Anti-ultraviolet heat-shrinkable material and preparation method thereof, and heat-shrinkable sleeve and manufacturing method thereof
The stability of the heat-shrink sleeve in alternating hot and humid environments was solved by adding modified 2-(2-hydroxy-5-phenylino)benzotriazole to the heat-shrink material and performing electron beam irradiation crosslinking. The performance and UV resistance problems enable longer service life and lower cost heat shrink tubes, suitable for applications in sun exposure components.
Patent Information
- Application Number
- CN202411225358.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-19
AI Technical Summary
The existing heat shrink sleeves are prone to electrochemical corrosion in alternate hot and cold and humid environments, with poor stability, high cost, and lack of UV resistance, which limits its application in sun exposure components.
Using UV heat shrinkage materials, the modified 2-(2-hydroxy-5-phenylino)benzotriazole is prepared through chemical modification and processing technology, and grafted it on polyethylene and inorganic flame retardant. In this case, a heat shrink tube with excellent UV resistance was prepared by cross-linking of electron beam irradiation.
It extends the service life of the heat shrink tube, improves its stability and waterproof performance under various environmental conditions, reduces costs, and is suitable for external sunlight applications such as automobiles and high-speed railways.
Smart Images

Figure CN118978758A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of material technology, and in particular to an anti-ultraviolet heat shrinkable material and a preparation method thereof, as well as a heat shrinkable sleeve and a manufacturing method thereof. Background Art
[0002] Heat shrink tubing is widely used to protect metal and non-metal parts. They can shrink when heated and fit tightly to the surface of the protected object to provide insulation, protection and identification functions.
[0003] In practical applications, heat shrink tubing is often exposed to alternating hot and cold and humid environmental conditions, which may cause electrochemical corrosion and affect the durability and protective effect of the tubing.
[0004] The commonly used solution at present is to use double-walled pipes, whose inner layer is hot melt adhesive, which can provide better adhesion. However, during long-distance transportation in summer, the inner wall of the double-walled pipe is easy to stick together, affecting its use.
[0005] In addition, the stability of double-walled pipes is poor, and it is difficult to control the amount of glue and tensile properties, which limits their use in certain application scenarios. In addition, the cost of double-walled pipes is high, which brings great cost pressure to enterprises.
[0006] For those protected parts that are exposed to sunlight, they usually need to be resistant to UV rays to prevent material aging and performance degradation caused by UV rays.
[0007] In view of the limitations of existing technology, the industry is in urgent need of a new type of heat shrinkable material that can maintain stability under various environmental conditions and provide good waterproof, wear-resistant and UV-resistant properties. Summary of the invention
[0008] In view of this, the anti-ultraviolet heat shrinkable material and heat shrinkable tube proposed in the present invention overcome the shortcomings of traditional heat shrinkable tubes through special chemical modification and processing technology, and provide a solution with better performance and lower cost.
[0009] On the one hand, the present application provides an anti-ultraviolet heat shrinkable material, characterized in that it includes the following components in parts by weight:
[0010] Polyethylene 100 parts;
[0011] 50-70 parts of inorganic flame retardant;
[0012] 3-10 parts of modified 2-(2-hydroxy-5-phenylamino)benzotriazole;
[0013] The modified 2-(2-hydroxy-5-phenylamino)benzotriazole is 2-(2-hydroxy-5-phenylamino)benzotriazole modified with enoyl chloride.
[0014] Optionally, the polyethylene has a melting point of 110-130° C. and a melt index of 3-10 g / 10 min.
[0015] Optionally, the inorganic flame retardant includes the following components by weight: 2 parts of titanium dioxide, 1 part of talc and 1 part of clay.
[0016] In a second aspect, the present application further provides a method for preparing an anti-ultraviolet heat shrinkable material, using the components as described in any one of the above items, and the method comprises:
[0017] The preparation of the modified 2-(2-hydroxy-5-phenylamino)benzotriazole comprises the following steps:
[0018] Take 2-(2-hydroxy-5-phenylamino)benzotriazole, a stabilizer, and an organic base, and add an enoyl chloride reagent dropwise to react;
[0019] After the reaction is completed, the precipitate is filtered and the stabilizer is evaporated to obtain modified 2-(2-hydroxy-5-phenylamino)benzotriazole;
[0020] Take the modified 2-(2-hydroxy-5-phenylamino)benzotriazole, add polyethylene and an inorganic flame retardant, and mix to obtain a mixture;
[0021] The mixture was extruded into pellets.
[0022] Optionally, the stabilizer is ethylene dichloride or toluene; and the organic base is triethylamine or pyridine.
[0023] Optionally, the enoyl chloride reagent is acryloyl chloride.
[0024] Optionally, in the step of taking 2-(2-hydroxy-5-phenylamino)benzotriazole, a stabilizer, and an organic base, and adding an enoyl chloride reagent dropwise to react, the reaction temperature is 0-20° C., the reaction time is 6-30 hours, and the stirring speed is 50-400 revolutions per minute.
[0025] In a second aspect, the present application also provides a heat shrinkable tube using the anti-ultraviolet heat shrinkable material as described above.
[0026] In a third aspect, the present application also provides a method for manufacturing a heat shrink tube, comprising: taking the anti-ultraviolet heat shrink material as described above; extruding the anti-ultraviolet heat shrink material into shape, and obtaining a heat shrink tube through radiation cross-linking and expansion molding.
[0027] Optionally, the radiation cross-linking method is electron beam irradiation, the irradiation dose is between 100-300 kGy, and the thermal extension of the expansion molding is controlled at 200%-240%.
[0028] The technical solution of the present application avoids the shortcomings of single-walled tubes and double-walled tubes in the prior art. By preparing modified 2-(2-hydroxy-5-phenylamino)benzotriazole and grafting it into the corresponding matrix material of the heat shrink tube, a heat shrink tube with excellent UV resistance is prepared, the stability and durability of the heat shrink tube are guaranteed, and the failure time of the heat shrink tube is extended. It is shrunk on the metal tube at the appropriate temperature and time, and can fit tightly, achieve excellent waterproof performance, and realize the application in the field of washing and cooling water pipes in automobiles, high-speed railways and other places exposed to sunlight.
[0029] The present invention adds modified 2-(2-hydroxy-5-phenylamino)benzotriazole during the processing and manufacturing process of the heat shrink tube, so that the heat shrink tube can have an anti-UV ultraviolet function during long-term use and prolong the failure time of the heat shrink tube.
[0030] The anti-UV heat shrink tube prepared by the present invention can cross-link the stable anti-UV material to the polymer matrix material after being irradiated by an electron accelerator, thereby ensuring the stability and durability of the anti-UV material filled in the polymer matrix;
[0031] The anti-UV material added and cross-linked in the present invention can strengthen the polarity of the base material and can strengthen the adhesion between the base material and the metal material under a specific temperature and time.
[0032] The inorganic material added in the present invention can enhance the ultraviolet reflection ability of the polymer matrix and enhance its anti-UV effect after being prepared in a suitable proportion. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings used in the description of the embodiments are briefly introduced below.
[0034] Figure 1 A schematic flow chart of a method for preparing an anti-ultraviolet heat shrinkable material provided in an embodiment of the present application;
[0035] Figure 2 A chemical formula for the preparation process of a modified 2-(2-hydroxy-5-phenylamino)benzotriazole provided in an embodiment of the present application;
[0036] Figure 3 This is the chemical formula of the modified 2-(2-hydroxy-5-phenylamino)benzotriazole enoyl chloride provided in the embodiment of the present application, which is cross-linked on a polymer matrix after being irradiated and cross-linked by an electron accelerator. DETAILED DESCRIPTION
[0037] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the specific implementation methods of the present application will be described below with reference to the accompanying drawings. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings and other implementation methods can be obtained based on these drawings without creative work.
[0038] In the description of the present application, the terms "first", "second", etc. are only used to distinguish and describe associated objects, and cannot be understood as indicating or implying the relative importance or order between the associated objects. The term "comprising: a combination of one or more of a1, a2, ..., an" (n is a positive integer greater than 2) means any one of the described objects, any combination of two objects, any combination of three objects, and any combination of n objects. For example, "combining one or more of a1, a2, a3" includes a1, a2, a3, a1 and a2, a1 and a3, a2 and a3, a1, a2, and a3.
[0039] In real-world applications, heat shrink tubing is often exposed to extreme environmental conditions, such as drastic temperature changes, humid environments, and prolonged exposure to direct sunlight. These conditions may cause electrochemical corrosion, which can affect the durability of the heat shrink tubing and its ability to protect the cables or pipes inside.
[0040] In order to solve these problems, the present application embodiment proposes a new heat shrink material development plan. This material significantly improves the overall performance of the heat shrink material through a specific component design, and effectively avoids the defects of traditional single-walled tubes and double-walled tubes. The heat shrink tube prepared by this method not only has excellent UV resistance, but also ensures its stability and durability in long-term use, thereby extending the service life of the heat shrink tube.
[0041] In addition, when this heat shrink tubing shrinks on the metal tube at the appropriate temperature and time, it can fit tightly and show excellent waterproof performance. This performance improvement makes the new heat shrink tubing very suitable for the exterior of vehicles such as automobiles and high-speed railways, especially in washing and cooling water pipe systems that are often exposed to sunlight. Such applications not only improve the reliability of the system, but also reduce maintenance costs and potential failure risks.
[0042] The components and preparation process of this heat shrinkable material are described below.
[0043] The anti-ultraviolet heat shrinkable material provided in this embodiment includes the following components by weight:
[0044] Polyethylene 100 parts;
[0045] 50-70 parts of inorganic flame retardant;
[0046] 3-10 parts of modified 2-(2-hydroxy-5-phenylamino)benzotriazole;
[0047] The modified 2-(2-hydroxy-5-phenylamino)benzotriazole is 2-(2-hydroxy-5-phenylamino)benzotriazole modified with enoyl chloride.
[0048] The modified 2-(2-hydroxy-5-phenylamino)benzotriazole prepared in the embodiment of the present application is grafted into the resin matrix material by means of radiation cross-linking modification. The heat shrinkable tube thus prepared not only has excellent UV resistance, but can also be grafted onto the polymer resin matrix in a long-lasting and stable manner.
[0049] In the examples of the present application, the polyethylene has a melting point of 110-130° C. and a melt index of 3-10 grams per 10 minutes (g / 10min).
[0050] In the embodiments of the present application, the inorganic flame retardant is titanium dioxide, talcum powder and clay, and the weight ratio of each component is 2:1:1.
[0051] When the inorganic flame retardant is added in the above proportion, not only the cost is reduced, but also because the added inorganic material has a higher refractive index, it can be evenly distributed on the surface of the polymer matrix, enhancing the reflection and scattering of ultraviolet rays by the heat shrinkable tube, thereby further enhancing the anti-UV function of the heat shrinkable material.
[0052] Combine the following Figure 1 Describe the preparation process of the UV-resistant heat shrinkable material. The components used in the preparation process are selected according to the above weight parts, such as Figure 1 As shown, the preparation process includes the following steps:
[0053] Step S10: preparing modified 2-(2-hydroxy-5-phenylamino)benzotriazole, specifically comprising the following steps:
[0054] Step S11: Take 2-(2-hydroxy-5-phenylamino)benzotriazole, a stabilizer, and an organic base, and dropwise add an enoyl chloride reagent to react;
[0055] In this embodiment, the stabilizer is ethylene dichloride or toluene, the organic base is triethylamine or pyridine, the reaction temperature is 0-20°C, the reaction time is 6-30 hours, and the stirring speed is 50-400 revolutions per minute (r / min).
[0056] Step S12: After the reaction is completed, the precipitate is filtered and the stabilizer is evaporated to obtain modified 2-(2-hydroxy-5-phenylamino)benzotriazole;
[0057] like Figure 2As shown in the chemical formula, the molar masses of 2-(2-hydroxy-5-phenylamino)benzotriazole, the organic base, and the enoyl chloride reagent are 0.1-0.5 mol, 0.01-0.05 mol, and 0.1-0.5 mol, respectively; and the volume of the stabilizer is 200-600 ml.
[0058] Step S20: taking the modified 2-(2-hydroxy-5-phenylamino)benzotriazole, adding polyethylene and an inorganic flame retardant, and mixing to obtain a mixture;
[0059] Step S30: extruding the mixture into granules.
[0060] The present application also provides a method for manufacturing a heat shrink tube using the above-mentioned anti-ultraviolet heat shrink material, comprising:
[0061] The master batch prepared from the anti-ultraviolet heat shrinkable material in the above embodiment is taken; the anti-ultraviolet heat shrinkable material is extruded and formed, and a heat shrinkable tube is obtained by radiation cross-linking and expansion forming.
[0062] The radiation cross-linking method is electron beam irradiation, the irradiation dosage is between 100-300 kGy, and the thermal extension of the expansion molding is controlled at 200%-240%.
[0063] Specifically, 3-10 parts of modified 2-(2-hydroxy-5-phenylamino)benzotriazole are added with 100 parts of polyethylene and 50-70 parts of inorganic flame retardant, and the mixture is blended and granulated, and then extruded into a tube by an extruder, and then cross-linked by electron beam irradiation. The cross-linking effect of irradiation is as follows: Figure 3 As shown, after modification of 2-(2-hydroxy-5-phenylamino)benzotriazole acyl chloride, after cross-linking by electron accelerator irradiation, it can be evenly and tightly cross-linked on the polymer matrix. Since 2-(2-hydroxy-5-phenylamino)benzotriazole itself can absorb ultraviolet rays, the stability and durability of the anti-UV material in the polymer matrix are guaranteed. At the same time, the inorganic flame retardant is titanium dioxide, talcum powder and clay. The added inorganic material has a high refractive index and can be evenly distributed on the surface of the polymer matrix to enhance the reflection and scattering of ultraviolet rays by the heat shrink tube. After oil bath expansion, the anti-UV ultraviolet heat shrink tube is obtained.
[0064] The UV-resistant heat shrink tubing prepared according to the above embodiment is sleeved on a metal tube such as an aluminum tube of a suitable size, and then baked in an oven at 200-220°C for 3-5 minutes. It can adhere tightly to the metal tube and has excellent waterproof performance. This may be because the cross-linked and grafted 2-(2-hydroxy-5-phenylamino)benzotriazole enhances the polarity of the polymer matrix and the adhesion between the polymer matrix and the metal material, thereby enhancing its waterproof performance. It can be used in the field of washing and cooling water pipes in automobiles, high-speed railways, etc. that are exposed to sunlight.
[0065] The following provides some specific examples, comparative examples and performance test results:
[0066] Example 1
[0067] Take 0.1 mol of 2-(2-hydroxy-5-phenylamino)benzotriazole and 0.05 mol of organic base in a round-bottom flask, then pour in 300 ml of stabilizer, magnetically stir, under nitrogen protection, dropwise add 0.1 mol of acryloyl chloride reagent, react at 10°C for 10 hours, filter the precipitate, and rotary evaporate the organic solvent to obtain modified 2-(2-hydroxy-5-phenylamino)benzotriazole;
[0068] Take 5 parts of modified 2-(2-hydroxy-5-phenylamino)benzotriazole, add 100 parts of polyethylene and 60 parts of inorganic flame retardant, the inorganic flame retardant is titanium dioxide, talcum powder and clay in a weight ratio of 2:1:1. Granulate through a twin-screw extruder, and then extrude into a hollow tube through a single-screw extruder. The tube is irradiated and cross-linked according to the heat extension standard of 200-240% by an electron accelerator, and then expanded to obtain a UV-resistant heat shrink tube.
[0069] Shrink the expanded UV-resistant heat shrink tubing onto an aluminum tube of appropriate size, and then bake it in an oven at 200°C for 5 minutes to ensure that it adheres tightly to the metal tube.
[0070] Example 2
[0071] 0.1 mol of 2-(2-hydroxy-5-phenylamino)benzotriazole and 0.05 mol of an organic base were placed in a round-bottom flask, and 300 ml of a stabilizer was added. The mixture was stirred magnetically and 0.1 mol of acryloyl chloride reagent was added dropwise under nitrogen protection. The mixture was reacted at 5°C for 12 hours, and the precipitate was filtered. The organic solvent was evaporated by rotary evaporation to obtain a modified 2-(2-hydroxy-5-phenylamino)benzotriazole.
[0072] Take 3 parts of modified 2-(2-hydroxy-5-phenylamino)benzotriazole, add 100 parts of polyethylene and 50 parts of inorganic flame retardant, the inorganic flame retardant is titanium dioxide, talcum powder and clay in a weight ratio of 2:1:1. Granulate through a twin-screw extruder, and then extrude into a hollow tube through a single-screw extruder. The tube is irradiated and cross-linked according to the heat extension standard of 200-240% by an electron accelerator, and then expanded to obtain a UV-resistant heat shrink tube.
[0073] Shrink the expanded UV-resistant heat shrink tubing onto an aluminum tube of appropriate size, and then bake it in an oven at 220°C for 3 minutes to ensure that it adheres tightly to the metal tube.
[0074] Example 3
[0075] Take 0.1 mol of 2-(2-hydroxy-5-phenylamino)benzotriazole and 0.05 mol of organic base in a round-bottom flask, then pour in 300 ml of stabilizer, stir magnetically, add 0.1 mol of acryloyl chloride reagent dropwise under nitrogen protection, react at 20°C for 14 hours, filter the precipitate, and rotary evaporate the organic solvent to obtain modified 2-(2-hydroxy-5-phenylamino)benzotriazole;
[0076] Take 10 parts of modified 2-(2-hydroxy-5-phenylamino)benzotriazole, add 100 parts of polyethylene and 70 parts of inorganic flame retardant, the inorganic flame retardant is titanium dioxide, talcum powder and clay in a weight ratio of 1:1:1. Granulate through a twin-screw extruder, and then extrude into a hollow tube through a single-screw extruder. The tube is irradiated and cross-linked according to the heat extension standard of 200-240% by an electron accelerator, and then expanded to obtain a UV-resistant heat shrink tube.
[0077] Shrink the expanded UV-resistant heat shrink tubing onto an aluminum tube of appropriate size, and then bake it in an oven at 210°C for 4 minutes to ensure that it adheres tightly to the metal tube.
[0078] In order to more clearly illustrate the beneficial technical effects achieved by the technical solution provided by the present application, the following comparative examples are given for comparison and explanation:
[0079] Comparative Example 1
[0080] This example is different from Example 1 in that modified 2-(2-hydroxy-5-phenylamino)benzotriazole is not added.
[0081] Comparative Example 2
[0082] This embodiment is different from Embodiment 1 in that no inorganic flame retardant is added.
[0083] Comparative Example 3
[0084] This example is different from Example 1 in that unmodified 2-(2-hydroxy-5-phenylamino)benzotriazole is added.
[0085] Performance Testing
[0086] Performance Test 1
[0087] According to ASTM D2671 standard, the tensile strength and elongation at break of the samples obtained in Examples 1-3 and Comparative Examples 1-8 were tested.
[0088] Performance Test 2
[0089] According to GB / T 16422.3 standard, use UV-A lamp to cycle according to exposure method 1, that is, first expose to radiation at a standard temperature of 60℃±3℃ for 4h, and then expose to radiation at a standard temperature of 50℃±3℃ for 4h as one cycle. Record the number of cycles when the surface of the heat shrink tube turns yellow and fails, and perform relevant experiments as integer multiples of 10.
[0090] Performance Test 3
[0091] The heat shrinkable tubes obtained in the embodiment and the comparative example were subjected to a peeling force test, and the specific steps were as follows:
[0092] S1. The high-ratio heat shrink tubing is shrunk at 200°C / 5min in a metal tube with a suitable inner diameter to form a test piece, wherein the high-ratio heat shrink tubing is shrunk to a distance of 12.5mm at one end of the metal tube, and the heat shrink tubing is extended to leave a pulling portion;
[0093] S2. Cut the specimen of set length and retain the pulling portion 30mm;
[0094] S3. Place the specimen vertically on the ground and hang a suitable weight below until the heat shrink tube is peeled off from the metal pipe;
[0095] S4. Record the force when the heat shrink tube is peeled off; the above peeling force test can effectively test the actual effect of the formula used in improving adhesion.
[0096] Performance Test 4
[0097] The waterproof performance of the samples obtained in Examples 1-3 and Comparative Examples 1-8 was tested according to GB4208-2008 to determine whether they could achieve IP67 waterproof performance, and the determination result was recorded as yes or no.
[0098] Performance Test Table
[0099]
[0100] From the above test data, we can see that:
[0101] 1. The technical solution of the embodiment of the present application adds modified 2-(2-hydroxy-5-phenylamino)benzotriazole during the processing and manufacturing process of the heat shrink tube, which can have UV resistance during long-term use and extend the failure time of the heat shrink tube;
[0102] 2. The anti-UV heat shrink tubing prepared in the embodiment of the present application can cross-link the stable anti-UV material to the polymer matrix material after being irradiated by an electron accelerator, thereby ensuring the stability and durability of the anti-UV material filled in the polymer matrix;
[0103] 3. The anti-UV material added and cross-linked in the embodiment of the present application can enhance the polarity of the base material and enhance its adhesion with the metal material under a specific temperature and time.
[0104] 4. The inorganic materials added in the embodiments of the present application, after being prepared in appropriate proportions, can enhance the ultraviolet reflection ability of the polymer matrix and enhance its anti-UV effect.
[0105] The technical solution of the embodiment of the present application avoids the shortcomings of single-walled tubes and double-walled tubes in the prior art, and provides a method for preparing a UV-resistant heat shrink tube and its application on a metal tube. The present application prepares a heat shrink tube with excellent UV resistance by preparing a modified 2-(2-hydroxy-5-phenylamino)benzotriazole and grafting it on the corresponding matrix material of the heat shrink tube, and shrinks it on the metal tube at a suitable temperature and time, so that it can fit tightly and achieve excellent waterproof performance, and realizes its application in the field of washing and cooling water pipes in automobiles, high-speed railways, etc. that are exposed to sunlight.
[0106] The above are only some embodiments of the present invention. For ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as within the scope of protection of the present invention.
Claims
1. An anti-ultraviolet heat shrinkable material, characterized in that: By weight, it includes the following components: Polyethylene 100 parts; 50-70 parts of inorganic flame retardant; 3-10 parts of modified 2-(2-hydroxy-5-phenylamino)benzotriazole; The modified 2-(2-hydroxy-5-phenylamino)benzotriazole is 2-(2-hydroxy-5-phenylamino)benzotriazole modified with enoyl chloride.
2. The anti-ultraviolet heat shrinkable material according to claim 1, characterized in that: The polyethylene has a melting point of 110-130° C. and a melt index of 3-10 g / 10 min.
3. The UV-resistant heat shrinkable material according to claim 1, characterized in that: The inorganic flame retardant comprises the following components by weight: 2 parts of titanium dioxide, 1 part of talcum powder and 1 part of clay.
4. A method for preparing an anti-ultraviolet heat shrinkable material, characterized in that: Using the components according to any one of claims 1 to 3, and the method comprising: The preparation of the modified 2-(2-hydroxy-5-phenylamino)benzotriazole comprises the following steps: Take 2-(2-hydroxy-5-phenylamino)benzotriazole, a stabilizer, and an organic base, and add an enoyl chloride reagent dropwise to react; After the reaction is completed, the precipitate is filtered and the stabilizer is evaporated to obtain modified 2-(2-hydroxy-5-phenylamino)benzotriazole; Take the modified 2-(2-hydroxy-5-phenylamino)benzotriazole, add polyethylene and an inorganic flame retardant, and mix to obtain a mixture; The mixture was extruded into pellets.
5. The method for preparing the UV-resistant heat shrinkable material according to claim 4, characterized in that: The stabilizer is ethylene dichloride or toluene; the organic base is triethylamine or pyridine.
6. The method for preparing the anti-ultraviolet heat shrinkable material according to claim 4, characterized in that: The enoyl chloride reagent is acryloyl chloride.
7. The method for preparing the anti-ultraviolet heat shrinkable material according to claim 4, characterized in that: In the step of taking 2-(2-hydroxy-5-phenylamino)benzotriazole, a stabilizer, and an organic base, and adding an enoyl chloride reagent dropwise to react, the reaction temperature is 0-20° C., the reaction time is 6-30 hours, and the stirring speed is 50-400 revolutions per minute.
8. A heat shrink tube, characterized in that: Use the UV-resistant heat shrinkable material as described in any one of claims 1 to 3.
9. A method for manufacturing a heat shrink tube, characterized in that: include: Take the anti-ultraviolet heat shrinkable material as described in any one of claims 1 to 3; The anti-ultraviolet heat shrinkable material is extruded and formed, and then irradiated, cross-linked and expanded to obtain a heat shrinkable tube.