Quaterphenyl pyridine derivative for electrochromic material as well as preparation method and application thereof

By introducing heavy atoms F, Cl, Br into the tetrabiphenylpyridine derivatives, the light absorption capacity and structural stability of electrochromic materials are improved, and the problem of insufficient response speed and cycle life of existing materials is solved, achieving high The light transmittance and fast response electrochromic effect is suitable for smart dimming windows and other fields.

CN118978478AActive Publication Date: 2024-11-19YILAICHUANG (BEIJING) INTELLIGENT MATERIAL TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411056883.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-19
Estimated Expiration
2044-08-02

AI Technical Summary

Technical Problem

Existing electrochromic materials have shortcomings in response speed, cycle life and optical contrast, which cannot meet the needs of fast dimming and are costly, and the preparation process is complicated.

Method used

Using tetrabiphenylpyridine derivatives, the light absorption capacity and structural stability of the material are improved by introducing heavy atoms F, Cl, Br, and specific preparation methods such as reaction with bromine alkanes and exchange of hexafluorophosphate. Electrochromic materials with high light transmittance and fast response are produced.

Benefits of technology

It realizes obvious color changes of the material at different voltages, high response speed and long cycle life, improves the practicality and reliability of electrochromic materials, and reduces resource consumption and waste generation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978478A_ABST
    Figure CN118978478A_ABST
Patent Text Reader

Abstract

Some embodiments disclose a tetrabiphenyl pyridine derivative for an electrochromic material, comprising a compound represented by the following general formula: # imgabs0 # wherein X is any one of F, Cl and Br, Y is ethyl or n-hexyl; the electrochromic material is prepared from the compound shown in the general formula. The obtained electrochromic material comprises the compound shown in the general formula, ferrocene, poly (vinylidene fluoride-co-hexafluoropropylene) and ionic liquid, and the molar ratio of the compound to the ferrocene to the poly (vinylidene fluoride-co-hexafluoropropylene) to the ionic liquid is 4: 1: 15: 60. The ionic liquid is 1-butyl-3-methylimidazolium bis (trifluoromethylsulfonyl) imine or 1-ethyl-3-methylimidazolium tetrafluoroborate, and the ionic liquid is 1-butyl-3-methylimidazolium bis (trifluoromethylsulfonyl) imine. Heavy atoms F, Cl and Br are introduced into a quaterphenyl pyridine structure, the light absorption capacity is effectively improved, the color change significance is enhanced, the thin-layer structure of the quaterphenyl pyridine derivative has excellent light transmittance, and meanwhile, the structural stability and durability of an electrochromic material in the electrochromic process are provided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electrochromic materials, and in particular relates to a quaternary biphenylpyridine derivative for electrochromic materials and a preparation method and application thereof. Background Art

[0002] With the development of modern architecture and the automotive industry, there is an increasing demand for smart dimming windows, which can automatically adjust transparency according to external light conditions, thereby improving energy efficiency, protecting privacy and improving indoor comfort.

[0003] In the current market, smart dimming window technology mainly relies on electrochromic (EC) materials. Traditional EC materials mainly include inorganic materials and organic materials. These materials have been widely used in smart dimming windows, rearview mirrors, displays and other fields. Inorganic materials usually have excellent stability and durability, but their response speed is slow, the preparation process is complex and the cost is high. Organic materials have the advantages of fast response speed, rich color changes and simple preparation process, but their cycle life and optical contrast are usually low.

[0004] Typical EC materials consist of an active layer, an ion conductive layer, and an electrode layer. The active layer is the key part to achieve color change. Under an applied voltage, the material undergoes oxidation and reduction through an electrochemical reaction, resulting in a change in color. The ion conductive layer is responsible for providing an ion conduction path, while the electrode layer is used to apply voltage and transmit current. The performance of EC materials is mainly evaluated through the following indicators: optical contrast: the difference in light transmittance of the material under different voltages; response time: the time required for the material to switch from one color state to another; cycle life: the performance stability of the material after multiple cycles; and transmittance: the light transmittance of the material in a transparent state.

[0005] In summary, although the existing EC materials have achieved certain applications in the field of smart dimming windows, there are still some problems that need to be solved. The color change response speed of inorganic materials is slow, which makes it difficult to meet the needs of fast dimming, while the cycle life of organic materials is short, and performance will decay after long-term use; the transmittance difference of some materials under different voltages is not obvious, and the optical contrast is low, which affects the dimming effect; the preparation process of some inorganic materials is complicated and costly, which limits their large-scale application. For example, patent CN106959564A discloses a window glass with electrochromic properties, which has a structure of two transparent conductive layer glasses with a layer of electrochromic liquid sandwiched between them and sealed with a polymer adhesive. The conductive layer is a glass with a thin film of indium tin oxide, polythiophene, etc. coated on the surface. The electrochromic liquid uses bipyridyl salt compounds as cathode color-changing materials, and ferrocene or phenazine compounds as anode color-changing materials. The invention has a simple process and low cost, and is suitable for window glass of smart buildings and vehicles. However, it has the following shortcomings:

[0006] The molar absorption coefficients of bipyridyl salts and ferrocene or phenazine compounds may have certain limitations in different wavelength ranges, and may show lower absorption capacity at certain wavelengths in the visible light range, resulting in less significant or uneven color changes, thus affecting the overall visual effect and performance of electrochromic window glass;

[0007] The molecular structures of bipyridyl salts and ferrocene or phenazine compounds may be non-planar to a certain extent, resulting in reduced intermolecular stacking efficiency, thereby affecting the electrochromic performance, causing the color change rate to slow down, the contrast to decrease, and the cycle life to shorten. Summary of the invention

[0008] In view of this, on the one hand, some embodiments disclose a quaternary pyridine derivative for electrochromic materials, comprising a compound represented by the following general formula (I), or a hexafluorophosphate of the compound represented by the general formula (I):

[0009]

[0010] Wherein, X is any one of F, Cl, and Br, and Y is ethyl or n-hexyl.

[0011] On the other hand, some embodiments disclose a method for preparing a quaternary biphenylpyridine derivative for an electrochromic material, comprising:

[0012] The compound represented by the general formula (II) is reacted with a brominated alkane to obtain a compound represented by the general formula (I);

[0013] The general formula (II) is:

[0014]

[0015] Wherein, X is any one of F, Cl, and Br, and the brominated alkane is methyl bromide or 1-bromohexane.

[0016] On the other hand, some embodiments disclose the use of quaternary biphenylpyridine derivatives for electrochromic materials, and the electrochromic materials are prepared using the compounds represented by the general formula (I).

[0017] The method for preparing a quaternary pyridine derivative for an electrochromic material disclosed in an embodiment of the present invention, wherein the prepared quaternary pyridine derivative introduces heavy atoms F, Cl, and Br into the quaternary pyridine structure, effectively increasing the light absorption capacity and enhancing the significance of color change, and the thin layer structure of the quaternary pyridine derivative has excellent light transmittance, while providing structural stability and durability of the electrochromic material during the electrochromic process. The quaternary pyridine derivative can show obvious color changes under different DC voltages, and this color change can be identified and distinguished by the RGB color model, so that the material can quickly and accurately adjust the light transmittance in practical applications; the electrochromic response is fast, the material completes color conversion in a short time, the color contrast is high, and obvious visual differences under different states are ensured; the cycle life is long, and the practicality and reliability of the electrochromic material are improved. DETAILED DESCRIPTION

[0018] The word "embodiment" used herein as an "exemplary" does not necessarily mean that any embodiment described is superior or better than other embodiments. Performance index tests in the embodiments of the present invention are performed using conventional test methods in the art unless otherwise specified. It should be understood that the terms described in the embodiments of the present invention are only used to describe specific implementation methods and are not intended to limit the contents disclosed in the embodiments of the present invention.

[0019] Unless otherwise specified, the technical and scientific terms used herein have the same meanings as commonly understood by ordinary technicians in the technical field to which the embodiments of the present invention belong; other experimental methods and technical means not specifically specified in the embodiments of the present invention refer to experimental methods and technical means commonly used by ordinary technicians in the field.

[0020] The terms "substantially" and "approximately" used herein are used to describe small fluctuations. For example, they can refer to less than or equal to ±5%, such as less than or equal to ±2%, such as less than or equal to ±1%, such as less than or equal to ±0.5%, such as less than or equal to ±0.2%, such as less than or equal to ±0.1%, such as less than or equal to ±0.05%. The numerical data represented or presented in the range format herein are used only for convenience and brevity, and should therefore be flexibly interpreted as including not only the values ​​clearly listed as the limits of the range, but also all independent values ​​or sub-ranges contained in the range. For example, the numerical range of "1-5%" should be interpreted as including not only the clearly listed values ​​of 1% to 5%, but also the independent values ​​and sub-ranges within the range shown. Therefore, independent values ​​such as 2%, 3.5% and 4% and sub-ranges such as 1%-3%, 2%-4% and 3%-5% are included in this numerical range. This principle also applies to the range of only one numerical value. In addition, such an interpretation applies regardless of the width of the range or the characteristics described.

[0021] In this document, including in the claims, transitional words such as "comprises," "includes," "with," "having," "containing," "involving," "accommodating," etc. are understood to be open-ended, i.e., meaning "including but not limited to." Only the transitional words "consisting of" and "composed of" are closed transitional words.

[0022] In order to better illustrate the present invention, numerous specific details are provided in the specific examples below. It should be understood by those skilled in the art that the present invention can be implemented without certain specific details. In the embodiments, some methods, means, instruments, equipment, etc. well known to those skilled in the art are not described in detail in order to highlight the gist of the present invention.

[0023] Under the premise of no conflict, the technical features disclosed in the embodiments of the present invention may be arbitrarily combined, and the resulting technical solutions belong to the contents disclosed in the embodiments of the present invention.

[0024] Some embodiments disclose a quaternary biphenylpyridine derivative for electrochromic materials, comprising a compound represented by the following general formula (I):

[0025]

[0026] Wherein, X is any one of F, Cl, and Br, and Y is ethyl or n-hexyl.

[0027] Some embodiments disclose a quaternary biphenylpyridine derivative for electrochromic materials, wherein X in the general formula (I) is F, Y is ethyl, and the compound is 3,3'-difluoro-1,1'-diethyl-[4,4'-bipyridine]-1,1'-diimine.

[0028] In some embodiments, the tetraphenylpyridine derivative for electrochromic materials disclosed in the general formula (I) is Cl, and Y is ethyl. The compound is 3,3'-dichloro-1,1'-diethyl-[4,4'-bipyridine]-1,1'-diimine.

[0029] Some embodiments disclose a quaternary biphenylpyridine derivative for electrochromic materials, wherein X in the general formula (I) is Br, Y is ethyl, and the compound is 3,3'-dibromo-1,1'-diethyl-[4,4'-bipyridine]-1,1'-diimine.

[0030] Some embodiments disclose a quaternary biphenylpyridine derivative for electrochromic materials, wherein X in the general formula (I) is F, Y is hexyl, and the compound is 3,3'-difluoro-1,1'-dihexyl-[4,4'-bipyridine]-1,1'-diimine.

[0031] Some embodiments disclose a quaternary biphenylpyridine derivative for electrochromic materials, wherein X in the general formula (I) is Cl, Y is hexyl, and the compound is 3,3'-dichloro-1,1'-dihexyl-[4,4'-bipyridine]-1,1'-diimine.

[0032] Some embodiments disclose a quaternary biphenylpyridine derivative for electrochromic materials, wherein X in the general formula (I) is Br, Y is hexyl, and the compound is 3,3'-dibromo-1,1'-dihexyl-[4,4'-bipyridine]-1,1'-diimine.

[0033] Some embodiments disclose a method for preparing a quaternary biphenylpyridine derivative for electrochromic materials, comprising:

[0034] The compound represented by the general formula (II) and the bromoalkane are dissolved in a solvent, condensed and refluxed at 80° C., and reacted for 24 hours. After the reaction is complete, a light yellow solid is precipitated to obtain the compound represented by the general formula (I); acetonitrile and dichloromethane can usually be selected as the solvent; dichloromethane is a more preferred solvent; using dichloromethane solvent can improve solubility and reaction efficiency, reduce energy consumption and reaction time, and at the same time, room temperature operation is safer and reduces the risk of high temperature operation;

[0035] The general formula (II) is:

[0036]

[0037] Wherein, X is any one of F, Cl, and Br, and the brominated alkane is methyl bromide or 1-bromohexane;

[0038] The compound represented by the general formula (I) is recrystallized from ethanol for purification;

[0039] The recrystallized product is dissolved in deionized water and heated to 60° C. to dissolve. After ammonium hexafluorophosphate is fully dissolved in deionized water, it is slowly added dropwise. The hexafluorophosphate ions exchange with the bromide ions to replace the bromide ions in the structure of the compound of the general formula (I), thereby obtaining the hexafluorophosphate salt of the compound of the general formula (I).

[0040] As an optional embodiment, the recrystallized product is dissolved in deionized water, heated to 40°C to dissolve, and after ammonium hexafluorophosphate is fully dissolved in deionized water, it is slowly added dropwise to perform an ion exchange reaction to replace the bromide ions in the structure of the compound of general formula (I). After the system is no longer turbid, the addition is stopped, and then heated to 60°C and stirred for 2 hours, and then filtered to obtain the hexafluorophosphate of the compound represented by general formula (I). By reducing the heating temperature during the ion exchange process, the possible decomposition risk can be reduced, and the stirring time can be increased to ensure that the reaction is complete, improve the purity and stability of the product, and ensure efficient production of the product.

[0041] Some embodiments disclose the application of a quaternary biphenylpyridine derivative for an electrochromic material, wherein the electrochromic material is prepared using a compound represented by the general formula (I); the electrochromic material comprises a compound represented by the general formula (I) or a hexafluorophosphate thereof, ferrocene, poly(vinylidene fluoride-co-hexafluoropropylene) and an ionic liquid, wherein the molar ratio is 4:1:15:60; the ionic liquid is 1-butyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide or 1-ethyl-3-methylimidazolium tetrafluoroborate. Typically, the compound represented by the general formula (I), ferrocene, poly(vinylidene fluoride-co-hexafluoropropylene) and the ionic liquid are dissolved in an acetone solution according to a set molar ratio to obtain an electrochromic solution.

[0042] Furthermore, the electrochromic solution was cast onto a glass slide to obtain a uniform free-standing EC gel.

[0043] To make an electrochromic device (ECD), we cut the EC gel into the desired shape with a razor blade and transferred it to the target location. Then, the gel was sandwiched between another substrate with an ITO coating and firmly fixed with double-sided tape to obtain an electrochromic device (ECD). The ECD was powered with different DC voltages to analyze the color development effect and operational stability. Among them, the ITO coating is a tin-doped indium oxide coating.

[0044] Generally, electrochromic materials derived from tetraphenylpyridine can be applied to smart dimming windows, which can automatically adjust transparency according to external light conditions and user needs. High response speed and optical contrast ensure that users can quickly obtain the desired dimming effect, improving the comfort of living and working environment; by adjusting the light and heat entering the room, it can effectively reduce the energy consumption of air conditioning and lighting, and help improve the energy efficiency of buildings.

[0045] The electrochromic materials derived from tetraphenylpyridine can also be applied to other optical adjustment devices, such as rearview mirrors, displays, and goggles, etc. Their fast response and excellent light transmittance make them perform well in these applications.

[0046] The technical details are further illustrated below in conjunction with embodiments.

[0047] Example 1

[0048] Preparation of Compound 1,1'-Diethyl-3,3'-difluoro-[4,4'-bipyridine]-1,1'-diimine

[0049] The basic reaction is:

[0050]

[0051] The preparation method comprises the steps of:

[0052] ① First, weigh 1g of 3,3'-difluoro-4,4'-bipyridine and 5g of ethyl bromide into a beaker, add acetonitrile to dissolve, condense and reflux at 80°C, react for 24h, and after the reaction is complete to precipitate a light yellow solid, filter and dry to obtain a light yellow solid 1,1'-diethyl-3,3'-difluoro-[4,4'-bipyridine]-1,1'-diimine;

[0053] ② Then, the obtained light yellow solid was recrystallized and purified with ethanol;

[0054] ③ Preferably, the purified product is dissolved in deionized water, heated to 60°C to dissolve, the ammonium hexafluorophosphate is fully dissolved in water and then slowly added dropwise into the reaction, and the addition is stopped when the system is no longer turbid, and then stirred for 1 hour and then filtered and dried to obtain the hexafluorophosphate salt of the compound: hexafluorophosphate-1,1'-diethyl-3,3'-difluoro-[4,4'-bipyridine]-1,1'-diimine.

[0055] Example 2

[0056] Preparation of Compound 3,3'-Dichloro-1,1'-diethyl-[4,4'-bipyridine]-1,1'-diimine

[0057] The basic reaction is:

[0058]

[0059] The preparation method comprises the steps of:

[0060] ① First, weigh 1g 3,3'-dichloro-4,4'-bipyridine and 5g ethyl bromide into a beaker, add acetonitrile to dissolve, condense and reflux at 80°C, react for 24h, and after the reaction is complete to precipitate a light yellow solid, filter and dry to obtain a light yellow solid 1,1'-diethyl-3,3'-dichloro-[4,4'-bipyridine]-1,1'-diimine;

[0061] ② Then, the obtained light yellow solid was recrystallized and purified with ethanol;

[0062] ③Finally, the purified product was dissolved in deionized water and heated to 60°C to dissolve. After the ammonium hexafluorophosphate was fully dissolved in water, it was slowly added dropwise into the reaction. The addition was stopped when the system was no longer turbid. After stirring for 1 hour, the mixture was filtered and dried to obtain the hexafluorophosphate salt of the compound: hexafluorophosphate-1,1'-diethyl-3,3'-dichloro-[4,4'-bipyridine]-1,1'-diimine.

[0063] Example 3

[0064] Preparation of Compound 3,3'-Dibromo-1,1'-diethyl-[4,4'-bipyridine]-1,1'-diimine

[0065] The basic reaction is:

[0066]

[0067] The preparation method comprises the steps of:

[0068] ① First, weigh 1g 3,3'-dibromo-4,4'-bipyridine and 5g bromoethane into a beaker, add acetonitrile to dissolve, condense and reflux at 80°C, react for 24h, and after the reaction is complete to precipitate a light yellow solid, filter and dry to obtain a light yellow solid 1,1'-diethyl-3,3'-dibromo-[4,4'-bipyridine]-1,1'-diimine;

[0069] ② Then, the obtained light yellow solid was recrystallized and purified with ethanol;

[0070] ③Finally, the purified product was dissolved in deionized water and heated to 60°C to dissolve. After the ammonium hexafluorophosphate was fully dissolved in water, it was slowly added dropwise into the reaction. The addition was stopped when the system was no longer turbid. After stirring for 1 hour, the mixture was filtered and dried to obtain the hexafluorophosphate salt of the compound: hexafluorophosphate-1,1'-diethyl-3,3'-dibromo-[4,4'-bipyridine]-1,1'-diimine.

[0071] Example 4

[0072] Preparation of Compound 3,3'-Difluoro-1,1'-dihexyl-[4,4'-bipyridine]-1,1'-diimine

[0073] The basic reaction is:

[0074]

[0075] The preparation method comprises the steps of:

[0076] ① First, weigh 1g 3,3'-difluoro-4,4'-bipyridine and 5g bromohexane into a beaker, add acetonitrile to dissolve, condense and reflux at 80°C, react for 24h, and after the reaction is complete to precipitate a light yellow solid, filter and dry to obtain a light yellow solid 1,1'-dihexyl-3,3'-difluoro-[4,4'-bipyridine]-1,1'-diimine;

[0077] ② Then, the obtained light yellow solid was recrystallized and purified with ethanol;

[0078] ③Finally, the purified product was dissolved in deionized water and heated to 60°C to dissolve. After the ammonium hexafluorophosphate was fully dissolved in water, it was slowly added dropwise into the reaction. The addition was stopped when the system was no longer turbid. After stirring for 1 hour, the mixture was filtered and dried to obtain the hexafluorophosphate salt of the compound: hexafluorophosphate-1,1'-dihexyl-3,3'-difluoro-[4,4'-bipyridine]-1,1'-diimine.

[0079] Example 5

[0080] Preparation of Compound 3,3'-Dichloro-1,1'-dihexyl-[4,4'-bipyridine]-1,1'-diimine

[0081] The basic reaction is:

[0082]

[0083] The preparation method comprises the steps of:

[0084] ① First, weigh 1g 3,3'-dichloro-4,4'-bipyridine and 5g bromohexane into a beaker, add acetonitrile to dissolve, condense and reflux at 80°C, react for 24h, and after the reaction is complete to precipitate a light yellow solid, filter and dry to obtain a light yellow solid 1,1'-dihexyl-3,3'-dichloro-[4,4'-bipyridine]-1,1'-diimine;

[0085] ② Then, the obtained light yellow solid was recrystallized and purified with ethanol;

[0086] ③Finally, the purified product was dissolved in deionized water and heated to 60°C to dissolve. After the ammonium hexafluorophosphate was fully dissolved in water, it was slowly added dropwise into the reaction. The addition was stopped when the system was no longer turbid. After stirring for 1 hour, the mixture was filtered and dried to obtain the hexafluorophosphate salt of the compound: hexafluorophosphate-1,1'-dihexyl-3,3'-dichloro-[4,4'-bipyridine]-1,1'-diimine.

[0087] Example 6

[0088] Preparation of Compound 3,3'-Dibromo-1,1'-dihexyl-[4,4'-bipyridine]-1,1'-diimine

[0089] The basic reaction is:

[0090]

[0091] The preparation method comprises the steps of:

[0092] ① First, weigh 1g 3,3'-dibromo-4,4'-bipyridine and 5g bromohexane into a beaker, add acetonitrile to dissolve, condense and reflux at 80°C, react for 24h, and after the reaction is complete to precipitate a light yellow solid, filter and dry to obtain a light yellow solid 1,1'-dihexyl-3,3'-dibromo-[4,4'-bipyridine]-1,1'-diimine;

[0093] ② Then, the obtained light yellow solid was recrystallized and purified with ethanol;

[0094] ③Finally, the purified product was dissolved in deionized water and heated to 60°C to dissolve. After the ammonium hexafluorophosphate was fully dissolved in water, it was slowly added dropwise into the reaction. The addition was stopped when the system was no longer turbid. After stirring for 1 hour, the mixture was filtered and dried to obtain the hexafluorophosphate salt of the compound: hexafluorophosphate-1,1'-dihexyl-3,3'-dibromo-[4,4'-bipyridine]-1,1'-diimine.

[0095] Example 7

[0096] Preparation of solid-state electrochromic devices

[0097] The six EC materials of Examples 1 to 6 were respectively dissolved in acetone at a molar ratio of 4:1:15:60 with ferrocene, poly(vinylidene fluoride-co-hexafluoropropylene), and ionic liquid 1-butyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide at 50°C;

[0098] The obtained solution was cast onto a glass slide to obtain a uniform free-standing EC gel with a thickness of approximately 60 μm;

[0099] Cut the EC gel into the desired shape using a razor blade and transfer it to the target location on the ITO-coated substrate;

[0100] The gel was sandwiched between another ITO-coated substrate and firmly fixed with double-sided tape to obtain a solid-state electrochromic device;

[0101] Different DC voltages were used to energize the device and the color rendering effect and operation stability were analyzed.

[0102] In Examples 1 to 6, the molecular structures and properties of the core molecules 3,3'-difluoro-4,4'-bipyridine, 3,3'-dichloro-4,4'-bipyridine, and 3,3'-dibromo-4,4'-bipyridine in the optimal conformation are shown in Table 1;

[0103] In Examples 1 to 6, the electrochromic EC molecules include tetraphenylpyridine derivatives 1,1'-diethyl-3,3'-difluoro-[4,4'-bipyridine]-1,1'-diimine, 3,3'-dichloro-1,1'-diethyl-[4,4'-bipyridine]-1,1'-diimine, 3,3'-dibromo-1,1'-diethyl-[4,4'-bipyridine]-1,1'-diimine, 3,3'- The molecular structures and properties of difluoro-1,1'-dihexyl-[4,4'-bipyridine]-1,1'-diimine, 3,3'-dichloro-1,1'-dihexyl-[4,4'-bipyridine]-1,1'-diimine, and 3,3'-dibromo-1,1'-dihexyl-[4,4'-bipyridine]-1,1'-diimine are shown in Table 2. In Example 7, the performance values ​​of the six compounds under different direct currents are shown in Table 3.

[0104] Table 1 List of molecular structures and properties of the optimal conformation of the parent core molecule

[0105]

[0106] Table 2 Molecular structures and properties of tetraphenylpyridine derivatives

[0107]

[0108]

[0109] Table 3 Performance numerical list of quaternary pyridine derivatives

[0110]

[0111] It can be seen from Tables 1 and 2 that after the introduction of heavy atoms F, Cl or Br, the MM2 energy of the EC molecular structure is significantly higher than that of the parent core molecular structure; the energy of the parent core molecular structure gradually increases with the introduction of heavy atoms from F to Br, from 14.3775 Kcal / mol to 26.6357 Kcal / mol; correspondingly, the energy change of the EC molecular structure is more significant, increasing from 53.2137 Kcal / mol to 70.4172 Kcal / mol; this shows that the introduction of heavy atoms reduces the stability of the parent core molecular structure, and more energy is required to maintain its conformation, which also shows that the structure is relatively schedulable.

[0112] From Tables 1 and 2, we can see that in the structure of the parent core molecule, the distance between the heavy atom and the adjacent hydrogen atom increases with the increase of the heavy atom volume. Increase to H(3)-Br(14) Similar distance changes can be observed in EC molecular structures, such as from H(20)-F(18) Increase to H(24)-Br(17) This increase in distance is due to the larger size of heavy atoms, which changes the spatial arrangement within the molecule.

[0113] As can be seen from Tables 1 and 2, the dihedral angle of the parent core molecular structure increases significantly with the increase of heavy atom volume, from 29.855° of C(4)-C(3)-C(7)-C(8) to 57.833°. In the EC molecular structure, the dihedral angle also increases with the increase of heavy atom volume, from 20.301° of C(2)-C(3)-C(7)-C(8) to 43.629°. This change indicates that the degree of distortion of the molecular plane increases after the introduction of heavy atoms, making the three-dimensional structure of the molecule more complex.

[0114] As can be seen from Table 3, the molar absorption coefficient of the molecule is significantly enhanced after the introduction of heavy atoms. This is because the electron cloud of heavy atoms is larger and can interact with photons more effectively and absorb more light. Therefore, after the introduction of heavy atoms, the light absorption capacity of the material is improved, enhancing its electrochromic performance. In practical applications, this means that the material can achieve significant color changes at lower concentrations, improving the efficiency of the material.

[0115] As can be seen from Table 3, although the introduction of heavy atoms increases the light absorption capacity of the molecule, it may also have a negative impact on the transmittance. Due to the enhanced light absorption, the material may become opaque and the transmittance decreases. However, by rationally designing the molecular structure and controlling the amount of heavy atoms introduced, it is possible to maintain a high transmittance while enhancing the molar absorptivity, which is crucial for applications such as electrochromic window glass, because the transmittance directly affects the transparency and practicality of the window glass.

[0116] In the present invention, under different DC voltages, the molar absorption coefficient of the long-chain EC material is larger than that of the short-chain EC material, and the transmittance is also higher. The main reason is that the long chain increases the conjugation effect of the electrons in the molecule and enhances the light absorption capacity. At the same time, the long chain structure helps to arrange the molecules more orderly, reduces the scattering and absorption of light, and thus improves the transmittance. Therefore, the long-chain EC material shows better effects in electrochromic performance and optical performance.

[0117] The preparation method of the quaternary pyridine derivative for electrochromic materials disclosed in the embodiment of the present invention is to prepare the quaternary pyridine derivative, heavy atoms F, Cl, and Br are introduced into the quaternary pyridine structure, which effectively increases the light absorption capacity, can absorb more light in the electrochromic process, and enhance the significance of color change. The thin layer structure of the quaternary pyridine derivative has excellent light transmittance, and at the same time provides the structural stability and durability of the electrochromic material in the electrochromic process. The quaternary pyridine derivative can show obvious color changes under different DC voltages, and this color change can be identified and distinguished by the RGB color model, so that the material can quickly and accurately adjust the light transmittance in practical applications; the electrochromic response is fast, the material completes the color conversion in a short time, the color contrast is high, and the obvious visual difference in different states is guaranteed; the cycle life is long, the practicality and reliability of the electrochromic material are improved, the frequency of replacement and maintenance is reduced, the resource consumption and waste generation are reduced, and the requirements of environmental protection and sustainable development are met. It has good application prospects in the fields of smart dimming windows, rearview mirrors, displays, goggles, etc.

[0118] The technical solutions disclosed in the embodiments of the present invention and the technical details disclosed in the embodiments are merely illustrative of the inventive concept of the present invention and do not constitute a limitation on the technical solutions of the embodiments of the present invention. Any conventional changes, replacements or combinations of the technical details disclosed in the embodiments of the present invention have the same inventive concept as the present invention and are within the protection scope of the claims of the present invention.

Claims

1. A quaternary pyridine derivative for electrochromic materials, characterized in that: Including compounds represented by the following general formula (I): Wherein, X is any one of F, Cl, and Br, and Y is ethyl or n-hexyl; Or a hexafluorophosphate of the compound represented by the general formula (I).

2. The quaternary biphenylpyridine derivative for electrochromic material according to claim 1, characterized in that: In the general formula (I), X is F and Y is ethyl.

3. The quaternary biphenylpyridine derivative for electrochromic material according to claim 1, characterized in that: In the general formula (I), X is Cl and Y is ethyl.

4. The quaternary biphenylpyridine derivative for electrochromic material according to claim 1, characterized in that: In the general formula (I), X is Br and Y is ethyl.

5. The quaternary biphenylpyridine derivative for electrochromic material according to claim 1, characterized in that: In the general formula (I), X is F and Y is hexyl.

6. The quaternary biphenylpyridine derivative for electrochromic material according to claim 1, characterized in that: In the general formula (I), X is Cl and Y is hexyl.

7. The quaternary biphenylpyridine derivative for electrochromic material according to claim 1, characterized in that: In the general formula (I), X is Br and Y is hexyl.

8. The method for preparing the quaternary biphenylpyridine derivative for electrochromic materials according to claim 1, characterized in that: include: The compound represented by the general formula (II) is reacted with a brominated alkane to obtain a compound represented by the general formula (I); The general formula (II) is: Wherein, X is any one of F, Cl, and Br, and the brominated alkane is methyl bromide or 1-bromohexane.

9. The method for preparing a quaternary biphenylpyridine derivative for electrochromic materials according to claim 8 is characterized in that: Also includes: Recrystallizing the compound represented by general formula (I); The recrystallized product is dissolved in deionized water and reacted with ammonium hexafluorophosphate to obtain the hexafluorophosphate of the compound represented by the general formula (I).

10. The use of the quaternary pyridine derivative for electrochromic materials according to claim 1, characterized in that: The electrochromic material is prepared by using the compound represented by the general formula (I).

Citation Information

Patent Citations

  • Electrochromic material and electrochromic device

    CN103059831A

  • Organic compound, electrochromic compound, and electrochromic element, optical filter, lens unit, imaging device, and window component having same

    US20170329195A1

  • Organic compound and electrochromic element

    US20230416222A1