Benzimidazole structure covalent triazine framework porous organic polymer as well as preparation method and application thereof

By designing the benzimidazole structure covalent triazine frame porous organic polymer, the problems of high energy consumption and low separation efficiency in the separation process of acetylene and carbon dioxide are solved, and efficient and economical C2H2/CO2 adsorption and separation are achieved, reducing environmental pollution .

CN118978655APending Publication Date: 2024-11-19NINGDE NORMAL UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411059131.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

In the separation process of acetylene (C2H2) and carbon dioxide (CO2), the prior art has problems of high energy consumption and low separation efficiency. The traditional separation method is costly and has a negative impact on the environment, and lacks efficient physical adsorbents.

Method used

A benzimidazole structure covalent triazine frame porous organic polymer was designed and prepared, and the dicyanobenzimidazole monomer was reverse synthesized by amine condensation, and the co-synthesis of the benzimidazole functional groups was synthesized through triazine frame polymerization. The valent triazine frame material CTF-CCx has a high specific surface area and a rich microporous structure, which enhances the adsorption and separation performance of C2H2/CO2.

Benefits of technology

This material significantly improves the adsorption and separation performance of C2H2/CO2, enhances the interaction force between polymer and guest molecules, and can efficiently separate C2H2/CO2, reduces production costs, and reduces environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978655A_ABST
    Figure CN118978655A_ABST
Patent Text Reader

Abstract

The invention discloses a benzimidazole structure covalent triazine framework porous organic polymer, and a preparation method thereof comprises the following steps: mixing p-cyanobenzaldehyde, 3, 4-diaminobenzene and sodium hydrogen sulfite into N, N-dimethylformamide, and after the reaction is completed, carrying out suction filtration on the reaction mixture to obtain a crude product 1; washing and drying the crude product 1, performing chromatography column passing, and drying again to obtain CCHBI; mixing the CCHBI and anhydrous zinc chloride, transferring into a tubular furnace, introducing nitrogen into the tubular furnace, heating to 400-600 DEG C at the rate of 1-10 DEG C / min, and reacting for 40 hours to obtain a crude product 2; taking out the crude product 2, putting into a mortar for grinding, pouring into deionized water for soaking, carrying out suction filtration and washing, and carrying out vacuum drying to obtain a crude product 3; pouring an HCl solution into the crude product 3, stirring for 24 hours, washing, respectively performing Soxhlet extraction by using water and acetone for 24 hours, and drying to obtain a sample CTF-CCx; according to the invention, the interaction force between the polymer and guest molecules and the adsorption and separation performance on C2H2 / CO2 are effectively enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of porous materials, and particularly relates to a benzimidazole structure covalent triazine framework porous organic polymer and a preparation method and application thereof. Background Art

[0002] Acetylene (C2H2) is an important industrial raw material and is widely used in synthetic rubber, plastics, synthetic fibers and other fields. However, the production process of C2H2 is often accompanied by the generation of CO2, which not only increases the production cost, but also has a negative impact on the environment, exacerbating the problem of greenhouse gas emissions and climate change. With the continuous deepening of the industrialization process and the increasing attention to environmental protection, C2H2 / CO2 separation has attracted much attention as a challenging and important technical issue. By improving the purity and yield of C2H2, not only can the production cost be reduced, but also the pollution to the environment can be reduced, which meets the requirements of sustainable development. At present, various separation technologies such as absorption, membrane separation, and chemical adsorption are widely used in C2H2 / CO2 separation, but they still face challenges such as high energy consumption and low separation efficiency. Traditional separation methods, such as separation using solvent extraction and cryogenic distillation, have defects such as high cost and high energy consumption. The use of physical adsorbents can achieve efficient adsorption separation with relatively low energy consumption. This makes physical adsorbents more economical, so the research and development of new physical adsorbents has received increasing attention in the field of scientific research.

[0003] Porous organic polymer materials are widely used in the field of adsorption separation due to their diverse porous structures, ultra-high BET specific surface area, flexible framework adjustability, and excellent physical / chemical stability. Chinese patent application number CN202110435545.5 discloses a covalent organic framework material that can be used for C2H2 / CO2 and C2H2 / CO2 adsorption separation. The preparation method is as follows: ultrasonically mix and disperse aldehyde precursors and amine precursors in an organic solvent, add an acid catalyst, cool with liquid nitrogen, freeze and thaw to degas, seal and react at 80-150°C for 3-9 days, and then post-treat to obtain the three-dimensional covalent organic framework material prepared by the invention. It has a very high specific surface area (347 5m 2 / g). Compared with methane, the prepared two-dimensional covalent organic framework material has better acetylene and carbon dioxide adsorption performance. The adsorption capacities of C2H2, CO2 and CH4 at 298K are 77.8, 39.4 and 9.6 cm-1, respectively. 3 / g, and under equal proportion mixed gas, its C2H2 / CH4 and C2H2 / CO2 separation selectivities are 306.2 and 4.8 respectively.

[0004] Covalent triazine frameworks (CTFs) are a class of important porous organic polymer materials. They have become the focus of gas adsorption and separation due to their high nitrogen content, excellent porosity and physicochemical stability. Covalent triazine frameworks (CTFs) are a class of porous organic polymers with triazine rings as the core structure. They have aromatic 1,3,5-triazine rings with planar π-conjugated properties as the main structural features, and can be changed into the required structure according to different synthesis conditions. CTFs materials are low in cost, and the conjugation effect between triazine rings and aromatic rings reduces the energy of the framework, which can improve the chemical stability of the polymer. The stable chemical structure gives it the advantages of long service life and good economic benefits. At present, it is rare to use covalent organic framework materials as adsorption materials for C2H2 / CO2. The present invention aims to "bind" nitrogen functional groups with high Lewis basicity to triazine organic frameworks, design and prepare a series of Lewis basic nitrogen-rich structure CTFs, and study their adsorption and separation performance. Summary of the invention

[0005] In order to solve the above problems, the present invention provides a method for preparing a benzimidazole covalent triazine framework porous organic polymer. The benzimidazole covalent triazine framework porous organic polymer prepared by the present invention has a large specific surface area and rich microporous structure, and can be used as an excellent material for a physical adsorbent.

[0006] The technical solution of the present invention is as follows:

[0007] One of the purposes of the present invention is to provide a benzimidazole structure covalent triazine framework porous organic polymer, the structural formula of the porous organic polymer is:

[0008]

[0009] The second object of the present invention is to provide a method for preparing a benzimidazole structure covalent triazine framework porous organic polymer, comprising the following steps:

[0010] S1: p-cyanobenzaldehyde, 3,4-diaminobenzonitrile and sodium bisulfite were mixed in N,N-dimethylformamide, reacted at 140°C for 24 hours, and the reaction mixture was filtered to obtain a crude product 1;

[0011] S2: washing the crude product 1 obtained in step S1, drying it, passing it through a chromatography column, and drying it again to obtain a pure sample of dicyanobenzimidazole monomer CCHBI;

[0012] S3: The CCHBI prepared in step S2 is mixed with anhydrous zinc chloride and transferred into a tube furnace, nitrogen is passed through the tube furnace for 15 minutes, and heated to 400-600°C at a rate of 1-10°C / min under a nitrogen atmosphere, and reacted for 40 hours to obtain a crude product 2;

[0013] S4: taking out the crude product 2 obtained in step S3, grinding it in a mortar, and soaking it in deionized water, filtering and washing it, and vacuum drying it to obtain a crude product 3;

[0014] S5: Pour HCl solution into the crude product 3 obtained in step S4 and stir for 24 hours. After washing, use water and acetone to Soxhlet extraction for 24 hours respectively, and obtain sample CTF-CCx after drying.

[0015] Furthermore, in step S1, the molar ratio of p-cyanobenzaldehyde, 3,4-diaminobenzonitrile and sodium bisulfite is 4:5:6.

[0016] Furthermore, in step S2, the crude product 1 is washed with deionized water, methanol, DMF, water and ethanol in sequence.

[0017] Furthermore, in step S2, the drying temperature is 85° C. and the drying time is 24 h.

[0018] Furthermore, in step S3, the molar ratio of CCHBI to anhydrous zinc chloride is 1:8.

[0019] Furthermore, in step S4, the crude product 2 is filtered and washed using water and methanol, and the number of times of filtration and washing is no less than 5 times.

[0020] Furthermore, in step S4, the vacuum drying time is 3 hours.

[0021] Furthermore, in step S5, deionized water and ethanol are used for washing.

[0022] The third object of the present invention is to provide a benzimidazole structure covalent triazine framework porous organic polymer for use in separation of C2H2 / CO2.

[0023] Compared with the prior art, the beneficial effects of the present invention are as follows: the present invention provides a method for preparing a benzimidazole structure covalent triazine framework porous organic polymer, utilizes amine condensation to reversely synthesize the dicyanobenzimidazole monomer CCHBI, and then synthesizes a series of covalent triazine framework materials CTF-CCx containing benzimidazole functional groups through triazine framework polymerization reaction, which has a very high specific surface area and rich microporous structure. Due to the benzimidazole and triazine structures, the binding ability of the covalent triazine framework material CTF-CCx with C2H2 is enhanced, and the polymer material has high adsorption and separation performance for C2H2 / CO2, and the present invention effectively enhances the interaction force between the polymer and the guest molecules and the adsorption and separation performance for C2H2 / CO2. The covalent triazine framework material CTF-CCx containing benzimidazole functional groups prepared by the present invention can be used as an excellent material of a physical adsorbent for separating C2H2 / CO2. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 Schematic diagram of the synthesis of dicyanobenzimidazole monomer CCHBI in the present invention;

[0025] Figure 2 Schematic diagram of the synthesis of CTF-CCx in the present invention;

[0026] Figure 3 The SEM images of the dicyanobenzimidazole monomers CCHBI and CTF-CCx in the present invention;

[0027] Figure 4 The infrared spectra of the dicyanobenzimidazole monomer CCHBI, 3,4-diaminobenzonitrile, p-cyanobenzaldehyde and CTF-CCx in the present invention;

[0028] Figure 5 is the hydrogen nuclear magnetic resonance spectrum of the dicyanobenzimidazole monomer CCHBI in the present invention;

[0029] Figure 6 The carbon nuclear magnetic resonance spectra of the dicyanobenzimidazole monomers CCHBI and CTF-CCx in the present invention;

[0030] Figure 7 XRD spectra of CTF-CCx prepared in Examples 1-7 of the present invention;

[0031] Figure 8 The XPS total spectrum and N1s fine spectrum of the dicyanobenzimidazole monomer CCHBI in the present invention and CTF-CCx prepared in Examples 1-7;

[0032] Fig. 9 The thermogravimetric diagrams of the dicyanobenzimidazole monomer CCHBI in the present invention and CTF-CCx prepared in Examples 1-7;

[0033] Fig.10 N2 adsorption and desorption isotherms of CTF-CCx prepared in Examples 1-7 at 77K and pore size distribution of CTF-CCx calculated by NLDFT method;

[0034] Fig.11 is the adsorption isotherms of CO2 and C2H2 of CTF-CC-5 and CTF-CC-6 at 296K and 273K;

[0035] Fig.12 Virial equation fitting curve parameters and adsorption heat curves of CTF-CC-5 and CTF-CC-6 for C2H2 in the present invention;

[0036] Fig.13 is the C2H2 / CO2 breakthrough curve of CTF-CC-5 in the present invention;

[0037] Fig.14 This is the C2H2 / CO2 breakthrough curve of CTF-CC-6 in the present invention. DETAILED DESCRIPTION

[0038] The following is combined with the preferred embodiment and with reference to the attached Figure 1-14 , the present invention is further described. The endpoints and any values ​​of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values; for numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, and these numerical ranges should be regarded as specifically disclosed herein; the materials, reagents, etc. used in the following examples, unless otherwise specified, can be obtained from commercial channels; the experimental methods in the following examples, unless otherwise specified, are all conventional methods.

[0039] Example 1

[0040] This embodiment provides a method for preparing a benzimidazole structure covalent triazine framework porous organic polymer, comprising the following steps:

[0041] S1: In a 250 mL round-bottom flask, 12 mmol of p-cyanobenzaldehyde, 15 mmol of 3,4-diaminobenzonitrile and 18 mmol of sodium bisulfite were mixed into 100 ml of N,N-dimethylformamide, and the mixture was reacted at 140 °C for 24 h. The reaction mixture was filtered to obtain a crude product 1;

[0042] S2: The crude product 1 obtained in step S1 is washed with deionized water, methanol, DMF, water, and ethanol in sequence, and dried at 85° C. for 24 hours, chromatographed, and dried again at 85° C. for 24 hours to obtain a pure sample of dicyanobenzimidazole monomer CCHBI; the synthesis schematic diagram of the dicyanobenzimidazole monomer CCHBI is as follows: Figure 1 As shown;

[0043] S3: CCHBI prepared in step S2 and anhydrous zinc chloride were mixed in a molar ratio of 1:8 and transferred into a tube furnace. Nitrogen was passed through the tube furnace for 15 min, and heated to 550° C. at a rate of 1° C. / min under a nitrogen atmosphere for 40 h to obtain a crude product 2;

[0044] S4: Open the tube furnace, take out the crude product 2 obtained in step S3, grind it in a mortar, soak it in deionized water, filter and wash it with water and ethanol five times each, and vacuum dry it for 3 hours to obtain a crude product 3;

[0045] S5: Pour HCl solution into the crude product 3 obtained in step S4 and stir for 24 hours to remove ZnCl2. After washing, use water and acetone to Soxhlet extract for 24 hours respectively, and obtain sample CTF-CC-1 after drying. The synthesis schematic diagram of CTF-CCx in this embodiment is as follows: Figure 2 shown.

[0046] Example 2

[0047] This embodiment provides a method for preparing a benzimidazole structure covalent triazine framework porous organic polymer, comprising the following steps:

[0048] S1: In a 250 mL round-bottom flask, 12 mmol of p-cyanobenzaldehyde, 15 mmol of 3,4-diaminobenzonitrile and 18 mmol of sodium bisulfite were mixed into 100 ml of N,N-dimethylformamide, and the mixture was reacted at 140 °C for 24 h. The reaction mixture was filtered to obtain a crude product 1;

[0049] S2: washing the crude product 1 obtained in step S1 with deionized water, methanol, DMF, water, and ethanol in sequence, drying at 85° C. for 24 h, column chromatography, and drying at 85° C. for 24 h again to obtain a pure sample of dicyanobenzimidazole monomer CCHBI;

[0050] S3: CCHBI prepared in step S2 and anhydrous zinc chloride were mixed in a molar ratio of 1:8 and transferred into a tube furnace. Nitrogen was passed through the tube furnace for 15 min, and heated to 550° C. at a rate of 5° C. / min under a nitrogen atmosphere. The mixture was reacted for 40 h to obtain a crude product 2.

[0051] S4: Open the tube furnace, take out the crude product 2 obtained in step S3, grind it in a mortar, soak it in deionized water, filter and wash it with water and ethanol five times each, and vacuum dry it for 3 hours to obtain a crude product 3;

[0052] S5: Pour HCl solution into the crude product 3 obtained in step S4 and stir for 24 hours to remove ZnCl2. After washing, use water and acetone to Soxhlet extraction for 24 hours respectively, and obtain sample CTF-CC-2 after drying.

[0053] Example 3

[0054] This embodiment provides a method for preparing a benzimidazole structure covalent triazine framework porous organic polymer, comprising the following steps:

[0055] S1: In a 250 mL round-bottom flask, 12 mmol of p-cyanobenzaldehyde, 15 mmol of 3,4-diaminobenzonitrile and 18 mmol of sodium bisulfite were mixed into 100 ml of N,N-dimethylformamide, and the mixture was reacted at 140 °C for 24 h. The reaction mixture was filtered to obtain a crude product 1;

[0056] S2: washing the crude product 1 obtained in step S1 with deionized water, methanol, DMF, water, and ethanol in sequence, drying at 85° C. for 24 h, column chromatography, and drying at 85° C. for 24 h again to obtain a pure sample of dicyanobenzimidazole monomer CCHBI;

[0057] S3: CCHBI prepared in step S2 and anhydrous zinc chloride were mixed in a molar ratio of 1:8 and transferred into a tube furnace. Nitrogen was passed through the tube furnace for 15 min, and heated to 550° C. at a rate of 10° C. / min under a nitrogen atmosphere. The mixture was reacted for 40 h to obtain a crude product 2.

[0058] S4: Open the tube furnace, take out the crude product 2 obtained in step S3, grind it in a mortar, soak it in deionized water, filter and wash it with water and ethanol five times each, and vacuum dry it for 3 hours to obtain a crude product 3;

[0059] S5: Pour HCl solution into the crude product 3 obtained in step S4 and stir for 24 hours to remove ZnCl2. After washing, use water and acetone to Soxhlet extraction for 24 hours respectively, and obtain sample CTF-CC-3 after drying.

[0060] Example 4

[0061] This embodiment provides a method for preparing a benzimidazole structure covalent triazine framework porous organic polymer, comprising the following steps:

[0062] S1: In a 250 mL round-bottom flask, 12 mmol of p-cyanobenzaldehyde, 15 mmol of 3,4-diaminobenzonitrile and 18 mmol of sodium bisulfite were mixed into 100 ml of N,N-dimethylformamide, and the mixture was reacted at 140 °C for 24 h. The reaction mixture was filtered to obtain a crude product 1;

[0063] S2: washing the crude product 1 obtained in step S1 with deionized water, methanol, DMF, water, and ethanol in sequence, drying at 85° C. for 24 h, column chromatography, and drying at 85° C. for 24 h again to obtain a pure sample of dicyanobenzimidazole monomer CCHBI;

[0064] S3: CCHBI prepared in step S2 and anhydrous zinc chloride were mixed in a molar ratio of 1:8 and transferred into a tube furnace. Nitrogen was passed through the tube furnace for 15 min, and heated to 400° C. at a rate of 5° C. / min under a nitrogen atmosphere. The mixture was reacted for 40 h to obtain a crude product 2.

[0065] S4: Open the tube furnace, take out the crude product 2 obtained in step S3, grind it in a mortar, soak it in deionized water, filter and wash it with water and ethanol five times each, and vacuum dry it for 3 hours to obtain a crude product 3;

[0066] S5: Pour HCl solution into the crude product 3 obtained in step S4 and stir for 24 hours to remove ZnCl2. After washing, use water and acetone to Soxhlet extraction for 24 hours respectively, and obtain sample CTF-CC-4 after drying.

[0067] Example 5

[0068] This embodiment provides a method for preparing a benzimidazole structure covalent triazine framework porous organic polymer, comprising the following steps:

[0069] S1: In a 250 mL round-bottom flask, 12 mmol of p-cyanobenzaldehyde, 15 mmol of 3,4-diaminobenzonitrile and 18 mmol of sodium bisulfite were mixed into 100 ml of N,N-dimethylformamide, and the mixture was reacted at 140 °C for 24 h. The reaction mixture was filtered to obtain a crude product 1;

[0070] S2: washing the crude product 1 obtained in step S1 with deionized water, methanol, DMF, water, and ethanol in sequence, drying at 85° C. for 24 h, column chromatography, and drying at 85° C. for 24 h again to obtain a pure sample of dicyanobenzimidazole monomer CCHBI;

[0071] S3: CCHBI prepared in step S2 and anhydrous zinc chloride were mixed in a molar ratio of 1:8 and transferred into a tube furnace. Nitrogen was passed through the tube furnace for 15 min, and heated to 450° C. at a rate of 5° C. / min under a nitrogen atmosphere. The mixture was reacted for 40 h to obtain a crude product 2.

[0072] S4: Open the tube furnace, take out the crude product 2 obtained in step S3, grind it in a mortar, soak it in deionized water, filter and wash it with water and ethanol five times each, and vacuum dry it for 3 hours to obtain a crude product 3;

[0073] S5: Pour HCl solution into the crude product 3 obtained in step S4 and stir for 24 hours to remove ZnCl2. After washing, use water and acetone to Soxhlet extraction for 24 hours respectively, and obtain sample CTF-CC-5 after drying.

[0074] Example 6

[0075] This embodiment provides a method for preparing a benzimidazole structure covalent triazine framework porous organic polymer, comprising the following steps:

[0076] S1: In a 250 mL round-bottom flask, 12 mmol of p-cyanobenzaldehyde, 15 mmol of 3,4-diaminobenzonitrile and 18 mmol of sodium bisulfite were mixed into 100 ml of N,N-dimethylformamide, and the mixture was reacted at 140 °C for 24 h. The reaction mixture was filtered to obtain a crude product 1;

[0077] S2: washing the crude product 1 obtained in step S1 with deionized water, methanol, DMF, water, and ethanol in sequence, drying at 85° C. for 24 h, column chromatography, and drying at 85° C. for 24 h again to obtain a pure sample of dicyanobenzimidazole monomer CCHBI;

[0078] S3: CCHBI prepared in step S2 and anhydrous zinc chloride were mixed in a molar ratio of 1:8 and transferred into a tube furnace. Nitrogen was passed through the tube furnace for 15 min, and heated to 500° C. at a rate of 5° C. / min under a nitrogen atmosphere. The mixture was reacted for 40 h to obtain a crude product 2.

[0079] S4: Open the tube furnace, take out the crude product 2 obtained in step S3, grind it in a mortar, soak it in deionized water, filter and wash it with water and ethanol five times each, and vacuum dry it for 3 hours to obtain a crude product 3;

[0080] S5: Pour HCl solution into the crude product 3 obtained in step S4 and stir for 24 hours to remove ZnCl2. After washing, use water and acetone to Soxhlet extraction for 24 hours respectively, and obtain sample CTF-CC-6 after drying.

[0081] Example 7

[0082] This embodiment provides a method for preparing a benzimidazole structure covalent triazine framework porous organic polymer, comprising the following steps:

[0083] S1: In a 250 mL round-bottom flask, 12 mmol of p-cyanobenzaldehyde, 15 mmol of 3,4-diaminobenzonitrile and 18 mmol of sodium bisulfite were mixed into 100 ml of N,N-dimethylformamide, and the mixture was reacted at 140 °C for 24 h. The reaction mixture was filtered to obtain a crude product 1;

[0084] S2: washing the crude product 1 obtained in step S1 with deionized water, methanol, DMF, water, and ethanol in sequence, drying at 85° C. for 24 h, column chromatography, and drying at 85° C. for 24 h again to obtain a pure sample of dicyanobenzimidazole monomer CCHBI;

[0085] S3: CCHBI prepared in step S2 and anhydrous zinc chloride were mixed in a molar ratio of 1:8 and transferred into a tube furnace. Nitrogen was passed through the tube furnace for 15 min, and heated to 600° C. at a rate of 5° C. / min under a nitrogen atmosphere. The mixture was reacted for 40 h to obtain a crude product 2.

[0086] S4: Open the tube furnace, take out the crude product 2 obtained in step S3, grind it in a mortar, soak it in deionized water, filter and wash it with water and ethanol five times each, and vacuum dry it for 3 hours to obtain a crude product 3;

[0087] S5: Pour HCl solution into the crude product 3 obtained in step S4 and stir for 24 hours to remove ZnCl2. After washing, use water and acetone to Soxhlet extraction for 24 hours respectively, and obtain sample CTF-CC-7 after drying.

[0088] Implementation effect evaluation:

[0089] The excellent effects achieved by the present invention are further illustrated by conducting specific tests on the benzimidazole covalent triazine framework porous organic polymers obtained in Examples 1-7:

[0090] Figure 3 The SEM images of CCHBI prepared in the present invention and CTF-CCx prepared in Examples 1-7 are as follows: Figure 3 As shown in the figure, ab is the SEM image of CCHBI magnified 10K times. Figure 3It can be seen from the figure that the CCHBI material is composed of regular small structures stacked together; ci is the SEM image of CTF-CCx prepared in Example 1-7. It can be seen from the figure that CTF-CC-1 is composed of irregular layered structures stacked together, which is a typical feature of organic porous polymers, while CCHBI does not have a similar structure, which proves that the present invention has successfully synthesized the triazine material. The layered structure may be caused by the rigid structure and π-π stacking structure of the polymer CTF-NH2.

[0091] Figure 4 The infrared spectra of the raw materials of the present invention, 3,4-diaminobenzonitrile, p-cyanobenzaldehyde, CCHBI and CTF-CCx prepared in Examples 1-7 are shown in FIG. Figure 4 As can be seen in (a), the 2229 cm-1 of 3,4-diaminobenzonitrile, p-cyanobenzaldehyde, and CCHBI -1 The characteristic peak of cyano group appears at , indicating that the present invention successfully synthesized CCHBI. Figure 4 As can be seen in (b), at 2229 cm -1 At , the characteristic peak of the nitrile group of CTF-CC-1 completely disappeared, indicating that the nitrile group of CCHBI had been completely reacted. Figure 4 (b) It can be found that the infrared spectrum of CTF-CC-1 has the peaks at 1590 and 1370 cm -1 The characteristic peak of the triazine ring appeared at the above results, indicating that the nitrile group has been converted into a triazine ring.

[0092] Figure 5 The CCHBI prepared by the present invention 1 H NMR spectrum, from Figure 5 It can be seen that CCHBI 1 The H NMR spectrum showed five hydrogen signals at δ8.34, 8.19, 8.04, 7.78, and 7.62 ppm, which were 2H on the benzene rings. The integrated areas of the peaks were 2, 1, 2, 1, and 1, respectively. The number of hydrogen atoms on the five benzene rings in CCHBI were 2, 1, 2, 1, and 1.

[0093] Figure 6 The CCHBI prepared in the present invention and the CTF-CCx prepared in Examples 1-7 are 13 C NMR spectrum, Figure 6 (a) is CCHBI 13 C NMR spectrum, Figure 6 (b) is CTF-CCx 13 C NMR spectrum. Figure 6 It can be seen that after the reaction, an aromatic carbon peak at 128.34 ppm was formed. Compared with the chemical shift of CCHBI, it changed, proving the successful synthesis of the material.

[0094] Figure 7 The XRD spectra of CTF-CCx prepared in Examples 1-7 of the present invention are shown in FIG. Figure 7 It can be seen that CTF-CCx is usually composed of amorphous structure and partial graphitization. The typical peaks of CTF-CC-2 to CTF-CC-7 near 24.41° indicate the amorphous nature of the polymer. The polymerization peak of CTF-CC-1 is at 25.84°, and the peak position is shifted. From the thermogravimetric data, it can be found that the monomer CCHBI begins to decompose at 300°C. This may be because the heating rate of CTF-CC-1 is low, and there is a longer reaction time in the temperature range above 300°C, which leads to more CCHBI being decomposed and destroyed, producing more amorphous structures. At the same time, it can be found that changing the temperature and the heating rate did not change the amorphous structure of the material.

[0095] Figure 8 The XPS total spectrum and N1s fine spectrum of CCHBI prepared in the present invention and CTF-CCx prepared in Examples 1-7 are shown. Figure 8 As shown, the overall spectrum of CTF-CCx shows that all materials have similar elemental compositions, namely C, N, and O. Figure 8 As can be seen from the figure, there are three forms of N in CTF-CC-1: pyridinic nitrogen (398 eV), i.e., N in the triazine ring; pyrrolic nitrogen (400.51 eV); and quaternary nitrogen, i.e., graphitized nitrogen (403.1 eV). Figure 4-8 As shown in (b), CCHBI only has pyridinic nitrogen and pyrrolic nitrogen. As CCHBI reacts, the pyridinic nitrogen decreases as the reaction occurs. This is because the polymerization of the triazine framework occurs and the cyano group is converted into a triazine ring. Figure 4-9 The binding energy of CTF-CC-4 is 396 eV, which belongs to nitride. This may be because the activation energy is too low at low temperature, and the cyanide generates an intermediate nitride. As the synthesis temperature increases, the nitride disappears.

[0096] Fig. 9 Thermogravimetric diagrams of CCHBI prepared in the present invention and CTF-CCx prepared in Examples 1-7 are shown in Table 1. Fig. 9It can be seen that the monomer CCHBI maintains excellent thermal stability at 300°C under nitrogen atmosphere, with almost no loss, and almost complete loss from 300°C to 400°C. After thermal ionic polymerization, CTF-CCx still retains a high weight residue at 800°C. CTF-CC-1 to CTF-CC-7 all retain more than 74% of their weight at 800°C. CTF-CC-4, CTF-CC-5, CTF-CC-6 and CTF-CC-7 retain 74.26%, 80.14%, 74.27% and 84.48% of their weight at 800°C, respectively. This provides support for CTF-CCx to perform gas separation adsorption in high temperature environments.

[0097] Fig.10 In the figure, (a) is the N2 adsorption and desorption isotherms of CTF-CCx prepared in Example 1-7 at 77K, and (b) is the pore size distribution of CTF-CCx calculated by the NLDFT method. Fig.10 It can be seen that with the increase of heating rate, the maximum nitrogen adsorption and BET specific surface area of ​​CTF-CCx show a trend of first increasing and then decreasing. With the increase of synthesis temperature, the maximum nitrogen adsorption and BET specific surface area generally show a trend of first increasing and then decreasing. This may be because as the final temperature increases, the triazine ring is destroyed, resulting in a decrease in micropores, a decrease in BET specific surface area and adsorption capacity. As shown in the table below, the BET specific surface area of ​​CTF-CC-5 in CTF-CCx is 1946m 2 ·g -1 , the maximum nitrogen adsorption capacity is 850cm 3 ·g -1 .like Fig.10 As shown, CTF-CC-5 has a typical type IV reversible curve under a higher relative pressure, indicating the presence of mesopores and / or macropores in the sample structure. At the same time, the average pore size of CTF-CC-5 is 2.7 nm, and the pore size distribution is concentrated in the range between 0.5 nm and 2.5 nm. This also proves the presence of mesopores and / or macropores in CTF-CC-5. The increase in the BET specific surface area and the maximum nitrogen adsorption capacity of CTF-CC-5 may be because this temperature is close to the activation energy of the conversion of triazine ring pyridine N to pyrrole N, resulting in the conversion of pyridine N to pyrrole N. This can be confirmed by the reduction of micropores and the increase of mesopores or mesopores. Fig.10 (b) is the pore size distribution of CTF-CCx calculated by the NLDFT method. It can be concluded that the pore size distribution of CTF-Ccx is concentrated below 2 nm, which is consistent with the pore size characteristics of porous organic polymers.

[0098] Table 1 Adsorption data of CTF-CCx

[0099] <![CDATA[Specific surface area (m 2 ·g -1 )]]> Pore ​​size (nm) <![CDATA[Adsorption capacity (cm 3 ·g -1 , STP)]]> CTF-CC-1 1503.87 0.88 424.83 CTF-CC-2 1641.01 0.67 496.11 CTF-CC-3 1534.39 0.80 468.53 CTF-CC-4 1249.64 1.02 369.08 CTF-CC-5 1946.77 0.95 850.11 CTF-CC-6 1839.35 0.99 531.58 CTF-CC-7 1714.71 1.01 532.02

[0100] Fig.11 The adsorption isotherms of CO2 and C2H2 of CTF-CC-5 and CTF-CC-6 at 296K and 273K. Fig.11 It can be seen that the maximum adsorption of C2H2 by CTF-CC-5 and CTF-CC-6 is 123.24 and 120.97 (296K, cm 3 ·g -1 , STP), and also higher than the adsorption capacity of TpPa-F (117 cm 3 ·g -1 ) is higher. The maximum adsorption of CO2 is 77.67 and 108.55 (296K, cm 3 ·g -1 , STP). Compared with CTF-CN-1 and CTF-NH2, they are greatly improved. This can be attributed to the abundant adsorption sites provided by the benzimidazole groups and triazine rings of CTF-CC-5 and CTF-CC-6, and secondly, the abundant ultra-microporous regions of CTF-CC-5. It is generally believed that narrow pores can enhance the interaction between C2H2 and CO2 and the surface of the triazine framework, and the microporous region is conducive to the adsorption of C2H2 and CO2.

[0101] Fig.12 The Virial equation fitting curve parameters and adsorption heat curves of C2H2 for CTF-CC-5 and CTF-CC-6 are shown in Figure 2. Fig.12 It can be seen that the zero-point adsorption heat of CTF-CC-5 and CTF-CC-6 for C2H2 and CO2 is 30.99 and 31.87 kJ·mol -1 , which proves that CTF-CC-5 and CTF-CC-6 have good adsorption capacity for C2H2 and CO2. Compared with CTF-CN-1 and CTF-NH2, they are all improved.

[0102] Fig.13 is the breakthrough curve of C2H2 / CO2 of CTF-CC-5, Fig.14 is the breakthrough curve of C2H2 / CO2 of CTF-CC-6. Figure 13-14It can be seen that at 296K and STP total pressure, the competitive adsorption test of equimolar C2H2 / CO2 mixed gas was carried out. For CTF-CC-5 and CTF-CC-6, the breakthrough time series at 296K showed that the breakthrough points of CTF-CC-5 and CTF-CC-6 for C2H2 were much higher than those for CO2. CTF-CC-5 and CTF-CC-6 showed excellent separation performance for C2H2 / CO2. The separation factors of CTF-CC-5 and CTF-CC-6 for C2H2 / CO2 were 2.49 and 2.52, respectively, and the dynamic adsorption capacities were 3.97 and 1.60 (mmol·g -1 ) and 3.84, 1.52 (mmol·g -1 ). Compared with the separation factor of 1.80 and 1.98 / 1.10 (mmol·g -1 ) separation capacity, the separation performance of CTF-CC-5 and CTF-CC-6 is better, and they can be used as excellent materials for C2H2 / CO2 separation.

[0103] In summary, the present invention utilizes amine condensation to synthesize the dicyanobenzimidazole monomer CCHBI, and then synthesizes a series of covalent triazine framework materials CTF-CCx containing benzimidazole functional groups through triazine framework polymerization reaction. Among them, CTF-CC-5 has the highest BET specific surface area (1946.77 m 2 ·g -1 ), but the adsorption-desorption curve shows a type IV hysteresis loop, indicating the presence of macropores in the structure. CTF-CC-6 has a BET specific surface area (1839.35 m 2 ·g -1 ), the pore size distribution is below 2nm, and it has a rich microporous structure. Due to the benzimidazole and triazine structures, the binding ability of CTF-CC-5 and CTF-CC-6 with C2H2 is enhanced, and the adsorption amount reaches 175.67cm 3 ·g -1 (273K, STP) and 174.28cm 3 ·g -1 (273K, STP). The C2H2 / CO2 separation factors of CTF-CC-5 and CTF-CC-6 were 2.49 and 2.52, respectively, and the dynamic adsorption capacities were 3.97 and 1.60 (mmol·g -1 ) and 3.84, 1.52 (mmol·g -1 ). Therefore, the CTF-CCx of the present invention can be used as an excellent material for physical adsorbent.

[0104] The above is only a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several modifications and improvements without departing from the inventive concept of the present invention, which all belong to the protection scope of the present invention.

Claims

1. A benzimidazole structure covalent triazine framework porous organic polymer, characterized in that: The structural formula of the porous organic polymer is:

2. The method for preparing a benzimidazole structure covalent triazine framework porous organic polymer according to claim 1, characterized in that: The following steps are involved: S1: p-cyanobenzaldehyde, 3,4-diaminobenzonitrile and sodium bisulfite were mixed in N,N-dimethylformamide, reacted at 140°C for 24 hours, and the reaction mixture was filtered to obtain a crude product 1; S2: washing the crude product 1 obtained in step S1, drying it, passing it through a chromatography column, and drying it again to obtain a pure sample of dicyanobenzimidazole monomer CCHBI; S3: The CCHBI prepared in step S2 is mixed with anhydrous zinc chloride and transferred into a tube furnace, nitrogen is passed through the tube furnace for 15 minutes, and heated to 400-600°C at a rate of 1-10°C / min under a nitrogen atmosphere, and reacted for 40 hours to obtain a crude product 2; S4: taking out the crude product 2 obtained in step S3, grinding it in a mortar, and soaking it in deionized water, filtering and washing it, and vacuum drying it to obtain a crude product 3; S5: Pour HCl solution into the crude product 3 obtained in step S4 and stir for 24 hours. After washing, use water and acetone to Soxhlet extraction for 24 hours respectively, and obtain sample CTF-CCx after drying.

3. The method for preparing a benzimidazole structure covalent triazine framework porous organic polymer according to claim 2, characterized in that: In step S1, the molar ratio of p-cyanobenzaldehyde, 3,4-diaminobenzonitrile and sodium bisulfite is 4:5:

6.

4. The method for preparing a benzimidazole structure covalent triazine framework porous organic polymer according to claim 2, characterized in that: In step S2, the crude product 1 is washed with deionized water, methanol, DMF, water and ethanol in sequence.

5. The method for preparing a benzimidazole structure covalent triazine framework porous organic polymer according to claim 2, characterized in that: In step S2, the drying temperature is 85°C and the drying time is 24 hours.

6. The method for preparing a benzimidazole structure covalent triazine framework porous organic polymer according to claim 2, characterized in that: In step S3, the molar ratio of CCHBI to anhydrous zinc chloride is 1:

8.

7. The method for preparing a benzimidazole structure covalent triazine framework porous organic polymer according to claim 2, characterized in that: In step S4, the crude product 2 is filtered and washed using water and methanol, and the number of times of the filtration and washing is no less than 5 times.

8. The method for preparing a benzimidazole structure covalent triazine framework porous organic polymer according to claim 2, characterized in that: In step S4, the vacuum drying time is 3 hours.

9. The method for preparing a benzimidazole structure covalent triazine framework porous organic polymer according to claim 2, characterized in that: In step S5, deionized water and ethanol are used for washing.

10. Use of a benzimidazole covalent triazine framework porous organic polymer according to claim 1 or a benzimidazole covalent triazine framework porous organic polymer prepared according to any one of the preparation methods of claims 2-9 in the separation of C2H2 / CO2.

Citation Information

Patent Citations

  • Covalent organic framework material as well as preparation method and application thereof

    CN113198423A

  • Nitrogen-rich porous polymer containing heteroatoms, imine and triazine ring structure and preparation method

    CN111285986A

  • Application of covalent triazine skeleton polymer in recovery of gold (I) in thiosulfate solution

    CN117448568A

  • Preparation method of triazine covalent organic polymer with high CO2 adsorption enthalpy

    CN118085209A