Polycaprolactone colloidal solution as well as preparation method and application thereof
By controlling the shear and extrusion parameters in the preparation of polycaprolactone microspheres, a nano micelle solution with moderate viscosity was prepared, which solved the problems of poor fluidity and high production cost of polycaprolactone microspheres, and achieved safe and efficient beauty filler applications.
Patent Information
- Application Number
- CN202411102199.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-19
AI Technical Summary
The existing polycaprolactone microspheres have poor high viscosity and poor fluidity and large particle size, which limit their application scope and complex process require organic solvents, resulting in high production costs and safety problems.
By shearing the molten polycaprolactone during the extrusion process, controlling the shear rate and extrusion rate, a nano micelle solution with a viscosity of 0.1Pa·s to 1Pa·s is prepared, and organic solvents and emulsifiers are avoided. Simplify the process flow.
A polycaprolactone colloidal solution with moderate viscosity and good flowability is prepared, which is suitable for whole-body filling, avoids particle accumulation and safety risks, and reduces production costs.
Smart Images

Figure CN118978713A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of polycaprolactone materials, and in particular to a polycaprolactone colloid solution and a preparation method and application thereof. Background Art
[0002] Polycaprolactone (PCL) is a linear aliphatic polyester obtained by ring-opening polymerization of ε-caprolactone (εCL). It is widely used in the field of medical beauty as a subcutaneous filler to improve wrinkles and stimulate the production of collagen. Due to its strong hydrophobicity, the conventional process for preparing polycaprolactone microspheres in the industry is to pre-dissolve polycaprolactone in an organic solvent, and then evaporate the organic solvent to prepare microspheres of about 20 to 100 μm dispersed in the gel by shearing and emulsifying into balls.
[0003] However, polycaprolactone microsphere fillers have the following problems:
[0004] 1. Due to its high viscosity, poor fluidity and large particle size, the current polycaprolactone microspheres can only be used for local filling, such as nasolabial folds, nasal base, etc., to stimulate local collagen production;
[0005] 2. Since polycaprolactone microspheres are dispersed in the gel system, there may be uneven dispersion, resulting in particle accumulation and clogging of the needle, causing subcutaneous nodules and tumors;
[0006] 3. The process is complicated and requires the use of organic phase dissolution, shear emulsification and solidification technology, which results in high production costs. Summary of the invention
[0007] The present application provides a polycaprolactone colloid solution and a preparation method and application thereof, which can produce a nanomicelle solution with a viscosity of 0.1 Pa·s to 1 Pa·s.
[0008] The embodiment of the present application is implemented as follows:
[0009] In a first aspect, the present application provides an example of a method for preparing a polycaprolactone colloidal solution, comprising: shearing columnar molten polycaprolactone while extruding it, the shear rate being 2000 rpm to 10000 rpm, and the extrusion rate of the molten polycaprolactone being 1 cm / s to 10 cm / s.
[0010] In the above technical scheme, the preparation method of the polycaprolactone colloid solution of the present application can be used to prepare a uniform nano-micelle solution with a viscosity of 0.1Pa·s to 1Pa·s. The obtained polycaprolactone colloid solution has moderate viscosity, good fluidity, and good diffusivity. It can be used as a cosmetic filler for full-position filling, and the sample is a particle-free flowing gel state, and will not cause nodules, thrombi, granulation and other phenomena after injection. At the same time, the preparation process of the polycaprolactone colloid solution does not require the introduction of organic solvents and emulsifiers and other auxiliary spheroidizing agents with certain toxicity, and the product is highly safe. In addition, the preparation method of the polycaprolactone colloid solution of the present application is simple, does not require the introduction of complex equipment, and has a low production cost.
[0011] In some possible embodiments, the temperature of the molten polycaprolactone is between 45°C and 80°C.
[0012] In the above technical solution, by making the temperature of polycaprolactone within the above range, the polycaprolactone can be kept in a molten state and thermal decomposition of the polycaprolactone can be avoided.
[0013] In some possible embodiments, before extrusion, the molten polycaprolactone is in a cylindrical shape, and the diameter of the cross section of the molten polycaprolactone is 0.2 cm to 1 cm.
[0014] In the above technical solution, by making the cross-sectional diameter of the molten polycaprolactone within the above range, it is advantageous to prepare a uniform nanomicelle solution with a viscosity of 0.1 Pa·s to 1 Pa·s.
[0015] In some possible embodiments, the shearing time is 5 min to 10 min.
[0016] In the above technical solution, by making the shear time within the above range, the particle size of polycaprolactone in the nanomicelle solution can be controlled to be 80 nm to 1 μm, and the entire preparation time can be reduced.
[0017] In some possible embodiments, the weight average molecular weight of the polycaprolactone is 20,000 g / mol to 35,000 g / mol.
[0018] In the above technical solution, by making the weight average molecular weight of polycaprolactone within the above range, it is not only beneficial to prepare a uniform nanomicelle solution, but also can keep polycaprolactone soluble in water to form a nanomicelle solution.
[0019] In some possible embodiments, the molten polycaprolactone is extruded and sheared into a container filled with water, and after the shearing is completed, the container is stirred at a rate of 100 rpm to 400 rpm.
[0020] In some possible implementation schemes, a stirring paddle is provided in the container, and the shortest distance from the stirring paddle to the inner wall of the container is 0.2 cm to 0.5 cm.
[0021] In the above technical solution, by making the shortest distance from the stirring blade to the inner wall of the container within the above range, it is possible to prevent the sheared nanomicelle solution from adhering to the inner wall of the container.
[0022] In some possible embodiments, the shear rate is 3000 rpm to 80000 rpm, and the extrusion rate of the molten polycaprolactone is 3 cm / s to 5 cm / s.
[0023] In a second aspect, the present application provides an example of a polycaprolactone colloid solution, which is prepared according to the preparation method of the polycaprolactone colloid solution in the above embodiment.
[0024] In the above technical scheme, the viscosity of the polycaprolactone colloidal solution of the present application is 0.1Pa·s~1Pa·s, and it has moderate viscosity, good fluidity, and good diffusivity. It can be used as a cosmetic filler for full-position filling, and the sample is a particle-free flowing gel state, and will not cause nodules, thrombi, granulation tissue, etc. after injection.
[0025] In a third aspect, the present application provides an example of using the above-mentioned polycaprolactone colloid solution in a tissue filler. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.
[0027] Figure 1 This is a schematic diagram of the structure of the melt extrusion device of the present application;
[0028] Figure 2 A cross-sectional view of the shearing machine of the present application;
[0029] Figure 3 This is a photograph of the polycaprolactone colloidal solution prepared in Example 1 of the present application.
[0030] Icons: 10-melt extrusion device; 100-extruder; 101-raw material inlet; 200-extrusion pipeline; 300-shearing machine; 400-container; 410-stirring paddle. DETAILED DESCRIPTION
[0031] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. In the examples, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0032] The following is a specific description of a polycaprolactone colloidal solution and its preparation method and application according to an embodiment of the present application:
[0033] The present application provides a method for preparing a polycaprolactone colloid solution, which comprises the following steps:
[0034] S1. Heating
[0035] The polycaprolactone material is heated to 45° C. to 80° C. to be molten, and the molten polycaprolactone is loaded into a device capable of simultaneously performing extrusion and shearing.
[0036] As an example, the temperature of the molten polycaprolactone may be 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, or 80°C.
[0037] In some exemplary embodiments, the weight average molecular weight of the polycaprolactone is 20,000 g / mol to 35,000 g / mol.
[0038] As an example, the weight average molecular weight of the polycaprolactone may be 20,000 g / mol, 25,000 g / mol, 30,000 g / mol or 35,000 g / mol.
[0039] By making the weight average molecular weight of polycaprolactone within the above range, it is not only beneficial to prepare a uniform nanomicelle solution, but also can keep polycaprolactone soluble in water to form a nanomicelle solution.
[0040] S2, extrude and cut
[0041] The columnar molten polycaprolactone is sheared while being extruded, and the sheared polycaprolactone enters a container filled with water, the shear rate is 2000rpm-10000rpm, the extrusion rate of the molten polycaprolactone is 1cm / s-10cm / s, and the container is stirred after the shearing is completed.
[0042] As an example, the shear rate may be 2000 rpm, 2500 rpm, 3000 rpm, 3500 rpm, 4000 rpm, 4500 rpm, 5000 rpm, 5500 rpm, 6000 rpm, 6500 rpm, 7000 rpm, 7500 rpm, 8000 rpm, 8500 rpm, 9000 rpm, 9500 rpm, or 10000 rpm.
[0043] Optionally, the shear rate is 3000 rpm to 80000 rpm.
[0044] As an example, the extrusion rate of the molten polycaprolactone may be 1 cm / s, 2 cm / s, 3 cm / s, 4 cm / s, 5 cm / s, 6 cm / s, 7 cm / s, 8 cm / s, 9 cm / s, or 10 cm / s.
[0045] Optionally, the extrusion rate of the molten polycaprolactone is 3 cm / s to 5 cm / s.
[0046] Before extrusion, the molten polycaprolactone is in a cylindrical shape, and the diameter of the cross section of the molten polycaprolactone is 0.2 cm to 1 cm.
[0047] As an example, the diameter of the cross section of molten polycaprolactone may be 0.2 cm, 0.3 cm, 0.4 cm, 0.5 cm, 0.6 cm, 0.7 cm, 0.8 cm, 0.9 cm, or 1 cm.
[0048] Optionally, the diameter of the cross section of the molten polycaprolactone is 0.2 cm to 0.5 cm.
[0049] When the diameter of the cross section of the molten polycaprolactone is within the above range, it is advantageous to prepare a uniform nanomicelle solution having a viscosity of 0.1 Pa·s to 1 Pa·s.
[0050] In some exemplary embodiments, the shearing time is 5 min to 10 min.
[0051] As an example, the shearing time may be 5 min, 6 min, 7 min, 8 min, 9 min or 10 min.
[0052] By making the shearing time within the above range, the particle size of polycaprolactone in the nanomicelle solution can be controlled to be 80 nm to 1 μm, and the entire preparation time can be reduced.
[0053] In some exemplary embodiments, the stirring rate in the container is 100 rpm to 400 rpm.
[0054] As an example, the stirring rate in the container may be 100 rpm, 150 rpm, 200 rpm, 250 rpm, 300 rpm, 350 rpm or 400 rpm.
[0055] In some exemplary embodiments, a stirring paddle is disposed in the container, and the shortest distance from the stirring paddle to the inner wall of the container is 0.2 cm to 0.5 cm.
[0056] As an example, the shortest distance from the stirring paddle to the inner wall of the container may be 0.2 cm, 0.3 cm, 0.4 cm or 0.5 cm.
[0057] By setting the shortest distance from the stirring blade to the inner wall of the container within the above range, it is possible to prevent the sheared nanomicelle solution from adhering to the inner wall of the container.
[0058] The preparation method of the polycaprolactone colloid solution of the present application can be used to prepare a uniform nano-micelle solution with a viscosity of 0.1Pa·s to 1Pa·s. The obtained polycaprolactone colloid solution has moderate viscosity, good fluidity, and good diffusivity. It can be used as a cosmetic filler for full-position filling, and the sample is in a particle-free flowing gel state, and will not cause nodules, thrombi, granulation and other phenomena after injection. At the same time, the preparation process of the polycaprolactone colloid solution does not require the introduction of auxiliary spheroidizing agents with certain toxicity such as organic solvents and emulsifiers, and the product is highly safe. In addition, the preparation method of the polycaprolactone colloid solution of the present application is simple, does not require the introduction of complex equipment, and has a low production cost.
[0059] The preparation process of the polycaprolactone colloid solution of the present application can be carried out in the following melt extrusion device:
[0060] See also Figure 1 and 2 The melt extrusion device 10 includes an extruder 100, an extrusion pipe 200, a shearing machine 300 and a container 400. The extruder 100 has two opposite ends, wherein one end of the extruder 100 has a raw material inlet 101, and the other end of the extruder 100 is connected to one end of the extrusion pipe 200. The cross section of the extrusion pipe 200 can be circular, and the diameter of the cross section is 0.2cm~1cm. The other end of the extrusion pipe 200 is connected to the shearing machine 300, and the shearing machine 300 includes a stator and a rotor. The outlet position of the extrusion pipe 200 is set between the stator and the rotor, so that the molten polycaprolactone material is directly sheared into pieces by the shearing head after extrusion. The shearing machine 300 is connected to the container 400, so that the extruded and sheared molten polycaprolactone can directly enter the container 400. A stirring paddle 410 is set in the container 400, and the shortest distance from the stirring paddle 410 to the inner wall of the container 400 is 0.2cm~0.5cm.
[0061] Optionally, the stirring paddle 410 is a double-helix stirring paddle.
[0062] The method for preparing the polycaprolactone colloid solution using the melt extrusion device 10 of the present application is as follows:
[0063] S1. Heating
[0064] The polycaprolactone material is added into the extruder 100 from the raw material inlet 101, and the polycaprolactone material is heated to 45° C. to 80° C. to melt.
[0065] S2, extrude and cut
[0066] The molten polycaprolactone material is extruded from the extrusion pipe 200 at an extrusion rate of 1 cm / s to 10 cm / s. The molten polycaprolactone is extruded to the shearing machine 300 and shredded at a shearing rate of 2000 rpm to 10000 rpm. The shredded polycaprolactone enters a container filled with water, and the container is started to stir.
[0067] The present application also provides a polycaprolactone colloid solution, which is prepared according to the preparation method of the polycaprolactone colloid solution in the above embodiment.
[0068] The viscosity of the polycaprolactone colloid solution of the present application is 0.1Pa·s~1Pa·s. It has moderate viscosity, good fluidity and good diffusivity. It can be used as a cosmetic filler for full-position filling. The sample is in a particle-free flowing gel state and will not cause nodules, thrombi, granulation and the like after injection.
[0069] The present application also provides a use of the polycaprolactone colloid solution in tissue fillers.
[0070] The tissue filler may be a skin tissue repair injection, a filler for beauty, or a filler for treatment.
[0071] The polycaprolactone colloid solution and the preparation method thereof of the present application are further described in detail below in conjunction with the examples.
[0072] Example 1
[0073] The present invention provides a polycaprolactone colloid solution and a preparation method thereof, which comprises the following steps:
[0074] S1. Heating
[0075] Polycaprolactone with a molecular weight of 30,000 g / mol was selected as a raw material, and a polycaprolactone colloidal solution was prepared using the melt extrusion device 10 of the present application. The polycaprolactone material was added into the extruder 100 from the raw material inlet 101, and the polycaprolactone material was heated to 55° C. to melt.
[0076] S2, extrude and cut
[0077] The molten polycaprolactone material is extruded from the extrusion pipe 200 at an extrusion rate of 3 cm / s. The cross section of the extrusion pipe 200 is circular, and the diameter of the cross section is 0.5 cm. The molten polycaprolactone is extruded to the shearing machine 300 and shredded at a shear rate of 3000 rpm for 8 min. The shredded polycaprolactone enters a container filled with water. The container is stirred at a stirring rate of 250 rpm. The shortest distance from the double-helix stirring paddle in the container to the inner wall of the container is 0.5 cm.
[0078] The photo of the obtained polycaprolactone colloidal solution is shown in Figure 3 shown.
[0079] Example 2
[0080] The present invention provides a polycaprolactone colloid solution and a preparation method thereof, which comprises the following steps:
[0081] S1. Heating
[0082] Polycaprolactone with a molecular weight of 30,000 g / mol was selected as a raw material, and a polycaprolactone colloidal solution was prepared using the melt extrusion device 10 of the present application. The polycaprolactone material was added into the extruder 100 from the raw material inlet 101, and the polycaprolactone material was heated to 55° C. to melt.
[0083] S2, extrude and cut
[0084] The molten polycaprolactone material is extruded from the extrusion pipe 200 at an extrusion rate of 5 cm / s. The cross section of the extrusion pipe 200 is circular, and the diameter of the cross section is 0.5 cm. The molten polycaprolactone is extruded to the shearing machine 300 for shearing at a shear rate of 8000 rpm for a shearing time of 8 min. The sheared polycaprolactone enters a container filled with water. The container is stirred at a stirring rate of 250 rpm. The shortest distance from the double-screw stirring paddle in the container to the inner wall of the container is 0.5 cm.
[0085] Example 3
[0086] The present invention provides a polycaprolactone colloid solution and a preparation method thereof, which comprises the following steps:
[0087] S1. Heating
[0088] Polycaprolactone with a molecular weight of 30,000 g / mol was selected as a raw material, and a polycaprolactone colloidal solution was prepared using the melt extrusion device 10 of the present application. The polycaprolactone material was added into the extruder 100 from the raw material inlet 101, and the polycaprolactone material was heated to 55° C. to melt.
[0089] S2, extrude and cut
[0090] The molten polycaprolactone material is extruded from the extrusion pipe 200 at an extrusion rate of 10 cm / s. The cross section of the extrusion pipe 200 is circular, and the diameter of the cross section is 0.5 cm. The molten polycaprolactone is extruded to the shearing machine 300 for shearing at a shear rate of 10000 rpm for a shearing time of 10 min. The sheared polycaprolactone enters a container filled with water. The container is stirred at a stirring rate of 250 rpm. The shortest distance from the double-screw stirring paddle in the container to the inner wall of the container is 0.5 cm.
[0091] Example 4
[0092] The present invention provides a polycaprolactone colloid solution and a preparation method thereof, which comprises the following steps:
[0093] S1. Heating
[0094] Polycaprolactone with a molecular weight of 30,000 g / mol was selected as a raw material, and a polycaprolactone colloidal solution was prepared using the melt extrusion device 10 of the present application. The polycaprolactone material was added into the extruder 100 from the raw material inlet 101, and the polycaprolactone material was heated to 55° C. to melt.
[0095] S2, extrude and cut
[0096] The molten polycaprolactone material is extruded from the extrusion pipe 200 at an extrusion rate of 1 cm / s. The cross section of the extrusion pipe 200 is circular and the diameter of the cross section is 0.5 cm. The molten polycaprolactone is extruded to the shearing machine 300 and shredded at a shear rate of 2000 rpm for a shearing time of 10 min. The shredded polycaprolactone enters a container filled with water. The container is stirred at a stirring rate of 250 rpm. The shortest distance from the double-helix stirring paddle in the container to the inner wall of the container is 0.5 cm.
[0097] Example 5
[0098] The present invention provides a polycaprolactone colloid solution and a preparation method thereof, which comprises the following steps:
[0099] S1. Heating
[0100] Polycaprolactone with a molecular weight of 30,000 g / mol was selected as a raw material, and a polycaprolactone colloidal solution was prepared using the melt extrusion device 10 of the present application. The polycaprolactone material was added into the extruder 100 from the raw material inlet 101, and the polycaprolactone material was heated to 55° C. to melt.
[0101] S2, extrude and cut
[0102] The molten polycaprolactone material is extruded from the extrusion pipe 200 at an extrusion rate of 3 cm / s. The cross section of the extrusion pipe 200 is circular, and the diameter of the cross section is 0.5 cm. The molten polycaprolactone is extruded to the shearing machine 300 for shearing at a shear rate of 3000 rpm for a shearing time of 5 min. The sheared polycaprolactone enters a container filled with water. The container is stirred at a stirring rate of 250 rpm. The shortest distance from the double-helix stirring paddle in the container to the inner wall of the container is 0.5 cm.
[0103] Example 6
[0104] The present invention provides a polycaprolactone colloid solution and a preparation method thereof, which comprises the following steps:
[0105] S1. Heating
[0106] Polycaprolactone with a molecular weight of 20,000 g / mol was selected as a raw material, and a polycaprolactone colloidal solution was prepared using the melt extrusion device 10 of the present application. The polycaprolactone material was added into the extruder 100 from the raw material inlet 101, and the polycaprolactone material was heated to 55° C. to melt.
[0107] S2, extrude and cut
[0108] The molten polycaprolactone material is extruded from the extrusion pipe 200 at an extrusion rate of 3 cm / s. The cross section of the extrusion pipe 200 is circular, and the diameter of the cross section is 0.5 cm. The molten polycaprolactone is extruded to the shearing machine 300 and shredded at a shear rate of 3000 rpm for 8 min. The shredded polycaprolactone enters a container filled with water. The container is stirred at a stirring rate of 250 rpm. The shortest distance from the double-helix stirring paddle in the container to the inner wall of the container is 0.5 cm.
[0109] Comparative Example 1
[0110] The comparative example of the present application provides a polycaprolactone colloid solution and a preparation method thereof, which comprises the following steps:
[0111] S1. Heating
[0112] Polycaprolactone with a molecular weight of 30,000 g / mol was selected as a raw material, and a polycaprolactone colloidal solution was prepared using the melt extrusion device 10 of the present application. The polycaprolactone material was added into the extruder 100 from the raw material inlet 101, and the polycaprolactone material was heated to 55° C. to melt.
[0113] S2, extrude and cut
[0114] The molten polycaprolactone material is extruded from the extrusion pipe 200 at an extrusion rate of 3 cm / s. The cross section of the extrusion pipe 200 is circular, and the diameter of the cross section is 0.5 cm. The molten polycaprolactone is extruded to the shearing machine 300 for shearing at a shear rate of 1000 rpm for a shearing time of 8 min. The sheared polycaprolactone enters a container filled with water. The container is stirred at a stirring rate of 250 rpm. The shortest distance from the double-helix stirring paddle in the container to the inner wall of the container is 0.5 cm.
[0115] Comparative Example 2
[0116] The comparative example of the present application provides a polycaprolactone colloid solution and a preparation method thereof, which comprises the following steps:
[0117] S1. Heating
[0118] Polycaprolactone with a molecular weight of 30,000 g / mol was selected as a raw material, and a polycaprolactone colloidal solution was prepared using the melt extrusion device 10 of the present application. The polycaprolactone material was added into the extruder 100 from the raw material inlet 101, and the polycaprolactone material was heated to 55° C. to melt.
[0119] S2, extrude and cut
[0120] The molten polycaprolactone material is extruded from the extrusion pipe 200 at an extrusion rate of 3 cm / s. The cross section of the extrusion pipe 200 is circular, and the diameter of the cross section is 0.5 cm. The molten polycaprolactone is extruded to the shearing machine 300 for shearing at a shear rate of 12000 rpm for a shearing time of 8 min. The sheared polycaprolactone enters a container filled with water. The container is stirred at a stirring rate of 250 rpm. The shortest distance from the double-helix stirring paddle in the container to the inner wall of the container is 0.5 cm.
[0121] Comparative Example 3
[0122] The comparative example of the present application provides a polycaprolactone colloid solution and a preparation method thereof, which comprises the following steps:
[0123] S1. Heating
[0124] Polycaprolactone with a molecular weight of 30,000 g / mol was selected as a raw material, and a polycaprolactone colloidal solution was prepared using the melt extrusion device 10 of the present application. The polycaprolactone material was added into the extruder 100 from the raw material inlet 101, and the polycaprolactone material was heated to 55° C. to melt.
[0125] S2, extrude and cut
[0126] The molten polycaprolactone material is extruded from the extrusion pipe 200 at an extrusion rate of 0.5 cm / s. The cross section of the extrusion pipe 200 is circular, and the diameter of the cross section is 0.5 cm. The molten polycaprolactone is extruded to the shearing machine 300 and shredded at a shear rate of 3000 rpm for 8 min. The shredded polycaprolactone enters a container filled with water. The container is stirred at a stirring rate of 250 rpm. The shortest distance from the double-screw stirring paddle in the container to the inner wall of the container is 0.5 cm.
[0127] Comparative Example 4
[0128] The comparative example of the present application provides a polycaprolactone colloid solution and a preparation method thereof, which comprises the following steps:
[0129] S1. Heating
[0130] Polycaprolactone with a molecular weight of 30,000 g / mol was selected as a raw material, and a polycaprolactone colloidal solution was prepared using the melt extrusion device 10 of the present application. The polycaprolactone material was added into the extruder 100 from the raw material inlet 101, and the polycaprolactone material was heated to 55° C. to melt.
[0131] S2, extrude and cut
[0132] The molten polycaprolactone material is extruded from the extrusion pipe 200 at an extrusion rate of 12 cm / s. The cross section of the extrusion pipe 200 is circular, and the diameter of the cross section is 0.5 cm. The molten polycaprolactone is extruded to the shearing machine 300 for shearing at a shear rate of 3000 rpm for a shearing time of 8 min. The sheared polycaprolactone enters a container filled with water. The container is stirred at a stirring rate of 250 rpm. The shortest distance from the double-helix stirring paddle in the container to the inner wall of the container is 0.5 cm.
[0133] Comparative Example 5
[0134] The comparative example of the present application provides a polycaprolactone colloid solution and a preparation method thereof, which comprises the following steps:
[0135] S1. Heating
[0136] Polycaprolactone with a molecular weight of 45000 g / mol was selected as a raw material, and a polycaprolactone colloidal solution was prepared by using the melt extrusion device 10 of the present application. The polycaprolactone material was added into the extruder 100 from the raw material inlet 101, and the polycaprolactone material was heated to 55° C. to melt.
[0137] S2, extrude and cut
[0138] The molten polycaprolactone material is extruded from the extrusion pipe 200 at an extrusion rate of 3 cm / s. The cross section of the extrusion pipe 200 is circular, and the diameter of the cross section is 0.5 cm. The molten polycaprolactone is extruded to the shearing machine 300 and shredded at a shear rate of 3000 rpm for 8 min. The shredded polycaprolactone enters a container filled with water. The container is stirred at a stirring rate of 250 rpm. The shortest distance from the double-helix stirring paddle in the container to the inner wall of the container is 0.5 cm.
[0139] Test Example 1
[0140] The polycaprolactone colloid solutions prepared in Examples 1 to 6 and Comparative Examples 1 to 5 were taken to measure the particle size and viscosity of the polycaprolactone, respectively. The results are shown in Table 1. The test method is as follows:
[0141] Particle size: Take this product, dilute it 200 times with purified water, and determine it according to the particle size and particle size distribution determination method of the 2020 edition of the Pharmacopoeia of the People's Republic of China (Volume 4) (0982 Method 3).
[0142] Viscosity (single-point viscosity): Direct sampling, at (25±0.2)°C, using a rheometer to perform a creep scan at a shear rate of 100 (1 / S).
[0143] Table 1 Parameters of polycaprolactone colloid solutions obtained in Examples 1 to 6 and Comparative Examples 1 to 5
[0144] project Particle size of polycaprolactone (nm) Viscosity (Pa·s) Appearance: Whether a colloidal solution is formed Example 1 542 0.52 yes Example 2 498 0.48 yes Example 3 821 0.21 yes Example 4 157 0.18 yes Example 5 379 0.45 yes Example 6 123 0.12 yes Comparative Example 1 / / no Comparative Example 2 65 0.045 yes Comparative Example 3 85 0.086 yes Comparative Example 4 / / no Comparative Example 5 / / no
[0145] It can be seen from Examples 1 to 6 that the method for preparing the polycaprolactone colloid solution of the present application can prepare a polycaprolactone colloid solution with a viscosity of 0.1 Pa·s to 1 Pa·s and a particle size of 80 nm to 1 μm.
[0146] From the comparison between Comparative Example 1 and Example 1, it can be seen that when the shear rate is too low, the polycaprolactone colloidal solution cannot be formed.
[0147] From the comparison between Comparative Examples 2 to 3 and Example 1, it can be seen that when the shear rate is too high or the extrusion rate is too low, the viscosity of the obtained polycaprolactone colloid solution is relatively low.
[0148] From the comparison between Comparative Example 4 and Example 1, it can be seen that when the extrusion rate is too high, the polycaprolactone colloidal solution cannot be formed.
[0149] From the comparison between Comparative Example 5 and Example 1, it can be seen that when the weight average molecular weight of polycaprolactone>
[0150] When the concentration of polycaprolactone is 35000 g / mol, no polycaprolactone colloidal solution can be formed.
[0151] The above description is only a specific embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.
Claims
1. A method for preparing a polycaprolactone colloid solution, characterized in that: The preparation method of the polycaprolactone colloid solution comprises: shearing columnar molten polycaprolactone while extruding it, the shear rate is 2000rpm-10000rpm, and the extrusion rate of the molten polycaprolactone is 1cm / s-10cm / s.
2. The method for preparing the polycaprolactone colloid solution according to claim 1, characterized in that: The temperature of the molten polycaprolactone is 45°C to 80°C.
3. The method for preparing the polycaprolactone colloid solution according to claim 1, characterized in that: Before extrusion, the molten polycaprolactone is cylindrical, and the diameter of the cross section of the molten polycaprolactone is 0.2 cm to 1 cm.
4. The method for preparing the polycaprolactone colloid solution according to claim 1, characterized in that: The shearing time is 5min to 10min.
5. The method for preparing the polycaprolactone colloid solution according to claim 1, characterized in that: The weight average molecular weight of the polycaprolactone is 20000 g / mol to 35000 g / mol.
6. The method for preparing the polycaprolactone colloid solution according to claim 1, characterized in that: The molten polycaprolactone is extruded and sheared into a container filled with water. After the shearing is completed, the container is stirred at a stirring rate of 100 rpm to 400 rpm.
7. The method for preparing the polycaprolactone colloid solution according to claim 6, characterized in that: The container is provided with a stirring paddle, and the shortest distance from the stirring paddle to the inner wall of the container is 0.2 cm to 0.5 cm.
8. The method for preparing a polycaprolactone colloid solution according to any one of claims 1 to 7, characterized in that: The shear rate is 3000 rpm to 80000 rpm, and the extrusion rate of the molten polycaprolactone is 3 cm / s to 5 cm / s.
9. A polycaprolactone colloid solution, characterized in that: The polycaprolactone colloid solution is prepared according to the preparation method of the polycaprolactone colloid solution according to any one of claims 1 to 8.
10. Use of the polycaprolactone colloidal solution according to claim 9 in tissue fillers.