Repair method for blocky SiCf / SiC ceramic matrix composite component

Through the connection of mortise and tenon structures and the cross-winding reinforcement of fiber lines, combined with the CVI deposition process, the material matching and performance stability problems in the repair of SiCf/SiC ceramic matrix composite materials are solved, and efficient and economical repair results are achieved, significantly reducing the repair Cost and operational complexity.

CN118978408AActive Publication Date: 2024-11-19INST OF ENGINEERING THERMOPHYSICS - CHINESE ACAD OF SCI +1

Patent Information

Application Number
CN202411063892.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-19
Estimated Expiration
2044-08-05

AI Technical Summary

Technical Problem

The existing SiCf/SiC ceramic matrix composite repair process has problems such as insufficient filling interface strength, complex bonding process and unstable mechanical properties, high fiber braiding cost and difficult interface processing, making it difficult to achieve good matching between the material and the matrix and overall stable performance. .

Method used

The dovetail-shaped convex structure connection, fiber line cross-winding reinforcement and CVI deposition repair process are adopted to form dovetail-shaped convex structure and groove connection through cutting pretreatment, fiber prefabricated body repair, fiber line reinforcement and CVI deposition repair steps to ensure that after repair The material properties are consistent with the raw materials and reduce repair costs and operational complexity.

Benefits of technology

The good matching between the repair material and the matrix material is achieved, the tensile and bending resistance after repair is improved, the repair cost and operation complexity is significantly reduced, and the stable repair at the fracture of the material is ensured and the stability of overall performance is ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978408A_ABST
    Figure CN118978408A_ABST
Patent Text Reader

Abstract

The invention discloses a repair method for a blocky SiCf / SiC ceramic matrix composite component. The repair method mainly comprises the steps of processing pretreatment, fiber preform repair, fiber line reinforcement, CVI deposition repair and the like. In the processing pretreatment step, a damaged material is cut and processed into a dovetail-shaped bulge, and the thickness of the part is slightly reduced, so that a space is reserved for winding of fiber wires. In the fiber prefabricated body repairing step, ceramic fibers are woven into a prefabricated body with the thickness consistent with that of the dovetail-shaped protrusion in a 2.5 D mode, an inner groove matched with the prefabricated body is machined, and the prefabricated body is spliced with a material to be repaired in a mortise and tenon joint structure mode. In the fiber line reinforcing step, SiC fiber lines are used for crosswise winding the tenon-and-mortise connection part in the mutually perpendicular direction for reinforcing. In the CVI deposition repairing step, fiber preforms and fiber lines are deposited by means of a CVI process to form the SiCf / SiC ceramic-based composite material, and the SiCf / SiC ceramic-based composite material is tightly connected with a to-be-repaired part by means of matching of a dovetail-shaped part and cross winding of the fiber lines, so that the damaged material is repaired.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of composite material repair, and relates to the preparation and repair technology of ceramic-based composite materials, and specifically is a SiC composite material that adopts mortise and tenon structure connection, fiber line cross winding reinforcement and CVI deposition repair processes. f Repair method of SiC ceramic matrix composite components. Background Art

[0002] SiC f / SiC ceramic matrix composite material is a new type of composite material with high strength, high temperature resistance, corrosion resistance and other characteristics. It is usually made of SiC fiber as reinforcement and SiC ceramic as matrix through chemical vapor infiltration (CVI) or liquid phase sintering (LPS) and other processes. It is widely used in the manufacture of key structural components in the fields of aerospace, chemical industry, vehicle manufacturing, etc., and plays an important role. In these applications, SiC f The high performance of SiC / SiC composites enables them to maintain stable physical and chemical properties in extreme environments.

[0003] However, in practical engineering applications, SiC f / SiC composite materials can be damaged due to changes in the service environment, long-term use or unexpected accidents. These damages may take the form of microcracks, holes, surface erosion or local fractures, affecting the structural integrity and performance stability of the material, making it impossible for the material to continue to serve and requiring replacement of components. f SiC fiber is an important raw material for SiC composite materials. The economic cost of SiC fiber is high, and it takes a lot of time to re-make parts that meet the requirements. Therefore, in order to save economic costs and shorten the project cycle, SiC fiber, which is mainly in block form, is used to manufacture parts that meet the requirements. f / SiC ceramic-based composite materials use repair technology to achieve the reuse of damaged materials while ensuring unchanged performance, which has certain engineering value.

[0004] Existing repair processes for bulk SiC f / SiC ceramic-based composite materials are repaired mainly by filling repair, interlayer bonding repair, fiber reinforcement repair and other methods. However, these processes adopted by the existing technology have certain limitations and shortcomings in practical applications, such as: (1) The filling material used in the filling repair process needs to have a high degree of matching with the matrix material. If the material used is not highly matched and the performance difference is large, it may lead to insufficient strength of the filling interface. (2) The interlayer bonding repair process requires precise control of parameters such as adhesive concentration, temperature, and pressure. The operation is relatively complicated and mistakes are prone to occur during the bonding process, affecting the experimental results. At the same time, the bonding interface only relies on the performance of the adhesive itself to connect the repair material and the matrix material, which can easily lead to changes in the mechanical properties of the repaired material at the fracture, weakening the tensile and bending resistance, and affecting the service life of the material after repair. (3) Common fiber-reinforced repairs use the damaged material as the matrix and re-weave the material with fibers. However, for SiC f / SiC ceramic-based composite materials, the consumption of re-weaving SiC fibers is too large and the cost is high. In addition, weaving based on damaged materials will make it difficult to handle the interface between the preform and the matrix, especially the repair of the fracture of the original damaged material, which is a more complicated operation.

[0005] In summary, the existing repair processes have limitations to varying degrees in practical applications. The filling repair process is difficult to ensure the strength and stability of the filling interface; the interlayer bonding repair process is complicated to operate, and the mechanical properties of the repaired material are unstable; the fiber reinforcement repair process is costly and difficult to deal with the interface problem between the preform and the matrix. Therefore, how to repair bulk SiC f / SiC ceramic-based composite materials, so that it can achieve the matching of repair materials and matrix materials on the basis of cost saving, the stability of the overall performance of the material after repair, and the repair treatment of the material fracture, have become technical problems that need to be solved urgently. Summary of the invention

[0006] (I) Purpose of the invention

[0007] For existing SiC f In order to solve at least one of the above and other technical problems in the prior art, the present invention aims to provide a method for repairing bulk SiC ceramic matrix composite materials, which has defects and shortcomings such as insufficient strength of the filling interface, complex bonding process and unstable mechanical properties, high fiber weaving cost and difficult interface treatment. fA repair method for SiC / SiC ceramic-based composite components is designed to process a dovetail-shaped protrusion structure at the fracture of the damaged material, and to process the same dovetail-shaped groove at the connection of the SiC fiber preform, and use the mortise and tenon connection of the two and the subsequent reinforcement of the SiC fiber line to solve the problems of mismatch between existing repair materials and raw materials, reduced tensile and bending properties of repaired materials and high repair costs. It not only achieves a good match between the repair material and the matrix material, ensures the overall stability of the repaired material, and effectively handles the repair of the material fracture, but also significantly reduces the repair cost and operation complexity, thereby having significant engineering value and economic benefits in practical applications.

[0008] (II) Technical solution

[0009] In order to achieve the purpose of the invention and solve the technical problems, the present invention adopts the following technical solutions:

[0010] The present invention provides a method for bulk SiC f / SiC ceramic matrix composite component repair method for repairing bulk SiC f The damaged part of the SiC ceramic matrix composite material at least includes the steps of cutting pretreatment, fiber preform repair, fiber wire reinforcement and CVI deposition repair. Specifically:

[0011] SS1. Cutting pre-treatment steps

[0012] For damaged bulk SiC f / SiC ceramic-based composite materials are cut and processed to remove the damaged part to form the material to be repaired, and a dovetail-shaped protrusion with reduced thickness is cut out at the original fracture surface to be connected with the repair part in the form of mortise and tenon joints;

[0013] SS2.Fiber preform repair steps

[0014] The SiC fiber woven preform is first processed into a shape that meets the requirements of the material to be repaired, and then installed in conjunction with the material to be repaired in the form of mortise and tenon joints to ensure the tensile strength of the material after repair. The shape of the SiC fiber preform is processed into the required contour of the block material, and the connection between the SiC fiber preform and the material to be repaired is processed into a groove with the same shape and similar size as the dovetail protrusion, and the thickness is consistent with the dovetail protrusion, so that the mortise and tenon joint can be closely matched during installation, and the repaired material can have stable tensile strength.

[0015] SS3. Fiber line reinforcement steps

[0016] At the mortise and tenon joints between the SiC fiber preform and the material to be repaired, SiC fiber wires are used to reinforce the mortise and tenon joints in the form of cross-winding. The winding directions of the SiC fiber wires are perpendicular to each other to form a grid structure. At the same time, the thickness reduction of the mortise and tenon joints provides space for the winding of the SiC fiber wires, ensuring that the size and roughness of the repaired material will not change due to the presence of the SiC fiber wires. Through this cross-winding method, while ensuring a stable connection between the two, the bending resistance of the material after repair is enhanced;

[0017] SS4.CVI Deposits Repair Steps

[0018] The material to be repaired, which is installed with a fiber preform and reinforced with fiber wire winding, is placed in a chemical vapor deposition furnace for chemical vapor deposition. During the CVI process, the SiC fiber preform and SiC fiber wire are deposited with a SiC matrix to make them the same and mutually matching ceramic matrix composite materials as the material to be repaired, ensuring that the repaired material is consistent with the original damaged material in composition and structure, thereby ensuring the matching of performance and achieving the goal of repairing the damaged SiC f Repair of SiC composites.

[0019] (III) Technical Effect

[0020] Compared with the prior art, the repair method for blocky SiCf / SiC ceramic matrix composite material components of the present invention has the following beneficial and significant technical effects:

[0021] (1) The material to be repaired and the repair part are connected by a mortise and tenon structure, and the connection interface is dovetail-shaped, which not only achieves a close fit between the fiber preform and the material to be repaired, but also ensures that the connection interface will not be separated due to external stretching with the help of the dovetail-shaped structure, thereby enhancing the tensile strength of the repaired material.

[0022] (2) Use SiC fiber wires to cross-wrap the material to be repaired and the repaired part to strengthen the connection between the two and further improve the tensile strength of the repaired material. At the same time, the cross-wrap fiber wires can also decompose the stress caused by bending of the material and improve the bending resistance of the repaired material. Due to the reduction in thickness of the mortise and tenon joint, space is left for the winding of the SiC fiber wire, so that the size and roughness of the repaired material will not change due to the SiC fiber wire.

[0023] (3) The repair part is a fiber preform woven from SiC fibers, and the fiber wire for winding reinforcement is also SiC fiber. Both become SiC after the SiC matrix is ​​deposited by the CVI process. f / SiC composite materials match the properties of the original damaged material and will not affect the performance of the repaired material due to differences in material properties.

[0024] (4) Since only a small amount of SiC fibers are used to make the repair part and the reinforcement part spliced ​​with the material to be repaired, and no large amount of fibers are used to reweave with the material to be repaired as the matrix, this method saves the economic cost and time cost of the repair material. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 is a flow chart of a method for repairing a bulk SiCf / SiC ceramic matrix composite component;

[0026] Figure 2 is a damaged bulk SiC used in the embodiments of the present invention f Schematic diagram of / SiC ceramic matrix composite material;

[0027] Figure 3 is a schematic diagram of cutting pretreatment steps in an embodiment of the present invention;

[0028] Figure 4 is a schematic diagram of the fiber preform repairing steps according to an embodiment of the present invention;

[0029] Figure 5 is a schematic diagram of fiber line reinforcement steps according to an embodiment of the present invention;

[0030] Figure 6 It is a complete block SiC after CVI deposition repair used in the embodiment of the present invention. f Schematic diagram of / SiC ceramic matrix composite material.

[0031] The technical features indicated by the reference numerals in the figure are:

[0032] 1. Damaged bulk SiC f / SiC ceramic matrix composite material; 2. Damaged part; 3. Dovetail protrusion; 4. SiC fiber preform; 5. SiC fiber line; 6. Complete block SiC f / SiC ceramic matrix composite materials. DETAILED DESCRIPTION

[0033] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0034] For existing SiC fThe present invention provides a method for repairing damaged SiC ceramic matrix composite materials. f The repair method of SiC / SiC ceramic matrix composite components mainly includes the steps of cutting pretreatment, fiber preform repair, fiber wire reinforcement and CVI deposition repair, which not only achieves a good match between the repair material and the matrix material, ensures the overall stability of the repaired material, effectively handles the repair of the material fracture, but also significantly reduces the repair cost and operation complexity, thereby having significant engineering value and economic benefits in practical applications.

[0035] Figure 2 Schematic diagram of damaged bulk SiCf / SiC ceramic matrix composite. As a specific example, Figure 1 As shown, for the repair of damaged bulk SiCf / SiC ceramic matrix composite materials, the repair method of the present invention mainly includes the following specific steps when implemented:

[0036] SS1. Cutting pre-treatment steps

[0037] For damaged bulk SiC f / SiC ceramic-based composite materials are cut and processed to remove the damaged part to form the material to be repaired, and a dovetail-shaped protrusion with a reduced thickness is cut out at the original fracture surface to be connected with the repair part in the form of mortise and tenon joints.

[0038] Specifically, if Figure 3 As shown, Figure 2 Damaged bulk SiC with damaged portion 2 f The / SiC ceramic matrix composite material 1 is subjected to cutting pretreatment, the damaged portion 2 is processed into a dovetail-shaped protrusion 3, and the thickness is reduced to facilitate installation and connection with the fiber preform during subsequent repair.

[0039] In a more preferred embodiment, the dovetail protrusion 3 obtained by cutting the damaged material should have a shape of a dovetail protrusion with a narrower inner side and a wider outer side. In order to achieve stable tensile properties at the connection between the material to be repaired and the repaired part, the outer cross-sectional area of ​​the dovetail protrusion 3 should be slightly larger than the inner cross-sectional area. In order to prevent stress concentration, the outer contour of the dovetail protrusion should be polished into an arc-shaped curve. In order to make the material after fiber wire winding and reinforcement consistent with the size of the raw material, it is necessary to reduce the thickness of the protruding part to leave space for the subsequent fiber wire winding and reinforcement. In addition, after cutting the dovetail protrusion 3, it is preferred to perform laser texturing on its surface; the laser parameters are: power 100-500W, scanning speed 50-200mm / s, spot diameter 50-200μm; by forming a microstructure on the surface, the contact area between the material to be repaired and the repaired part can be increased, and the interface bonding strength can be improved.

[0040] SS2.Fiber preform repair steps

[0041] The SiC fiber woven preform is first processed into a shape that meets the requirements of the material to be repaired, and then installed in conjunction with the material to be repaired in the form of mortise and tenon joints to ensure the tensile strength of the material after repair. The shape of the SiC fiber preform is processed into the required contour of the block material, and the connection between it and the material to be repaired is processed into a groove with the same shape and similar size as the dovetail protrusion, and its thickness is consistent with the dovetail protrusion, so that a tight fit of the mortise and tenon joint can be achieved during installation, and at the same time, the repaired material can have stable tensile strength.

[0042] Specifically, if Figure 4 As shown, the SiC fiber preform 4 used for repair is processed so that it has a groove of the same shape and the same thickness as the dovetail protrusion 3 at the connection point, so as to fit tightly with the part to be repaired through the mortise and tenon connection and enhance the tensile strength of the material after repair.

[0043] In a more preferred embodiment, the processed SiC fiber preform 4 is used as the repair part to ensure that the damaged material can be consistent with the raw material after CVI deposition repair. After the SiC fiber is woven into a block preform with the same thickness as the dovetail protrusion 3 by the 2.5D method, a dovetail-shaped groove needs to be processed on the side where the preform 4 is spliced ​​with the material to be repaired, so as to achieve the mortise and tenon connection and precise installation with the material to be repaired with the dovetail-shaped protrusion. The dovetail-shaped groove should be consistent with the shape and size of the dovetail-shaped protrusion of the material to be repaired, and in order to prevent stress concentration, the inner contour should be polished into an arc-shaped curve.

[0044] SS3. Fiber line reinforcement steps

[0045] In the mortise and tenon connection part between the SiC fiber preform and the material to be repaired, SiC fiber wires are used to reinforce the mortise and tenon connection part in the form of cross-winding. The winding directions of the SiC fiber wires are perpendicular to each other to form a grid structure. At the same time, the thickness reduction of the mortise and tenon connection part provides space for the winding of the SiC fiber wires, ensuring that the size and roughness of the repaired material will not change due to the presence of the SiC fiber wires. Through this cross-winding method, while ensuring the stable connection between the two, the bending resistance of the material after repair is enhanced.

[0046] Specifically, if Figure 5 As shown, the SiC fiber wire 5 is used to reinforce the material on which the SiC fiber preform 4 is installed. The specific method is to cross-wrap the SiC fiber wire 5 around the thickness reduction part of the mortise and tenon connection, and the winding directions are perpendicular to each other.

[0047] In a more preferred embodiment, the fiber wire 5 used for winding and reinforcing the material to be repaired and the repaired part should be SiC fiber, so that the damaged material can be consistent with the raw material after CVI deposition repair. The winding of the fiber wire 5 should be carried out only in the mortise and tenon joint part with thickness reduction. When winding and reinforcing, first select an edge perpendicular to the material fracture as the starting edge, and start winding from this edge in a direction at an angle of 45° to the edge of the material, and then start from the opposite side of the starting edge, and continue winding perpendicular to the direction of the existing coil, and finally fix the fiber wire used for winding. This step realizes the reinforcement of the material to be repaired and the repaired part, and also improves the bending resistance of the repaired material. In addition, the SiC fiber wire is preferably surface-modified before winding, and chemically treated with a silane coupling agent, the immersion time is 1-3 hours, and the temperature is 60-80°C, so as to improve the interface bonding strength between the SiC fiber wire and the matrix, reduce the interface debonding phenomenon, and improve the overall mechanical properties of the repaired part.

[0048] SS4.CVI Deposits Repair Steps

[0049] The material to be repaired, which is installed with a fiber preform and reinforced with fiber wire winding, is placed in a chemical vapor deposition furnace for chemical vapor deposition. During the CVI process, the SiC fiber preform and SiC fiber wire are deposited with a SiC matrix to make them the same and mutually matching ceramic matrix composite materials as the material to be repaired, ensuring that the repaired material is consistent with the original damaged material in composition and structure, thereby ensuring the matching of performance and achieving the goal of repairing the damaged SiC f Repair of SiC composites.

[0050] Specifically, if Figure 6 As shown, the repaired material is subjected to a CVI process to deposit the SiC fiber preform 4 and the SiC fiber wire 5 into SiC f / SiC ceramic matrix composite material, matching the original damaged material, and at the same time making the repaired part and the material to be repaired closely combined to form a complete block of SiC f / SiC ceramic matrix composites6.

[0051] In a more preferred embodiment, the deposition temperature of the CVI deposition repair step is preferably controlled between 800°C and 1200°C, the deposition pressure is maintained in the range of 10-100 Pa, the deposition time is 10 to 20 hours, and the deposition gas should be a gas mixture containing silicon and carbon, specifically including methyltrichlorosilane and hydrogen, with a gas flow ratio of 1:5 to 1:10. By precisely controlling these parameters, it is possible to ensure that the SiC matrix is ​​uniformly deposited on the SiC fiber preform and the SiC fiber line, thereby obtaining a repair effect consistent with the performance of the raw materials, and improving the overall performance and service life of the repaired material. In addition, the CVI deposition process can also use pulsed CVI technology, that is, the flow rate and pressure of the reaction gas are periodically changed during the deposition process; the pulse period is 30-120 seconds, and the duty cycle is 40-60%; this method can increase the penetration depth of the SiC matrix inside the fiber preform, reduce the porosity, and improve the density and mechanical properties of the repaired part.

[0052] In a further preferred embodiment, after completing the above steps SS1 to SS4, the repaired material can also be heat treated at a temperature of 1200-1400°C for 2-5 hours in an inert gas argon environment to release the residual stress generated during the repair process, improve the structural stability of the material, and promote interface bonding, thereby further improving the repair effect.

[0053] In addition, after completing the above steps SS1 to SS4, the repaired material surface can be further subjected to plasma spraying treatment, with the spraying material being SiC, the same as the substrate, and the spraying thickness being 50-200 μm, to further seal the surface pores, improve the surface density and oxidation resistance of the material, and repair possible surface microscopic defects, thereby improving the overall performance and appearance quality of the material.

[0054] Repairing bulk SiC according to the present invention f The method of making a preform repair part and a fiber line reinforcement part by using a small amount of SiC fiber, and at the same time, by processing the connection between the repair part and the material to be repaired, the stability of the performance of the material after repair is ensured, the tensile and bending resistance of the material is improved, and the economic cost and time cost of repair are saved.

[0055] Through the above embodiments, the purpose of the present invention is fully and effectively achieved. Those skilled in the art can understand that the present invention includes but is not limited to the contents described in the drawings and the above specific embodiments. Although the present invention has been described with respect to the most practical and preferred embodiments currently considered, it should be understood that the present invention is not limited to the disclosed embodiments, and any modification that does not deviate from the functional and structural principles of the present invention will be included in the scope of the claims.

Claims

1. A SiC f / SiC ceramic matrix composite material component repair method, characterized in that: The repair method comprises at least the following steps: SS1. Damaged bulk SiC f / SiC ceramic-based composite materials are cut and processed to remove the damaged part to form the material to be repaired, and a dovetail-shaped protrusion with reduced thickness is cut out at the original fracture surface to be connected with the repair part in the form of mortise and tenon joints; SS2. First, the SiC fiber woven preform is processed into a shape that meets the requirements of the material to be repaired, and it is used as the repair part, and then installed with the material to be repaired in the form of mortise and tenon joints to ensure the tensile strength of the material after repair. The shape of the SiC fiber preform is processed into the required contour of the block material, and the connection between it and the material to be repaired is processed into a groove with the same shape and similar size as the dovetail protrusion, and the thickness of the groove is consistent with the dovetail protrusion, so that the mortise and tenon joint can be closely matched during installation, and the repaired material has stable tensile strength. SS3. At the mortise and tenon joints between the SiC fiber preform and the material to be repaired, SiC fiber wires are used for reinforcement in the form of cross winding. The winding directions of the SiC fiber wires are perpendicular to each other and form a grid structure. At the same time, the thickness reduction of the dovetail-shaped protrusion provides space for the winding of the SiC fiber wires, ensuring that the size and roughness of the repaired material will not change due to the presence of the SiC fiber wires; SS4. The material to be repaired, which is installed with SiC fiber preform and reinforced with SiC fiber wire, is placed in a chemical vapor deposition furnace for chemical vapor deposition. During the CVI process, SiC matrix is ​​deposited on the SiC fiber preform and SiC fiber wire to make them into ceramic matrix composite materials that are the same as and match the material to be repaired, ensuring that the repaired material is consistent with the original damaged material in composition and structure, thereby ensuring the matching of performance and achieving the goal of repairing the damaged SiC. f Repair of SiC composites.

2. The repair method according to claim 1, characterized in that: In the above step SS1, the shape of the raised part obtained by cutting the damaged material should be a dovetail-shaped protrusion with a narrower inner side and a wider outer side. The outer cross-sectional area of ​​the dovetail-shaped protrusion should be slightly larger than the inner cross-sectional area to enhance the tensile strength of the connection between the material to be repaired and the repaired part; and in order to prevent stress concentration, the outer contour of the dovetail-shaped protrusion should be polished into an arc-shaped curve; at the same time, in order to make the material after SiC fiber wire winding and reinforcement consistent with the size of the raw material, it is necessary to reduce the thickness of the raised part to leave space for the subsequent winding and reinforcement of the fiber wire.

3. The repair method according to claim 1, characterized in that: In the above step SS1, after cutting the dovetail-shaped protrusion, the surface is laser texturing processed, and the laser parameters are power 100-500W, scanning speed 50-200mm / s, and spot diameter 50-200μm. By forming a microstructure on the surface, the contact area between the material to be repaired and the repair part is increased.

4. The repair method according to any one of claims 1 to 3, characterized in that: In the above step SS2, the processed SiC fiber preform is used as the repair part to ensure that the damaged material can be consistent with the raw material after CVI deposition repair. After the SiC fiber is woven into a block preform with the same thickness as the dovetail-shaped protrusion by the 2.5D method, a dovetail groove needs to be processed on the side where the preform is spliced ​​with the material to be repaired, so as to achieve the mortise and tenon connection and precise installation with the material to be repaired having the dovetail-shaped protrusion, and the dovetail groove should be consistent with the shape and size of the dovetail protrusion of the material to be repaired, and in order to prevent stress concentration, the inner contour of the dovetail groove should be polished into an arc curve.

5. The repair method according to claim 1, characterized in that: In the above step SS3, the fiber wire used for winding and reinforcing the material to be repaired and the repaired part should be SiC fiber, so that the damaged material can be consistent with the original material after CVI deposition repair; the winding of the SiC fiber wire should only be carried out on the mortise and tenon connection part with thickness reduction, and when winding and reinforcing, first select an edge perpendicular to the material fracture as the starting edge, and start winding from this edge in a direction at an angle of 45° to the edge of the material, and then start from the opposite side of the starting edge, continue winding perpendicular to the direction of the existing coil, and finally fix the fiber wire used for winding.

6. The repair method according to claim 1, characterized in that: In the above step SS3, the SiC fiber line is surface modified before winding, and chemically treated with a silane coupling agent, with an immersion time of 1-3 hours and a temperature of 60-80°C to improve the interface bonding strength between the fiber line and the matrix and reduce interface debonding.

7. The repair method according to claim 1, characterized in that: In the above step SS4, the deposition temperature of the CVI deposition repair step should be controlled between 800°C and 1200°C, the deposition pressure should be maintained in the range of 10-100Pa, the deposition time should be 10 to 20 hours, and the deposition gas should be a gas mixture containing silicon and carbon, specifically including methyltrichlorosilane and hydrogen, with a gas flow ratio of 1:5 to 1:

10.

8. The repair method according to claim 1, characterized in that: In the above step SS4, the CVI deposition process adopts pulse CVI technology, and the flow rate and pressure of the reaction gas are periodically changed during the deposition process. The pulse period is 30-120 seconds and the duty cycle is 40-60% to increase the penetration depth of the SiC matrix inside the fiber preform and reduce the porosity.

9. The repair method according to claim 1, characterized in that: After completing the above steps SS1 to SS4, the repaired material is heat treated at a temperature of 1200-1400°C for 2-5 hours in an inert gas argon environment to release the residual stress generated during the repair process, improve the structural stability of the material, and promote interface bonding.

10. The repair method according to claim 1, characterized in that: After completing the above steps SS1 to SS4, the repaired material surface is subjected to plasma spraying treatment. The spraying material is SiC, which is the same as the substrate, and the spraying thickness is 50-200 μm, so as to further seal the surface pores, improve the surface density and oxidation resistance of the material, and repair possible surface microscopic defects to improve the overall performance and appearance quality of the material.

Citation Information

Patent Citations

  • Method for repairing heat damage crackles of ceramic based composite material

    CN104446666A

  • Defect repair method of carbon fiber reinforced carbon fiber composite material

    CN106986664A

  • SiC nanowire toughened PyC / SiC composite interface of SiCf / SiC composite material and preparation method of SiC nanowire toughened PyC / SiC composite interface

    CN114315395A

  • Method for repairing carbon fiber toughened ceramic matrix composite component

    CN115536436A

  • Method for repairing local damage and microcrack of small and medium-sized SiCf / SiC composite material

    CN116143549A

Cited By

  • SiC / SiC composite material in-situ weaving repairing method and application

    CN121110267A

  • SiC / SiC composite material in-situ weaving repair method and application

    CN121110267B

  • SiC / SiC composite material sewing repair method and application

    CN121132908A