Polycarboxylate-type water reducer, modifier for reducing loess absorption of water in pile foundation pouring material, and development method and application of polycarboxylate-type water reducer and modifier for reducing loess absorption of water in pile foundation pouring material
By using high-performance polycarboxylate superplasticizers and compounding agents in pile foundation construction in collapsible loess areas, the problem of limited water-reducing performance was solved, the fluidity and early strength of the grout were improved, and the construction quality and stability were ensured.
Patent Information
- Application Number
- CN202411266437.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-11-19
AI Technical Summary
Existing water-reducing agents have limited water-reducing performance in pile foundation construction in collapsible loess areas, affecting the fluidity and mechanical properties of the grout, leading to increased construction costs and extended construction periods.
Using high-performance polycarboxylate superplasticizer as the core component, and compounded with inorganic salt early strength agent, retarder, dispersant and water-retaining agent, the fluidity and early strength of the grout are improved by optimizing the component ratio and preparation process, and the absorption of water by loess is reduced.
It significantly improves the fluidity and early strength of the grout, ensuring the construction quality and stability of the pile foundation, while also having good environmental friendliness and economic benefits.
Smart Images

Figure CN118978648A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of civil engineering materials, and more specifically, relates to a polycarboxylic acid-based water reducing agent, a modifier for reducing the water absorption of loess into pile foundation grouting materials, and a preparation method and application thereof. Background Art
[0002] Collapsible loess, as a special geological type, is widely distributed in Northwest my country. This type of loess is prone to collapse and deformation when it comes into contact with water, posing a severe challenge to pile foundation construction. During the pouring of pile foundations, the water in the pouring material is often absorbed by the loess in large quantities, resulting in reduced fluidity of the pouring material and slow development of early strength, which in turn affects the bearing capacity and stability of the pile foundation. Although traditional methods such as increasing the water-cement ratio of the pouring material and extending the mixing time can alleviate this problem to a certain extent, they often bring about unfavorable factors such as increased construction costs and extended construction periods. At the same time, most of the existing modifiers have problems such as unstable performance, high costs or complex construction operations, making it difficult to be widely used in actual projects.
[0003] Therefore, developing a modifier that can effectively reduce the absorption of water by loess into pile foundation castables has become a hot topic in current research.
[0004] After searching, patent CN107474196A is a polycarboxylic acid water-reducing agent for small slump concrete and its preparation method. The water-reducing agent is made of the following raw materials in parts by weight: 120-180 parts of methoxy polyoxyethylene ether, 0.5-0.8 parts of catalyst, 0.1-0.3 parts of inhibitor, 5-10 parts of water-carrying agent, 17-35 parts of one or two components of unsaturated acid and acid anhydride, 14-20 parts of functional monomer, 0.8-1.5 parts of initiator, 0.8-1.6 parts of chain transfer agent, and 286-322 parts of deionized water. Patent CN108484842A discloses an ester-based low-sensitivity polycarboxylate water reducer and its preparation method, the molecular weight of its effective ingredient is 10,000 to 15,000, and the ester-based low-sensitivity polycarboxylate water reducer prepared by the invention preparation method has a two-stage polyether structure with ester groups connected at both ends, which can significantly reduce the sensitivity of the product and achieve that the product is not affected by changes in concrete production factors such as ambient temperature, water consumption per cubic meter, aggregate mud content, and water reducer dosage. The water reducer in the above patents has a cumbersome preparation process, is not suitable for large-scale production, and has limited usage scenarios.
[0005] Patent CN110451839A discloses an early-strength polycarboxylate water-reducing agent and its preparation method and application. The early-strength polycarboxylate water-reducing agent includes the following components: polycarboxylate high-efficiency water-reducing agent mother liquor, early-strength component, defoamer, accelerator, fluorosilicate; the early-strength component includes an organic early-strength component and an inorganic early-strength component, and the mass ratio of the organic early-strength component to the inorganic early-strength component is 1: (0.8-1.2); the polycarboxylate high-efficiency water-reducing agent mother liquor includes the following raw materials in parts by weight: 20-45 parts of methoxy polyethylene glycol, 15-20 parts of 1,2,4,5-pyromellitic anhydride, 5-14 parts of sodium methacrylic acid sulfonate, 15-20 parts of p-toluenesulfonic acid, 35-40 parts of deionized water, 1-5 parts of inhibitor, 2.5-5 initiator, and 1-3 parts of pH regulator. However, the early-strength component is not added in this patent, and the early strength of concrete is not significantly improved.
[0006] Patent CN106542767A discloses a composite high-efficiency water reducer and its preparation method and use. The water reducer is made of the following components in weight percentage: 0-50% polycarboxylic acid water reducer, 0-50% naphthalene high-efficiency water reducer, 0-50% melamine resin water reducer, 0-50% aliphatic water reducer, 10-50% lignin sulfonate, 0-50% aminosulfonate water reducer, 0.1-5% sodium gluconate, 0.1-5% sodium dodecyl sulfate, 0.1-10% water glass, 0.1-10% potassium methyl silicate, 0.1-10% sodium thiocyanate, 0.1-10% sodium metaphosphate, 0.1-10% triethanolamine, 0.1-10% potassium persulfate and 10-65% water. The water reducer improves the freeze-thaw resistance by adding air entraining agent, but the gas increases the pores of concrete, resulting in no obvious improvement in its later strength.
[0007] The water reducing agent in the above patents is used in concrete, but its water reducing performance for castables such as concrete is limited, which affects the flowability of the castables and further affects the mechanical properties of the castables. Therefore, it is necessary to develop a water reducing agent and a modifier containing the water reducing agent to improve the water reducing performance and thereby ensure the mechanical properties of the castables. Summary of the invention
[0008] 1. Problem to be solved
[0009] In view of the problem that the existing water reducing agent has limited water reducing performance and affects the mechanical properties of the cast material, the first object of the present invention is to provide a polycarboxylic acid-based water reducing agent and a preparation method thereof, wherein the polycarboxylic acid-based water reducing agent has excellent water reducing performance, effectively improves the flowability of the cast material, and thus ensures the mechanical properties of the cast material;
[0010] The second object of the present invention is to provide a modifier and a preparation method for reducing the water absorption of the pile foundation grouting material by loess, wherein the modifier improves the fluidity and early strength of the grouting material;
[0011] The third purpose of the present invention is to provide an application of the modifier, which can be widely used in pile foundation construction in collapsible loess areas.
[0012] 2. Technical solution
[0013] In order to solve the above problems, the technical solution adopted by the present invention is as follows:
[0014] Aiming at the problem that the water content of the grouting material is easily absorbed by the loess during pile foundation construction in collapsible loess areas, the present invention proposes a modifier for reducing the water content of the pile foundation grouting material absorbed by the loess and a preparation method thereof. The modifier achieves effective control of the water absorption of the loess by optimizing the proportion of each component and the preparation process, and significantly improves the fluidity and early strength of the grouting material.
[0015] Specifically, the present invention firstly selects high-performance polycarboxylic acid water-reducing agent as the core component, and uses its excellent water-reducing and dispersing properties to improve the fluidity of the grouting material; at the same time, an inorganic salt early strength agent is compounded to accelerate the hardening process of the grouting material; in addition, auxiliary components such as retarders, dispersants and water-retaining agents are added to further adjust the performance of the grouting material. Through scientific and reasonable ratio design, the various components work synergistically to jointly play the effect of reducing the water absorption of loess and improving the performance of the grouting material.
[0016] The invention provides a polycarboxylic acid-based water reducer, wherein the water reduction rate of the polycarboxylic acid-based water reducer is not less than 25%.
[0017] The molecular structure of the polycarboxylic acid water reducer is a comb-like structure, and the molecular weight of its active ingredient is 10,000 to 15,000. Figure 1 As shown, the structural formula of its active ingredient is:
[0018]
[0019] Among them, R1, R2, R3, R4, R5 and R6 are alkyl groups containing 1-30 carbon atoms, a=4-6; b=4-6; c=4-6; d=4-6. The main chain of the polymer is mainly composed of a long carbon chain with an appropriate molecular weight, and a variety of active functional groups are grafted on the molecular chain. By introducing carboxylic acid groups (R-COOH) and strong anionic sulfonic acid groups (R-SO3 - ) as adsorption groups, these groups can be adsorbed on the surface of cement particles, making them negatively charged, thereby generating electrostatic repulsion between particles, forming a strong electric repulsion between cement particles, and inhibiting the coagulation tendency of cement paste. In addition, the adsorption group also expands the contact area between cement particles and water, promotes the full hydration of cement, and effectively improves the strength of concrete.
[0020] The main chain is also grafted with polar groups with strong water affinity, such as hydroxyl, amine and alkoxy groups. These groups enhance the dispersion and fluidity of cement particles, reduce the friction resistance between particles, and reduce the free energy of the interface between cement particles and water through surface active effects such as adsorption, dispersion, wetting and lubrication, thereby improving the workability of fresh concrete.
[0021] The steric repulsion effect of polycarboxylic acid molecules, i.e., spatial hindrance, is achieved by grafting long polyalkoxy nonionic hydrophilic long side chains (the average molecular weight of the side chains is as high as 3000 or more) on the main chain of the polymer. The water reducer molecules are adsorbed on the surface of cement particles in a "comb-shaped" structure to form a thicker adsorption layer, and through the mutual crossing and entanglement between the molecular adsorption layers, a strong steric hindrance effect is generated to prevent the formation of cement cohesive structure in the early stage. This characteristic gives polycarboxylic acid water reducers stronger dispersibility and water reduction capabilities than other systems, which is an important feature that distinguishes them from traditional water reducers.
[0022] The polycarboxylate water reducer is prepared by the following method:
[0023] 1) preparing an esterified macromonomer: mixing methoxy polyethylene glycol and methacrylic acid at a ratio of (0.8-0.9):1, adding a polymerization inhibitor and a naphthalene-based high-efficiency water reducer, reacting at 70-80° C. under the action of a catalyst for 6-8 hours to perform esterification to obtain an esterified macromonomer;
[0024] 2) Preparation of polycarboxylic acid water reducer: The prepared esterified macromonomer and methacrylic acid are mixed at a ratio of 1: (0.7-0.8), and uniformly added dropwise to a flask containing a sulfonic acid monomer, and an initiator is added dropwise at the same time, and the mixture is kept warm at 70-80° C. for 30-40 min. After the reaction is completed, the pH is adjusted to 6-7, and a molecular weight regulator is added to react for 20-30 min to obtain a polycarboxylic acid water reducer.
[0025] Wherein, the polymerization inhibitor is at least one of phenothiazine, hydroquinone and diphenylamine;
[0026] The catalyst is at least one of concentrated sulfuric acid, periodic acid, benzenesulfonic acid, p-toluenesulfonic acid and ethylsulfonic acid;
[0027] The sulfonic acid monomer is one or more of sodium p-styrene sulfonate or 2-acrylamide-2-methylpropane sulfonic acid;
[0028] The initiator is a water-soluble redox initiator system or a water-soluble azo initiator;
[0029] The molecular weight regulator is at least one of thioglycolic acid, mercaptopropionic acid, mercaptoethanol, isopropanol, sodium hypophosphite, trisodium phosphate, sodium formate, sodium acetate and dodecanethiol; and is added to the mixture in the form of an aqueous solution.
[0030] The pH is adjusted with alkali.
[0031] In step 1), the mass fraction of the methoxy polyethylene glycol is 10%-15%, the mass fraction of methacrylic acid required for preparing the esterification macromonomer is 12%-19%, the mass fraction of the inhibitor is 10%-12%, the mass fraction of the catalyst is 9%-15%, and the rest is naphthalene-based high-efficiency water reducer.
[0032] In step 2), the mass fraction of the esterified macromonomer is 18%-36%, the mass fraction of methacrylic acid required for preparing the polycarboxylic acid water reducer is 15%-25%, the mass fraction of the sulfonic acid monomer is 3%-5%, the mass fraction of the initiator is 2%-3%, the mass fraction of the molecular weight regulator is 10%-13%, and the rest is water.
[0033] The preparation principle of esterification macromonomer is as follows Figure 2 As shown, since the esterification reaction is reversible, the esterification rate of the reaction cannot reach 100%, so it is necessary to increase the amount of one of the reactants to increase the esterification rate. In view of the fact that methoxy polyethylene glycol has no role in the subsequent synthesis of polycarboxylic acid-based water reducers, an excess of methacrylic acid should be used in the reaction. In addition, in order to speed up the reaction rate and shorten the reaction time, one of concentrated sulfuric acid, periodic acid, benzenesulfonic acid, p-toluenesulfonic acid or ethylsulfonic acid can be added as a catalyst, which will dissolve in methoxy polyethylene glycol to form a homogeneous system. In view of the fact that methacrylic acid and the esterification macromonomer (polyethylene glycol monomethyl ether methacrylate) are prone to self-polymerization, a certain amount of inhibitor needs to be added in the reaction.
[0034] A modifier for reducing the moisture absorbed by loess in pile foundation grouting material, comprising the above-mentioned polycarboxylic acid water reducer, the modifier comprises the following components by weight percentage: 20%-40% polycarboxylic acid water reducer, 10%-30% inorganic salt early strength agent, 5%-15% retarder, 3%-8% dispersant, 2%-6% water retaining agent, and the balance is water, the sum of the components being 100%.
[0035] Furthermore, the inorganic salt early strength agent is selected from one or more combinations of calcium chloride, sodium sulfate, and calcium nitrate, which has a significant early strength effect and can accelerate the hardening process of the injection material.
[0036] Furthermore, the retarder is sodium gluconate or citric acid, which is used to adjust the setting time of the grouting material to prevent construction difficulties caused by too fast setting.
[0037] Furthermore, the dispersant is lignin sulfonate or naphthalene-based high-efficiency water reducer, which helps to improve the fluidity of the injection material and reduce pumping resistance.
[0038] Furthermore, the water retaining agent is polyacrylamide or acrylic acid-based super absorbent resin, which can effectively retain the moisture in the pouring material and reduce the water absorption of loess.
[0039] Furthermore, the molecular weight regulator is thioglycolic acid, which can adjust the molecular weight of the polycarboxylic acid water reducer, thereby affecting its water reducing performance.
[0040] The application controls the amount of initiator to be 2%-3%. The initiator is one or a mixture of several of ammonium persulfate, sodium persulfate, hydrogen peroxide and tert-butyl hydroperoxide. As the amount of initiator increases, the fluidity of the cement slurry gradually increases. When the amount of initiator reaches 2.8%, the fluidity of the slurry reaches the maximum value, showing the best dispersion effect, and the fluidity loss after 1 hour is minimal. The amount of initiator has a significant effect on the polymerization reaction, and its concentration is inversely proportional to the square of the relative molecular weight of the water reducer. When the amount of initiator is small, the molecular weight of the water reducer is large and the dispersibility is poor; when the amount of initiator is large, the molecular weight of the water reducer may be small, or an explosion phenomenon may occur, which will lead to a decrease in dispersibility. Therefore, in order to ensure that it achieves the best fluidity, the amount of initiator is 2%-3%.
[0041] The present application controls the polymerization temperature to be 70-80°C. The polymerization temperature will affect the decomposition rate of the initiator, thereby changing its half-life and affecting the concentration of the initiator free radicals in the polymerization solution. When the polymerization temperature is low, the initiator decomposes slowly, the half-life is long, and the free radical concentration in the reaction system is low, resulting in a slow polymerization rate and a large relative molecular mass of the generated polymer. On the contrary, when the polymerization temperature is high, the initiator decomposes quickly, the half-life is short, the free radical concentration in the reaction system is high, the polymerization rate is fast, and the generated polymer has a small relative molecular mass. At the same time, if the reaction temperature is too high, the decomposition rate of the initiator may be too fast, resulting in a too fast polymerization rate, thereby producing too many side chains, resulting in extremely uneven polymer molecular weight. Therefore, in order to ensure that the synthesized water reducer can exert the best dispersibility, the polymerization temperature needs to be maintained at 70-80°C.
[0042] The present application controls the polymerization concentration of the esterified macromonomer to be 18%-36%, that is, the mass concentration of the esterified macromonomer. When the polymerization concentration is low, the collision opportunities between the reaction molecules are reduced, resulting in a low conversion rate. As the polymerization concentration increases, the conversion rate will also increase, and at the same time, the degree of polymerization of the water reducer molecules increases, thereby increasing the relative molecular mass of the water reducer. Therefore, in order to obtain a water reducer with good performance, the polymerization concentration is selected to be 30%-40%.
[0043] The present application improves the fluidity of the grouting material by adding a high-performance polycarboxylate water-reducing agent and improving the dispersion performance of cement particles.
[0044] Among them, the water-reducing performance of polycarboxylic acid-based water-reducing agents is mainly based on the electrostatic effect on the surface of cement particles. The surface of cement particles will be charged under the action of electrostatics. These charges not only exist on the surface of the particles, but also are distributed in the free charges adsorbed by the gas. When the water-reducing agent is not used, the charges between the particles are in an unbalanced state, resulting in the mutual attraction between the charged particles due to the Coulomb force, which makes the particles close to each other and agglomerate; when the distance between the particles exceeds the range of the charge, the electrostatic repulsion causes the particles to disperse. When the water-reducing agent is added, the water-reducing agent molecules will be adsorbed on the surface of the cement particles, further enhancing the electrostatic repulsion, thereby reducing the agglomeration of the particles and improving the dispersion performance and fluidity of the cement. At the same time, the side chains and groups in the water-reducing agent can produce adsorption and repulsion effects on the surface of the particles, further enhancing the dispersion effect of the cement paste.
[0045] The molecular structure of polycarboxylic acid-based water-reducing agents is usually composed of different active groups, such as polyoxyethylene chains, carboxyl groups, sulfonic acid groups, etc. These groups will induce electrostatic effects and steric hindrance effects on the surface of cement particles, thereby significantly improving the water-reducing performance and durability.
[0046] The dispersibility of this high-performance polycarboxylate water reducer is mainly attributed to the steric hindrance effect, followed by electrostatic repulsion. In addition, the complexation of calcium ions in inorganic salts and the lubrication of hydration film also have a certain influence on the dispersibility.
[0047] According to the steric hindrance theory, when the polycarboxylate water-reducing agent molecules first contact cement particles, the negatively charged main chain in the molecule will be adsorbed on the surface of the positively charged cement particles, forming an "anchoring" phenomenon. At the same time, the long side chains in the polycarboxylate water-reducing agent molecules expand in the liquid phase of the cement paste to form an adsorption layer of a certain thickness. These long side chains are intertwined with the long side chains in other molecules to form a three-dimensional cross structure. When the cement particles move toward each other, these adsorption layers will overlap. The greater the overlap, the stronger the repulsion between the cement particles, thereby improving the dispersibility of the cement particles. Studies have shown that the thick adsorption layer formed by the polycarboxylate water-reducing agent molecules on the surface of cement particles helps to improve the dispersion of cement particles.
[0048] According to the electrostatic repulsion theory, polycarboxylate water-reducing agent molecules contain anionic groups (such as sulfonate and carboxylate), while cement particles carry positive charges during the early hydration process. Therefore, anionic polycarboxylate water-reducing agent molecules will adsorb to the surface of these positively charged cement particles. In this process, the polar groups in the polycarboxylate water-reducing agent molecules adsorbed on the surface of cement particles will interact with the same electrical charges in the liquid phase to form a double electric layer. Studies have shown that the strength of electrostatic repulsion is from large to small: -SO3>-COO>-O>-OH.
[0049] According to the complexation of calcium ions, the calcium ions in the inorganic salts will interact with the carboxylate radicals in the polycarboxylate water-reducing agent molecules in the cement paste to form a calcium coordination complex. This complexation reaction reduces the concentration of calcium ions in the liquid phase and reduces the formation of CHS gel particles, thereby slowing down the hydration rate of cement and inhibiting further hydration of cement.
[0050] According to the lubricating effect of the hydration film, the polycarboxylate water-reducing agent molecules contain strong polar groups such as carboxyl, sulfonic acid and ether groups, and have strong hydrophilicity. When the polycarboxylate water-reducing agent is added to the cement paste, its negatively charged carboxyl and sulfonic acid groups will be directional adsorbed on the surface of the cement particles. The polar groups in the polycarboxylate water-reducing agent form hydrogen bonds with water molecules, and the strength of this hydrogen bond is greater than the van der Waals force between the polycarboxylate water-reducing agent molecules and the cement particles. Therefore, a stable and strong solvated water film is formed on the surface of the cement particles. This water film reduces the direct contact between the cement particles, thereby playing a lubricating role, reducing the coagulation of cement particles, and ultimately improving the fluidity of the cement paste macroscopically.
[0051] The present invention also discloses a method for preparing the above-mentioned modifier for reducing the water absorption of the pile foundation grouting material by loess, such as Figure 3 As shown, the following steps are included:
[0052] a) Add water into a stirring container, turn on the stirrer, slowly add the polycarboxylate water reducer, and stir until it is completely dissolved;
[0053] b) adding an inorganic salt early strength agent, a retarder, a dispersant and a water retaining agent to the solution obtained in step a) in sequence, and each additive needs to be fully stirred after being added until it is uniform;
[0054] c) Continue stirring the mixture for 30-40 minutes until all components are fully reacted and evenly dispersed to obtain the finished modifier.
[0055] The feeding sequence of the present invention is to dissolve the polycarboxylic acid water reducer first and then add other additives to ensure that each component can fully react and be evenly dispersed in water. At the same time, the process parameters such as stirring time and temperature are strictly controlled to ensure the stability and consistency of the finished modifier.
[0056] The modifier proposed in the present invention can be widely used in pile foundation construction in collapsible loess areas, and can reduce the absorption of loess on the water content of the grouting material, thereby improving the fluidity and early strength of the grouting material, thereby ensuring the construction quality and stability of the pile foundation. At the same time, the modifier also has good environmental friendliness and economic benefits, and is expected to be widely promoted and applied in actual projects.
[0057] In view of the above problems, the present invention proposes a new type of modifier and its preparation method, aiming to solve the difficult problems in pile foundation construction in collapsible loess areas through scientific and reasonable component ratio and preparation process. The modifier uses polycarboxylic acid water reducer as the core component, and is compounded with various auxiliary components such as inorganic salt early strength agent. By optimizing the ratio of each component and the preparation process, it realizes the effective control of loess water absorption and significantly improves the fluidity and early strength of the grouting material. At the same time, the present invention also proposes corresponding test methods and mix ratios, which provide a scientific basis for the practical application of the modifier.
[0058] 3. Beneficial effects
[0059] Compared with the prior art, the present invention has the following beneficial effects:
[0060] (1) The polycarboxylic acid-based water reducer of the present invention has excellent water reducing performance, effectively improving the dispersibility of the cast material, thereby improving the fluidity of the cast material;
[0061] (2) The modifier of the present invention uses a polycarboxylic acid-based water reducer as a core component and is compounded with a variety of auxiliary components such as an inorganic salt early strength agent. By optimizing the proportion of each component and the preparation process, the water absorption of loess is effectively controlled, and the fluidity and early strength of the grouting material are significantly improved;
[0062] (3) The modifier of the present invention can be widely used in pile foundation construction in collapsible loess areas, by reducing the absorption of loess on the water content of the grouting material, improving the fluidity and early strength of the grouting material, thereby ensuring the construction quality and stability of the pile foundation. BRIEF DESCRIPTION OF THE DRAWINGS
[0063] The technical solution of the present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments, but it should be understood that these drawings are designed only for explanation purposes and are not intended to limit the scope of the present invention. In addition, unless otherwise specified, these drawings are intended only to conceptually illustrate the structural configurations described herein and are not necessarily drawn to scale.
[0064] Figure 1 is the structural formula of the polycarboxylic acid water reducer of the present invention;
[0065] Figure 2 The preparation principle of the esterification macromonomer of the present invention;
[0066] Figure 3 The present invention is a flow chart of the preparation process of the modifier. DETAILED DESCRIPTION
[0067] The following detailed description of exemplary embodiments of the present invention refers to the accompanying drawings, which form a part of the description, and in which exemplary embodiments of the present invention that can be implemented are shown as examples. Although these exemplary embodiments are described in sufficient detail to enable those skilled in the art to implement the present invention, it should be understood that other embodiments can be implemented and various changes can be made to the present invention without departing from the spirit and scope of the present invention. The following more detailed description of the embodiments of the present invention is not intended to limit the scope of the claimed invention, but is only for the purpose of illustrating and not limiting the description of the characteristics and features of the present invention, so as to propose the best mode for performing the present invention and to enable those skilled in the art to implement the present invention. Therefore, the scope of the present invention is limited only by the appended claims.
[0068] Unless otherwise specified, the materials in the present invention are all commercially available.
[0069] The modifier of the invention can be widely used in pile foundation construction in collapsible loess areas, and can reduce the absorption of loess on water content of the grouting material, thereby improving the fluidity and early strength of the grouting material and ensuring the construction quality and stability of the pile foundation.
[0070] Embodiment 1-3 is applied to the process of controlling water loss in the loess during the construction of rotary bored piles for the base reinforcement of a collapsible loess tunnel, and comprises the following steps:
[0071] Raw material preparation: Weigh different proportions of polycarboxylic acid water reducer, calcium chloride early strength agent, sodium gluconate retarder, lignin sulfonate dispersant, and polyacrylamide water retaining agent according to weight percentage, and the balance is water.
[0072] Preparation of modifier: Add water to a stirring container, turn on the stirrer, slowly add polycarboxylic acid water reducer, and stir until completely dissolved; add calcium chloride, sodium gluconate, lignin sulfonate and polyacrylamide in sequence, and stir each additive thoroughly until uniform after adding; continue to stir the mixture for 30 minutes to ensure that each component is fully reacted and evenly dispersed to obtain the finished modifier.
[0073] Performance testing: Conduct fluidity test, early strength test and loess water absorption test on the finished modifier to ensure that it meets the construction requirements.
[0074] On-site construction: During the construction of rotary bored piles for the reinforcement of the collapsible loess tunnel base, the prepared modifier is added to the grouting material in a certain proportion, and the grouting is performed after being fully stirred. The modifier effectively reduces the absorption rate of the loess to the water of the grouting material, ensures the fluidity and early strength of the grouting material, and improves the bearing capacity and stability of the pile foundation.
[0075] Embodiment 4-6 is applied to the process of controlling water loss in micro-piling of collapsible loess roadbed slope, which comprises the following steps:
[0076] Raw material preparation: Weigh polycarboxylic acid water reducer, sodium sulfate early strength agent, citric acid retarder, naphthalene high efficiency water reducer dispersant, acrylic acid super absorbent resin water retaining agent according to weight percentage, and the balance is water.
[0077] Preparation of modifier: The operation steps are the same as those for controlling water loss in the loess reinforced by rotary bored piles for collapsible loess tunnel base.
[0078] Performance testing: The finished modifier is also tested for fluidity, early strength and loess water absorption to ensure that it meets the construction requirements.
[0079] On-site construction: During the construction of micro-piles on collapsible loess roadbed slopes, the prepared modifier is added to the grouting material in a certain proportion, and the mixture is poured after being fully stirred. Through the action of the modifier, the absorption rate of the loess on the water of the grouting material is also effectively reduced, the fluidity and early strength of the grouting material are improved, and thus the quality of the micro-piles and the stability of the slope are improved.
[0080] Example 1
[0081] The polycarboxylate water reducer of Example 1 is prepared by the following method:
[0082] 1) preparing an esterified macromonomer: mixing methoxy polyethylene glycol and methacrylic acid at a ratio of 0.8:1, adding a polymerization inhibitor and a naphthalene-based high-efficiency water reducer, reacting at 75° C. under a catalyst for 7 hours, and performing esterification to obtain an esterified macromonomer;
[0083] 2) Preparation of polycarboxylic acid water reducer: The prepared esterified macromonomer and methacrylic acid were mixed at a ratio of 1:0.75, and evenly added to a flask containing a sulfonic acid monomer. An initiator was added at the same time, and the mixture was kept warm at 75°C for 30 minutes. After the reaction was completed, the pH was adjusted to 6.5, and a molecular weight regulator was added dropwise into water for reaction for 20 minutes to obtain a polycarboxylic acid water reducer.
[0084] Wherein, the polymerization inhibitor is hydroquinone;
[0085] The catalyst is p-toluenesulfonic acid;
[0086] The sulfonic acid monomer is one or more of sodium p-styrene sulfonate or 2-acrylamide-2-methylpropane sulfonic acid;
[0087] The initiator is hydrogen peroxide;
[0088] The molecular weight regulator is thioglycolic acid;
[0089] The pH was adjusted using caustic soda.
[0090] In step 1), the mass fraction of the methoxy polyethylene glycol is 10%, when preparing the esterification macromonomer, the mass fraction of methacrylic acid is 12%, the mass fraction of hydroquinone is 10%, the mass fraction of p-toluenesulfonic acid is 9%, and the rest is naphthalene-based high-efficiency water reducer.
[0091] In step 2), the mass fraction of the esterified macromonomer is 20%, the mass fraction of methacrylic acid is 15% when preparing the polycarboxylate water reducer, the mass fraction of the sulfonic acid monomer is 3%, the mass fraction of the initiator is 2%, the mass fraction of the molecular weight regulator is 10%, and the rest is water.
[0092] The structure of the obtained polycarboxylic acid water reducer is:
[0093]
[0094] Among them, a=4, b=6, c=5, d=6, and the molecular weight is 8000-10000.
[0095] Example 2
[0096] The polycarboxylate water reducer of Example 2 is prepared by the following method:
[0097] 1) preparing an esterified macromonomer: mixing methoxy polyethylene glycol and methacrylic acid at a ratio of 0.8:1, adding a polymerization inhibitor and a naphthalene-based high-efficiency water reducer, reacting at 75° C. under a catalyst for 7 hours, and performing esterification to obtain an esterified macromonomer;
[0098] 2) Preparation of polycarboxylic acid water reducer: The prepared esterified macromonomer and methacrylic acid were mixed at a ratio of 1:0.75, and evenly added to a flask containing a sulfonic acid monomer. An initiator was added at the same time, and the mixture was kept warm at 75°C for 30 minutes. After the reaction was completed, the pH was adjusted to 6.5, and a molecular weight regulator was added dropwise into water for reaction for 20 minutes to obtain a polycarboxylic acid water reducer.
[0099] Wherein, the inhibitor is phenothiazine;
[0100] The catalyst is p-toluenesulfonic acid;
[0101] The sulfonic acid monomer is sodium p-styrene sulfonate;
[0102] The initiator is an aqueous solution of ascorbic acid;
[0103] The molecular weight regulator is mercaptoethanol;
[0104] The pH was adjusted using caustic soda.
[0105] In step 1), the mass fraction of the methoxy polyethylene glycol is 10%, when preparing the esterification macromonomer, the mass fraction of methacrylic acid accounts for 12%, the mass fraction of phenothiazine is 10%, the mass fraction of p-toluenesulfonic acid is 9%, and the rest is naphthalene-based high-efficiency water reducer.
[0106] In step 2), the mass fraction of the esterified macromonomer is 20%, the mass fraction of methacrylic acid is 15% when preparing the polycarboxylate water reducer, the mass fraction of the sulfonic acid monomer is 3%, the mass fraction of the initiator is 2%, the mass fraction of the molecular weight regulator is 10%, and the rest is water.
[0107] The structure of the obtained polycarboxylic acid water reducer is:
[0108]
[0109] Among them, a=5, b=5, c=6, d=4, and the molecular weight is 9000-13000.
[0110] Example 3
[0111] The polycarboxylate water reducer of Example 3 is prepared by the following method:
[0112] 1) preparing an esterified macromonomer: mixing methoxy polyethylene glycol and methacrylic acid at a ratio of 0.8:1, adding a polymerization inhibitor and a naphthalene-based high-efficiency water reducer, reacting at 75° C. under a catalyst for 7 hours, and performing esterification to obtain an esterified macromonomer;
[0113] 2) Preparation of polycarboxylic acid water reducer: The prepared esterified macromonomer and methacrylic acid were mixed at a ratio of 1:0.8, and evenly added to a flask containing a sulfonic acid monomer. An initiator was added at the same time, and the mixture was kept warm at 75°C for 30 minutes. After the reaction was completed, the pH was adjusted to 6.5, and a molecular weight regulator was added dropwise into water for reaction for 20 minutes to obtain a polycarboxylic acid water reducer.
[0114] Wherein, the polymerization inhibitor is hydroquinone;
[0115] The catalyst is ethylsulfonic acid;
[0116] The sulfonic acid monomer is 2-acrylamide-2-methylpropane sulfonic acid;
[0117] The initiator is hydrogen peroxide;
[0118] The molecular weight regulator is mercaptopropionic acid;
[0119] The pH was adjusted using caustic soda.
[0120] In step 1), the mass fraction of the methoxy polyethylene glycol is 10%, when preparing the esterification macromonomer, the mass fraction of methacrylic acid is 12%, the mass fraction of hydroquinone is 10%, the mass fraction of ethyl sulfonic acid is 9%, and the rest is naphthalene-based high-efficiency water reducer.
[0121] In step 2), the mass fraction of the esterified macromonomer is 18%, methacrylic acid accounts for 15% when preparing the polycarboxylic acid water reducer, the mass fraction of the sulfonic acid monomer is 3%, the mass fraction of the initiator is 2%, the mass fraction of the molecular weight regulator is 10%, and the rest is water.
[0122] The structure of the obtained polycarboxylic acid water reducer is:
[0123]
[0124] Among them, a=6, b=6, c=5, d=4, and the molecular weight is 10000-13000.
[0125] Example 4
[0126] The modifier of Example 4 includes, by mass fraction, 30% of a polycarboxylic acid water reducer, 20% of a calcium chloride early strength agent, 10% of a sodium gluconate retarder, 6% of a lignin sulfonate dispersant, 4% of a polyacrylamide water retaining agent, and the remainder is water, wherein the polycarboxylic acid water reducer adopts the polycarboxylic acid water reducer prepared in Example 1.
[0127] The preparation process of the modifier comprises the steps of:
[0128] a) Add water into a stirrer, turn on the stirrer, slowly add the polycarboxylate water reducer, and stir until it is completely dissolved to form a uniform solution;
[0129] b) adding calcium chloride, sodium gluconate, lignin sulfonate and polyacrylamide in sequence, and stirring each additive thoroughly until uniform after addition to ensure that each component is fully dispersed;
[0130] c) Continue stirring the mixture for 30 minutes, keeping the stirring speed and temperature constant to ensure that all components react fully and are evenly dispersed to form a stable finished modifier.
[0131] The dosage of the modifier is 0.3wt% of the concrete, and the distribution ratio of each component in the pouring material is: cement: gravel: sand: water: modifier = 1: 2.61: 2.13: 0.41: 0.015.
[0132] Example 5
[0133] The modifier of Example 5 includes, by mass fraction, 30% of a polycarboxylic acid water reducer, 20% of a sodium sulfate early strength agent, 10% of a sodium gluconate retarder, 6% of a lignin sulfonate dispersant, 4% of a polyacrylamide water retaining agent, and the balance is water, wherein the polycarboxylic acid water reducer adopts the polycarboxylic acid water reducer prepared in Example 1.
[0134] The preparation process of the modifier comprises the steps of:
[0135] a) Add water into a stirrer, turn on the stirrer, slowly add the polycarboxylate water reducer, and stir until it is completely dissolved to form a uniform solution;
[0136] b) adding sodium sulfate, sodium gluconate, lignin sulfonate and polyacrylamide in sequence, and stirring each additive thoroughly until uniform after addition to ensure that each component is fully dispersed;
[0137] c) Continue stirring the mixture for 30 minutes, keeping the stirring speed and temperature constant to ensure that all components react fully and are evenly dispersed to form a stable finished modifier.
[0138] The dosage of the modifier is 0.3wt% of the concrete, and the distribution ratio of each component in the pouring material is: cement: gravel: sand: water: modifier = 1: 2.61: 2.13: 0.41: 0.015.
[0139] Example 6
[0140] The modifier of Example 6 includes, by mass fraction, 30% of a polycarboxylic acid water reducer, 20% of a mixed early strength agent of calcium chloride and sodium sulfate (the mass ratio of calcium chloride to sodium sulfate is 1:1), 10% of a sodium gluconate retarder, 6% of a lignin sulfonate dispersant, 4% of a polyacrylamide water retaining agent, and the balance is water, wherein the polycarboxylic acid water reducer adopts the polycarboxylic acid water reducer prepared in Example 1.
[0141] The preparation process of the modifier comprises the steps of:
[0142] a) Add water into a stirrer, turn on the stirrer, slowly add the polycarboxylate water reducer, and stir until it is completely dissolved to form a uniform solution;
[0143] b) adding calcium chloride and sodium sulfate mixture, sodium gluconate, lignin sulfonate and polyacrylamide in sequence, and stirring each additive thoroughly until uniform after adding to ensure that each component is fully dispersed;
[0144] c) Continue stirring the mixture for 30 minutes, keeping the stirring speed and temperature constant to ensure that all components react fully and are evenly dispersed to form a stable finished modifier.
[0145] The dosage of the modifier is 0.3wt% of the concrete, and the distribution ratio of each component in the pouring material is: cement: gravel: sand: water: modifier = 1: 2.61: 2.13: 0.41: 0.015.
[0146] Example 7
[0147] The modifier of Example 7 includes, by mass fraction, 25% of polycarboxylic acid water reducer, 15% of calcium chloride early strength agent, 8% of citric acid retarder, 5% of naphthalene high-efficiency water reducer dispersant, 3% of acrylic acid super absorbent resin water retaining agent, and the balance is water, wherein the polycarboxylic acid water reducer adopts the polycarboxylic acid water reducer prepared in Example 1.
[0148] The preparation process of the modifier comprises the steps of:
[0149] a) Add water into a stirrer, turn on the stirrer, slowly add the polycarboxylate water reducer, and stir until it is completely dissolved to form a uniform solution;
[0150] b) Add calcium chloride, citric acid retarder, high-efficiency water reducing agent dispersant and acrylic acid super absorbent resin water retaining agent amine in sequence. After adding each additive, stir thoroughly until uniform to ensure that each component is fully dispersed;
[0151] c) Continue stirring the mixture for 30 minutes, keeping the stirring speed and temperature constant to ensure that all components react fully and are evenly dispersed to form a stable finished modifier.
[0152] The dosage of the modifier is 0.3wt% of the concrete, and the distribution ratio of each component in the pouring material is: cement: gravel: sand: water: modifier = 1: 2.61: 2.13: 0.41: 0.015.
[0153] Example 8
[0154] The modifier of Example 8 includes, by mass fraction, 25% of polycarboxylic acid water reducer, 15% of calcium chloride early strength agent, 8% of citric acid retarder, 5% of naphthalene high-efficiency water reducer dispersant, 3% of acrylic acid super absorbent resin water retaining agent, and the balance is water, wherein the polycarboxylic acid water reducer adopts the polycarboxylic acid water reducer prepared in Example 1.
[0155] The preparation process of the modifier comprises the steps of:
[0156] a) Add water into a stirrer, turn on the stirrer, slowly add the polycarboxylate water reducer, and stir until it is completely dissolved to form a uniform solution;
[0157] b) Add calcium chloride, citric acid retarder, high-efficiency water reducing agent dispersant and acrylic acid super absorbent resin water retaining agent amine in sequence. After adding each additive, stir thoroughly until uniform to ensure that each component is fully dispersed;
[0158] c) Continue stirring the mixture for 30 minutes, keeping the stirring speed and temperature constant to ensure that all components react fully and are evenly dispersed to form a stable finished modifier.
[0159] The dosage of the modifier is 0.3wt% of the concrete, and the distribution ratio of each component in the pouring material is: cement: gravel: sand: water: modifier = 1: 2.61: 2.13: 0.41: 0.015.
[0160] Example 9
[0161] The modifier of Example 9 includes, by mass fraction, 25% of polycarboxylic acid water reducer, 15% of calcium chloride and sodium sulfate early strength agent, 8% of citric acid retarder, 5% of naphthalene high-efficiency water reducer dispersant, 3% of acrylic acid super absorbent resin water retaining agent, and the balance is water, wherein the polycarboxylic acid water reducer adopts the polycarboxylic acid water reducer prepared in Example 1.
[0162] The preparation process of the modifier comprises the steps of:
[0163] a) Add water into a stirrer, turn on the stirrer, slowly add the polycarboxylate water reducer, and stir until it is completely dissolved to form a uniform solution;
[0164] b) Add calcium chloride and sodium sulfate mixture, citric acid retarder, high-efficiency water reducing agent dispersant and acrylic acid super absorbent resin water retaining agent amine in sequence. After adding each additive, stir thoroughly until uniform to ensure that each component is fully dispersed;
[0165] c) Continue stirring the mixture for 30 minutes, keeping the stirring speed and temperature constant to ensure that all components react fully and are evenly dispersed to form a stable finished modifier.
[0166] The dosage of the modifier is 0.3wt% of the concrete, and the distribution ratio of each component in the pouring material is: cement: gravel: sand: water: modifier = 1: 2.61: 2.13: 0.41: 0.015.
[0167] Comparative Example 1
[0168] The proportions of the components in the perfusion material are the same as those in Example 4, except that no modifier is added.
[0169] Comparative Example 2
[0170] The proportions of the components in the pouring material are the same as those in Example 4, except that no polycarboxylic acid water reducer is added to the modifier.
[0171] Comparative Example 3
[0172] The proportions of the components in the pouring material are the same as those in Example 4, except that no early strength agent is added to the modifier.
[0173] Comparative Example 4
[0174] The proportions of the components in the pouring material are the same as those in Example 4, except that no retarder is added to the modifier.
[0175] Comparative Example 5
[0176] The proportions of the components in the pouring material are the same as those in Example 4, except that no dispersant is added to the modifier.
[0177] Comparative Example 6
[0178] The proportions of the components in the pouring material are the same as those in Example 4, except that no water retaining agent is added to the modifier.
[0179] Comparative Example 7
[0180] The ratio of each component in the pouring material is the same as that in Example 4. The difference from Example 4 is that the ratio of each component of the modifier is: 10% polycarboxylic acid water reducer, 5% inorganic salt early strength agent, 5% retarder, 3% dispersant, 2% water retaining agent, and the balance is water, and the sum of each component is 100%.
[0181] Performance testing: Conduct fluidity test, early strength test and loess water absorption test on the finished modifier to ensure that it meets the construction requirements.
[0182] Concrete fluidity test: carried out in accordance with the national standard "GB / T 50080-2016 Concrete Engineering Construction Quality Acceptance Code".
[0183] The test should be carried out as follows:
[0184] (1) Place the funnel on a flat plate and use a steel needle to make a small hole in the center of the bottom of the funnel;
[0185] (2) Stir the sample evenly and then divide it into 3 parts;
[0186] (3) Pour the first sample into the funnel and open the small hole at the bottom to allow it to flow freely;
[0187] (4) After the first portion of the sample has completely flowed out, vibrate the outside of the funnel 45 times with a vibrating rod;
[0188] (5) Pour the second sample into the funnel and repeat steps (3) and (4);
[0189] (6) Pour the third sample into the funnel, repeat steps (3) and (4), and then close the small hole at the bottom;
[0190] (7) Lift the funnel upward so that the sample flows from the funnel onto the flatness plate;
[0191] (8) Vibrate the flatness plate 45 times;
[0192] (9) Use a steel needle to measure the distance between the highest point and the lowest point of the sample on the star flatness plate and record it as the fluidity.
[0193] Table 1 shows the cement paste fluidity of the embodiments and comparative examples.
[0194] category Initial net slurry fluidity / mm Fluidity after 60min / mm Fluidity after 120min / mm Example 1 275 267 254 Example 2 268 262 251 Example 3 277 271 263 Example 4 271 264 253 Example 5 271 264 253 Example 6 275 269 261 Comparative Example 1 269 257 249
[0195] It can be seen from the data in Table 1 that the fluidity of the pure slurry prepared according to Examples 1-6 after adding the modifier is good, and the fluidity loss after 1 hour and 2 hours is small.
[0196] Comparing Examples 4 and 7 with Examples 5 and 8 and Examples 6 and 9, it can be seen that the modifier added to the pouring material uses calcium chloride and sodium sulfate early strength agent, and the fluidity loss is small.
[0197] Concrete mechanical properties test
[0198] According to the methods of Examples 4-9 and Comparative Examples 1-7, a polycarboxylic acid-based water reducer was prepared and added to concrete in a ratio of cement: gravel: sand: water: modifier = 1: 2.61: 2.13: 0.41: 0.015. The cement was 42.5R cement, the fly ash was Class F secondary fly ash, the fineness modulus of the sand was 3.12, the maximum particle size of the gravel was 31.5 mm, the stirring time was 90 seconds, the vibration time was 15 seconds, and the concrete was cured at (20±3)°C for 12 hours. After demolding, a standard test block was made. The properties of the concrete were tested according to the following standards, and the test results are recorded in Table 2.
[0199] 1. Compressive strength: Tested in accordance with GB / T50081-2002 "Standard for Test Methods of Mechanical Properties of Ordinary Concrete";
[0200] 2. Stability test: Test in accordance with GB / T1346-2011 "Test methods for water consumption, setting time and stability of cement standard consistency";
[0201] 3. Setting time: Tested in accordance with GB / T8076-2008 "Concrete Admixtures";
[0202] 4. Standard consistency water consumption: Test in accordance with GB / T1346-2011 "Test methods for water consumption, setting time and stability of cement standard consistency";
[0203] 5. Slump: Test in accordance with GB / T50080-2016 "Standard for Test Methods for Performance of Ordinary Concrete Mixtures".
[0204] Table 2 Mechanical properties test of concrete in the embodiments and comparative examples
[0205]
[0206] It can be seen from the data in Table 2 that after adding the modifier to the grouting material of Examples 4-9, the compressive strength thereof is significantly improved, and has no adverse effect on the later strength improvement. The 7-day compressive strength reaches 34.8-37.2 MPa, and the 28-day compressive strength is 42.3-45.1 MPa. In addition, the water consumption of the standard consistency is low, the setting time is fast, the shrinkage is small, the slump is low, and the fluidity is good.
[0207] Comparing Examples 4 and 7 with Examples 5 and 8 and Examples 6 and 9, it can be seen that the modifier added to the injection material uses calcium chloride and sodium sulfate early strength agent, which has a good strength improvement effect.
[0208] The grouting material of Comparative Example 1 did not contain any modifier, and in Comparative Example 2, no polycarboxylic acid water reducer was added to the modifier. The early strength of the grouting materials prepared by Comparative Example 1 and Comparative Example 2 was poor, and the later strength growth was slow. Comparative Example 2 did not contain any polycarboxylic acid water reducer, and its standard consistency water consumption was high, up to 36%.
[0209] In comparative example 3, no early strength agent was added to the modifier, and its early strength was poor, only 27.1 MPa.
[0210] In comparative example 4, no retarder is added to the modifier, and the initial setting and retarding time are relatively early, which has an adverse effect on the early strength of concrete.
[0211] In comparative example 5, no dispersant was added to the modifier, and the concrete showed problems such as cracking, fissures, and deformation, resulting in a decrease in strength.
[0212] In Comparative Example 6, no water retaining agent was added to the modifier, and the water consumption at standard consistency was high, and the slump loss was large.
[0213] The difference between the modifier added in Comparative Example 7 and Examples 1-6 is that the ratio of the components of the modifier is: 10% polycarboxylic acid water reducer, 5% inorganic salt early strength agent, 5% retarder, 3% dispersant, 2% water retaining agent, and the balance is water, and the sum of the components is 100%. The water reducer is less, the early strength is poor, and the water consumption of the standard consistency is higher.
[0214] Through the detailed description of the above embodiments and comparative examples, it can be seen that the modifier for reducing the absorption of water of pile foundation grouting material by loess proposed by the present invention is effective and feasible in practical applications. The modifier can significantly reduce the absorption rate of loess to the water of the grouting material, improve the fluidity and early strength of the grouting material, thereby ensuring the construction quality and stability of the pile foundation. At the same time, the modifier also has good environmental friendliness and economic benefits, and is expected to be widely promoted and applied in practical projects.
[0215] The above description is only a preferred embodiment of the present application and an explanation of the technical principles used. Those skilled in the art should understand that the scope involved in the present application is not limited to the technical solution formed by a specific combination of the above-mentioned technical features, but should also cover other technical solutions formed by any combination of the above-mentioned technical features or their equivalent features without departing from the inventive concept, such as a technical solution formed by replacing the above-mentioned features with (but not limited to) technical features with similar functions disclosed in this application.
[0216] Except for the technical features described in the specification, the remaining technical features are known technologies to those skilled in the art. In order to highlight the innovative features of the present invention, the remaining technical features will not be described here in detail.
Claims
1. A polycarboxylic acid water reducing agent, characterized in that: The structural formula of the polycarboxylate water reducer is: In the formula, R1, R2, R3, R4, R5 and R6 are alkyl groups containing 1 to 30 carbon atoms, a=4-6, b=4-6, c=4-6, d=4-6.
2. The polycarboxylic acid water reducing agent according to claim 1, characterized in that: The molecular weight of the polycarboxylic acid water reducer is 10,000 to 15,000.
3. A method for preparing the polycarboxylic acid water reducer according to any one of claims 1 to 2, characterized in that: Includes steps: 1) preparing an esterified macromonomer: mixing methoxy polyethylene glycol and methacrylic acid in a ratio of (0.8-0.9):1, adding a polymerization inhibitor and a naphthalene-based high-efficiency water reducer, reacting at 70-80° C. under the action of a catalyst for 6-8 hours to perform esterification to obtain an esterified macromonomer; 2) Preparation of polycarboxylic acid water reducer: The prepared esterified macromonomer and methacrylic acid are mixed in a ratio of 1: (0.7-0.8), and uniformly added dropwise to a flask containing a sulfonic acid monomer, and an initiator is added dropwise at the same time, and the mixture is kept warm at 70-80° C. for 30-40 min. After the reaction is completed, the pH value is adjusted to 6-7, and a molecular weight regulator is added to react for 20-30 min to obtain a polycarboxylic acid water reducer.
4. A modifier for reducing the water absorption of loess into pile foundation grouting material, characterized in that: The invention comprises the polycarboxylic acid water reducer according to any one of claims 1 to 2, and the modifier comprises the following components by weight percentage: 20%-40% polycarboxylic acid water reducer, 10%-30% inorganic salt early strength agent, 5%-15% retarder, 3%-8% dispersant, 2%-6% water retaining agent, and the balance is water, and the sum of the components is 100%.
5. The modifier according to claim 4, characterized in that The inorganic salt early strengthening agent is selected from one or more combinations of calcium chloride, sodium sulfate and calcium nitrate.
6. The modifier according to claim 4, characterized in that The retarder is sodium gluconate or citric acid.
7. The modifying agent according to claim 4, characterized in that The dispersant is lignin sulfonate or naphthalene-based high-efficiency water reducer.
8. The modifying agent according to claim 4, characterized in that The water retaining agent is polyacrylamide or acrylic acid super absorbent resin.
9. A method for preparing the modifying agent according to any one of claims 4 to 8, comprising the following steps: a) Slowly add the polycarboxylate water reducer into water and stir until it is completely dissolved; b) adding an inorganic salt early strength agent, a retarder, a dispersant and a water retaining agent to the solution obtained in step a) in sequence and stirring evenly; c) Continue stirring the mixture for 30-40 minutes until it is fully reacted and evenly dispersed to obtain the finished modifier.