dispersibility and sphericity, and a tap density (1.77 g / cm³) and specific surface area (10.66 μm³). 2 The ternary precursor ( / g) is then processed by sieving and demagnetizing the dried material to obtain the corresponding precursor product, which is then used for cathode sintering.
[0247] The key physicochemical properties of the ternary precursors obtained in Comparative Example 2 are shown in Table 6 below:
[0248] Table 6 Key physicochemical properties of the ternary precursors obtained in Comparative Example 1
[0249] project D50(um) <![CDATA[BET(m 2 / g)]]> Tap density (g / m3) index 2.01 10.66 1.77
[0250] The SEM images and particle size distributions of the obtained ternary precursors are as follows: Figure 11 and Figure 12 As shown:
[0251] Comparative Examples 1-2 show that as the granulation pH increases (>13.0) and the particle size at shutdown is <1.5µm, the particles exhibit an amorphous distribution and a non-normal particle size distribution, with very low tap density and high specific surface area. Furthermore, as the pH increases during the growth stage (>11.60), the particle morphology becomes denser, with the primary particles gradually changing from lath-like to spindle-shaped, and unidentified small whiskers adhering to the particle surface. It is initially suspected that this is due to the increased particle density at higher pH levels, resulting in fewer remaining active sites on the surface, preventing newly generated crystal nuclei from effectively growing on the existing whiskers. This phenomenon, leading to a slight increase in the tap density and specific surface area, is mainly attributed to the influence of small surface particles.
[0252] The differences in physicochemical properties between the examples and the comparative examples are more intuitively illustrated in Table 7:
[0253] name D50(um) <![CDATA[BET(m 2 / g)]]> <![CDATA[Tap density (g / m 3 )]]> Example 1 1.604 38.07 1.00 Example 2 2.05 28.17 1.24 Example 3 1.99 17.17 1.52 Example 4 2.09 8.98 1.71 Comparative Example 1 1.14 55.99 0.74 Comparative Example 2 2.01 10.66 1.77
[0254] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a highly spherical ultra-small particle precursor, comprising the following steps, characterized in that: S1. Prepare solution: prepare nickel-cobalt-manganese salt solution, sodium hydroxide solution and ammonia solution; S2, pretreatment: introduce submerged nitrogen protective gas into the sealed main reactor, and at the same time add pure water into the main reactor to cover the upper edge of the upper stirring blade, and start stirring; S3, base liquid preparation: add complexing agent ammonia water and sodium hydroxide solution to the main reactor to adjust the ammonia value and pH of the system, which serve as the base liquid and starting condition for the reaction; S4. Adjust the atmosphere of the reactor to avoid oxidation of particles; S5, precipitation mixing: adding nickel-cobalt-manganese salt solution, sodium hydroxide solution and ammonia solution into the reaction kettle at the same time and maintaining the inert gas flow to perform precipitation; S6. Production and development of slurry crystal seeds: Lowering the pH of the reaction system and increasing the temperature at the same time facilitates the development and growth of particles; low pH is conducive to the growth of particles, and high temperature is conducive to the perfect accumulation of particle crystals. S7, clearing and concentration: When the main kettle is full, the overflow valve is opened to overflow to the secondary kettle. After the secondary kettle is submerged by the built-in filter element, the clearing is opened for concentration; S8, slurry aging and washing: the slurry is placed in an aging tank for aging, and the slurry in the aging tank is pumped into a washing device for washing; S9, drying and molding: placing the washed ternary precursor filter cake in an oven for drying to obtain a ternary precursor, and then sieving and demagnetizing the dried material to obtain the corresponding precursor finished product.
2. The method for preparing a highly spherical ultra-small particle precursor according to claim 1, characterized in that: Solution preparation: nickel-cobalt-manganese salt solution, sodium hydroxide solution and ammonia solution are prepared, specifically including: Prepare a nickel-cobalt-manganese salt solution with a metal ion concentration of 1-2.5 mol / L, a sodium hydroxide solution with a concentration of 8-15 mol / L, and an ammonia solution with a concentration of 100-150 g / L.
3. The method for preparing a highly spherical ultra-small particle precursor according to claim 1, characterized in that: Pretreatment: introduce submerged nitrogen protective gas into the sealed main reactor, add pure water to the main reactor to cover the upper edge of the upper stirring blade, and start stirring, specifically including: Pass submerged nitrogen protective gas into the sealed main reactor for 1-3 hours at a flow rate of 300-600L / h. During the process, add pure water to the main reactor to cover the upper edge of the upper stirring blade, start stirring at 500-650rpm, and control the temperature at 35-45℃.
4. The method for preparing a highly spherical ultra-small particle precursor according to claim 1, characterized in that: Base liquid preparation: add complexing agent ammonia water and sodium hydroxide solution to the main reactor to adjust the ammonia value and pH of the system, as the base liquid and starting conditions for the reaction, specifically including: Add complexing agent ammonia water to the main reactor in sequence, control the ammonia value at 1.0-3.0 g / L, and add sodium hydroxide solution to adjust the pH of the system to 12.0-13.0, which serves as the base liquid and starting condition for the reaction.
5. The method for preparing a highly spherical ultra-small particle precursor according to claim 1, characterized in that: Adjust the reactor atmosphere: Avoid particle oxidation, including: After the above S1 and S3 conditions are prepared, adjust the atmosphere of the reactor to 300-600 L / h of lower nitrogen and 100-300 L / h of upper nitrogen to avoid particle oxidation throughout the process.
6. The method for preparing a highly spherical ultra-small particle precursor according to claim 1, characterized in that: Precipitation mixing: Add nickel-cobalt-manganese salt solution, sodium hydroxide solution and ammonia solution into the reactor at the same time, and maintain the inert gas to precipitate, specifically including: Add nickel-cobalt-manganese salt solution, sodium hydroxide solution and ammonia solution into the reaction kettle at the same time and keep the inert gas flowing. During this period, the pH of the system is maintained at 12.0-13.0 and the ammonia value is maintained at 1.0-3.0 g / L to start the coprecipitation synthesis.
7. The method for preparing a high sphericity ultra-small particle precursor according to claim 1, characterized in that: Slurry seed generation and development growth: Lower the pH of the reaction system and increase the temperature to improve the efficiency of particle development and growth, including: After the above S4 conditions are maintained for 60-240 minutes, the required seed crystals are generated. On this basis, in order to further grow the seed crystal slurry, the growth pH of the reaction system is reduced. The process uses a ramp to reduce the pH to between 10.40-11.60, which takes 4-10 hours. This is mainly because directly closing the alkali solution (rapid drop) will cause the pH to drop rapidly, which in turn leads to excessive growth rate and particle agglomeration. After the pH drops to the right level, the temperature rises to 45-60°C to improve the efficiency of particle development and growth.
8. The method for preparing a high sphericity ultra-small particle precursor according to claim 1, characterized in that: Clearing and concentration: When the main kettle is full, the overflow valve is opened to overflow to the secondary kettle. After the secondary kettle is submerged by the built-in filter element, the clearing is opened for concentration, which specifically includes: 2 hours before the main reactor is full, start the secondary reactor with nitrogen at a flow rate of 300-600L / h to replace the air in the reactor. After the main reactor is full, open the overflow valve to overflow to the secondary reactor. After the secondary reactor passes through the built-in filter element, start the clearing to concentrate. During this period, adjust the size of the clearing according to the liquid levels of the main and secondary reactors to maintain the stability of the system.
9. The method for preparing a highly spherical ultra-small particle precursor according to claim 1, characterized in that: Slurry aging and washing: The slurry is placed in the aging tank for aging, and the slurry in the aging tank is sent to the washing equipment for washing, which specifically includes: When the reaction particle size D50 = 1.5-2.1um, the reaction is terminated and the machine is shut down, nitrogen is retained, and after 30-150 minutes of shutdown, the particle size is re-measured and no abnormality is found. The slurry is placed in an aging tank for aging before washing. The slurry in the aging tank is then pumped into a washing device and washed with a sodium hydroxide solution with a concentration of 30-80g / L.
10. The method for preparing a high sphericity ultra-small particle precursor according to claim 1, characterized in that: Drying and molding: The washed ternary precursor filter cake is placed in an oven for drying to obtain a ternary precursor, and then the dried material is screened and demagnetized to obtain the corresponding precursor finished product, which specifically includes: The washed ternary precursor filter cake is placed in an oven for static drying. When the moisture content is qualified, the drying is completed, and a primary particle with high consistency, secondary particle dispersion and high sphericity, and a tap density (1.00-1.80g / cm 3 ) and ratio table (8-45m 2 / g) to produce a controllable ternary precursor. Finally, the dried material is screened and demagnetized to obtain the corresponding precursor product for positive electrode sintering.
Citation Information
Patent Citations
An ultra-small particle size nickel-cobalt-manganese hydroxide and its preparation method
CN108946827B
Cited By
Preparation method and application of high-nickel majority crystal ternary precursor
CN119145049A
A preparation method and application of a high-nickel polycrystalline ternary precursor
CN119145049B
Preparation method of high-BET high-nickel low-cobalt ternary large-particle precursor
CN120589809A