Anti-flowing water synchronous grouting material for muck foundation in water-rich karst area and preparation method of anti-flowing water synchronous grouting material
By using anti-moving water-resistant synchronous grouting materials composed of sulfate cement in the karst area, the problems of uncontrollable diffusion and high cost of existing grouting materials are solved, and a green, efficient and environmentally friendly filling effect in the karst area is achieved.
Patent Information
- Application Number
- CN202411052113.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-01
AI Technical Summary
In the construction of underground engineering in karst areas, the diffusion distance of existing grouting materials is uncontrollable, which can easily induce groundwater pollution, is expensive, and the urban environment is fragile, making it difficult to meet the needs of green and efficient filling.
It is made of sulfate cement, quicklime, slag, fly ash, hydroxypropyl methylcellulose, 2-ethylhexylphosphate-2-ethylhexylphosphate, sodium tripolyphosphate, sodium dodecyl sulfate, poly The slag-based anti-moving water-resistant synchronous grouting material composed of acrylamide and calcium formate in water-rich karst areas can improve the anti-shrinkage performance and fluidity of the materials through the synergistic effect of components, achieving green and non-toxic synchronous grouting.
It achieves efficient and environmentally friendly filling in the urban environment of karst areas, reduces costs, has good anti-shrink performance and water retention rate, and meets the needs of synchronous grouting.
Abstract
Description
Technical Field
[0001] The invention relates to the field of underground engineering, and in particular to a synchronous grouting material for slag foundation anti-dynamic water in a water-rich karst area and a preparation method thereof. Background Art
[0002] The statements herein merely provide background information related to the present invention and do not necessarily constitute prior art.
[0003] Karst areas account for nearly 1 / 3 of my country's land area, and many cities are located in karst areas. During the construction of underground projects in karst areas, there are many disaster sources such as water-rich fissures, caves, and pipelines, which often show characteristics such as large water volume and high flow rate. In particular, the urban environment is fragile. During tunnel construction, the diffusion distance of grouting materials is uncontrollable and the slurry materials are not environmentally friendly, which can easily induce groundwater pollution and threaten the water safety of residents. In addition, the cost of grouting materials in karst areas is currently high. Summary of the invention
[0004] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a synchronous grouting material for slag foundation in water-rich karst areas and a preparation method thereof. The synchronous grouting material has good anti-scouring performance and can achieve green and efficient filling under urban karst water conditions.
[0005] In order to achieve the above object, the present invention is implemented through the following technical solutions:
[0006] In the first aspect, the present invention provides a synchronous grouting material for slag-based anti-dynamic water in water-rich karst areas, which is composed of the following components, measured by mass: 15 to 18 parts of sulfate cement, 1 to 2 parts of quicklime, 90 to 120 parts of slag, 10 to 12 parts of fly ash, 0.1 to 0.2 parts of hydroxypropyl methylcellulose, 0.3 to 0.4 parts of 2-ethylhexyl phosphate-2-ethylhexyl ester, 0.2 to 0.4 parts of sodium tripolyphosphate, 0.4 to 0.5 parts of sodium dodecyl sulfate, 0.05 to 0.1 parts of polyacrylamide, 0.6 to 0.9 parts of calcium formate, and 60 to 80 parts of water.
[0007] The effects of each component and the synergistic effects between the components are:
[0008] Sulfate cement: Sulphoaluminate cement has the characteristic of rapid solidification, which can ensure the initial solidification of the slurry before the protective layer is washed away, thereby improving the solidification rate of the slurry.
[0009] Slag: It is used as aggregate to fill the slurry and contains certain silicon and aluminum minerals. It has certain gelling activity and can reduce the amount of cement and fly ash.
[0010] Fly ash: It has volcanic ash effect, can be used as a cementitious material to enhance the strength of the slurry, and has micro-aggregate effect, which can fill pores and improve the impermeability of the slurry structure; it has micro-ball effect, has lubricity, and can improve the fluidity of the slurry.
[0011] Quicklime: It can stimulate the activity of slag and fly ash, thereby improving the strength of the slurry.
[0012] Hydroxypropyl methylcellulose: It can form a three-dimensional network structure inside the slurry, thereby improving the slurry's anti-scouring performance.
[0013] 2-Ethylhexyl Phosphate: Stimulates the activity of admixtures in the material, effectively improves the fluidity of the material, and improves the cohesiveness of the material.
[0014] Sodium tripolyphosphate: Promotes the absorption of water in cement, improves the fluidity and ductility of cement, thereby enhancing the strength and toughness of the material; improves the material's anti-permeability.
[0015] Sodium dodecyl sulfate: superplasticizer. When the clay content increases, the slurry viscosity becomes too high, resulting in poor fluidity. This material can significantly improve the slurry's resistance to mud.
[0016] Polyacrylamide: It has lubricity and flocculation effects, improving the injectability and anti-scouring ability of the slurry.
[0017] Calcium formate: It can form a complex with the cementitious material, thereby promoting the rapid coagulation and solidification of the material.
[0018] In some embodiments, the mesh size of the quicklime is 150-200 meshes. If the mesh size is too large, the reaction is too intense, resulting in too high a slurry temperature and accelerated coagulation. If the mesh size is too small, the specific surface area is large, the contact is insufficient, and the activity of the slag cannot be effectively stimulated.
[0019] In some embodiments, the specific surface area of sulphoaluminate cement is 400 to 600 m 2 / kg. The setting time of this cement with a water-cement ratio of 0.5 is 5 to 20 minutes.
[0020] In some embodiments, the fly ash has a specific surface area of 200 to 500 m 2 / kg, density is 2.2-2.6g / cm 3 .
[0021] In some embodiments, the molecular weight of polyacrylamide is 10 million to 18 million.
[0022] In some embodiments, sodium tripolyphosphate, sodium dodecyl sulfate, 2-ethylhexyl phosphate, and calcium formate are all analytically pure.
[0023] In a second aspect, the present invention provides a method for preparing the water-rich karst area slag-based anti-water synchronous grouting material, comprising the following steps: uniformly mixing the components according to a mass ratio to obtain the material.
[0024] The beneficial effects achieved by one or more embodiments of the present invention are as follows:
[0025] The water-rich karst area slag-based anti-water dynamic synchronous grouting material of the present invention is green, non-toxic, and highly erosion-resistant, and can meet the synchronous grouting needs of underground projects in urban environments in karst areas. The main materials are easy to obtain, and both water dynamic resistance and low-cost grouting are taken into account. DETAILED DESCRIPTION
[0026] It should be noted that the following detailed descriptions are illustrative and intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0027] The present invention will be further described below in conjunction with the embodiments.
[0028] Example 1
[0029] The invention discloses a synchronous grouting material for slag-based water-dynamic resistance in water-rich karst areas, which is composed of the following components in parts by mass: 18 parts of sulfate cement, 105 parts of slag, 12 parts of fly ash, 1.5 parts of quicklime, 0.3 parts of sodium tripolyphosphate, 0.4 parts of sodium lauryl sulfate, 0.3 parts of 2-ethylhexyl phosphate-2-ethylhexyl ester, 0.1 parts of hydroxypropyl methylcellulose, 0.05 parts of polyacrylamide, 0.8 parts of calcium formate and 75 parts of water.
[0030] The selected sulphoaluminate cement setting time is 10 min, and the fly ash specific surface area is 500 m 2 / kg, density 2.4g / cm 3 , the mesh number of quicklime is 180 mesh, and the molecular weight of polyacrylamide is 15 million.
[0031] The components are mixed uniformly according to the mass ratio to form the synchronous grouting material for slag foundation anti-dynamic water in water-rich karst area.
[0032] Specifically, the slurry prepared according to the above ratio was mixed and tested by the inverted cup method. The initial setting time was 4 hours, the final setting time was 10 hours, the truncated cone flow distance of the slurry was greater than 20 cm, the material solidity rate was 99%, and the 28-day compressive strength was 3 MPa.
[0033] After the fluidity test was carried out using a truncated cone test mold, a covering scouring test was carried out on the round cake formed by the material. The water flow velocity was 0.4m / s and the dynamic water retention rate was 95%.
[0034] Example 2
[0035] A synchronous grouting material for slag-based anti-dynamic water in water-rich karst areas, comprising the following components in parts by mass:
[0036] 18 parts of sulfate cement, 105 parts of slag, 12 parts of fly ash, 1.5 parts of quicklime, 0.3 parts of sodium tripolyphosphate, 0.1 parts of hydroxypropyl methylcellulose, 0.05 parts of polyacrylamide, 0.8 parts of calcium formate, and 75 parts of water.
[0037] The selected sulphoaluminate cement setting time is 10 min, and the fly ash specific surface area is 500 m 2 / kg, density 2.4g / cm 3 , the mesh number of quicklime is 180 mesh, and the molecular weight of polyacrylamide is 15 million.
[0038] The components are mixed uniformly according to the mass ratio to form the synchronous grouting material for slag foundation anti-dynamic water in water-rich karst area.
[0039] Specifically, the slurry prepared according to the above ratio has an initial setting time of 3.5 hours, a final setting time of 9 hours, a truncated cone flow distance of 16 cm, a material solidity rate of 98.5%, and a 28-day compressive strength of 2.8 MPa.
[0040] After the fluidity test was carried out using a truncated cone test mold, a covering scouring test was carried out on the round cake formed by the material. The water flow velocity was 0.4m / s and the dynamic water retention rate was 96%.
[0041] Example 3
[0042] A synchronous grouting material for slag-based anti-dynamic water in water-rich karst areas, comprising the following components in parts by mass:
[0043] According to the mass ratio, add 18 parts of sulfate cement, 105 parts of slag, 12 parts of fly ash, 1.5 parts of quicklime, 0.3 parts of sodium tripolyphosphate, 0.4 parts of sodium dodecyl sulfate, 0.3 parts of 2-ethylhexyl phosphate-2-ethylhexyl ester, 0.1 parts of hydroxypropyl methylcellulose, 0.05 parts of polyacrylamide and 75 parts of water.
[0044] The selected sulphoaluminate cement setting time is 10 min, and the fly ash specific surface area is 500 m 2 / kg, density 2.4g / cm 3 , the mesh number of quicklime is 180 mesh, and the molecular weight of polyacrylamide is 15 million.
[0045] The components are mixed uniformly according to the mass ratio to form the synchronous grouting material for slag foundation anti-dynamic water in water-rich karst area.
[0046] Specifically, the slurry prepared according to the above ratio has an initial setting time of 6 hours, a final setting time of 15 hours, a truncated cone flow distance of the slurry greater than 20 cm, a material solidity rate of 94%, and a 28-day compressive strength of 2.6 MPa.
[0047] After the fluidity test was carried out using a truncated cone test mold, a covering scouring test was carried out on the round cake formed by the material. The water flow velocity was 0.4m / s and the dynamic water retention rate was 88%.
[0048] Comparative Example 1
[0049] The difference from Example 1 is that quicklime is omitted, and the rest is the same as Example 1.
[0050] Specifically, the slurry prepared according to the above ratio has an initial setting time of 5 hours, a final setting time of 14 hours, a truncated cone flow distance of the slurry greater than 22 cm, a material solidity rate of 90%, and a 28-day compressive strength of 2.2 MPa.
[0051] After the fluidity test was carried out using a truncated cone test mold, a covering scouring test was carried out on the round cake formed by the material. The water flow velocity was 0.4m / s and the dynamic water retention rate was 80%.
[0052] Comparative Example 2
[0053] The difference from Example 1 is that hydroxypropyl methylcellulose is omitted, and the rest is the same as Example 1.
[0054] Specifically, the slurry prepared according to the above ratio has an initial setting time of 3.5 hours, a final setting time of 8 hours, a truncated cone flow distance of the slurry greater than 24 cm, a material solidity rate of 85%, and a 28-day compressive strength of 2.8 MPa.
[0055] After the fluidity test was carried out using a truncated cone test mold, a covering scouring test was carried out on the round cake formed by the material. The water flow velocity was 0.4m / s and the dynamic water retention rate was 30%.
[0056] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A synchronous grouting material for slag foundation against dynamic water in water-rich karst areas. Features: The invention is composed of the following components in parts by mass: 15-18 parts of sulfate cement, 1-2 parts of quicklime, 90-120 parts of slag, 10-12 parts of fly ash, 0.1-0.2 parts of hydroxypropyl methylcellulose, 0.3-0.4 parts of 2-ethylhexyl phosphate-2-ethylhexyl ester, 0.2-0.4 parts of sodium tripolyphosphate, 0.4-0.5 parts of sodium dodecyl sulfate, 0.05-0.1 parts of polyacrylamide, 0.6-0.9 parts of calcium formate and 60-80 parts of water.
2. The water-rich karst area slag foundation anti-dynamic water synchronous grouting material according to claim 1, Features: The invention is composed of the following components by mass: 15-18 parts of sulfate cement, 1-2 parts of quicklime, 90-110 parts of slag, 10-12 parts of fly ash, 0.1-0.2 parts of hydroxypropyl methylcellulose, 0.3-0.4 parts of 2-ethylhexyl phosphate-2-ethylhexyl ester, 0.2-0.4 parts of sodium tripolyphosphate, 0.4-0.5 parts of sodium lauryl sulfate, 0.05-0.1 parts of polyacrylamide, 0.6-0.9 parts of calcium formate and 60-70 parts of water.
3. The water-rich karst area slag foundation anti-dynamic water synchronous grouting material according to claim 2, Features: The invention is composed of the following components in parts by mass: 15-18 parts of sulfate cement, 1-2 parts of quicklime, 100-110 parts of slag, 10-12 parts of fly ash, 0.1-0.2 parts of hydroxypropyl methylcellulose, 0.3-0.4 parts of 2-ethylhexyl phosphate-2-ethylhexyl ester, 0.2-0.4 parts of sodium tripolyphosphate, 0.4-0.5 parts of sodium lauryl sulfate, 0.05-0.1 parts of polyacrylamide, 0.6-0.9 parts of calcium formate and 60-70 parts of water.
4. The water-rich karst area slag-based water-resistant synchronous grouting material according to any one of claims 1 to 3, Features: The mesh number of the quicklime is 150 to 200 meshes.
5. The water-resistant synchronous grouting material for slag foundation in water-rich karst areas according to any one of claims 1 to 3, Features: The specific surface area of sulphoaluminate cement is 400~600m 2 / kg.
6. The water-rich karst area slag foundation water-resistant synchronous grouting material according to any one of claims 1 to 3, Features: The specific surface area of fly ash is 200~500m 2 / kg.
7. The water-rich karst area slag foundation anti-dynamic water synchronous grouting material according to claim 6, Features: The density of fly ash is 2.2-2.6g / cm 3 .
8. The synchronous grouting material for slag foundation in water-rich karst areas according to any one of claims 1 to 3, Features: The molecular weight of polyacrylamide is 10 million to 18 million.
9. The synchronous grouting material for slag foundation in water-rich karst areas according to any one of claims 1 to 3, Features: Sodium tripolyphosphate, sodium dodecyl sulfate, 2-ethylhexyl phosphate, and calcium formate were all analytically pure.
10. The method for preparing the water-rich karst area slag-based anti-water synchronous grouting material according to any one of claims 1 to 9, comprising the following steps: uniformly mixing the components according to the mass ratio to obtain the material.
Citation Information
Patent Citations
Water-dispersion-resistant slurry with controllable initial setting time for shield synchronous grouting and preparation method
CN110183189A
Dispersion-resistant and high-impermeability grouting material under flowing water condition as well as preparation method and application thereof
CN115504747A
Subway muck slurry modification method and low-carbon concrete based on modified subway muck slurry
CN117361996A
Early-strength and high-toughness grouting material and preparation method thereof
CN117720363A
Novel green dispersion-resistant synchronous grouting material for water-rich stratum and preparation method of novel green dispersion-resistant synchronous grouting material
CN117865593A