Organic electroluminescent material and organic electroluminescent device
By adjusting the spatial structure of compounds on furan rings and pyridine rings, doped materials with specific molecular structures are designed, solving the problems of low efficiency and short lifetime in existing organic light-emitting devices, and realizing organic electroluminescent materials with long lifetime, high efficiency and low driving voltage.
Patent Information
- Application Number
- CN202411040090.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-19
AI Technical Summary
In the existing technology, phosphorescent materials have low efficiency and short lifespan when applied to organic light-emitting devices, making it difficult to achieve organic electroluminescent materials with long lifespan, high efficiency, and low driving voltage.
By employing doped materials with specific atomic structures and adjusting the spatial configuration and size of compounds through methods such as furan rings and pyridine rings, organic electroluminescent materials with specific molecular structures are designed for use in organic electroluminescent devices.
This achieves the characteristics of long lifespan, high efficiency, and low driving voltage in organic electroluminescent devices, thus improving device performance.
Smart Images

Figure BDA0004972159290000011 
Figure BDA0004972159290000021 
Figure BDA0004972159290000031
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of organic electroluminescent materials and relates to an organic electroluminescent material and an organic electroluminescent device. Background Art
[0002] OLEDs utilize organic thin films that emit light when a voltage is applied across the device. OLEDs are becoming an increasingly attractive technology for use in applications such as flat panel displays, lighting, and backlighting.
[0003] Optoelectronic devices utilizing organic materials are becoming increasingly popular for a variety of reasons. Many materials used to make the devices are relatively inexpensive, so organic optoelectronic devices have the potential to have cost advantages over inorganic devices. In addition, the inherent properties of organic materials (e.g., their flexibility) can make them more suitable for specific applications, such as manufacturing on flexible substrates. Examples of organic optoelectronic devices include organic light emitting diodes / devices (OLEDs), organic phototransistors, organic photovoltaic cells, and organic photodetectors. For OLEDs, organic materials can have performance advantages over conventional materials.
[0004] However, the phosphorescent materials used in the prior art have low efficiency and short lifespan in organic light-emitting devices. Therefore, how to provide an organic electroluminescent material with long lifespan, high efficiency and low driving voltage is an urgent problem to be solved by those skilled in the art. Summary of the invention
[0005] In view of the shortcomings of the prior art, the object of the present invention is to provide an organic electroluminescent material and an organic electroluminescent device. The organic electroluminescent device provided by the present invention adopts a doping material with a specific atomic structure, and adjusts the spatial stereo configuration and size of the obtained compound molecular structure through the furan ring and pyridine and pyridine ring, etc. After the obtained organic compound is used in the organic electroluminescent device, the device has the characteristics of long life, high efficiency and low driving voltage.
[0006] To achieve this object, the present invention adopts the following technical solutions:
[0007] In one aspect, the present invention provides an organic electroluminescent material having a structure as shown below: A )2(L B );
[0008] The ligand L A and L B The structure is as follows:
[0009]
[0010] Wherein, p is an integer between 0 and 4, q is an integer between 0 and 3, n is an integer between 0 and 2, and m is an integer between 0 and 6;
[0011] Ring H is a cyclic structure, which is a five-membered ring, a six-membered ring or a condensed ring structure;
[0012] R1, R2, R3 are independently selected from any one of -H, -D (deuterium), -T (tritium), -F, -CN, -CH3, -CD3, -CT3, -CF3, -CH2F, -CHF2, -Ge(Me)3, -Si(Me)3, substituted or unsubstituted C2-C6 alkyl, substituted or unsubstituted C3-C20 cycloalkyl, substituted or unsubstituted C6-C10 aryl and substituted or unsubstituted 4-8 membered aromatic heterocyclic group;
[0013] Ar1, Ar2, Ar3, and Ar4 are independently selected from any one of -H, -D (deuterium), -T (tritium), -F, -CN, -CH3, -CD3, -CT3, -CF3, -CH2F, -CHF2, -Ge(Me)3, -Si(Me)3, substituted or unsubstituted C2-C20 alkyl, substituted or unsubstituted C3-C20 cycloalkyl, substituted or unsubstituted C6-C20 aryl, substituted or unsubstituted C4-C20 condensed ring and substituted or unsubstituted 4-20 membered aromatic heterocyclic group;
[0014] wherein m Ar1 groups exist independently or any two of them form a ring structure;
[0015] M is metal Ir;
[0016] The hydrogen in the above groups may be substituted with deuterium.
[0017] Preferably, L A Any of the following structures:
[0018]
[0019] Among them, Ar2, Ar3, Ar4 and p, q, n are consistent with those described above and will not be repeated here.
[0020] m1 is an integer between 0 and 2 (e.g., 0, 1 or 2), m2 is an integer between 0 and 4 (e.g., 0, 1, 2, 3 or 4), and m3, m4, m5, and m6 are integers between 0 and 6 (e.g., 0, 1, 2, 3, 4, 5 or 6);
[0021] X is O or S;
[0022] Ar 11 ,Ar 12 ,Ar 13 ,Ar14 ,Ar 15 ,Ar 16 Each of them is independently selected from -H, -D (deuterium), -T (tritium), -F, -CN, -CH3, -CD3, -CT3, -CF3, -CH2F, -CHF2, -Ge(Me)3, -Si(Me)3, substituted or unsubstituted C2-C20 alkyl, substituted and unsubstituted C3-C20 cycloalkyl, substituted or unsubstituted C6-C20 aryl, substituted and unsubstituted C4-C20 condensed ring and substituted or unsubstituted 4-20 membered aromatic heterocyclic group.
[0023] Preferably, the Ar 11 ,Ar 12 ,Ar 13 ,Ar 14 ,Ar 15 ,Ar 16 The alkyl groups in Ar2, Ar3, Ar4, R1, R2 and R3 are each independently selected from any one of substituted or unsubstituted straight-chain alkyl groups, substituted or unsubstituted branched-chain alkyl groups and substituted or unsubstituted cycloalkyl groups.
[0024] Preferably, Ar 11 ,Ar 12 ,Ar 13 ,Ar 14 ,Ar 15 ,Ar 16 The heteroatoms in the heteroaryl groups in Ar2, Ar3, Ar4, R1, R2 and R3 are each independently selected from at least one of Si, Ge, N, S and O.
[0025] Furthermore, R1-R3, Ar1-Ar 16Selected from the following groups: -H, -D (deuterium), -T (tritium), -F, -CN, -CH3, -CD3, -CT3, -CF3, -CH2F, -CHF2, -Ge(Me)3, -Si(Me)3, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, tetrahydrofuran, pyrrolidine, thiolane, tetrahydropyran, phenyl, biphenyl, terphenyl, naphthyl, fluorenyl, phenanthrenyl, anthracenyl, indenyl, triphenylene, pyrenyl, naphthyl, peryl, chrysene, tetraphenyl, fluoranthenyl, furanyl, thienyl, pyrrolyl, imidazolyl, pyrazolyl, thiazolyl, thiadiazolyl, isothiazolyl, isoxazolyl, oxazolyl, oxadiazolyl, triazinyl, tetrazinyl, triazolyl, tetrazolyl, furazolyl, pyridyl, pyrazinyl, pyrimidinyl, pyridazinyl, benzofuranyl, benzothiophenyl, isobenzofuranyl, dibenzofuranyl, dibenzothiophenyl, benzimidazolyl, benzothiazolyl, benzisothiazolyl, benzisoxazolyl, benzoxazolyl, isoindolyl, indolyl, indazolyl, benzothiadiazolyl, quinolyl, isoquinolyl, cinnolinyl, quinazolinyl, quinoxalinyl, carbazolyl, phenoxazinyl, phenanthridinyl, benzodioxolyl and the like.
[0026] Preferably, the organometallic compound is selected from one of the following structures:
[0027]
[0028]
[0029]
[0030]
[0031]
[0032]
[0033]
[0034]
[0035]
[0036]
[0037]
[0038]
[0039]
[0040]
[0041]
[0042]
[0043]
[0044]
[0045]
[0046]
[0047]
[0048]
[0049]
[0050]
[0051]
[0052]
[0053]
[0054]
[0055]
[0056]
[0057]
[0058]
[0059]
[0060]
[0061]
[0062]
[0063]
[0064]
[0065]
[0066]
[0067]
[0068]
[0069]
[0070]
[0071]
[0072]
[0073]
[0074]
[0075]
[0076]
[0077]
[0078]
[0079]
[0080]
[0081]
[0082]
[0083]
[0084]
[0085]
[0086]
[0087]
[0088]
[0089]
[0090]
[0091]
[0092]
[0093]
[0094] In the present invention, the preparation process of the compound of formula I is as follows:
[0095]
[0096] The definitions of the groups in the above formula are the same as above and will not be repeated here.
[0097] On the other hand, the present invention provides an organic electroluminescent device, which includes an anode and a cathode and an organic thin film layer arranged between the anode and the cathode, the organic thin film layer includes a light-emitting layer, the light-emitting layer includes a main material and a doping material, and the doping material includes the organic electroluminescent material as described above.
[0098] The light-emitting layer may include a light-emitting dye (i.e., a dopant) that can emit light of different wavelength spectra, and may also include a host material (Host) at the same time. The light-emitting layer may be a monochrome light-emitting layer that emits a single color such as red, green, or blue. A plurality of monochrome light-emitting layers of different colors may be arranged in a plane according to a pixel pattern, or may be stacked together to form a color light-emitting layer. When light-emitting layers of different colors are stacked together, they may be separated from each other or may be connected to each other. The light-emitting layer may also be a single color light-emitting layer that can simultaneously emit different colors such as red and green.
[0099] According to different technologies, the luminescent layer material can be made of different materials such as phosphorescent electroluminescent materials and thermally activated delayed fluorescent luminescent materials. In an OLED device, a single luminescent technology can be used, or a combination of multiple different luminescent technologies can be used. These different luminescent materials classified by technology can emit light of the same color or different colors.
[0100] Preferably, the organic thin film layer further includes at least one of a hole injection layer, a hole transport layer, an electron blocking layer, a light emitting layer, an electron transport layer or an electron injection layer.
[0101] Preferably, the organic electroluminescent device comprises an anode, a hole injection layer, a hole transport layer, an electron blocking layer, a light-emitting layer, an electron transport layer, an electron injection layer and a cathode which are arranged in sequence.
[0102] Generally speaking, an organic electroluminescent device includes a first electrode, a second electrode, and an organic material layer between the electrodes. The organic material can be divided into multiple regions. For example, the organic material layer can include a hole transport region, a light emitting layer, and an electron transport region.
[0103] In a specific embodiment, a substrate may be used below the first electrode or above the second electrode. The substrate is a glass or polymer material with excellent mechanical strength, thermal stability, water resistance, and transparency. In addition, a thin film transistor (TFT) may also be provided on the substrate used as a display.
[0104] The first electrode can be formed by sputtering or depositing a material used as the first electrode on a substrate. When the first electrode is used as an anode, transparent conductive oxide materials such as indium tin oxide (ITO), indium zinc oxide (IZO), tin dioxide (SnO2), zinc oxide (ZnO) and any combination thereof can be used. In addition, the anode material can also be selected from materials and combinations thereof that facilitate hole injection other than the listed anode materials, including materials known to be suitable for anodes. When the first electrode is used as a cathode, metals or alloys such as magnesium (Mg), silver (Ag), aluminum (Al), aluminum-lithium (Al-Li), calcium (Ca), magnesium-indium (Mg-In), magnesium-silver (Mg-Ag) and any combination thereof can be used. In addition to the cathode materials listed above, the cathode material can also be a material and a combination thereof that facilitates electron injection, including materials known to be suitable for cathodes.
[0105] The organic material layer can be formed on the electrode by vacuum thermal evaporation, spin coating, printing and the like. The compound used as the organic material layer can be an organic small molecule, an organic macromolecule and a polymer, and a combination thereof. The hole transport region is located between the anode and the light-emitting layer. The hole transport region can be a hole transport layer (HTL) of a single-layer structure, including a single-layer hole transport layer containing only one compound and a single-layer hole transport layer containing multiple compounds. The hole transport region can also be a multilayer structure including at least one layer of a hole injection layer (HIL), a hole transport layer (HTL), and an electron blocking layer (EBL).
[0106] The material of the hole transport layer can be selected from, but not limited to, phthalocyanine derivatives such as CuPc, conductive polymers or polymers containing conductive dopants such as polyphenylene ethylene, polyaniline / dodecylbenzenesulfonic acid (Pani / DBSA), poly(3,4-ethylenedioxythiophene) / poly(4-styrenesulfonate) (PEDOT / PSS), polyaniline / camphorsulfonic acid (Pani / CSA), polyaniline / poly(4-styrenesulfonate) (Pani / PSS), aromatic amine derivatives such as the compounds shown in HT-1 to HT-34 below; or any combination thereof.
[0107]
[0108]
[0109]
[0110] But it is not limited to the above materials.
[0111] The hole injection layer is located between the anode and the hole transport layer. The hole injection layer can be a single compound material or a combination of multiple compounds. For example, the hole injection layer can use one or more compounds of HT-1 to HT-34 mentioned above, or one or more compounds of HI-1 to HI-3 below; or one or more compounds of HT-1 to HT-34 can be doped with one or more compounds of HI-1 to HI-3 below:
[0112]
[0113] But it is not limited to the above materials.
[0114] The OLED organic material layer may further include an electron transport region between the light emitting layer and the cathode. The electron transport region may be a single-layer electron transport layer (ETL), including a single-layer electron transport layer containing only one compound and a single-layer electron transport layer containing multiple compounds. The electron transport region may also be a multilayer structure including at least one layer of an electron injection layer (EIL), an electron transport layer (ETL), and a hole blocking layer (HBL).
[0115] In one aspect of the present invention, the electron transport layer material can be selected from, but not limited to, one or more combinations of ET-1 to ET-57 listed below.
[0116]
[0117]
[0118]
[0119] But it is not limited to the above materials.
[0120] The device may also include an electron injection layer located between the electron transport layer and the cathode. The electron injection layer material includes but is not limited to one or more combinations of the following: LiF, NaCl, CsF, Li2O, Cs2CO3, BaO, Na, Li, Ca.
[0121] Compared with the prior art, the present invention has the following beneficial effects:
[0122] 1. By adding an acene ring and a pyridine ring to the furan ring, the spatial structure size and morphology of the obtained substance are adjusted, so that when the compound is used in an organic electroluminescent device, the starting voltage is reduced, the efficiency is improved, and the life is increased.
[0123] 2. In the study of the diketone ligand part of the iridium complex, a complete theoretical system has not yet been formed. Because the carbon atoms on the side chain do not participate in conjugation, they have a certain influence on the electron cloud distribution but the influence is not significant. At the same time, the study found that the length, configuration, and group size of the side chain alkyl group will have a certain degree of influence on the performance indicators such as the wavelength, half-peak width, efficiency, life, and CIE coordinates of the doped material. More importantly, for different RH materials, the molecular structure of the diketone ligand is regulated to match RH and RD with each other. At present, there is basically no directional guidance for this kind of matching in the existing technology, and it needs to be verified through massive experiments.
[0124] The light-emitting layer of the organic electroluminescent device of the present invention adopts a structure composed of specific doping materials and main materials, and cooperates with other layer materials to make the obtained organic electroluminescent device effectively reduce the starting and dropping voltage, improve the efficiency, and improve the problem of low lifespan. DETAILED DESCRIPTION
[0125] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0126] Synthesis example 1
[0127] This synthesis example provides an organometallic compound Ⅰ-3, i.e., a compound numbered Ⅰ-3. The specific synthesis steps are as follows:
[0128]
[0129] Some of the synthesis methods are shown in patent CN116813670A.
[0130] Under nitrogen protection system, weigh the compound 8-bromo-1-chlorobenzo[4,5]thieno[2,3-c]pyridine (CAS: 2926783-50-6) (330mmol), isobutylboric acid (CAS: 84110-40-7) (363mmol), anhydrous potassium carbonate (990mmol) and put into the reaction system, add 1000ml toluene, 500ml anhydrous ethanol, 500ml purified water, add Pd(PPh3)4 (3.3mmol) under nitrogen protection, reflux at 100℃ for 24h under nitrogen protection, after the reaction is completed, separate the liquids, extract with ethyl acetate, wash three times with saturated brine, and concentrate under reduced pressure. 400 ml of dichloromethane was added to dissolve, and the solution was subjected to column chromatography (200-300 mesh, 600 g) with a developing solvent of DCM:PE=1:1. The receiving solution was vortexed until no liquid flowed out to obtain the compound formula C-3 (47.32 g, yield 52%). The intermediate compound formula C-3 was subjected to the following analytical tests:
[0131] HPLC purity: greater than 99.5%;
[0132] Mass spectrum: Test value is 275.21.
[0133] Elemental analysis: calculated values are C, 65.33; H, 5.12; Cl, 12.85; N, 5.08; S, 11.62. Measured values are C, 65.35; H, 5.10; Cl, 12.86; N, 5.09; S, 11.61.
[0134] Under nitrogen protection system, weigh the compound 2-methoxynaphthalene (CAS: 93-04-9) (240mmol) and dissolve it in 3L THF solvent. In nitrogen atmosphere, drop n-BuLi (2.5M, 115mL) at -20°C, keep warm for 3h and then cool to -80°C, then drop B(C4H9)3 (300mmol), and naturally heat to an internal temperature higher than -10°C after completion, and the reaction process is completed. The reaction solution is concentrated under reduced pressure, acidified with hydrochloric acid, and crystallized with PE to obtain a white solid, and the compound formula D-3 (37.3g, yield 77%) is obtained. The intermediate compound formula D-3 is subjected to the following analytical tests:
[0135] HPLC purity: greater than 99.5%;
[0136] Mass spectrum: Test value is 202.16.
[0137] Under nitrogen protection system, weigh compound D-3 (180mmol), compound C-3 (160mmol), anhydrous potassium carbonate (480mmol) and put them into the reaction system, add 500ml toluene, 250mL anhydrous ethanol, 250mL pure water, add Pd(PPh3)4 (1.8mmol) under nitrogen protection, reflux at 100℃ for 24h under nitrogen protection, after the reaction is completed, separate the liquid, extract with ethyl acetate, wash three times with saturated brine, and concentrate under reduced pressure. Add 400ml dichloromethane to dissolve, column chromatography (200-300 mesh, 600g) of the solution with developing agent DCM:PE=1:1, rotate the receiving liquid until no liquid flows out, and obtain the compound formula B-3 (57.2g, yield 90%) shown, and the intermediate compound formula B-3 is subjected to the following analysis and test:
[0138] HPLC purity: greater than 99.5%;
[0139] Mass spectrum: Test value is 397.34.
[0140] Under nitrogen protection, compound B-3 (140 mmol) was weighed and dissolved in 800 mL of DMF solvent. NBS (140 mmol) was added in batches at 0°C. After the reaction was completed, the reaction solution was poured into a large amount of water, the precipitated solid was filtered, and then slurried and dispersed with ethanol to obtain an off-white solid compound A-3 (38 g, yield 88%). The intermediate compound A-3 was subjected to the following analytical tests:
[0141] HPLC purity: greater than 99.5%;
[0142] Mass spectrum: Test value is 475.19.
[0143] Under nitrogen protection system, 3-chloro-6-methylpyridine (CAS: 56960-77-1) (135mmol), biboric acid pinacol ester (202.5mmol), X-Phos (8.1mmol), palladium acetate (4.05mmol), potassium acetate (270mmol) and dioxane (1000mL) were added to the reaction system in sequence, N2 was replaced three times and N2 was protected, and heated and stirred at 100°C overnight. After the reaction was completed, diatomaceous earth and anhydrous magnesium sulfate were filtered, ethyl acetate was washed twice, and the organic phase was collected and concentrated under reduced pressure to obtain the crude intermediate E-3, which was directly used in the next step.
[0144] Under nitrogen protection system, compound E-3 (132mmol), compound A-3 (120mmol), anhydrous potassium carbonate (360mmol) were weighed and put into the reaction system, 800ml toluene, 400mL anhydrous ethanol, 400mL pure water were added, Pd(PPh3)4 (1.2mmol) was added under nitrogen protection, refluxed at 100℃ for 24h under nitrogen protection, after the reaction was completed, liquid separation, ethyl acetate extraction, saturated brine washing three times, and reduced pressure concentration. 400ml dichloromethane was added to dissolve, the solution was column chromatographed (200-300 mesh, 600g) with developing agent DCM:PE=1:1, the receiving liquid was vortexed until no liquid flowed out, and the compound formula IV-3 (47.75g, yield 79%) was obtained, and the intermediate compound formula IV-3 was subjected to the following analysis and test:
[0145] HPLC purity: greater than 99.5%;
[0146] Mass spectrum: Test value is 503.46.
[0147] Under nitrogen protection, compound IV-3 (90 mmol) was weighed and dissolved in 400 mL of THF in the reaction system. After the internal temperature reached 55°C, heating was stopped, copper acetate (90 mmol) was added, and then 50 mL of THF solution containing tert-butyl nitrite (108 mmol) was carefully dripped into the above system. The system released heat and gas. After the dropwise addition was completed, the reaction was continued for 1 hour to complete the reaction. The reaction solution was directly concentrated to dryness under reduced pressure, and then 800 mL of DCM was added to reflux and dissolve to make it clear. The solution was passed through a silica gel column, and the column liquid was collected and concentrated under reduced pressure to a remaining volume of about 100 ml. Solids precipitated, and the temperature was lowered to below 20°C, filtered, dried, and dried to obtain a slightly yellow solid powder compound III-3 (26.80 g, with a yield of 63%). The intermediate compound III-3 was subjected to the following analytical tests:
[0148] HPLC purity: greater than 99.5%;
[0149] Mass spectrum: Test value 472.30.
[0150] Elemental analysis: calculated values are C, 78.78; H, 5.12; N, 5.93; O, 3.39; S, 6.78. Measured values are C, 78.79; H, 5.11; N, 5.94; O, 3.38; S, 6.79.
[0151] Under nitrogen protection, weigh ligand III-3 (50mmol), IrC13·3H2O (22mmol) into the reaction system, add 420mL ethylene glycol ethyl ether and 140mL pure water mixed solution, reflux for 26 hours under nitrogen protection, then cool to room temperature, precipitate, filter the precipitate, rinse with water, anhydrous ethanol, and petroleum ether, and dry it in turn. The bridged ligand II-3 (14.68, yield 57%) was obtained as a dark red powder.
[0152] Weigh the bridged ligand II-3 (5.5 mmol), add anhydrous potassium carbonate (55 mmol), then add 190 mL of ethylene glycol ether to the system, replace nitrogen three times, add 3,7-diethylnonane-4,6-dione (CAS: 872802-98-7) (16.5 mmol) under nitrogen, reflux for 22 hours under nitrogen protection, cool, filter, wash with alcohol, and dry. Use dichloromethane as solvent, use neutral alumina column chromatography, concentrate the filtrate and precipitate the solid, and finally obtain the organic phosphorescent material shown in I-3 (3.7 g, with a yield of 25%);
[0153] The organometallic compound I-3 was subjected to the following analytical tests:
[0154] HPLC purity: greater than 99.5%;
[0155] Mass spectrum: test value is 1346.52;
[0156] Elemental analysis: calculated values are C, 66.89; H, 5.16; N, 4.16; O, 4.75; S, 4.76. Test values are C, 66.88; H, 5.17; N, 4.19; O, 4.74; S, 4.75;
[0157] 1 H NMR (400MHz, deuterated chloroform) δ8.87(d,2H),8.13(dd,2H),8.09(dd,4H),7.91(dd,2H),7.81(d,2H),7.58(t,2H),7.47(td,2H),7.42(td,2H),7.26–7.21( m,2H),7.15(dd,2H),5.65(dd,1H),2.76(pd,1H),2.60(d,4H),2.53(d, 6H),2.48(pd,1H),1.91(dp,2H),1.61–1.41(m,8H),0.92–0.82(m,24H).
[0158] Synthesis example 2
[0159] This synthesis example provides an organometallic compound I-76, i.e., a compound numbered I-76. The specific synthesis steps are as follows:
[0160]
[0161] Among them, the synthesis method of formula IIIA-76 is consistent with that of Synthesis Example 1 and will not be repeated here.
[0162] Under nitrogen protection system, add formula IIIA-76 (100mmol), DMSO-d6 (4000mmol), KOH (600mmol), N2 replacement three times and N2 protection, and heat the reaction at 100°C for 36h. After the reaction is completed, extract with ethyl acetate, wash with saturated brine three times, and concentrate under reduced pressure. The crude product is purified by column chromatography, eluted with DCM:EA=50:1 to 10:1 (v / v) gradient, and the intermediate III-76 is 27.68g in mass and 58% in yield.
[0163] HPLC purity: greater than 99.5%;
[0164] Mass spectrum: Test value is 477.24.
[0165] Elemental analysis: calculated values are C, 77.95; H, 6.12; N, 5.87; O, 3.35; S, 6.71. Measured values are C, 77.93; H, 6.14; N, 5.88; O, 3.36; S, 6.70.
[0166] 1H NMR (400 MHz, deuterated chloroform) δ8.90 (d, 1H), 8.14–8.06 (m, 2H), 8.01–7.93 (m, 2H), 7.87 (d, 1H), 7.75 (d, 1H), 7.60 (t, 1H), 7.50 (td, 1H), 7.45 (td, 1H), 7.22 (d, 1H), 7.17 (dd, 1H), 2.01 (p, 1H), 0.84 (d, 6H).
[0167] Under nitrogen protection, weigh ligand III-76 (55mmol), IrC13·3H2O (20mmol) into the reaction system, add 450ml of ethylene glycol ethyl ether and 150ml of pure water, reflux for 26 hours under nitrogen protection, then cool to room temperature, precipitate, filter the precipitate, rinse with water, anhydrous ethanol, and petroleum ether, and dry it in turn. The mass of the dark red powder bridged ligand II-76 is 14.2g, and the yield is 60%.
[0168] Weigh the bridged ligand II-76 (5.5 mmol), add anhydrous potassium carbonate (55 mmol), then add 150 ml of ethylene glycol ether to the system, replace nitrogen three times, add 3,7-diethyl-3,7-dimethylnonane-4,6-dione (CAS: 865193-73-3) (16.5 mmol) under nitrogen, reflux for 22 hours under nitrogen protection, cool, filter, wash with alcohol, and dry. Use dichloromethane as solvent, use neutral alumina column chromatography, concentrate the filtrate and precipitate solids, and finally obtain the organic phosphorescent material shown in I-76, with a mass of 4.29 g and a yield of 31%.
[0169] The organometallic compound I-76 was subjected to the following analytical tests:
[0170] HPLC purity: greater than 99.5%;
[0171] Mass spectrum: test value is 1384.71.
[0172] Elemental analysis: calculated values are C, 66.78; H, 6.04; N, 4.05; O, 4.62; S, 4.63. Test values are C, 66.79; H, 6.03; N, 4.08; O, 4.60; S, 4.62;
[0173] 1H NMR (400 MHz, deuterated chloroform) δ8.87 (d, 2H), 8.16–8.06 (m, 6H), 7.91 (dd, 2H), 7.81 (d, 2H), 7.61 (t, 2H), 7.47 (td, 2H), 7.42 (td, 2H), 7.24 (d, 2H), 7.18 (dd, 2H), 5.56 (s, 1H), 2.01 (hept, 2H), 1.78–1.62 (m, 8H), 1.18 (s, 3H), 1.09 (s, 3H), 0.89–0.81 (m, 24H).
[0174] Synthesis example 3
[0175] This synthesis example provides an organometallic compound Ⅰ-200, i.e., a compound numbered Ⅰ-200. The specific synthesis steps are as follows:
[0176]
[0177] The synthesis method of formula A-200 is consistent with that of Synthesis Example 1 and will not be repeated here.
[0178] Under nitrogen protection, (6-aminopyridin-2-yl)boric acid (CAS: 1220910-24-6) (825 mmol), trimethylsilyl chloride (CAS: 75-77-4) (750 mmol), and anhydrous potassium carbonate (2250 mmol) were weighed and put into the reaction system, and 1200 ml of toluene, 600 ml of anhydrous ethanol, and 600 ml of purified water were added. Pd(PPh3)4 (7.5 mmol) was added under nitrogen protection, and the mixture was refluxed at 100°C for 24 h under nitrogen protection. After the reaction was completed, the mixture was separated, extracted with ethyl acetate, washed three times with saturated brine, and concentrated under reduced pressure. 400 ml of dichloromethane was added to dissolve, and the solution was subjected to column chromatography (200-300 mesh, 600 g) with a developing solvent of DCM:PE=1:1. The receiving solution was vortexed until no liquid flowed out to obtain the compound K-200 (59.87 g, a yield of 48%). The intermediate compound K-200 was subjected to the following analytical tests:
[0179] HPLC purity: greater than 99.5%;
[0180] Mass spectrum: Test value is 166.18.
[0181] Elemental analysis: Calculated values are C, 57.78; H, 8.49; N, 16.85; Si, 16.89. Measured values are C, 57.79; H, 8.48; N, 16.88; Si, 16.87.
[0182] Under nitrogen protection system, compound K-200 (550mmol) and DMAP (110mmol) were weighed and put into the reaction system, and 1000mL of DCM was added. When the internal temperature was 15°C, 500mL of DCM solution of Boc2O (550mmol) was added dropwise. The reaction was kept warm for 24h until the raw materials were basically complete. After the solvent and low boiling point products were concentrated under reduced pressure, a semi-solid was obtained, which was then slurried and dispersed by PE to obtain the compound F-200 (96.78g, yield 70%). The intermediate compound F-200 was subjected to the following analysis and test:
[0183] HPLC purity: greater than 99.5%;
[0184] Mass spectrum: Test value is 251.35.
[0185] Under nitrogen protection system, compound F-200 (250 mmol) was weighed and dissolved in 900 mL of THF, N,N-tetramethylethylenediamine (500 mmol) was added, and the temperature was lowered to -75 ° C under nitrogen atmosphere, and n-BuLi (2.5M, 120 mL) was added dropwise. After stirring for 1 hour, the temperature was further lowered to -85 ° C, triisopropyl borate (300 mmol) was added dropwise, and then the temperature was raised to room temperature. The reaction preparation was completed; the reaction solution was concentrated, the ammonium chloride aqueous solution was dissociated, and PE was dispersed and crystallized to obtain the compound formula E-200 (28.89 g, yield 55%), and the intermediate compound formula E-200 was subjected to the following analysis and test:
[0186] HPLC purity: greater than 99.5%;
[0187] Mass spectrum: Test value is 210.18.
[0188] Under nitrogen protection system, compound E-200 (132mmol), compound A-200 (120mmol), anhydrous potassium carbonate (360mmol) were weighed and put into the reaction system, 1100ml toluene, 550mL anhydrous ethanol, 550mL pure water were added, Pd(PPh3)4 (1.2mmol) was added under nitrogen protection, refluxed at 100℃ for 24h under nitrogen protection, after the reaction was completed, liquid separation, ethyl acetate extraction, saturated brine washing three times, and reduced pressure concentration. 400ml dichloromethane was added to dissolve, the solution was column chromatographed (200-300 mesh, 900g) with developing agent DCM:PE=1:2, the receiving liquid was vortexed until no liquid flowed out, and the compound IV-200 (53.93g, yield 80%) was obtained, and the intermediate compound IV-200 was subjected to the following analysis and test:
[0189] HPLC purity: greater than 99.5%;
[0190] Mass spectrum: Test value is 561.41.
[0191] Under nitrogen protection, compound IV-200 (90 mmol) was weighed and dissolved in 600 mL of THF in the reaction system. After the internal temperature reached 55°C to 57°C, heating was stopped, copper acetate (90 mmol) was added, and then 50 mL of THF solution containing tert-butyl nitrite (108 mmol) was carefully dripped into the above system. The system released heat and gas. After the dropwise addition was completed, the reaction was continued for 1 hour to complete the reaction. The reaction solution was directly concentrated to dryness under reduced pressure, and then 1000 mL of DCM was added to reflux and dissolve to make it clear. The solution was passed through a silica gel column, and the column liquid was collected and concentrated under reduced pressure to a remaining volume of about 150 ml. After solid precipitation, the temperature was lowered to below 20°C, filtered, drained, and dried to obtain the compound III-200 (32.48 g, with a yield of 68%). The intermediate compound III-200 was subjected to the following analytical tests:
[0192] HPLC purity: greater than 99.5%;
[0193] Mass spectrum: Test value is 530.36.
[0194] Elemental analysis: calculated values are C, 74.68; H, 5.70; N, 5.28; O, 3.01; S, 6.04; Si, 5.29. Measured values are C, 74.66; H, 5.72; N, 5.27; O, 3.02; S, 6.06; Si, 5.27.
[0195] Under nitrogen protection, weigh ligand III-200 (50mmol), IrC13·3H2O (22mmol) into the reaction system, add 420ml of ethylene glycol ethyl ether and 140ml of pure water, reflux for 26 hours under nitrogen protection, then cool to room temperature, precipitate, filter the precipitate, rinse with water, anhydrous ethanol, and petroleum ether, and dry it in turn. The mass of the dark red powder bridged ligand II-200 is 15.86g, and the yield is 56%.
[0196] Weigh the bridged ligand II-200 (5.5 mmol), add anhydrous potassium carbonate (7.59 g, 55 mmol), then add 150 ml of ethylene glycol ether to the system, replace nitrogen three times, add 3,7-diethyl-1,1,1-trifluoroketone-4,6-dione (CAS: 2529711-94-0) (16.5 mmol) under nitrogen, reflux for 22 hours under nitrogen protection, cool, filter, wash with alcohol, and dry. Use dichloromethane as solvent, use neutral alumina column chromatography, concentrate the filtrate and precipitate solids, and finally obtain the organic phosphorus luminescent material shown in I-200, with a mass of 4.70 g and a yield of 31%.
[0197] The organometallic compound I-200 was subjected to the following analytical tests:
[0198] HPLC purity: greater than 99.5%;
[0199] Mass spectrum: test value is 1516.62.
[0200] Elemental analysis: calculated values are C, 62.55; H, 5.18; F, 3.76; N, 3.69; O, 4.22; S, 4.23; Si, 3.70. Test values are C, 62.57; H, 5.16; F, 3.76; N, 3.68; O, 4.23; S, 4.21; Si, 3.72;
[0201] 1H NMR (400MHz, deuterated chloroform) δ8.87(d,2H),8.16–8.06(m,4H),7.91(dd,2H),7.81(d,2 H),7.78(dd,2H),7.64(d,2H),7.58(t,2H),7.47(td,2H),7.42(td,2H),7.15 (dd,2H),5.65(dd,1H),2.97(pd,1H),2.76(pd,1H),2.60(d,4H),2.39(dtd, 1H),1.97–1.83(m,3H),1.59–1.42(m,6H),0.94–0.79(m,21H),0.48(s,18H).
[0202] Synthesis example 4
[0203] This synthesis example provides an organometallic compound I-557, i.e., a compound numbered I-557. The specific synthesis steps are as follows:
[0204]
[0205] The synthesis methods of Formula D-557 and Formula E-557 are the same as those in Synthesis Example 1 and will not be described in detail.
[0206] Under nitrogen protection system, compound D-557 (1535mmol), 2,7-dichloro-3-methylthieno[2,3-c]pyridine (CAS: 3022861-39-5) (1535mmol), anhydrous potassium carbonate (4605mmol) were weighed and put into the reaction system, 2000ml toluene, 1000ml anhydrous ethanol, 1000ml purified water were added, Pd(PPh3)4 (15.35mmol) was added under nitrogen protection, refluxed at 100°C for 24h under nitrogen protection, after the reaction was completed, the liquids were separated, extracted with ethyl acetate, washed three times with saturated brine, and concentrated under reduced pressure. 500 ml of dichloromethane was added to dissolve, and the solution was subjected to column chromatography (200-300 mesh, 1000 g) with a developing solvent of DCM:PE=1:3. The receiving solution was vortexed until no liquid flowed out to obtain the compound B-557 (219.1 g, yield 42%). The intermediate compound B-557 was subjected to the following analytical tests:
[0207] HPLC purity: greater than 99.5%;
[0208] Mass spectrum: Test value is 339.47.
[0209] Elemental analysis: Calculated values are C, 67.15; H, 4.15; Cl, 10.43; N, 4.12; O, 4.71; S, 9.43. Measured values are C, 67.18; H, 4.12; Cl, 10.44; N, 4.10; O, 4.72; S, 9.44.
[0210] Under nitrogen protection, compound B-557 (645 mmol) was weighed and dissolved in 1500 mL of DMF solvent. NBS (645 mmol) was added in batches at 0°C to 10°C. After the reaction was completed, the reaction solution was poured into a large amount of water, the precipitated solid was filtered, and then slurried and dispersed with ethanol to obtain an off-white solid compound A-557 (132.33 g, yield 49%). The intermediate compound A-557 was subjected to the following analytical tests:
[0211] HPLC purity: greater than 99.5%;
[0212] Mass spectrum: Test value is 416.98.
[0213] Under nitrogen protection, compound A-557 (315 mmol), formula E-557 (315 mmol), anhydrous potassium carbonate (28.98 g, 945 mmol) were weighed and put into the reaction system, 1000 ml of toluene, 500 ml of anhydrous ethanol, 500 ml of purified water were added, Pd(PPh3)4 (3.15 mmol) was added under nitrogen protection, refluxed at 100 ° C for 24 h under nitrogen protection, then cooled to 25 ° C, filtered, and filtered. The cake was rinsed with petroleum ether, the filter cake was vacuum dried, 300 ml of dichloromethane was added to dissolve, the solution was column chromatographed (200-300 mesh, 650 g) with a developing agent of DCM:PE=2:1, the receiving liquid was vortexed until no liquid flowed out, petroleum ether was added and stirred for 20 min, filtered, the filter cake was rinsed with petroleum ether, and the filter cake was vacuum dried to obtain the compound of formula IV-557 (61.23 g, yield 45%), and the intermediate compound of formula IV-557 was subjected to the following analytical tests:
[0214] HPLC purity: greater than 99.5%;
[0215] Mass spectrum: Test value is 431.16.
[0216] Under nitrogen protection, compound IV-557 (125 mmol) was weighed and dissolved in 1200 mL of THF in the reaction system. After the internal temperature reached 55°C, heating was stopped, copper acetate (125 mmol) was added, and then 50 mL of THF solution containing tert-butyl nitrite (150 mmol) was carefully dripped into the above system. The system released heat and gas. After the dropwise addition was completed, the reaction was continued for 1 hour to complete the reaction. The reaction solution was directly concentrated to dryness under reduced pressure, and then 1000 mL of DCM was added to reflux and dissolve to make it clear. The solution was passed through a silica gel column, and the column liquid was collected and concentrated under reduced pressure to a remaining volume of about 200 ml. Solids precipitated, and the temperature was lowered to below 20°C, filtered, drained, and dried to obtain the compound IIIA-557 (31.12 g, with a yield of 60%). The intermediate compound IIIA-557 was subjected to the following analytical tests:
[0217] HPLC purity: greater than 99.5%;
[0218] Mass spectrum: Test value is 414.34.
[0219] Under nitrogen protection, compound IIIA-557 (75 mmol), 4-isobutylphenylboronic acid (CAS: 153624-38-5) (90 mmol), anhydrous potassium carbonate (225 mmol) were weighed and put into the reaction system, 900 ml of toluene, 450 ml of anhydrous ethanol, 450 ml of purified water were added, Pd (PPh3) 4 (0.75 mmol) was added under nitrogen protection, refluxed at 100 ° C for 24 h under nitrogen protection, and then cooled to 25 ° C. , filtrate with suction, rinse the filter cake with petroleum ether, dry the filter cake in vacuum, add 300 ml of dichloromethane to dissolve, column chromatography (200-300 mesh, 550 g) of the solution with a developing agent of DCM: PE = 1: 3, vortex the receiving solution until no liquid flows out, add petroleum ether and stir for 20 min, filter with suction, rinse the filter cake with petroleum ether, dry the filter cake in vacuum to obtain the compound of formula III-557 (32.68 g, yield 85%), and perform the following analytical tests on the intermediate compound of formula III-557:
[0220] HPLC purity: greater than 99.5%;
[0221] Mass spectrum: Test value is 512.33.
[0222] Elemental analysis: Calculated values are C, 79.66; H, 5.51; N, 5.46; O, 3.12; S, 6.25. Found values are C, 79.67; H, 5.50; N, 5.49; O, 3.10; S, 6.24.
[0223] Under nitrogen protection, weigh ligand III-557 (55mmol), IrC13·3H2O (22mmol) into the reaction system, add 480ml of ethylene glycol ethyl ether and 160mL of pure water, reflux for 26 hours under nitrogen protection, then cool to room temperature, precipitate, filter the precipitate, rinse with water, anhydrous ethanol, and petroleum ether, and dry it in turn. The mass of the dark red powder bridged ligand II-557 is 17.06g, and the yield is 62%.
[0224] Weigh the bridged ligand II-557 (6mmol), add anhydrous potassium carbonate (60mmol), then add 300ml of ethylene glycol ether to the system, replace nitrogen three times, add 3,7-diethylnonane-4,6-dione (CAS: 872802-98-7) (24mmol) under nitrogen, reflux for 22 hours under nitrogen protection, cool, filter, wash with alcohol, and dry. Use dichloromethane as solvent, use neutral alumina column chromatography, concentrate the filtrate and precipitate solids, and finally obtain the organic phosphorus luminescent material shown in I-557, with a mass of 6.16g and a yield of 36%.
[0225] The organometallic compound I-557 was subjected to the following analytical tests:
[0226] HPLC purity: greater than 99.5%;
[0227] Mass spectrum: test value is 1426.62.
[0228] Elemental analysis: calculated values are C, 68.18; H, 5.44; N, 3.93; O, 4.49; S, 4.49. Test values are C, 68.19; H, 5.43; N, 3.97; O, 4.47; S, 4.47;
[0229] 1H NMR (400 MHz, deuterated chloroform) δ8.47 (d, 2H), 8.13 (dd, 2H), 8.09 (d, 2H), 7.91 (dd, 2H), 7.67 (d, 2H), 7.51–7.43 (m, 6H), 7.42 (td, 2H), 7.24 (dt, 2H), 7.10 (dt, 4H), 5.65 (dd, 1H), 2.76 (pd, 1H), 2.55–2.43 (m, 11H), 2.40 (s, 6H), 1.87 (dp, 2H), 1.61–1.41 (m, 8H), 0.92–0.84 (m, 24H).
[0230] Synthesis example 5
[0231] This synthesis example provides an organometallic compound Ⅰ-660, i.e., a compound numbered Ⅰ-660. The specific synthesis steps are as follows:
[0232]
[0233] The synthesis method of Formula IIIA-660 is the same as that in Synthesis Example 4 and will not be described in detail.
[0234] Under nitrogen protection, compound IIIA-660 (80 mmol), isobutylboric acid (CAS: 84110-40-7) (96 mmol), anhydrous potassium carbonate (240 mmol) were weighed and put into the reaction system, 1500 ml of toluene, 750 ml of anhydrous ethanol, 750 ml of purified water were added, Pd(PPh3)4 (0.8 mmol) was added under nitrogen protection, refluxed at 100 ° C for 24 h under nitrogen protection, then cooled to 25 ° C, and pumped. Filter, rinse the filter cake with petroleum ether, vacuum dry the filter cake, add 300 ml of dichloromethane to dissolve, and perform column chromatography (200-300 mesh, 600 g) with a developing agent of DCM: PE = 1: 2. Rotate the receiving solution until no liquid flows out, add petroleum ether and stir for 20 min, filter with suction, rinse the filter cake with petroleum ether, and vacuum dry the filter cake to obtain the compound of formula III-660 (27.24 g, yield 78%). The intermediate compound of formula III-660 is subjected to the following analytical tests:
[0235] HPLC purity: greater than 99.5%;
[0236] Mass spectrum: Test value is 436.28.
[0237] Elemental analysis: calculated values are C, 77.03; H, 5.54; N, 6.42; O, 3.66; S, 7.34. Measured values are C, 77.05; H, 5.52; N, 6.40; O, 3.68; S, 7.35.
[0238] Under nitrogen protection, weigh ligand III-660 (60mmol), IrC13·3H2O (20mmol) into the reaction system, add 540mL ethylene glycol ethyl ether and 180mL pure water mixed solution, reflux for 26 hours under nitrogen protection, then cool to room temperature, precipitate, filter the precipitate, rinse with water, anhydrous ethanol, and petroleum ether, and dry it in turn. The mass of the dark red powder bridged ligand II-660 is 11.43g, and the yield is 52%.
[0239] Weigh the bridged ligand II-660 (5mmol), add anhydrous potassium carbonate (50mmol), then add 290ml of ethylene glycol ether to the system, replace nitrogen three times, add 3,7-diethyl-1,1,1-trifluoroketone-4,6-dione (CAS: 2529711-94-0) (15mmol) under nitrogen, reflux for 22 hours under nitrogen protection, cool, filter, wash with alcohol, and dry. Use dichloromethane as solvent, use neutral alumina column chromatography, concentrate the filtrate and precipitate solids, and finally obtain the organic phosphorus luminescent material shown in I-660, with a mass of 4.51g and a yield of 35%.
[0240] The organometallic compound I-660 was subjected to the following analytical tests:
[0241] HPLC purity: greater than 99.5%;
[0242] Mass spectrum: test value is 1288.72.
[0243] Elemental analysis: calculated values are C, 65.24; H, 5.55; N, 4.35; O, 4.97; S, 4.98. Test values are C, 65.26; H, 5.53; N, 4.39; O, 4.95; S, 4.96;
[0244] 1H NMR (400MHz, deuterated chloroform) δ8.46(d,2H),8.13(dd,2H),8.09(d,2H),7.91(dd,2H),7.65(d,2H),7.47(td,2H),7.42(td,2H),7.24(dq,2H),5.62(d, 1H),2.61(d,4H),2.56–2.46(m,7H),2.25(d,6H),1.94(dp,2H),1.69( qd,4H),1.61–1.41(m,4H),1.10(s,3H),0.97(d,12H),0.87(dt,12H).
[0245] The synthesis methods of other compounds are the same as above, and are not described one by one here. The mass spectra or molecular formulas of other synthesis examples are shown in Table 1 below:
[0246] Table 1
[0247] Compound Molecular formula Mass spectrometry test value Yield (%) Formula Ⅰ-1 <![CDATA[C 65 H 49 IrN4O4S2]]> 1206.43 34 Formula I-148 <![CDATA[C 74 H 65 F2IrN4O4S2]]> 1368.47 31 Formula I-259 <![CDATA[C 69 H 46 D8F3IrN4O4S2]]> 1324.50 24 Formula I-303 <![CDATA[C 77 H 70 F3IrN4O4S2]]> 1428.62 16 Formula I-380 <![CDATA[C 83 H 86 F3IrN4O4S2Si2]]> 1572.75 39 Formula I-438 <![CDATA[C 79 H 65 D 12 IrN4O4S2]]> 1414.98 28 Formula I-529 <![CDATA[C 79 H 77 IrN4O4S2]]> 1402.71 31 Formula I-687 <![CDATA[C 87 H 85 D8IrN4O4S2Si2]]> 1578.41 19 Formula I-720 <![CDATA[C 71 H 73 IrN4O4S2]]> 1302.54 24 Formula I-737 <![CDATA[C 75 H 62 F3IrN4O4S2]]> 1396.40 21 Formula I-847 <![CDATA[C 103 H 105 IrN4O4S2]]> 1718.95 18
[0248] Example 1
[0249] Device fabrication
[0250] All example devices were fabricated by high vacuum (<10-7 Torr) thermal evaporation. Indium tin oxide (ITO). The cathode is made of Liq (8-hydroxyquinoline lithium) and subsequently All devices were packaged with epoxy-sealed glass lids in a nitrogen glove box (H2O and O2 <1 ppm) immediately after fabrication, and a desiccant was incorporated inside the package. The organic stack of the device example consisted of the following in order: an ITO surface, a HT-16; as hole transport layer (HTL) HT-17; as an electron blocking layer (EBL) EBM; containing RH-01 as a red host and 3% of the emitter formula Ⅰ-1 compound of an emission layer (EML); and an electron transport layer (ETL) doped with 35% ET-16 Table 2 shows the thickness and materials of the device layers.
[0251] Table 2: Device layer materials and thicknesses
[0252]
[0253] Example 2
[0254] The method of the above-mentioned embodiment 1 is referred to, with the only difference being that the doping material I-1 is replaced by I-3.
[0255] Example 3
[0256] Refer to the method of the above-mentioned embodiment 1, the only difference is that the doping material Ⅰ-1 is replaced by Ⅰ-76.
[0257] Example 4
[0258] Refer to the method of the above-mentioned embodiment 1, the only difference is that the doping material I-1 is replaced by I-148.
[0259] Example 5
[0260] The method of the above-mentioned embodiment 1 is referred to, with the only difference being that the doping material I-1 is replaced by I-200.
[0261] Example 6
[0262] Refer to the method of the above-mentioned embodiment 1, the only difference is that the doping material I-1 is replaced by I-259.
[0263] Example 7
[0264] The method of the above-mentioned embodiment 1 is referred to, with the only difference being that the doping material Ⅰ-1 is replaced by Ⅰ-303.
[0265] Example 8
[0266] The method of the above-mentioned embodiment 1 is referred to, with the only difference being that the doping material Ⅰ-1 is replaced by Ⅰ-380.
[0267] Example 9
[0268] Refer to the method of the above-mentioned embodiment 1, the only difference is that the doping material I-1 is replaced by I-438.
[0269] Example 10
[0270] Refer to the method of the above-mentioned embodiment 1, the only difference is that the doping material I-1 is replaced by I-529.
[0271] Embodiment 11
[0272] Refer to the method of the above-mentioned embodiment 1, the only difference is that the doping material I-1 is replaced by I-557.
[0273] Example 12
[0274] Refer to the method of the above-mentioned embodiment 1, the only difference is that the doping material I-1 is replaced by I-660.
[0275] Embodiment 13
[0276] Refer to the method of the above-mentioned embodiment 1, the only difference is that the doping material I-1 is replaced by I-687.
[0277] Embodiment 14
[0278] The method of the above-mentioned embodiment 1 is referred to, with the only difference being that the doping material I-1 is replaced by I-720.
[0279] Embodiment 15
[0280] Refer to the method of the above-mentioned embodiment 1, the only difference is that the doping material I-1 is replaced by I-737.
[0281] Example 16
[0282] Refer to the method of the above-mentioned embodiment 1, the only difference is that the doping material I-1 is replaced by I-847.
[0283] Comparative Example 1
[0284] An organic electroluminescent device was prepared in the same manner as in Example 1, except that the compound of the structure of Comparative Example 1 was used instead of the compound of doping compound I-1 in Example 1.
[0285] Comparative Example 2
[0286] An organic electroluminescent device was prepared in the same manner as in Example 1, except that the compound of the structure of Comparative Example 2 was used instead of the doping compound I-1 in Example 1.
[0287] Comparative Example 3
[0288] An organic electroluminescent device was prepared in the same manner as in Example 1, except that the compound of the structure of Comparative Example 3 was used instead of the compound of doping compound I-1 in Example 1.
[0289] Comparative Example 4
[0290] An organic electroluminescent device was prepared in the same manner as in Example 1, except that the compound of the structure of Comparative Example 4 was used instead of the compound of doping compound I-1 in Example 1.
[0291] The structure used is as follows:
[0292]
[0293] The driving voltage, luminous efficiency and life of the organic electroluminescent devices obtained in the above device embodiments and device comparative examples were characterized at a brightness of 1000 (nits). The test results are shown in Table 3 below:
[0294] Table 3
[0295]
[0296]
[0297] It can be seen from Table 3 that, compared with the organic electroluminescent device prepared by using the compound provided by the present invention as the doping material of the light-emitting layer, the present invention selects a specific ligand compound, and changes the spatial configuration and stereostructure between molecules by adding an acene ring and a pyridine ring to the furan ring, sets the molecular orientation, and matches the device structure of the present invention, so that the OLED device has the advantages of long life, high efficiency, and low driving voltage.
[0298] The above embodiments only list the effect data of devices made of a part of the structural formulas. This is a representative sampling test. According to the experimental data, the overall data is not much different and can represent the effects of other unlisted structures.
[0299] It will be apparent to those skilled in the art that many modifications and variations of the present invention are possible without departing from the spirit and scope of the present invention. It is therefore contemplated that the present invention covers modifications and variations of the present invention provided within the scope of the appended claims and their equivalents.
[0300] The applicant declares that the present invention illustrates the organic electroluminescent material and the organic electroluminescent device of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned embodiments, that is, it does not mean that the present invention must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. An organic electroluminescent material, characterized in that: The organic electroluminescent material has the following structure: A )2(L B ); The ligand L A and L B The structure is as follows: Wherein, p is an integer between 0 and 4, q is an integer between 0 and 3, n is an integer between 0 and 2, and m is an integer between 0 and 6; Ring H is a cyclic structure, which is a five-membered ring, a six-membered ring or a condensed ring structure; R1, R2, R3 are independently selected from any one of -H, deuterium, tritium, -F, -CN, -CH3, -CD3, -CT3, -CF3, -CH2F, -CHF2, -Ge(Me)3, -Si(Me)3, substituted or unsubstituted C2-C6 alkyl, substituted or unsubstituted C3-C20 cycloalkyl, substituted or unsubstituted C6-C10 aryl and substituted or unsubstituted 4-8 membered aromatic heterocyclic group; Ar1, Ar2, Ar3, and Ar4 are independently selected from any one of -H, deuterium, tritium, -F, -CN, -CH3, -CD3, -CT3, -CF3, -CH2F, -CHF2, -Ge(Me)3, -Si(Me)3, substituted or unsubstituted C2-C20 alkyl, substituted or unsubstituted C3-C20 cycloalkyl, substituted or unsubstituted C6-C20 aryl, substituted or unsubstituted C4-C20 condensed ring and substituted or unsubstituted 4-20 membered aromatic heterocyclic group; wherein m Ar1 groups exist independently or any two of them form a ring structure; M is metal Ir; The hydrogen in the above groups may be substituted with deuterium.
2. The organic electroluminescent material according to claim 1, characterized in that: L A Any of the following structures: wherein Ar2, Ar3, Ar4 and p, q, n are the same as those in claim 1; m1 is an integer between 0 and 2, m2 is an integer between 0 and 4, and m3, m4, m5, and m6 are integers between 0 and 6; X is O or S; Ar 11 ,Ar 12 ,Ar 13 ,Ar 14 ,Ar 15 ,Ar 16 Each of them is independently selected from -H, deuterium, tritium, -F, -CN, -CH3, -CD3, -CT3, -CF3, -CH2F, -CHF2, -Ge(Me)3, -Si(Me)3, substituted or unsubstituted C2-C20 alkyl, substituted and unsubstituted C3-C20 cycloalkyl, substituted or unsubstituted C6-C20 aryl, substituted and unsubstituted C4-C20 condensed ring and substituted or unsubstituted 4-20 membered aromatic heterocyclic group.
3. The organic electroluminescent material according to claim 2, characterized in that: The Ar 11 ,Ar 12 ,Ar 13 ,Ar 14 ,Ar 15 ,Ar 16 The alkyl groups in Ar2, Ar3, Ar4, R1, R2 and R3 are each independently selected from any one of substituted or unsubstituted straight-chain alkyl groups, substituted or unsubstituted branched-chain alkyl groups and substituted or unsubstituted cycloalkyl groups.
4. The organic electroluminescent material according to claim 2, characterized in that: Ar 11 ,Ar 12 ,Ar 13 ,Ar 14 ,Ar 15 ,Ar 16 The heteroatoms in the heteroaryl groups in Ar2, Ar3, Ar4, R1, R2 and R3 are each independently selected from at least one of Si, Ge, N, S and O.
5. The organic electroluminescent material according to any one of claims 1 to 4, characterized in that: R1-R3, Ar1-Ar 16 Selected from the following groups: -H, deuterium, tritium, -F, -CN, -CH3, -CD3, -CT3, -CF3, -CH2F, -CHF2, -Ge(Me)3, -Si(Me)3, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, tetrahydrofuran, pyrrolidine, thiolane, tetrahydropyran, phenyl, biphenyl, terphenyl, naphthyl, fluorenyl, phenanthrenyl, anthracenyl, indenyl, triphenylene, pyrenyl, naphthacene, peryl, chrysene, fused tetraphenyl, fluoranthenyl, furanyl, thienyl, pyrrolyl, imidazolyl , pyrazolyl, thiazolyl, thiadiazolyl, isothiazolyl, isoxazolyl, oxazolyl, oxadiazolyl, triazinyl, tetrazinyl, triazolyl, tetrazolyl, furazolyl, pyridinyl, pyrazinyl, pyrimidinyl, pyridazinyl, benzofuranyl, benzothiophenyl, isobenzofuranyl, dibenzofuranyl, dibenzothiophenyl, benzimidazolyl, benzothiazolyl, benzisothiazolyl, benzisoxazolyl, benzoxazolyl, isoindolyl, indolyl, indazolyl, benzothiadiazolyl, quinolyl, isoquinolyl, cinnolinyl, quinazolinyl, quinoxalinyl, carbazolyl, phenoxazinyl, phenanthridinyl, or benzodioxolyl.
6. The organic electroluminescent material according to any one of claims 1 to 5, characterized in that: The organometallic compound is selected from one of the following structures:
7. An organic electroluminescent device, characterized in that: The organic electroluminescent device comprises an anode and a cathode and an organic thin film layer arranged between the anode and the cathode, the organic thin film layer comprises a light-emitting layer, the light-emitting layer comprises a main material and a doping material, and the doping material comprises the organic electroluminescent material as described in any one of claims 1-6.
8. The organic electroluminescent device according to claim 7, characterized in that: The organic thin film layer further includes at least one of a hole injection layer, a hole transport layer, an electron blocking layer, a light emitting layer, an electron transport layer or an electron injection layer.
Citation Information
Patent Citations
Large-steric-hindrance C-C coupling palladium ligand and synthesis method
CN116813670A
Cited By
Organic electroluminescent doping material and luminescent device
CN119371464A