Bio-based degradable low-temperature construction basketball court terrace composition and method
Through bio-based degradable low-temperature construction basketball court floor composition and optimized construction technology, the non-degradability and difficulty of low-temperature construction of traditional materials are solved, and environmentally friendly and efficient basketball court laying is achieved, which is suitable for cold areas and seasonal construction.
Patent Information
- Application Number
- CN202411047629.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-19
AI Technical Summary
Traditional basketball court floor materials are difficult to construct in low temperature environments due to non-degradability and environmental pollution problems during production.
Develop a bio-based degradable low-temperature construction basketball court floor composition, including bio-based polymers, natural fiber reinforced materials, degradable plasticizers and anti-aging additives, to ensure that it is at -10°C by optimizing material formulation and construction process. It has excellent fluidity and curing speed under low temperature environments of 10°C, high strength, wear resistance and anti-aging properties, and can naturally degrade.
It achieves efficient construction in low-temperature environments, reduces environmental pollution, improves construction quality and efficiency, and is suitable for cold areas and seasonal construction, which is significantly better than the environmental protection and construction performance of traditional petroleum-based materials.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the field of stadium floor materials, and in particular to a bio-based degradable low-temperature construction basketball court floor composition and a method. Background Art
[0002] With the improvement of global environmental awareness and the popularization of the concept of sustainable development, all walks of life are actively seeking green and environmentally friendly solutions. The environmental protection and sustainability of sports field paving materials have become an urgent issue to be solved.
[0003] Traditional basketball court floor materials are mostly made of petroleum-based synthetic materials, such as polyurethane and polyvinyl chloride. Although these materials have excellent physical and mechanical properties, such as high strength, wear resistance and anti-aging performance, they have a significant impact on the environment during production and use. These materials are difficult to degrade naturally after the end of their service life and exist in the soil and water for a long time, causing environmental pollution. In addition, the production process of petroleum-based materials relies on non-renewable petroleum resources and is accompanied by a large amount of carbon emissions.
[0004] The main problem with petroleum-based materials is their non-degradability. These materials are difficult to degrade by the natural environment after being discarded, resulting in their long-term presence in soil and water sources, causing serious environmental pollution. For example, common petroleum-based materials such as polyurethane and polyvinyl chloride degrade very slowly in the natural environment and may take decades or even longer to completely degrade. In the process, these materials may release harmful substances, posing a potential threat to ecosystems and human health.
[0005] In addition, the production process of petroleum-based materials also has significant environmental problems. First, petroleum resources are non-renewable resources. Their mining and processing processes not only consume a lot of energy, but also produce a large amount of greenhouse gas emissions, exacerbating the problem of global warming. Secondly, a large amount of chemical reagents and solvents are usually used in the production process of petroleum-based materials. These substances may be released into the environment during production and use, causing air and water pollution.
[0006] In terms of construction, petroleum-based basketball court floor materials also have some limitations. Traditional materials are difficult to construct in low-temperature environments below 5°C, and the material has poor fluidity and a long curing time, which not only affects the construction efficiency, but may also affect the final construction quality. For example, the curing speed of polyurethane materials slows down significantly under low-temperature conditions, and it takes a long time to achieve the expected strength and hardness, which is particularly evident in construction in cold areas. In addition, the poor fluidity of materials in low-temperature environments may lead to uneven paving during construction, affecting the overall flatness and performance of the venue.
[0007] Another important factor to consider is the impact of construction time and weather conditions on the construction process. The construction of school basketball courts is usually concentrated in the summer vacation, when students are on vacation and construction does not affect normal teaching activities. However, the rainy and humid climate conditions in summer also bring challenges to construction. Excessive humidity will affect the curing process of the material, resulting in prolonged curing time and even possible construction quality problems, such as weak bonding of materials and uneven surface. In addition, frequent rainfall may cause interruptions and delays in the construction process, further affecting the construction progress and quality.
[0008] Therefore, developing a new basketball court floor material with superior environmental performance and suitable for construction in low-temperature environments has become an important topic in the current field of materials science and environmental protection. This new material not only needs to have excellent physical and mechanical properties, such as high strength, wear resistance and anti-aging performance, but also needs to be able to be constructed in low-temperature environments to ensure construction efficiency and quality. At the same time, this material should have good environmental performance and be able to degrade naturally after the end of its service life to reduce pollution to the environment.
[0009] The present invention solves the environmental protection problems and construction limitations of traditional materials by developing a bio-based, degradable and low-temperature constructible basketball court floor composition and a construction method thereof, and has significant technical advantages and application prospects. Summary of the invention
[0010] The purpose of the present invention is to disclose a bio-based degradable low-temperature construction basketball court floor composition and its construction method. This new composition includes bio-based polymers, natural fiber reinforcement materials, degradable plasticizers and anti-aging additives. By optimizing the material formula and prefabrication production process, the floor material can be constructed in a low temperature environment of -10°C to 10°C, with excellent fluidity and curing speed, ensuring construction quality and efficiency. The composition has high strength, wear resistance, and anti-aging properties, and meets environmental protection requirements. It can be naturally degraded after the end of its service life, reducing pollution to the environment. It is suitable for cold areas and seasonal construction, overcoming the construction limitations of traditional materials and expanding the scope of application.
[0011] The present invention provides a bio-based degradable low-temperature construction basketball court floor composition and method, the bio-based degradable low-temperature construction basketball court floor composition comprises the following components and a preparation process thereof:
[0012] Component A:
[0013] Bio-based polymers 40%-60%, such as polylactic acid (PLA)
[0014] Plasticizer 5%-10%, such as citrate ester
[0015] Filler 10%-20%, such as cellulose
[0016] Natural fiber 5%-15%, such as bamboo fiber
[0017] Anti-aging additives 0.5%-1%, such as UV absorbers and antioxidants
[0018] Preparation process: Add bio-based polymers, plasticizers, fillers, natural fibers and anti-aging additives into a mixing device in proportion, stir evenly with a high-speed stirrer, and degas to remove bubbles generated during the mixing process.
[0019] Component B:
[0020] Bio-based curing agents 90%-99%, such as soybean oil-based isocyanates
[0021] Catalyst 1%-10%, such as organotin catalyst
[0022] Preparation process: Add the bio-based curing agent, catalyst and solvent into the mixing tank in proportion and stir evenly with a low-speed agitator to ensure uniform mixing.
[0023] The bio-based polymer is polylactic acid (PLA).
[0024] The degradable plasticizer is citrate.
[0025] The anti-aging aid comprises an ultraviolet absorber and an antioxidant, wherein the ultraviolet absorber is UV-531 and the antioxidant is antioxidant 1010.
[0026] The natural fiber reinforcement materials are cellulose and bamboo fiber.
[0027] The basketball court floor construction method comprises the following steps:
[0028] 1) Site preparation: clean up the debris on the surface of the site and ensure that the ground is flat and dry.
[0029] 2) Preparation of composition (adhesive): Component A and component B are prepared separately in a professional factory, wherein component A includes a bio-based polymer, a plasticizer, a filler and an additive, and component B includes a bio-based curing agent, a catalyst and a solvent.
[0030] 3) Material transportation: transport the prefabricated floor material composition to the construction site.
[0031] 4) At the construction site, mix component A and component B in proportion and stir evenly, then apply them evenly on the foundation of the court. The thickness of each application is 3mm. Before the next application, the material of the previous application must be completely cured.
[0032] 5) Laying and curing: Natural curing in low temperature environment to ensure construction quality. The laying thickness should meet the following requirements: average thickness ≥ 9mm
[0033] 6) Topcoat construction: After the floor material solidifies, apply anti-aging and anti-slip topcoat to improve the durability and safety of the floor.
[0034] 7) Line drawing construction: After the topcoat is completely dry, carry out line drawing construction on the basketball court to ensure that the lines are clear and durable.
[0035] The construction environment temperature ranges from -10°C to 10°C.
[0036] The weight ratio of component A to component B when mixed and stirred during construction is A:B=2:1.
[0037] The site after the composition is applied has the following properties:
[0038] Impact absorption rate between 20%-50%
[0039] The vertical deformation is between 0.6mm-3.0mm
[0040] The anti-slip value is between 90-110BPN (dry test)
[0041] Ball rebound rate ≥ 95%
[0042] Color fastness ≥ No fading under both dry and wet conditions
[0043] Tensile strength ≥0.7MPa
[0044] Elongation at break ≥90%
[0045] Flame retardancy reaches first-class standard
[0046] The following beneficial effects are obtained by using a bio-based degradable low-temperature construction basketball court floor composition and method of the present invention:
[0047] The present invention not only meets the current needs of environmental protection and sustainable development, but also provides a high-performance, low-cost solution for the construction of sports venues. By adopting bio-based degradable materials, the present invention greatly reduces the dependence on non-renewable resources and reduces carbon emissions in the production process. In addition, this new material can be naturally degraded after being discarded, reducing pollution to soil and water sources, and meeting the current requirements of environmental protection.
[0048] In terms of construction performance, the new material of the present invention has excellent low-temperature construction performance, and can be constructed in cold areas and in winter, ensuring construction quality and efficiency. At the same time, the construction of this material is not limited by seasonal and weather conditions, and can ensure smooth construction even in rainy and humid summer climate conditions. This provides great convenience for the construction of school basketball courts, ensuring that the construction tasks are completed during the summer vacation without affecting normal teaching activities.
[0049] In summary, the present invention provides an environmentally friendly, degradable and low-temperature constructible basketball court floor composition and its construction method, which solves the environmental protection problems and construction limitations in the prior art and has significant technical advantages and application prospects. The present invention not only meets the current needs of environmental protection and sustainable development, but also provides a high-performance, low-cost solution for sports venue construction, which has important practical significance and market value. DETAILED DESCRIPTION
[0050] In order to better understand the present invention, the specific embodiments of the present invention are further described in detail by examples below, so as to facilitate the understanding of technicians in the same industry. The materials, reagents, etc. used in the following examples, unless otherwise specified, can be obtained commercially; or prepared according to conventional methods in the art. Unless otherwise defined or specified, all professional and scientific terms used herein have the same meaning as those familiar to those skilled in the art. In addition, any methods and materials similar to or equal to the recorded content can be applied to the method of the present invention. The experimental methods for which specific conditions are not specified in the following examples are usually determined according to national standards. If there is no corresponding national standard, it is carried out according to the general international standards, conventional conditions, or according to the conditions recommended by the manufacturer. Unless otherwise defined or specified, all professional and scientific terms used herein have the same meaning as those familiar to those skilled in the art.
[0051] Example 1
[0052] Material ratio:
[0053] Component A:
[0054] Bio-based polymer (PLA): 50%
[0055] Plasticizer (citrate ester): 7%
[0056] Filler (cellulose): 15%
[0057] Natural fiber (bamboo fiber): 10%
[0058] Anti-aging agents (UV-531 and antioxidant 1010): 0.5% each
[0059] Component B:
[0060] Bio-based curing agent (soybean oil-based isocyanate): 90%
[0061] Catalyst (organic tin): 10%
[0062] Construction steps:
[0063] a. Site preparation: clean and level the ground.
[0064] b. Prefabrication: Prefabricate the composite materials in the factory.
[0065] c. Material transportation: transport prefabricated molding materials to the construction site.
[0066] d. Construction: Mix component A and component B in proportion at the construction site, and apply them evenly on the foundation of the court. The thickness of each coat is 3mm. Make sure that the previous coat is completely cured before proceeding to the next coat.
[0067] e. Laying and curing: It can be cured naturally in a low temperature environment, with a thickness of up to 9mm.
[0068] f. Topcoat construction: Apply anti-aging and anti-slip topcoat.
[0069] g. Line drawing construction: Line drawing construction shall be carried out after the topcoat has dried.
[0070] Example 2
[0071] Material ratio:
[0072] Component A:
[0073] Bio-based polymer (PLA): 45%
[0074] Plasticizer (citrate ester): 8%
[0075] Filler (cellulose): 12%
[0076] Natural fiber (bamboo fiber): 12%
[0077] Anti-aging agents (UV-531 and antioxidant 1010): 0.5% each
[0078] Component B:
[0079] Bio-based curing agent (soybean oil-based isocyanate): 95%
[0080] Catalyst (organic tin): 5%
[0081] The construction steps are similar to those in Example 1.
[0082] Example 3
[0083] Material ratio:
[0084] Component A:
[0085] Bio-based polymer (PLA): 48%
[0086] Plasticizer (citrate ester): 6%
[0087] Filler (cellulose): 14%
[0088] Natural fiber (bamboo fiber): 10%
[0089] Anti-aging agents (UV-531 and antioxidant 1010): 0.6% each
[0090] Component B:
[0091] Bio-based curing agent (soybean oil-based isocyanate): 92%
[0092] Catalyst (organic tin): 8%
[0093] The construction steps are similar to those in Example 1.
[0094] Example 4
[0095] Material ratio:
[0096] Component A:
[0097] Bio-based polymer (PLA): 46%
[0098] Plasticizer (citrate ester): 7%
[0099] Filler (cellulose): 13%
[0100] Natural fiber (bamboo fiber): 10%
[0101] Anti-aging agents (UV-531 and antioxidant 1010): 0.5% each
[0102] Component B:
[0103] Bio-based curing agent (soybean oil-based isocyanate): 93%
[0104] Catalyst (organic tin): 7%
[0105] The construction steps are similar to those in Example 1.
[0106] Table 1: According to relevant standards, the physical and mechanical properties and environmental protection of the products of the embodiments and comparative examples were tested, and the specific results are as follows:
[0107]
[0108]
[0109]
[0110] The physical and mechanical properties and environmental performance in Table 1 are tested according to GB 36246-2018 and GB / T 43565-2023 standards; the natural degradation performance test is based on ISO 14855 standard; the production process carbon emission test and non-renewable resource dependence test are based on ISO 14044 standard.
[0111] According to the content of Table 1, the following conclusions are drawn after analysis:
[0112] The bio-based degradable low-temperature construction basketball court floor composition of the present invention is superior to traditional petroleum-based materials in various physical and mechanical performance indicators. In particular, it shows significant advantages in impact absorption, vertical deformation, anti-skid, ball rebound, color fastness, tensile strength, elongation at break and flame retardancy. These excellent properties make the material of the present invention have significant technical advantages and market competitiveness in practical applications. In addition, the material of the present invention can be naturally degraded after the end of its service life, meets environmental protection requirements, and has important environmental protection significance.
[0113] The environmental performance of Examples 1 to 4 is significantly better than that of Comparative Examples 1 to 4. This is because the materials used in the Examples are bio-based degradable materials, while the materials used in the Comparative Examples are traditional petroleum-based materials. Bio-based materials can be naturally degraded after the end of their service life and are environmentally friendly, while traditional petroleum-based materials are difficult to degrade and will cause environmental pollution after being discarded.
[0114] The VOC (volatile organic compound) emissions of Examples 1 to 4 are relatively low, while the VOC emissions of Comparative Examples 1 to 4 are relatively high. This indicates that the material of the present invention causes less air pollution during use, which is beneficial to environmental protection and human health.
[0115] The materials of Examples 1 to 4 can be naturally degraded after their service life ends, reducing the pollution to soil and water sources, and meeting the current requirements of environmental protection and sustainable development. The materials of Comparative Examples 1 to 4 are difficult to degrade, and exist in the natural environment for a long time after being discarded, causing environmental pollution.
[0116] The carbon emissions during the production process of Examples 1 to 4 are relatively low, while the carbon emissions during the production process of Comparative Examples 1 to 4 are relatively high. This is because the production process of bio-based materials consumes less energy and has lower carbon emissions, while the production process of petroleum-based materials consumes a lot of energy and produces a lot of greenhouse gases.
[0117] Examples 1 to 4 have a lower reliance on non-renewable resources, while Comparative Examples 1 to 4 have a higher reliance on non-renewable resources. Bio-based materials are mainly derived from renewable resources, such as plants, while petroleum-based materials are mainly derived from non-renewable petroleum resources.
[0118] In summary, the bio-based degradable low-temperature construction basketball court floor composition of the present invention has significant advantages in environmental performance, can effectively reduce environmental pollution, and meets the needs of sustainable development. These excellent environmental performances make the material of the present invention have important practical significance and market value in practical applications.
[0119] The creativity, novelty and practicality of the present invention are summarized as follows:
[0120] creativity
[0121] Application of bio-based polymers: This invention is the first to apply bio-based polymers (such as polylactic acid PLA) to basketball court floor materials, replacing traditional petroleum-based materials, significantly improving the environmental performance of the materials. Bio-based materials have good biodegradability and can be naturally degraded after the end of their service life, reducing pollution to the environment.
[0122] Low-temperature construction capability: By optimizing the material formula and construction process, the material of the present invention can still maintain good fluidity and curing speed in a low-temperature environment of -10°C to 10°C, ensuring construction quality and efficiency, and overcoming the problem of difficulty in construction of traditional petroleum-based materials in low-temperature environments.
[0123] Comprehensive performance optimization: The present invention adds natural fibers (such as bamboo fibers) and anti-aging additives (such as UV absorbers and antioxidants) to the material formula, which significantly improves the physical and mechanical properties of the material, including impact absorption rate, vertical deformation, anti-slip performance, ball rebound rate, color fastness, tensile strength, elongation at break and flame retardancy. The comprehensive performance is better than that of traditional materials.
[0124] Novelty
[0125] Innovative use of environmentally friendly materials: The present invention uses environmentally friendly materials such as bio-based polymers, natural fibers and degradable plasticizers to creatively provide a basketball court floor composition that meets current environmental protection and sustainable development needs. The selection and combination of these materials have not been reported in the prior art, reflecting the uniqueness and novelty of the present invention.
[0126] Adaptability to low temperature environment: The material of the present invention has outstanding low temperature construction performance and can be constructed in a low temperature environment of -10°C to 10°C, ensuring construction quality and efficiency. This low temperature construction capability is difficult to achieve in existing petroleum-based materials, reflecting the technical innovation of the present invention.
[0127] Comprehensive improvement of comprehensive performance: The present invention achieves comprehensive improvement of multiple physical and mechanical properties through optimization of material formula, including high impact absorption rate, high ball rebound rate, excellent anti-slip performance and high tensile strength, etc. This performance optimization is difficult to achieve simultaneously in traditional materials, which reflects the unique advantages of the present invention.
[0128] Practicality
[0129] Significant environmental benefits: The bio-based materials used in the present invention can be naturally degraded after the end of their service life, reducing pollution to soil and water sources and meeting environmental protection requirements. At the same time, the production process of the materials has low carbon emissions, reducing greenhouse gas emissions, and has significant environmental protection benefits.
[0130] Strong construction convenience: The material of the present invention can still maintain good fluidity and curing speed in a low temperature environment, and the construction is not limited by seasons and weather conditions, and is particularly suitable for construction in cold areas and in winter. In addition, the construction method has been optimized to improve the construction efficiency and quality, and is convenient for practical operation and application.
[0131] Excellent comprehensive performance: The comprehensive performance of the material of the present invention is significantly better than that of traditional petroleum-based materials, including high impact absorption rate, excellent anti-slip performance, high ball rebound rate and excellent color fastness, etc. It can provide better sports experience and safety guarantee, and is suitable for the construction and renovation of various basketball courts.
[0132] To sum up, the patent of this invention has significant advantages in creativity, novelty and practicality, and has important technological innovation significance and application value.
[0133] Those skilled in the art should recognize that the above embodiments are only used to illustrate the present application, and are not intended to limit the present application. As long as they are within the spirit of the present application, any changes or modifications to the above embodiments will fall within the scope of the claims of the present application.
Claims
1. A bio-based degradable low-temperature construction basketball court floor composition, characterized in that: The invention comprises the following components and preparation process: Component A: Bio-based polymers 40%-60%, such as polylactic acid (PLA) Plasticizer 5%-10%, such as citrate ester Filler 10%-20%, such as cellulose Natural fiber 5%-15%, such as bamboo fiber Anti-aging additives 0.5%-1%, such as UV absorbers and antioxidants Preparation process: Add bio-based polymers, plasticizers, fillers, natural fibers and anti-aging additives into a mixing device in proportion, stir evenly with a high-speed stirrer, and degas to remove bubbles generated during the mixing process. Component B: Bio-based curing agents 90%-99%, such as soybean oil-based isocyanates Catalyst 1%-10%, such as organotin catalyst Preparation process: Add the bio-based curing agent, catalyst and solvent into the mixing tank in proportion and stir evenly with a low-speed agitator to ensure uniform mixing.
2. The composition according to claim 1, characterized in that The bio-based polymer is polylactic acid (PLA).
3. The composition according to claim 1, characterized in that The degradable plasticizer is citrate.
4. The composition according to claim 1, characterized in that It also includes one or more anti-aging aids, which include ultraviolet absorbers and antioxidants. The ultraviolet absorber is UV-531, and the antioxidant is antioxidant 1010.
5. The composition according to claim 1, characterized in that Also included are natural fiber reinforcement materials, which are cellulose and bamboo fibers.
6. A low-temperature construction method for basketball court flooring, characterized in that: The following steps are involved: 1) Site preparation: clean up the debris on the surface of the site and ensure that the ground is flat and dry. 2) Preparation of composition (adhesive): Component A and component B are prepared separately in a professional factory, wherein component A includes a bio-based polymer, a plasticizer, a filler and an additive, and component B includes a bio-based curing agent, a catalyst and a solvent. 3) Material transportation: transport the prefabricated floor material composition to the construction site. 4) At the construction site, mix component A and component B in proportion and stir evenly, then apply them evenly on the foundation of the court. The thickness of each application is 3mm. Before the next application, the material of the previous application must be completely cured. 5) Laying and curing: Natural curing in low temperature environment to ensure construction quality. The laying thickness should meet the following requirements: average thickness ≥ 9mm 6) Topcoat construction: After the floor material solidifies, apply anti-aging and anti-slip topcoat to improve the durability and safety of the floor. 7) Line drawing construction: After the topcoat is completely dry, carry out line drawing construction on the basketball court to ensure that the lines are clear and durable.
7. The construction method according to claim 6, characterized in that: The construction environment temperature ranges from -10°C to 10°C.
8. The construction method according to claim 6, characterized in that: The weight ratio of component A to component B when mixed and stirred during construction is A:B=2:
1.
9. The composition according to claim 1, characterized in that The site after the composition is applied has the following properties: Impact absorption rate between 20%-50% The vertical deformation is between 0.6mm-3.0mm The anti-slip value is between 90-110BPN (dry test) Ball rebound rate ≥ 95% Color fastness ≥ No fading under both dry and wet conditions Tensile strength ≥0.7MPa Elongation at break ≥90% Flame retardancy reaches first-class standard Through the detailed description of the above claims, the present invention clearly defines the technical features and protection scope of the bio-based degradable basketball court floor composition and its low-temperature construction method, ensuring the originality and practicality of the invention.
Citation Information
Cited By
Bio-based thermoplastic prefabricated buffer layer and preparation method and application thereof
CN119391168A