Preparation method of combined AG effect glass cover plate
Through one-time etching treatment and sandblasting process, the existing combined AG effect glass cover preparation process is solved, and the smooth transition and feel of AG effect are achieved, and the production process is simplified.
Patent Information
- Application Number
- CN202411150413.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-19
AI Technical Summary
The preparation process of the existing combined AG effect glass cover is complex, requiring at least 2 etchings, which is high cost, and the height difference between the two AG effects is large, which affects the feel and combination effect of the product.
By using a one-time etching treatment method, by sticking the film on the glass cover plate and sandblasting, and then etching in the etching liquid, the combination of two AG effects is achieved, the transition at the junction is smooth, the height difference is <0.01mm, and the process is simplified and Reduce costs.
The smooth transition between the two AG effects is achieved, which improves the feel of the product, saves multiple silk screening processes, significantly reduces costs and process cycles, simplifies operations, and is suitable for the production of combined AG effect glass covers.
Smart Images

Figure CN118978342A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of glass processing, and in particular to a method for preparing a combined AG effect glass cover plate. Background Art
[0002] Glass cover plates used for mobile phones, computers, etc. usually have only one AG effect. In order to increase the diversity of the appearance of glass cover plates, a glass cover plate with a combined AG effect is proposed, which can form a variety of combined effects by splicing at least two AG effects.
[0003] Taking the glass cover with combined AG effect formed by the combination of two AG effects as an example, the current preparation process of the glass cover with combined AG effect is generally: first protect the second preset area with silk screen ink, then etch the first preset area once, then remove the ink layer of the second preset area, then protect the silk screen ink of the first preset area, etch it twice, and then remove the ink layer of the first preset area, so as to obtain the combined AG effect. This process is complicated and cumbersome, and requires at least 2 etchings, and the etching process and etching liquid of the 2 etchings are not the same, which makes the production cost high, and after 2 etchings, the height difference at the junction of the two AG effects is greater than 0.025mm, which will obviously affect the feel of the product; in addition, there will be a problem of deviation when silk screen printing ink, generally the deviation is 0.15-0.25mm, and repeated silk screen printing will further increase the error, thereby affecting the overall combination effect of the product. Summary of the invention
[0004] Based on the technical problems existing in the background technology, the present invention proposes a preparation method for a combined AG effect glass cover plate. The preparation method of the present invention can achieve two AG effects after one etching treatment, and the transition at the junction of the two AG effects is smooth, and the height difference is less than 0.01mm, thereby improving the feel of the product; and the method has low cost, short process cycle, simple operation and easy production.
[0005] The present invention provides a preparation method of a combined AG effect glass cover plate, comprising the following steps: pasting a film on one side of the glass cover plate to form a film pasting area, then sandblasting the entire glass surface pasted with the film, then removing the film, placing the glass surface in an etching solution for etching, and obtaining the combined AG effect glass cover plate.
[0006] Preferably, after the sandblasting process, evenly distributed pits are formed in the area of the glass where the film is not applied, and there are no pits in the area where the film is applied.
[0007] Preferably, the depth of the pits is ≤ 0.01 μm.
[0008] Preferably, the combined AG effect is formed by the cooperation of two AG effects, and the height difference at the junction of the two AG effects is less than 0.01 mm.
[0009] The preparation method of the present invention can achieve two AG effects through one etching treatment, and the transition between the two AG effects is smooth without height difference, which can increase the feel of the product, eliminate multiple silk screen processes, and only perform one etching treatment, which can greatly save costs and shorten the process cycle.
[0010] Before the etching process, the glass may be ultrasonically cleaned to remove impurities.
[0011] The portion of the glass cover plate that does not require etching may be protected by a film or a silk-screen coating.
[0012] The above-mentioned etching liquid can be a commercially available ordinary AG etching liquid, a low-flash AG etching liquid, etc.; the etching parameters are not limited, and the etching liquid and etching parameters are selected according to different combined AG effects.
[0013] Preferably, the thickness of the film is 0.08-1.0 mm.
[0014] Preferably, the film is a polyethylene film.
[0015] The film can be cut into a preset pattern in advance and then pasted on the glass cover; the film has a base film and an adhesive layer, which is convenient for pasting and tearing. The thickness of the film is the total thickness of the base film and the adhesive layer.
[0016] Preferably, the sand number of the sandblasting is 420-600#, the sandblasting pressure is 1.0-2.0 bar, and the distance between the sandblasting port and the glass surface is 20-30 cm.
[0017] During the above-mentioned sandblasting treatment, the moving speed of the material-carrying conveyor belt is 6-20 mm / s, and the swing frequency of the spray gun is 30-45 r / min.
[0018] Preferably, the sandblasting material is one of green silicon carbide, corundum and ceramic sand.
[0019] The present invention selects a suitable film and sandblasting process, and after sandblasting the entire glass surface with the film, evenly distributed pits are formed in the area without the film, and there are no pits in the area with the film; thus, a combined AG effect is formed after etching.
[0020] The preparation method of the present invention can achieve two AG effects through one etching process, and the transition between the two AG effects is smooth, and the height difference is less than 0.01mm, thereby improving the feel of the product; and multiple silk-screen processes are omitted, and only one etching process is performed, which can reduce the cost by 30-40% compared with the existing process, and has a short process cycle, simple operation, and is easy to produce. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 These are cross-sectional photographs of the interface between two AG effects in the combined AG effect glass cover plate obtained in Example 3 and Comparative Example 4, wherein a is Example 3 and b is Comparative Example 4.
[0022] Figure 2 This is a photo of the combined AG effect glass cover plate prepared in Example 2.
[0023] Figure 3 This is a photo of the combined AG effect glass cover plate prepared in Example 3. DETAILED DESCRIPTION
[0024] The technical solution of the present invention is described in detail below through specific embodiments.
[0025] Example 1
[0026] A method for preparing a combined AG effect glass cover plate comprises the following steps:
[0027] Take a polyethylene film with a thickness of 0.1 mm (the polyethylene film includes: a polyethylene base film, an adhesive layer and a release paper), cut it into a preset pattern by laser, then remove the release paper, and stick the film on one side of the 2D glass cover to form a film-sticking area;
[0028] Then put it on the conveyor belt, and sandblast the entire glass surface with the film. The sandblasting material is green silicon carbide, the sand number is 420#, the sandblasting pressure is 2.0bar, and the distance between the sandblasting port and the glass surface is 20cm. The moving speed of the conveyor belt is 20mm / s, and the swing frequency of the spray gun is 30r / min.
[0029] Then the film was torn off and ultrasonically cleaned with water. On the obtained glass cover plate, evenly distributed pits were formed in the area without film on the sandblasted surface, and there were no pits in the area with film, and the depth of the pits was 0.01 μm.
[0030] Then, it was placed in an etching solution (the etching solution was purchased from Zhengzhou Henghao Optical Technology Co., Ltd.) for etching treatment, etched at 30-32°C for 4 minutes, taken out, washed with water, and dried to obtain a combined AG effect glass cover plate, which was formed by the combination of two AG effects, and the height difference at the junction of the two AG effects was 0.009mm.
[0031] Example 2
[0032] A method for preparing a combined AG effect glass cover plate comprises the following steps:
[0033] Take a polyethylene film with a thickness of 1.0 mm (the polyethylene film includes: a polyethylene base film, an adhesive layer and a release paper), cut it into a preset pattern by laser, then remove the release paper, and stick the film on one side of the 2D glass cover to form a film-sticking area;
[0034] Then put it on the conveyor belt, and sandblast the entire glass surface with the film. The sandblasting material is green silicon carbide, the sand number is 500#, the sandblasting pressure is 1.5bar, and the distance between the sandblasting port and the glass surface is 25cm. The moving speed of the conveyor belt is 10mm / s, and the swing frequency of the spray gun is 45r / min.
[0035] Then the film was torn off and ultrasonically cleaned with water. On the obtained glass cover plate, evenly distributed pits were formed in the area without film on the sandblasted surface, and there were no pits in the area with film, and the depth of the pits was 0.007 μm.
[0036] Then, it was placed in a low-flash etching solution (the low-flash etching solution was purchased from Zhengzhou Henghao Optical Technology Co., Ltd.) for etching treatment, etched at 30-32°C for 4 minutes, taken out, washed with water, and dried to obtain a combined AG effect glass cover plate, which is formed by the combination of two AG effects, and the height difference at the junction of the two AG effects is 0.005mm.
[0037] Example 3
[0038] A method for preparing a combined AG effect glass cover plate comprises the following steps:
[0039] Take a polyethylene film with a thickness of 0.1 mm (the polyethylene film includes: a polyethylene base film, an adhesive layer and a release paper), cut it into a preset pattern by laser, then remove the release paper, and stick the film on one side of the 2D glass cover to form a film-sticking area;
[0040] Then put it on the conveyor belt, and sandblast the entire glass surface with the film. The sandblasting material is green silicon carbide, the sand number is 500#, the sandblasting pressure is 1.0 bar, and the distance between the sandblasting port and the glass surface is 30cm. The moving speed of the conveyor belt is 10mm / s, and the swing frequency of the spray gun is 30r / min.
[0041] Then the film was torn off and ultrasonically cleaned with water. On the obtained glass cover plate, evenly distributed pits were formed in the area without film on the sandblasted surface, and there were no pits in the area with film, and the depth of the pits was 0.004 μm.
[0042] Then, it was placed in an etching solution (the etching solution was purchased from Zhengzhou Henghao Optical Technology Co., Ltd.) for etching treatment, etched at 30-32°C for 4 minutes, taken out, washed with water, and dried to obtain a combined AG effect glass cover plate, which was formed by the combination of two AG effects, and the height difference at the junction of the two AG effects was 0.003mm.
[0043] Comparative Example 1
[0044] The sandblasting pressure is 3.0 bar, the distance between the sandblasting port and the glass surface is 15 cm, and the rest is the same as in Example 3. The obtained combined AG effect glass cover plate is formed by combining two AG effects, but the fragmentation rate during the sandblasting process reaches 25%, and the sandblasting pressure is too high, which affects the performance of the subsequent glass after strengthening.
[0045] Comparative Example 2
[0046] The sandblasting pressure is 0.5 bar, the distance between the sandblasting port and the glass surface is 35 cm, and the rest is the same as in Example 3. There is only one AG effect on the glass cover plate, and no combined AG effect can be formed.
[0047] Comparative Example 3
[0048] The thickness of the polyethylene film is 0.05 mm. Other aspects are the same as those of Example 3. There is only one AG effect on the glass cover plate, and no combined AG effect can be formed.
[0049] Comparative Example 4 (Existing Process)
[0050] A method for preparing a combined AG effect glass cover plate comprises the following steps:
[0051] First, the silk-screen ink of the second preset area is protected, and then the first preset area is etched once at 30-32°C for 4 minutes, and then the ink layer of the second preset area is removed, and then the silk-screen ink of the first preset area is protected, and a second etching is performed at 16-20°C for 90s, and then the ink layer of the first preset area is removed, so as to obtain a combined AG effect.
[0052] The etching solution used in the first etching and the second etching in the above-mentioned comparative example 4 is the same as the etching solution in the embodiment 3.
[0053] Figure 1 These are cross-sectional photographs of the interface between two AG effects in the combined AG effect glass cover plate obtained in Example 3 and Comparative Example 4, wherein a is Example 3 and b is Comparative Example 4.
[0054] Depend on Figure 1It can be seen that in the AG effect glass cover plate obtained in Example 3, the height difference at the junction of the two AG effects is only 0.003 mm, while the height difference at the junction of the two AG effects in Comparative Example 4 is 0.025 mm, which is much greater than that in Example 3.
[0055] Figure 2 This is a photo of the combined AG effect glass cover plate prepared in Example 2.
[0056] Figure 3 This is a photo of the combined AG effect glass cover plate prepared in Example 3.
[0057] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for preparing a combined AG effect glass cover plate, characterized in that: The method comprises the following steps: pasting a film on one side of a glass cover plate to form a film pasting area, then sandblasting the entire glass surface pasted with the film, then removing the film, placing the glass surface into an etching solution for etching, and obtaining a combined AG effect glass cover plate.
2. The method for preparing the combined AG effect glass cover plate according to claim 1, characterized in that: After sandblasting, evenly distributed pits are formed in the unfilmed area of the glass, while there are no pits in the filmed area.
3. The method for preparing the combined AG effect glass cover plate according to claim 2, characterized in that: The depth of the pit is ≤0.01μm.
4. The method for preparing the combined AG effect glass cover plate according to any one of claims 1 to 3, characterized in that: The combined AG effect is formed by the cooperation of two AG effects, and the height difference at the junction of the two AG effects is less than 0.01 mm.
5. The method for preparing the combined AG effect glass cover plate according to any one of claims 1 to 4, characterized in that: The thickness of the film is 0.08-1.0 mm.
6. The method for preparing the combined AG effect glass cover plate according to any one of claims 1 to 5, characterized in that: The film is a polyethylene film.
7. The method for preparing the combined AG effect glass cover plate according to any one of claims 1 to 6, characterized in that: The sand number for sandblasting is 420-600#, the sandblasting pressure is 1.0-2.0bar, and the distance between the sandblasting port and the glass surface is 20-30cm.
8. The method for preparing the combined AG effect glass cover plate according to any one of claims 1 to 7, characterized in that: The sandblasting material is one of green silicon carbide, corundum and ceramic sand.
Citation Information
Patent Citations
Glass with matte paper effect and preparation method thereof
CN113716875A
Glass cover plate with starry sky AG effect and preparation method thereof
CN115550479A