Preparation method and application of graphene composite nickel sulfide

The in-situ synthesis of graphene composite nickel sulfide by solution reaction of nickel citrate and thiourea and high-temperature calcination method, solving the complex process, high cost and environmental safety problems in the existing technology, significantly improving the electrochemical performance and stability of the material , has promoted the development of sodium ion batteries.

CN118978196AActive Publication Date: 2024-11-19SOUTHWEST JIAOTONG UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411075493.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-19
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

The existing preparation methods for graphene composite nickel sulfide have complex processes, high costs, environmental and safety hazards, and unstable material structure and performance, making it difficult to achieve efficient, low-cost and safe preparation of nickel sulfide electrode materials.

Method used

Nickel citrate and thiourea are used as precursor materials, and graphene composite nickel sulfide is synthesized in situ by solution reaction and high-temperature calcination to simplify the preparation process, improve the conductivity and structural stability of the material, and optimize the material's performance by using high-temperature heat treatment.

Benefits of technology

The high conductivity and structural stability of graphene composite nickel sulfide has been achieved, which significantly improves its electrochemical performance, reduces production costs, improves the environmental friendliness and safety of the preparation process, and broadens its in sodium ion batteries. Application potential.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978196A_ABST
    Figure CN118978196A_ABST
Patent Text Reader

Abstract

The invention belongs to but not limited to the technical field of energy storage materials, and discloses a preparation method and application of graphene composite nickel sulphide. A nickel source, a carbon source and a sulfur source compound are added into a certain amount of deionized water, and after violent stirring is conducted for a period of time, a green clear solution is obtained; freezing the clarified solution with liquid nitrogen, putting into a freeze dryer, and drying at a certain temperature for a plurality of hours to obtain a precursor material; placing the prepared precursor material in a high-temperature tube furnace, and performing high-temperature heat treatment in an inert atmosphere to obtain graphene composite nickel sulfide; the nickel source compound and the carbon source compound are nickel citrate, the sulfur source compound is thiourea, and the mass ratio of the nickel source compound to the sulfur source compound is 1: 6-5: 4. The method has the advantages of simplicity, high efficiency, low preparation cost and the like; the prepared graphene composite nickel sulfide has high conductivity and excellent structural stability, and shows excellent electrochemical performance as a sodium ion battery negative electrode.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to but is not limited to the technical field of energy storage materials, and in particular relates to a preparation method of graphene composite nickel sulfide and application thereof. Background Art

[0002] Sodium-ion batteries (SIBs) are gaining attention as a potential alternative to lithium-ion batteries (LIBs) in large-scale energy storage systems due to their significant cost-effectiveness and the abundance of sodium resources in nature. Similar to LIBs, electrode materials are one of the key factors determining the electrochemical performance of SIBs. However, the larger ionic radius of sodium ions ( contrast Therefore, finding suitable sodium storage materials is of great significance for promoting the development of sodium ion batteries.

[0003] As a transition metal sulfide (TMCs) anode material based on a conversion mechanism, nickel sulfide shows great potential as anode for SIBs. Nickel sulfide is not only abundant in the earth's crust and low in cost, but also has a high theoretical capacity (591 mAhg-1 for NiS and 446 mAhg-1 for NiS) through multi-electron conversion reactions, which far exceeds the capacity of current LIBs graphite anodes. However, there are also some challenges for nickel sulfide as a sodium storage anode material. First, its inherent low conductivity limits the transmission efficiency of electrons within the material, which in turn affects the electrochemical performance. Secondly, during the charge and discharge process, the nickel sulfide material will undergo a huge volume change, resulting in the instability of the electrode structure, which accelerates the capacity decay and affects the rate performance. Therefore, improving the conductivity of the material and optimizing the stability of the electrode structure are the key to developing high-performance nickel sulfide anodes.

[0004] Constructing a composite nanostructure of carbonaceous materials is an effective way to improve the electrochemical performance of nickel sulfide sodium storage. The strong willpower of carbonaceous materials can buffer the volume change during charging and discharging and ensure the structural stability of the electrode; at the same time, the conductive network constructed by the composite of carbonaceous materials can promote the rapid transmission of electrons and increase the electronic conductivity of the material; in addition, the construction of nanostructures can increase the specific surface area of ​​the material and shorten the transmission distance of electrons / ions, thereby significantly improving the sodium storage capacity and rate performance of nickel sulfide materials. The carbonaceous materials currently used mainly include graphene, carbon nanotubes and conductive polymers. Among them, graphene is the most widely used carbon-based composite material due to its unique two-dimensional layered structure, extremely high theoretical specific surface area, high conductivity and good structural stability. However, the current synthesis of graphene is mainly obtained by the reduction of graphene oxide. The Brodie method, Staudenmaier method and Hummers method are traditional methods for preparing graphene oxide, all of which are based on the reaction of graphite with a large amount of concentrated nitric acid, concentrated sulfuric acid, potassium permanganate and other composite strong oxidants. Although these methods have a long history and mature technology, they have disadvantages such as explosion risk, serious pollution, and long reaction cycle, making it difficult to achieve large-scale application. In addition, the existing composites of graphene and nickel sulfide are completed by physical and chemical methods through simple mechanical and chemical bonding. Due to the weak composite force between the two, it is difficult to achieve a significant improvement in the material's conductivity and structural stability. Summary of the invention

[0005] In view of the problems existing in the prior art, the present invention provides an efficient and convenient method for preparing graphene composite nickel sulfide, and examines its electrochemical performance as the negative electrode of a sodium ion battery; the present invention significantly increases the electrical conductivity and structural stability of the nickel sulfide material by constructing a carbonaceous material composite nanostructure, thereby achieving high capacity, long cycle and high rate of the nickel sulfide sodium storage negative electrode.

[0006] The present invention is achieved by a method for preparing graphene composite nickel sulfide, comprising the following steps:

[0007] (1) Preparing a precursor: adding a nickel source, a carbon source, and a sulfur source compound to a certain amount of deionized water, and after a period of vigorous stirring, a green clear solution is obtained. The clear solution is frozen with liquid nitrogen and placed in a freeze dryer. After drying at a certain temperature for several hours, a precursor material is obtained;

[0008] (2) Preparing graphene-composite nickel sulfide: placing the precursor material prepared in step (1) in a high-temperature tube furnace, and performing high-temperature heat treatment in an inert atmosphere to obtain graphene-composite nickel sulfide;

[0009] In the step (1), the nickel source and carbon source compound is nickel citrate, and the sulfur source compound is thiourea, and the mass ratio of the two added is 1:6 to 5:4.

[0010] Furthermore, in the step (1), the amount of deionized water added is 50 to 200 ml.

[0011] Furthermore, in the step (1), the stirring time is 0.5 to 12 hours.

[0012] Furthermore, in the step (1), the freeze-drying temperature is -30 to -60°C.

[0013] Furthermore, in the step (1), the freeze-drying time is 12 to 72 hours.

[0014] Furthermore, in the step (2), the heating rate of the high temperature heat treatment process is 2 to 5°C / min.

[0015] Furthermore, in the step (2), the insulation temperature range of the high temperature heat treatment process is 400 to 1000° C.; and the insulation time range is 1 to 10 hours.

[0016] Furthermore, in step (2), the inert atmosphere is one or both of argon and nitrogen.

[0017] The object of the present invention is to provide a graphene composite nickel sulfide prepared by the preparation method of the graphene composite nickel sulfide.

[0018] Another object of the present invention is to provide a sodium ion battery, comprising: a negative electrode, a positive electrode, a separator between the positive and negative electrodes, and an electrolyte, wherein the negative electrode is prepared from the above-mentioned graphene composite nickel sulfide.

[0019] In combination with the above technical solutions and the technical problems solved, the advantages and positive effects of the technical solutions to be protected by the present invention are as follows:

[0020] First, the present invention uses nickel citrate and thiourea as raw materials, and synthesizes the graphene uniformly composite nickel sulfide material in situ through solution reaction and high-temperature calcination method;

[0021] The method of the present invention synthesizes graphene materials in situ during the preparation of nickel sulfide, and realizes the composite of nickel sulfide and graphene. Compared with other preparation technologies, this method does not require the cumbersome graphene preparation process, and realizes the synthesis of graphene and nickel sulfide in situ during the synthesis of nickel sulfide and graphene, and has the advantages of simplicity, high efficiency and low preparation cost;

[0022] The graphene composite nickel sulfide prepared by the present invention has high electrical conductivity and excellent structural stability, and exhibits excellent electrochemical performance as a sodium storage negative electrode.

[0023] Second, the main parameters of the present invention:

[0024] 1. Nickel source, carbon source and sulfur source compounds:

[0025] Nickel and carbon source: nickel citrate

[0026] Sulfur source: Thiourea

[0027] Mass ratio: 1:6~5:4

[0028] 2. Deionized water:

[0029] Addition amount: 50~200ml

[0030] 3. Mixing time:

[0031] 0.5~12 hours

[0032] 4. Freeze drying:

[0033] Temperature: -30~-60℃

[0034] Time: 12 to 72 hours

[0035] 5. High temperature heat treatment:

[0036] Heating rate: 2~5℃ / min

[0037] Insulation temperature: 400~1000℃

[0038] Insulation time: 1 to 10 hours

[0039] Inert atmosphere: Argon or nitrogen

[0040] Technical problems solved by the prior art:

[0041] 1. Complex preparation process and high cost issues:

[0042] The conventional preparation method of graphene composite nickel sulfide often involves multi-step reactions, which is complex and costly. The present invention prepares the precursor material in a one-step method and performs high-temperature heat treatment, which simplifies the preparation process and reduces the production cost.

[0043] 2. Material structure and performance instability issues:

[0044] In the prior art, the structure and performance of the composite material are often unstable, which affects its effect in practical applications. The present invention ensures the structural stability and excellent performance of the graphene composite nickel sulfide material by precisely controlling the stirring time, freeze-drying temperature and time, and high-temperature heat treatment conditions.

[0045] 3. Environmental and safety issues:

[0046] Some chemical reagents used in traditional preparation methods are potentially harmful to the environment and operators. The present invention selects safe and non-toxic nickel citrate and thiourea as precursor materials, which improves the environmental friendliness and safety of the preparation process.

[0047] 4.Improvement of electrochemical performance of materials:

[0048] The existing graphene composite nickel sulfide materials have limitations in electrochemical performance. The present invention significantly improves the conductivity and electrochemical stability of the material by optimizing the material preparation parameters, such as the temperature and time of high-temperature heat treatment, so that it performs well in battery energy storage applications.

[0049] Significant technological advances achieved:

[0050] 1. Process simplification and cost reduction:

[0051] By preparing the precursor material in a one-step method and performing heat treatment under an inert atmosphere in a high-temperature tube furnace, the present invention simplifies the traditional complex preparation process, greatly reduces the production cost, and improves the feasibility of industrial production.

[0052] 2. High stability and excellent performance:

[0053] Precise control of preparation parameters ensures the structural stability of graphene-composite nickel sulfide materials, improves the performance stability and durability of the materials in electrochemical applications, and broadens their application areas.

[0054] 3. Environmental friendliness and operational safety:

[0055] The selection of safe and non-toxic compounds such as nickel citrate and thiourea as precursor materials improves the environmental friendliness of the preparation process, reduces health hazards to operators, and complies with the principles of green chemistry.

[0056] 4. Significant improvement in electrochemical performance:

[0057] By optimizing the high-temperature heat treatment conditions, the conductivity and electrochemical properties of the material were significantly improved, greatly increasing its application potential in sodium-ion battery energy storage devices and promoting the development of the energy materials field.

[0058] In summary, the present invention not only solves the problems of complex process, high cost, environmental safety and material performance stability in the prior art by optimizing preparation parameters and selecting environmentally friendly and safe precursor materials, but also significantly improves the electrochemical properties of graphene composite nickel sulfide materials, providing a solid technical foundation for their application in energy storage and conversion equipment, and demonstrating significant technological progress and application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0059] Figure 1 It is a flow chart of a method for preparing graphene composite nickel sulfide provided by an embodiment of the present invention;

[0060] Figure 2 The X-ray diffraction pattern (XRD) of the graphene composite nickel sulfide material obtained in Example 1 of the present invention;

[0061] Figure 3 This is a transmission electron microscope image (TEM) of the graphene composite nickel sulfide material obtained in Example 1 of the present invention;

[0062] Figure 4 The graphene composite nickel sulfide material obtained in Example 1 of the present invention is subjected to 200 mAg -1 Cyclic performance diagram at current density of ;

[0063] Figure 5 is the X-ray diffraction pattern (XRD) of the graphene composite nickel sulfide material obtained in Example 2 of the present invention;

[0064] Figure 6 This is a transmission electron microscope image (TEM) of the graphene composite nickel sulfide material obtained in Example 2 of the present invention;

[0065] Figure 7 The graphene composite nickel sulfide material obtained in Example 2 of the present invention is subjected to 200 mAg -1 Cyclic performance diagram at current density of ;

[0066] Figure 8 The X-ray diffraction pattern (XRD) of the graphene composite nickel sulfide material obtained in Example 3 of the present invention;

[0067] Fig. 9 This is a transmission electron microscope image (TEM) of the graphene composite nickel sulfide material obtained in Example 3 of the present invention;

[0068] Fig.10 The graphene composite nickel sulfide material obtained in Example 3 of the present invention is subjected to 200 mAg -1 Cycling performance diagram at current density of . DETAILED DESCRIPTION

[0069] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0070] The following are two embodiments of the preparation method of the graphene composite nickel sulfide:

[0071] Application Example 1:

[0072] 1. Preparation of precursor:

[0073] Nickel source, carbon source compound: nickel citrate, 10g

[0074] Sulfur source compound: thiourea, 24 g (mass ratio is 1:2.4, within the range of 1:6 to 5:4)

[0075] Deionized water: 100ml (within the range of 50-200ml)

[0076] Stirring time: 6h (within the range of 0.5 to 12h)

[0077] Freeze drying temperature: -45℃ (within the range of -30~-60℃)

[0078] Freeze drying time: 48h (within the range of 12 to 72h)

[0079] 2. Preparation of graphene composite nickel sulfide:

[0080] High temperature heat treatment heating rate: 3℃ / min (within the range of 2~5℃ / min)

[0081] High temperature heat treatment holding temperature: 600℃ (within the range of 400~1000℃)

[0082] High temperature heat treatment holding time: 5h (within the range of 1 to 10h)

[0083] Inert atmosphere: Argon

[0084] Application Example 2:

[0085] 1. Preparation of precursor:

[0086] Nickel source, carbon source compound: nickel citrate, 20g

[0087] Sulfur source compound: thiourea, 16 g (mass ratio is 5:4, in the range of 1:6 to 5:4)

[0088] Deionized water: 200ml (within the range of 50-200ml)

[0089] Stirring time: 12h (within the range of 0.5 to 12h)

[0090] Freeze drying temperature: -60℃ (within the range of -30~-60℃)

[0091] Freeze drying time: 72h (within the range of 12 to 72h)

[0092] 2. Preparation of graphene composite nickel sulfide:

[0093] High temperature heat treatment heating rate: 5℃ / min (within the range of 2~5℃ / min)

[0094] High temperature heat treatment holding temperature: 1000℃ (within the range of 400~1000℃)

[0095] High temperature heat treatment holding time: 10h (within the range of 1 to 10h)

[0096] Inert atmosphere: Nitrogen

[0097] In these two examples, all parameters are within the ranges specified in the claims, demonstrating how to specifically apply the method for preparing graphene-composite nickel sulfide.

[0098] like Figure 1 As shown, a method for preparing graphene composite nickel sulfide provided by an embodiment of the present invention comprises the following steps:

[0099] (1) Preparing a precursor: adding a nickel source, a carbon source, and a sulfur source compound to a certain amount of deionized water, and after a period of vigorous stirring, a green clear solution is obtained. The clear solution is frozen with liquid nitrogen and placed in a freeze dryer. After drying at a certain temperature for several hours, a precursor material is obtained;

[0100] (2) Preparing graphene-composite nickel sulfide: placing the precursor material prepared in step (1) in a high-temperature tube furnace, and performing high-temperature heat treatment in an inert atmosphere to obtain graphene-composite nickel sulfide;

[0101] In the step (1), the nickel source and carbon source compound is nickel citrate, and the sulfur source compound is thiourea, and the mass ratio of the two added is 1:6 to 5:4.

[0102] Example 1

[0103] This embodiment includes the following steps:

[0104] (1) Nickel citrate and thiourea were added to 50 ml of deionized water in a mass ratio of 1:3, and the mixture was vigorously stirred for 2 h to obtain a green clear solution. The solution was frozen in a liquid nitrogen environment and then placed in a freeze dryer and dried at -60 °C for 12 h to obtain a precursor material.

[0105] (2) The obtained precursor material is subjected to high-temperature heat treatment. The specific heating program is: heating at a rate of 5°C / min and keeping at 600°C for 2h. The entire high-temperature heat treatment process is carried out in an argon atmosphere to obtain the target product.

[0106] Figure 2 The X-ray diffraction pattern (XRD) of the graphene composite nickel sulfide material obtained in Example 1 of the present invention is as follows: Figure 2 It can be seen that the X-ray diffraction peak of the graphene composite nickel sulfide obtained in Example 1 is similar to that of NiS 1.03 (JCPDS 02-1273) standard card, proving that the synthesized nickel sulfide is NiS 1.03 .

[0107] Figure 3 The transmission electron microscopy (TEM) image of the graphene composite nickel sulfide material obtained in Embodiment 1 of the present invention is as follows: Figure 3 It can be seen that in Example 1 of the present invention, the nickel sulfide obtained is nanoparticles of 50-100 nm and is evenly coated in the flaky graphene.

[0108] Figure 4 The graphene composite nickel sulfide material obtained in Example 1 of the present invention is subjected to 200 mAg -1 Cycling performance diagram under current density, Figure 4 The material has a capacity of 638.6 mAhg -1 The first-week capacity and the first-week coulomb efficiency are 77.9%, and the sodium storage capacity after 300 cycles is 348.1 mAh g -1 , the capacity retention rate is 54.5%.

[0109] Example 2

[0110] This embodiment includes the following steps:

[0111] (1) Nickel citrate and thiourea were added to 80 ml of deionized water in a mass ratio of 2:3, and stirred vigorously for 2 h to obtain a green clear solution. The solution was frozen in a liquid nitrogen environment and placed in a freeze dryer and dried at -60 °C for 24 h to obtain a precursor material.

[0112] (2) The obtained precursor material is subjected to high-temperature heat treatment. The specific heating program is: heating at a rate of 8°C / min and keeping at 600°C for 2h. The entire high-temperature heat treatment process is carried out in an argon atmosphere to obtain the target product.

[0113] Figure 5 The X-ray diffraction pattern (XRD) of the graphene composite nickel sulfide material synthesized in Example 2 of the present invention is as follows: Figure 5 It can be seen that the X-ray diffraction peak of the graphene composite nickel sulfide obtained in Example 2 is similar to that of NiS1.03 (JCPDS 02-1273) standard card, proving that the synthesized nickel sulfide is NiS 1.03 .

[0114] Figure 6 The transmission electron microscopy (TEM) image of the graphene composite nickel sulfide material obtained in Embodiment 2 of the present invention is as follows: Figure 6 It can be seen that in Example 2 of the present invention, the nickel sulfide obtained is nanoparticles of 100-120 nm and is evenly coated in the flaky graphene.

[0115] Figure 7 The graphene composite nickel sulfide material obtained in Example 2 of the present invention is subjected to 200 mAg -1 Cycling performance diagram under current density, Figure 7 The material has a 259 mAhg -1 The first-week capacity and the first-week coulomb efficiency are 71.2%, and the sodium storage capacity after 300 cycles is 231.1 mAh g -1 , the capacity retention rate is 89.2%.

[0116] Example 3

[0117] This embodiment includes the following steps:

[0118] (1) Nickel citrate and thiourea were added to 100 ml of deionized water in a mass ratio of 1:1, and the mixture was vigorously stirred for 4 h to obtain a green clear solution. The solution was frozen in a liquid nitrogen environment and then placed in a freeze dryer and dried at -60 °C for 48 h to obtain a precursor material.

[0119] (2) The obtained precursor material is subjected to high-temperature heat treatment. The specific heating program is: heating at a rate of 5°C / min and keeping at 600°C for 2h. The entire high-temperature heat treatment process is carried out in an argon atmosphere to obtain the target product.

[0120] Figure 8 The X-ray diffraction pattern (XRD) of the graphene composite nickel sulfide material synthesized in Example 3 of the present invention is as follows: Figure 8 It can be seen that the X-ray diffraction peak of the graphene composite nickel sulfide obtained in Example 3 is similar to that of NiS 1.03 (JCPDS 02-1273) standard card, proving that the synthesized nickel sulfide is NiS 1.03 .

[0121] Fig. 9 The transmission electron microscopy (TEM) image of the graphene composite nickel sulfide material obtained in Embodiment 3 of the present invention is shown in FIG. Fig. 9 It can be seen that in Example 3 of the present invention, the nickel sulfide obtained is nanoparticles of 20-50 nm and is evenly coated in the flaky graphene.

[0122] Fig.10 The graphene composite nickel sulfide material obtained in Example 3 of the present invention is subjected to 200 mAg -1 Cycling performance diagram under current density, Fig.10 The material has a 361.5 mAh g -1 The first-week capacity, the first-week coulomb efficiency is 76.9%, there is no attenuation after 300 cycles, and the sodium storage capacity is 386.3mAhg -1 .

[0123] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any modifications, equivalent substitutions and improvements made by any technician familiar with the technical field within the technical scope disclosed by the present invention and within the spirit and principle of the present invention should be covered by the protection scope of the present invention.

Claims

1. A method for preparing graphene composite nickel sulfide, characterized in that: The following steps are involved: (1) Preparing a precursor: adding a nickel source, a carbon source, and a sulfur source compound to a certain amount of deionized water, and after a period of vigorous stirring, a green clear solution is obtained. The clear solution is frozen with liquid nitrogen and placed in a freeze dryer. After drying at a certain temperature for several hours, a precursor material is obtained; (2) Preparing graphene-composite nickel sulfide: placing the precursor material prepared in step (1) in a high-temperature tube furnace, and performing high-temperature heat treatment in an inert atmosphere to obtain graphene-composite nickel sulfide; In the step (1), the nickel source and carbon source compound is nickel citrate, and the sulfur source compound is thiourea, and the mass ratio of the two added is 1:6 to 5:

4.

2. The method for preparing graphene composite nickel sulfide according to claim 1, characterized in that: In the step (1), the amount of deionized water added is 50 to 200 ml.

3. The method for preparing graphene composite nickel sulfide according to claim 1, characterized in that: In the step (1), the stirring time is 0.5 to 12 hours.

4. The method for preparing graphene composite nickel sulfide according to claim 1, characterized in that: In the step (1), the freeze-drying temperature is -30 to -60°C.

5. The method for preparing graphene composite nickel sulfide according to claim 1, characterized in that: In the step (1), the freeze-drying time is 12 to 72 hours.

6. The method for preparing graphene composite nickel sulfide according to claim 1, characterized in that: In the step (2), the heating rate of the high temperature heat treatment process is 2 to 5°C / min.

7. The method for preparing graphene-composite nickel sulfide according to claim 1, characterized in that: In the step (2), the insulation temperature range of the high temperature heat treatment process is 400 to 1000° C.; the insulation time range is 1 to 10 hours.

8. The method for preparing graphene-composite nickel sulfide according to claim 1, characterized in that: In the step (2), the inert atmosphere is one or both of argon and nitrogen.

9. A graphene composite nickel sulfide prepared by the method for preparing graphene composite nickel sulfide according to any one of claims 1 to 8.

10. A sodium ion battery, comprising a negative electrode, a positive electrode, a separator between the positive and negative electrodes, and an electrolyte, characterized in that: The negative electrode is prepared from the graphene composite nickel sulfide according to claim 9.

Citation Information

Patent Citations

  • Nano-NiS / graphene composite anode material and preparation method thereof

    CN104134783A

  • Preparation method for nitrogen-doped graphene-coated nickel sulfide composite electrode material

    CN105895882A

  • Preparation method of composite cathode material for aluminum ion battery, and aluminum ion battery

    CN111668459A

  • NiS / graphene and carbon composite material as well as preparation method and application thereof

    CN114388763A

  • Hierarchical mesoporous graphene / Ni-Co-S array on 3-dimensional nickel foam composite and preparation method thereof

    KR1020170094872A