Total-hot-melt tread rubber polymer with ultrahigh grip under low-temperature condition
By using styrene butadiene rubber and other fillers of different glass transition temperatures in hot melt tread rubber polymer, the problem of insufficient grip performance under low temperature conditions is solved, and high grip performance in low temperature environments is achieved, ensuring The safety and performance of the game.
Patent Information
- Application Number
- CN202411276771.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-11-19
AI Technical Summary
The grip performance of existing hot tires under low temperature conditions cannot meet the competition needs, resulting in slow tire warming and insufficient grip, affecting drivers' safety and racing performance.
Using a fully heat-melting tread rubber polymer with ultra-high grip at low temperatures, combining carbon black, sunflower oil and functional resins by using two different glass transition temperatures of styrene butadiene rubber (SBR1 and SBR2) To improve the formula, optimize the formula to reduce the glass transition temperature of the tread and improve the low-temperature grip performance.
Provide ultra-high grip performance under low temperature conditions, ensure smooth competition in areas with low temperatures, reduce tire warming time, and improve drivers' safety and racing performance.
Smart Images

Figure BDA0005040424070000081 
Figure BDA0005040424070000091 
Figure BDA0005040424070000111
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of tire rubber formulations, and in particular to a full hot-melt tread rubber polymer with ultra-high grip under low temperature conditions. Background Art
[0002] For ease of understanding, the professional terms involved in the present invention are as follows:
[0003] Graining: One of the common faults of racing tires. The main reason for this is that the tires have not been fully warmed up, or the tires have not reached their optimal operating temperature due to vehicle tuning or unreasonable parameter settings. The driver then makes intense operation. Since the tire tread has not yet melted, the tread rubber contacts the bumps on the track surface, which acts like a scraper, causing abnormal wear on the tread rubber. Figure 1 , refer to the photo of tire wear with graining phenomenon Figure 2 .
[0004] Racing sports have a long history of more than 100 years. According to the competition venue, they are mainly divided into track racing and non-track racing. Track racing is completed in a closed track, such as F1 Formula One competition. Non-track racing is a race on a route designated on normal roads, cities, villages, and the wild. Compared with track racing, the risk factor is higher and the uncertainty during the competition is greater. Track racing currently includes drift racing, formula racing, GT endurance racing, and drag racing. Although the types of competitions are different, the models used, horsepower, and torque are different, they all have high requirements for tire performance, especially for tire grip performance.
[0005] At present, for track racing, due to the extremely high requirements for vehicle speed, the requirements for tire grip are more stringent. In order to meet the high grip requirements of racing tires, full hot melt tires came into being. Because there are two main types of rubber grip mechanisms, one is the pitting effect, which mainly utilizes the viscoelastic hysteresis effect of rubber. The greater the hysteresis loss Tanδ of the rubber, the greater the friction generated between the rubber and the ground protrusion after the force is applied. The commonly used civilian tread grip mechanism is mainly the pitting effect. The other is the adhesion effect, which mainly utilizes the molecular-level van der Waals force generated between the adhesion characteristics of rubber molecules and the road surface. The tread grip mechanism of the event is the combined effect of the pitting effect and the adhesion effect, and the adhesion effect plays a dominant role. The full hot melt tire is designed to generate heat through friction with the ground, and the tire surface forms a gel, and the tread becomes soft, increasing the contact area with the ground, greatly improving the grip of the car, and improving the cornering limit and handling performance of the car. Because the characteristics of racing tires must reach a certain working temperature (generally 60-120℃) to play out, most of the current races are held in areas with higher temperatures. In addition to commercial value considerations, weather is one of the important factors that need to be considered. The temperature conditions of each race are as good as possible, with an average temperature of more than 20℃, but there will still be extreme weather conditions. The requirements for tires during the race are more stringent, and the tires need to be able to reach the required working temperature in a very short time. At present, the common racing tires on the market will be melted after being warmed up in a high temperature environment, which can quickly increase the grip of the tires with the ground. However, in a low temperature environment, the tires cannot be fully warmed up in a short time and reach a melted state. At this time, the driver's aggressive driving is likely to cause the tire graining phenomenon, the tire's contact area with the ground is reduced, and the tire's grip performance with the ground becomes worse, which will greatly affect the driver's lap time, and in severe cases, it will even cause huge safety hazards to the driver's life safety.
[0006] In order to solve the above problems, the present invention provides a full hot-melt tread rubber polymer with ultra-high grip under low temperature conditions. Summary of the invention
[0007] The purpose of the present invention is to provide a full hot melt tread rubber polymer with ultra-high grip under low temperature conditions to solve the problems raised in the background technology:
[0008] The grip performance of existing hot melt tires cannot meet the competition requirements in low temperature areas.
[0009] In order to achieve the above object, the present invention adopts the following technical solutions:
[0010] A full hot-melt tread rubber polymer with ultra-high grip under low temperature conditions, wherein the tread rubber polymer is prepared by mixing raw materials including the following components based on 100 parts by weight of the rubber component: 100 parts of the rubber component, 80-160 parts of the filler component, 50-100 parts of the plasticizer, 10-60 parts of the functional resin, 3-6 parts of the antioxidant, 2-6 parts of the activator, 1-5 parts of the vulcanizer and 1-6 parts of the accelerator;
[0011] The rubber component is styrene-butadiene rubber, i.e., SBR. The SBR includes 0-40 parts of SBR1 and 60-100 parts of SBR2. Both SBR1 and SBR2 are prepared by mixing styrene and vinyl in different proportions. The styrene content of SBR1 accounts for more than 30% of the total content of SBR1, the vinyl content is lower than 35% of the total content of SBR1, and the glass transition temperature is lower than -20°C; the styrene content of SBR2 accounts for more than 30% of the total content of SBR2, the vinyl content accounts for more than 35% of the total content of SBR2, and the glass transition temperature is higher than -20°C.
[0012] Preferably, both SBR1 and SBR2 of the styrene-butadiene rubber are filled with 0-50 parts of TDAE as a plasticizer.
[0013] Preferably, the filler component is carbon black, and the amount used is 80-160 parts, more preferably 100 parts; the specific surface area of the carbon black is 100-200m 2 / g, more preferably 120-180m 2 / g, and the particle size is 0.1-1 μm, more preferably 0.2-0.8 μm.
[0014] Preferably, the plasticizer is sunflower oil, and the amount used is 5-100 parts, more preferably 80 parts.
[0015] Preferably, the functional resin includes one or more of C5 petroleum resin, C9 petroleum resin, α-methylstyrene resin, indene resin, phenolic resin, and terpene resin, and the amount used is 10-60 parts, more preferably 20 parts.
[0016] Preferably, the antioxidant includes a physical antioxidant and a chemical antioxidant, wherein the physical antioxidant includes one or more of paraffin wax and microcrystalline wax, and the chemical antioxidant includes one or more of RD, 4010, 4010NA, 4020, and DTPD.
[0017] Preferably, the active agents include zinc oxide and stearic acid.
[0018] Preferably, the vulcanizing agent includes one or more of common sulfur, insoluble sulfur, sulfur-containing compounds, and peroxides.
[0019] Preferably, the accelerator is one or more of N-cyclohexyl-2-benzothiazole sulfenamide, amide N-tert-butyl-2-benzothiazole sulfenamide, 2-(4-morpholinethio)benzothiazole, N,N-dicyclohexyl-2-benzothiazole sulfenamide, tetrabenzylthiuram disulfide, tetramethylthiuram disulfide, diphenylguanidine, o-tolylbiguanide, and di-o-tolylguanidine.
[0020] A mixing method for a full hot-melt tread rubber polymer with ultra-high grip under low temperature conditions comprises the following steps:
[0021] Put all raw materials into the internal mixer at one time according to the components, control the rotor speed of the internal mixer to 40-50rpm, the upper bolt pressure to 0.6Mpa, the cooling water temperature of the internal mixer to 25±3℃, and carry out a master batching, which specifically includes the following process steps:
[0022] Add all the raw materials, press the top bolt, and keep it for 60 seconds, or heat the raw materials to 110℃;
[0023] Raise the top bolt, add plasticizer, press the top bolt and hold for 30 seconds;
[0024] Raise the top bolt and hold for 10 seconds;
[0025] Press the top bolt and hold for 30 seconds;
[0026] Raise the top bolt and hold for 10 seconds;
[0027] Press the top bolt and keep it for 90 seconds to perform the debinding operation, or heat the material to 150℃ to perform the debinding operation;
[0028] The rotor speed of the internal mixer is controlled to be 40-50rpm, the upper bolt pressure is 0.6Mpa, the cooling water temperature of the internal mixer is 25±3℃, and the second-stage masterbatch is carried out. The specific process steps include the following:
[0029] Add all the masterbatch from the first stage of masterbatch
[0030] Press the top bolt and hold for 30 seconds;
[0031] Raise the top bolt and hold for 10 seconds;
[0032] Press the top bolt and keep it for 90 seconds to perform the debinding operation, or heat the material to 150℃ to perform the debinding operation;
[0033] The rotor speed of the internal mixer is controlled to be 20-30rpm, the upper bolt pressure is 0.6Mpa, and the cooling water temperature of the internal mixer is 25±3℃. The final mixing is carried out, which specifically includes the following process steps:
[0034] Press the top bolt and hold for 30 seconds;
[0035] Raise the top bolt and hold for 10 seconds;
[0036] Press the top bolt and hold it for 90 seconds to perform the debinding operation, or heat the material to 100℃ to perform the debinding operation.
[0037] Compared with the prior art, the present invention provides a full hot-melt tread rubber polymer with ultra-high grip under low temperature conditions, which has the following beneficial effects:
[0038] The present invention uses two SBRs with different Tg and optimizes the number of combined parts, thereby reducing the Tg of the competition tread as much as possible while ensuring grip, and improving the grip performance of the competition tread at low temperatures. Sunflower oil with a glass transition temperature lower than that of conventional operating oil is used as a softener to improve the low-temperature performance of the formula and the hysteresis loss under low-temperature environments; at the same time, fillers and functional resins are added in appropriate proportions to ensure the grip performance of the rubber while improving the low-temperature performance of the rubber. The rubber polymer prepared in this way can still provide ultra-high grip performance under low-temperature conditions, which is conducive to the smooth progress of competitions in areas with lower temperatures and to cope with the problems of slow tire warm-up and insufficient grip caused by sudden temperature drops during competitions, and also protects the personal safety of drivers. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 The normal racing tire wear diagram mentioned in the background technology of the present invention;
[0040] Figure 2 This is the tire wear diagram of the graining phenomenon mentioned in the background technology of the present invention. DETAILED DESCRIPTION
[0041] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0042] The present invention uses two SBRs with different Tg and optimizes the number of combined parts, while ensuring grip, reducing the Tg of the competition tread as much as possible, and improving the grip performance of the competition tread at low temperatures. Sunflower oil with a glass transition temperature lower than that of conventional operating oil is used as a softener to improve the low-temperature performance of the formula and the hysteresis loss in a low-temperature environment; at the same time, fillers and functional resins in appropriate proportions are added to ensure the grip performance of the rubber while improving the low-temperature performance of the rubber. The rubber polymer prepared in this way can still provide ultra-high grip performance under low-temperature conditions, which is conducive to the smooth progress of competitions in areas with lower temperatures and to cope with the problems of slow tire warm-up and insufficient grip caused by sudden temperature drops during competitions, and also protects the personal safety of the driver. Specifically include the following contents.
[0043] SBR-1: SL5563 (JSR), styrene content: 41%, vinyl content: 57%, Tg: -11°C, filled with 37.5 parts of TDAE;
[0044] SBR-2: SBR1739 (Dow), styrene content: 40%, vinyl content: 18%, Tg: -36°C, filled with 37.5 parts of TDAE;
[0045] Carbon black: N115 (Jiangxi Black Cat), specific surface area 130m 2 / g;
[0046] Functional resin: one or more of C5 petroleum resin, C9 petroleum resin, α-methylstyrene resin, indene resin, phenolic resin, and terpene resin;
[0047] Sunflower oil: COREYSA-SPAIN, Tg<-90℃;
[0048] TDAE: Viavatec (Han Sheng Company, Germany);
[0049] Others: antioxidants, active agents, vulcanizing agents, accelerators, etc.; antioxidants include physical antioxidants and chemical antioxidants, wherein physical antioxidants include one or more of paraffin wax and microcrystalline wax, and chemical antioxidants include one or more of RD, 4010, 4010NA, 4020, and DTPD; active agents include zinc oxide and stearic acid; vulcanizing agents include one or more of common sulfur, insoluble sulfur, sulfur-containing compounds, and peroxides. The vulcanizing agent is one or more of sulfur or insoluble sulfur; the accelerator is one or more of N-cyclohexyl-2-benzothiazole sulfenamide, amide N-tert-butyl-2-benzothiazole sulfenamide, 2-(4-morpholinethio)benzothiazole, N,N-dicyclohexyl-2-benzothiazole sulfenamide, tetrabenzylthiuram disulfide, tetramethylthiuram disulfide, diphenylguanidine, o-tolylbiguanidine, and di-o-tolylguanidine.
[0050] Reference group:
[0051] The raw material composition is as follows: 100 parts of rubber component, 100 parts of carbon black, 35 parts of TDAE as a plasticizer, 10 parts of functional resin, 5 parts of antioxidant, 5 parts of activator, 2.5 parts of vulcanizer and 3 parts of accelerator; wherein the rubber component is styrene-butadiene rubber, and the styrene-butadiene rubber includes 100 parts of SBR-1.
[0052] Example Group 1:
[0053] Raw material composition: 100 parts of rubber component, 100 parts of carbon black, 35 parts of TDAE as plasticizer, 10 parts of functional resin, 5 parts of antioxidant, 5 parts of activator, 2.5 parts of vulcanizer, 3 parts of accelerator; wherein, the rubber component is styrene-butadiene rubber, styrene-butadiene rubber includes SBR-1 and SBR-2, and the combination results refer to Table 1:
[0054] Table 1 Additive components of SBR-1 and SBR-2 in different schemes
[0055] Components Solution 1-1 Solution 1-2 Scheme 1-3 Scheme 1-4 Scheme 1-5 SBR-1 80 60 40 20 0 SBR-2 20 40 60 80 100
[0056] Example Group 2:
[0057] Raw material composition: 100 parts of rubber component, 80-160 parts of carbon black, 35 parts of TDAE as plasticizer, 10 parts of functional resin, 5 parts of antioxidant, 5 parts of activator, 2.5 parts of vulcanizer, 3 parts of accelerator; wherein, the rubber component is styrene-butadiene rubber, and styrene-butadiene rubber includes 100 parts of SBR-1. The addition results of carbon black refer to Table 2:
[0058] Table 2 Added components of carbon black in different schemes
[0059] Components Solution 2-1 Solution 2-2 Scheme 2-3 Scheme 2-4 Scheme 2-5 Carbon Black 80 100 120 140 160
[0060] Example Group 3:
[0061] Raw material composition: 100 parts of rubber component, 100 parts of carbon black, 0-100 parts of sunflower oil as plasticizer, 10 parts of functional resin, 5 parts of antioxidant, 5 parts of activator, 2.5 parts of vulcanizer, 3 parts of accelerator; wherein, the rubber component is styrene-butadiene rubber, styrene-butadiene rubber includes 100 parts of SBR-1, and the number of sunflower oil used is shown in Table 3:
[0062] Table 3 Added components of sunflower oil in different schemes
[0063]
[0064]
[0065] Example Group 4:
[0066] Raw material composition: 100 parts of rubber component, 100 parts of carbon black, 35 parts of TDAE as plasticizer, 10-60 parts of functional resin, 5 parts of antioxidant, 5 parts of activator, 2.5 parts of vulcanizer, 3 parts of accelerator; wherein, the rubber component is styrene-butadiene rubber, styrene-butadiene rubber includes 100 parts of SBR-1, wherein the number of functional resins used is referred to Table 4:
[0067] Table 4 Added components of functional resin in different schemes
[0068] Components Solution 4-1 Solution 4-2 Solution 4-3 Scheme 4-4 Scheme 4-5 Scheme 4-6 Functional resin 10 20 30 40 50 60
[0069] Example Group 5:
[0070] The raw material composition is as follows: 100 parts of rubber component, 100 parts of carbon black, 80 parts of sunflower oil as a plasticizer, 20 parts of functional resin, 5 parts of antioxidant, 5 parts of activator, 2.5 parts of vulcanizer and 3 parts of accelerator; wherein the rubber component is styrene-butadiene rubber, and styrene-butadiene rubber includes 20 parts of SBR-1 and 80 parts of SBR-2.
[0071] The reference group and sample groups 1-5 were processed according to the same masterbatch and final batching process:
[0072] Put all raw materials into the internal mixer at one time according to the components, control the rotor speed of the internal mixer to 40-50rpm, the upper bolt pressure to 0.6Mpa, the cooling water temperature of the internal mixer to 25±3℃, and carry out a master batching, which specifically includes the following process steps:
[0073] Add all the raw materials, press the top bolt, and keep it for 60 seconds, or heat the raw materials to 110℃;
[0074] Raise the top bolt, add plasticizer, press the top bolt and hold for 30 seconds;
[0075] Raise the top bolt and hold for 10 seconds;
[0076] Press the top bolt and hold for 30 seconds;
[0077] Raise the top bolt and hold for 10 seconds;
[0078] Press the top bolt and keep it for 90 seconds to perform the debinding operation, or heat the material to 150℃ to perform the debinding operation;
[0079] The rotor speed of the internal mixer is controlled to be 40-50rpm, the upper bolt pressure is 0.6Mpa, the cooling water temperature of the internal mixer is 25±3℃, and the second-stage masterbatch is carried out. The specific process steps include the following:
[0080] Add all the masterbatch from the first stage of masterbatch
[0081] Press the top bolt and hold for 30 seconds;
[0082] Raise the top bolt and hold for 10 seconds;
[0083] Press the top bolt and keep it for 90 seconds to perform the debinding operation, or heat the material to 150℃ to perform the debinding operation;
[0084] The rotor speed of the internal mixer is controlled to be 20-30rpm, the upper bolt pressure is 0.6Mpa, and the cooling water temperature of the internal mixer is 25±3℃. The final mixing is carried out, which specifically includes the following process steps:
[0085] Press the top bolt and hold for 30 seconds;
[0086] Raise the top bolt and hold for 10 seconds;
[0087] Press the top bolt and hold it for 90 seconds to perform the debinding operation, or heat the material to 100℃ to perform the debinding operation.
[0088] The final mixed rubber was vulcanized at 160°C for 10 minutes using a flat vulcanizer to obtain a vulcanized rubber, and the performance of the vulcanized rubber was tested according to the following test methods:
[0089] 1. Shore hardness: GB / T531.1-2008
[0090] 2. Tensile stress strain: GB / T528-2009
[0091] DMA temperature scan: test temperature -30℃~70℃, dynamic 0.3%, static 3%
[0092] Based on the above test standards, the reference group and sample groups 1-5 were tested. The test results can be found in Table 5-9:
[0093] Table 5 Test results of properties of vulcanized rubber prepared by reference group and example group 1
[0094]
[0095] Table 6 Test results of properties of vulcanized rubber prepared by reference group and example group 2
[0096]
[0097] Table 7 Test results of properties of vulcanized rubber prepared by reference group and example group 3
[0098]
[0099] Table 8 Test results of properties of vulcanized rubber prepared by reference group and example group 4
[0100]
[0101]
[0102] Table 9 Test results of properties of vulcanized rubber prepared by reference group and example group 5
[0103] plan Reference group Example Group 5 Shore Hardness 63 43 Breaking strength Ts 14.5 10.5 Elongation at break Eb 550 670 -25℃E’ 2800 450 25℃Tanδ 0.320 0.365 60℃Tanδ 0.245 0.270 Peak Tg -5.5 -22.5
[0104] The specific meanings of the performance items in Table 5-9 are as follows:
[0105] Shore hardness: The value obtained by measuring the standard sample using a Shore hardness tester, which represents the ability of rubber to resist external stress deformation. The smaller the value, the larger the contact area between the rubber and the ground under the same stress.
[0106] Breaking strength Ts: The strength of the standard tensile specimen when it breaks, together with the breaking elongation, characterizes the rubber's ability to resist damage. The larger the product of Ts*Eb, the better the physical properties of the rubber compound.
[0107] Elongation at break Eb: The elongation at which the standard tensile specimen breaks after being stretched. Together with the tear strength, it characterizes the rubber's ability to resist damage. The larger the product of Ts*Eb, the better the physical properties of the rubber compound.
[0108] -25℃E': The modulus of rubber at -25℃. According to the room temperature equivalent principle of viscoelastic materials, it can be used to characterize the low-temperature grip performance of rubber. The smaller the E' at -25℃, the better the low-temperature grip performance of rubber.
[0109] 25℃Tanδ: hysteresis loss Tanδ of rubber at 25℃, often used to characterize the grip performance of rubber. The larger the 25℃Tanδ, the better the grip performance of the rubber at room temperature.
[0110] 60℃Tanδ: hysteresis loss Tanδ of rubber at 60℃. According to the room temperature equivalent principle of viscoelastic materials, it can be used to characterize the rolling resistance of rubber, that is, the heat generation rate of the rubber. The larger the 60℃Tanδ, the faster the heat generation rate, that is, the faster the rubber becomes soft and sticky and exerts the molecular adhesion effect.
[0111] Peak Tg: The glass transition temperature Tg of rubber. According to the room temperature equivalence principle of viscoelastic materials, it can be used to characterize the low-temperature performance of rubber. The lower the Peak Tg, the better the low-temperature performance of the rubber.
[0112] For the above performance, please refer to Table 10 according to the classification of importance:
[0113] Table 10 Classification results of importance of vulcanized rubber properties
[0114]
[0115] Based on the above test results, compared with the reference group, it can be seen that in Example Group 1, as the number of SBR-1 used decreases and the number of SBR-2 used increases, the performance of Schemes 1-1 to 1-5 presents the following trends:
[0116] Low temperature performance:
[0117] 1. -25℃E': It shows a gradual downward trend, and schemes 1-4 and 1-5 are better;
[0118] 2. Peak Tg: presents a gradually decreasing trend, with Schemes 1-4 and 1-5 being the best;
[0119] Grip performance:
[0120] 1. 25℃ tand: There is little difference among the schemes, and schemes 1-4 are the best;
[0121] 2. 60℃ tand: There is little difference among the schemes, and schemes 1-4 are the best;
[0122] Physical and mechanical properties:
[0123] 1. Anti-destruction capability Ts*Eb: It shows a trend of first increasing and then decreasing, and schemes 1-4 are the best;
[0124] In summary, Schemes 1-4 in Example Group 1 have relatively balanced low-temperature performance, grip performance, and physical properties, and are the optimal schemes.
[0125] Based on the above test results, compared with the reference group, it can be seen that in Example Group 2, as the number of fillers used increases, the performance of Schemes 2-1 to 2-5 presents the following trends:
[0126] Low temperature performance:
[0127] 1. -25℃E': It shows a gradual upward trend, and Schemes 2-1 and 2-2 are better;
[0128] 2. Peak Tg: It shows a gradual upward trend, and Schemes 2-1 and 2-2 are better;
[0129] Grip performance:
[0130] 1. 25℃tand: showing a gradual upward trend, schemes 2-4 and 2-5 are better;
[0131] 2. 60℃ tand: showing a gradual upward trend, schemes 2-4 and 2-5 are better;
[0132] Physical and mechanical properties:
[0133] 1. Anti-destruction capability Ts*Eb: It shows a trend of first increasing and then decreasing, and scheme 2-2 is the best;
[0134] In summary, Scheme 2-2 in Example Group 2 has relatively balanced low-temperature performance, grip performance, and physical properties, and is the optimal solution.
[0135] Based on the above test results, compared with the reference group, it can be seen that in Example Group 3, as the number of sunflower oil used increases, the performance of Schemes 3-1 to 3-5 presents the following trends:
[0136] Low temperature performance:
[0137] 1. -25℃E': It shows a gradual downward trend, and schemes 3-5 and 3-6 are better;
[0138] 2. Peak Tg: presents a gradually decreasing trend, with schemes 3-5 and 3-6 being the best;
[0139] Grip performance:
[0140] 1. 25℃tand: showing a gradual downward trend, scheme 3-1 is the best;
[0141] 2. 60℃tand: showing a gradual downward trend, scheme 3-1 is the best;
[0142] Physical and mechanical properties:
[0143] 1. Anti-destruction capability Ts*Eb: presents a downward trend, and scheme 3-1 is the best;
[0144] In summary, Scheme 3-5 in Example Group 3 has relatively balanced low-temperature performance, grip performance, and physical performance, and is the optimal scheme.
[0145] Based on the above test results, compared with the reference group, it can be seen that in Example Group 4, as the number of functional resins used increases, the performance of Schemes 4-1 to 4-5 presents the following trends:
[0146] Low temperature performance:
[0147] 1. -25℃E': It shows a gradual downward trend, and schemes 4-5 and 4-6 are better;
[0148] 2. Peak Tg: It shows a gradual downward trend, and Schemes 4-1 and 4-2 are better;
[0149] Grip performance:
[0150] 1. 25℃ tand: showing a gradual upward trend, schemes 4-5 and 4-6 are better;
[0151] 2. 60℃ tand: showing a gradual upward trend, schemes 4-5 and 4-6 are better;
[0152] Physical and mechanical properties:
[0153] 1. Anti-destruction capability Ts*Eb: It shows a trend of first increasing and then decreasing, and scheme 4-3 is the best;
[0154] In summary, Scheme 4-3 in Example Group 4 has relatively balanced low-temperature performance, grip performance, and physical performance, and is the optimal solution.
[0155] Based on the above test results, compared with the reference group, Example Group 5 uses the optimal components of Example Groups 1, 2, 3, and 4, that is, 20 parts of SBR-1 and 80 parts of SBR-2, 100 parts of filler, 80 parts of sunflower oil, and 20 parts of functional resin. Compared with the reference group, Example Group 5 has the following advantages:
[0156] 1) Low temperature performance: Tg is significantly reduced, E' is significantly reduced at -25℃, the mobility of rubber molecular segments is greatly improved under low temperature conditions, and the low temperature performance of the rubber compound is significantly improved;
[0157] 2) Grip performance: Both 25℃ Tanδ and 60℃ Tanδ have been significantly improved. The grip of the rubber compound due to the pitting effect has been significantly improved. At the same time, due to the increase in 60℃ Tanδ, the heat generation rate of the rubber compound has been accelerated. Under the same conditions, the time it takes to reach a gel state and exert an adhesion effect is shorter, and the overall grip performance has been significantly improved;
[0158] 3) Ground contact area: As the Shore hardness of the rubber compound decreases, the tire tread ground contact area becomes larger under the same stress conditions, and the contact between the rubber and the ground protrusions becomes more complete;
[0159] The rubber polymers prepared in the reference group and example group 5 were applied to the tire treads of racing cars and were tested on a track. Except that the tire treads used the reference group and example group 5, respectively, the other conditions remained the same.
[0160] The test vehicle parameter information is as follows:
[0161] Vehicle: Prosche GTR3 R
[0162] Maximum horsepower: 480NM
[0163] Weight: 1200kg
[0164] Vehicle parameter settings can refer to Table 11:
[0165] Table 11 Vehicle parameters
[0166]
[0167] Test track: Shanghai International Circuit, track length 5.45km.
[0168] The test conditions can be found in Table 12:
[0169] Table 12 Vehicle test environment conditions
[0170] Air temperature Track temperature weather -3℃ 3℃ partly cloudy
[0171] The test results can be found in Table 13:
[0172] Table 13 Racing car test results of the reference group and sample group 5
[0173] Group Reference group Example Group 5 Fastest lap time 2.15.701 1.59.948
[0174] Based on actual feedback, the tires of sample group 5 heat up quickly, and the grip brought by the adhesion effect can be felt after one lap of warm-up, allowing for intense control. The grip of the reference group is still poor after 4 laps of warm-up, and graining occurs. From the fastest lap time, the fastest lap of sample group 5 is more than 15 seconds faster than that of the reference group, which shows that the grip of sample group 5 is better than that of the reference group under low temperature conditions.
[0175] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A full hot melt tread rubber polymer with ultra-high grip under low temperature conditions, characterized in that: The tread rubber polymer is prepared by mixing raw materials including the following components based on 100 parts by weight of the rubber component: 100 parts of the rubber component, 80-160 parts of the filler component, 5-100 parts of the plasticizer, 10-60 parts of the functional resin, 3-6 parts of the antioxidant, 2-6 parts of the activator, 1-5 parts of the vulcanizer and 1-6 parts of the accelerator; The rubber component is styrene-butadiene rubber, i.e., SBR. The SBR includes 0-40 parts of SBR1 and 60-100 parts of SBR2. Both SBR1 and SBR2 are prepared by mixing styrene and vinyl in different proportions. The styrene content of SBR1 accounts for more than 30% of the total content of SBR1, the vinyl content is lower than 35% of the total content of SBR1, and the glass transition temperature is lower than -20°C; the styrene content of SBR2 accounts for more than 30% of the total content of SBR2, the vinyl content accounts for more than 35% of the total content of SBR2, and the glass transition temperature is higher than -20°C.
2. The full hot melt tread rubber polymer with ultra-high grip under low temperature conditions according to claim 1, characterized in that: The styrene-butadiene rubber SBR1 and SBR2 are both filled with 0-50 parts of TDAE as a plasticizer.
3. The full hot melt tread rubber polymer with ultra-high grip under low temperature conditions according to claim 1, characterized in that: The filler component is carbon black, and the amount used is 80-160 parts, and more preferably 100 parts; the specific surface area of the carbon black is 100-200m 2 / g, more preferably 120-180m 2 / g, and the particle size is 0.1-1 μm, more preferably 0.2-0.8 μm.
4. The full hot melt tread rubber polymer with ultra-high grip under low temperature conditions according to claim 1, characterized in that: The plasticizer is sunflower oil, and the usage amount is 5-100 parts, more preferably 80 parts.
5. The full hot melt tread rubber polymer with ultra-high grip under low temperature conditions according to claim 1, characterized in that: The functional resin includes one or more of C5 petroleum resin, C9 petroleum resin, α-methylstyrene resin, indene resin, phenolic resin and terpene resin, and the amount used is 10-60 parts, and more preferably 20 parts.
6. The full hot melt tread rubber polymer with ultra-high grip under low temperature conditions according to claim 1, characterized in that: The antioxidants include physical antioxidants and chemical antioxidants, wherein the physical antioxidants include one or more of paraffin wax and microcrystalline wax, and the chemical antioxidants include one or more of RD, 4010, 4010NA, 4020, and DTPD.
7. The full hot melt tread rubber polymer with ultra-high grip under low temperature conditions according to claim 1, characterized in that: The active agents include zinc oxide and stearic acid.
8. The full hot melt tread rubber polymer with ultra-high grip under low temperature conditions according to claim 1, characterized in that: The vulcanizing agent includes one or more of common sulfur, insoluble sulfur, sulfur-containing compounds, and peroxides.
9. The full hot melt tread rubber polymer with ultra-high grip under low temperature conditions according to claim 1, characterized in that: The accelerator is one or more of N-cyclohexyl-2-benzothiazole sulfenamide, amide N-tert-butyl-2-benzothiazole sulfenamide, 2-(4-morpholinethio)benzothiazole, N,N-dicyclohexyl-2-benzothiazole sulfenamide, tetrabenzylthiuram disulfide, tetramethylthiuram disulfide, diphenylguanidine, o-tolylbiguanide, and di-o-tolylguanidine.
10. A mixing method for a full hot-melt tread rubber polymer with ultra-high grip under low temperature conditions as claimed in any one of claims 1 to 9, characterized in that: The steps include: Put all raw materials into the internal mixer at one time according to the components, control the rotor speed of the internal mixer to 40-50rpm, the upper bolt pressure to 0.6Mpa, the cooling water temperature of the internal mixer to 25±3℃, and carry out a master batching, which specifically includes the following process steps: Add all the raw materials, press the top bolt, and keep it for 60 seconds, or heat the raw materials to 110℃; Raise the top bolt, add plasticizer, press the top bolt and hold for 30 seconds; Raise the top bolt and hold for 10 seconds; Press the top bolt and hold for 30 seconds; Raise the top bolt and hold for 10 seconds; Press the top bolt and keep it for 90 seconds to perform the debinding operation, or heat the material to 150℃ to perform the debinding operation; The rotor speed of the internal mixer is controlled to be 40-50rpm, the upper bolt pressure is 0.6Mpa, the cooling water temperature of the internal mixer is 25±3℃, and the second-stage masterbatch is carried out. The specific process steps include the following: Add all the masterbatch from the first stage of masterbatch Press the top bolt and hold for 30 seconds; Raise the top bolt and hold for 10 seconds; Press the top bolt and keep it for 90 seconds to perform the debinding operation, or heat the material to 150℃ to perform the debinding operation; The rotor speed of the internal mixer is controlled to be 20-30rpm, the upper bolt pressure is 0.6Mpa, and the cooling water temperature of the internal mixer is 25±3℃. The final refining is carried out, which specifically includes the following process steps: Press the top bolt and hold for 30 seconds; Raise the top bolt and hold for 10 seconds; Press the top bolt and hold it for 90 seconds to perform the debinding operation, or heat the material to 100℃ to perform the debinding operation.