Cationic thermocuring ink composition and preparation method thereof
Through the reaction of epoxy resin with cationic initiator and the coordination of nano core-shell rubber, the shortcomings of existing thermally cured inks in terms of ultraviolet resistance, water resistance and heat resistance are solved, and high-performance cationic thermally cured inks are achieved. It solves the problems of environmental pollution and safety hazards and is suitable for the high-demand home appliance and furniture industry.
Patent Information
- Application Number
- CN202411276638.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-11-19
AI Technical Summary
The existing thermal curing inks have shortcomings in UV resistance, water resistance and heat resistance, and the solvent-based epoxy amine system causes environmental pollution and safety hazards, making it difficult to meet the high requirements of the home appliance and furniture industry.
Using the epoxy-cationic curing agent scheme, the reaction of epoxy resin and latent cationic initiator can achieve full-solid solvent-free curing, combined with nano core-shell rubber and specific resin to form a high-performance cationic thermal curing ink composition, with Excellent adhesion, heat resistance, boiling resistance and UV resistance.
Achieve green and environmentally friendly ink curing, reduces curing shrinkage, improves adhesion and surface hardness, has excellent UV resistance, temperature and UV resistance, is suitable for inorganic substrates such as glass, and expands ink in furniture and appliances. and the application of the photovoltaic industry.
Smart Images

Figure BDA0005040386430000021 
Figure BDA0005040386430000031 
Figure BDA0005040386430000091
Abstract
Description
Technical Field
[0001] This invention belongs to the field of coating and ink technology, and particularly relates to a cationic thermosetting ink composition and its preparation method. Background Technology
[0002] As a type of coating that protects the substrate, ink plays an important role in decoration and beautification. The UV resistance, water resistance, and heat resistance of ink are crucial performance indicators. With the continuous improvement of people's living standards, the requirements for ink are constantly increasing, thus creating an urgent need for inks with excellent resistance to UV yellowing, water resistance, and heat resistance.
[0003] Currently, most thermosetting inks use solvent-based epoxy amine systems. During use, the solvent needs to be dried, which can cause serious environmental pollution and safety hazards to production workers. At the same time, the cured products have poor resistance to temperature and UV yellowing, making it difficult to meet the current requirements of the home appliance and furniture industry for weather resistance and temperature resistance.
[0004] Therefore, there is a need for a cationic thermosetting system composition with low shrinkage, excellent adhesion (to inorganic substrates such as glass), and resistance to damp heat and boiling water, for use in the furniture, home appliance and photovoltaic industries. Summary of the Invention
[0005] To address the shortcomings of the prior art, this invention provides a cationic thermosetting ink composition and its preparation method, the specific technical solution of which is as follows:
[0006] The first objective of this invention is to provide a cationic thermosetting ink composition comprising component A and component B.
[0007] Component A comprises the following components in parts by weight:
[0008] 40-80 parts epoxy resin, 10-30 parts toughening agent, 10-30 parts diluent, 10-70 parts filler, 0.5-5 parts coupling agent, and 0-5 parts additives;
[0009] Component B comprises the following components in parts by weight:
[0010] 0.2-5 parts of latent cationic initiator, 0.2-100 parts of initiator diluent;
[0011] The mass ratio of component A to component B is 100:5-20.
[0012] The advantages of the above technical solution are that the present invention adopts an epoxy-cationic curing agent solution, which utilizes the epoxy groups in the epoxy resin structure to react with the cationic initiator to complete the curing. It is a completely solid solvent-free composition that is green and environmentally friendly. At the same time, the curing reaction is not affected by oxygen, the curing shrinkage rate is small, there is a dark reaction, and it has excellent adhesion and surface hardness, outstanding water resistance and acid and alkali resistance, and excellent resistance to ultraviolet yellowing and temperature yellowing.
[0013] The composition of this invention can be cured within 10 minutes at 160-180℃. The cured ink has excellent adhesion properties, exhibiting excellent adhesion to inorganic substrates such as glass (5B in cross-cut adhesion test); it also has excellent resistance to damp heat and boiling water, with 5B adhesion after boiling in water at 100℃ for 2 hours, 5B adhesion after damp heat at 85℃ / 85%RH for 500 hours, 5B adhesion after immersion in 5% NaOH for 24 hours, and 5B adhesion after immersion in 5% HCl for 24 hours; no significant color change after 1 hour of temperature aging at 180℃ (Δb<1); and Δb<2 after 400 hours of UV aging.
[0014] Furthermore, the epoxy resin is a variety of alicyclic epoxy resin, modified alicyclic epoxy resin, hydrogenated bisphenol A type epoxy resin, bisphenol A type epoxy resin, and bisphenol F type epoxy resin.
[0015] Furthermore, the alicyclic epoxy resin is one or more of the following resins:
[0016]
[0017]
[0018] Furthermore, the modified alicyclic epoxy resin is a dihydroxy alcohol-modified alicyclic epoxy resin or a fatty acid-modified alicyclic epoxy resin, such as DE1701, DE1601, and DE1801 from Yantai Donghua New Materials Co., Ltd.
[0019] Further, the toughening agent includes toughening agent B1 and toughening agent B2, wherein, by weight, toughening agent B1 is 5-30 parts and toughening agent B2 is 0-15 parts; the epoxy toughening agent B1 is a glycidyl ether or glycidyl ester toughening agent; and the toughening agent B2 is a nano-core-shell rubber.
[0020] The advantages of the above-mentioned further solutions are that the toughening agent B1 of the present invention is an epoxy resin containing flexible segments such as ether bonds and long carbon chains, and the terminal epoxy groups participate in the cross-linking reaction, introducing the flexible segments in the molecular structure into the polymer backbone structure to provide toughness; the outer shell of the toughening agent B2 nano-core-shell rubber is an epoxy resin layer, which improves the compatibility and dispersibility between the nano-core-shell rubber and the epoxy resin matrix, and at the same time participates in the reaction, and has excellent adhesion at the interface of the co-curing system; the inner core layer is a rubber elastomer with a low glass transition temperature and excellent toughness; the nano-core-shell rubber, as the stress concentration center, can work together with the core and shell when subjected to external force to absorb more energy and enhance the crack resistance and impact resistance of the material.
[0021] Further, the toughening agent B1 is one or more of the following: cyclohexane-1,2-dicarboxylic acid diglycidyl ester, adipic acid diglycidyl ester, 3-ethyl-3-oxabutane, 3,3'-[oxybis(methylene)]bis[3-ethyl]oxabutane, ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, dipropylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, butanediol diglycidyl ether, epoxidized soybean oil, neopentyl glycol diglycidyl ether, hydrogenated bisphenol A diglycidyl ether, hexanediol diglycidyl ether, cyclohexanediol diglycidyl ether, cyclohexanediol diglycidyl ether, and C16 to C16 tetradecyl diglycidyl ether.
[0022] Furthermore, the core layer of the toughening agent B2 is a rubber elastomer, and the outer shell layer is an epoxy resin. The rubber elastomer is polybutadiene rubber, nitrile rubber, or silicone rubber; the epoxy resin of the outer shell layer is an alicyclic epoxy resin, bisphenol A type epoxy resin, or bisphenol F type epoxy resin.
[0023] Furthermore, the diluent is one or more of polyols, hydroxyl-terminated acrylates, hydroxyl-terminated vinyl ethers, or oxetanes.
[0024] Furthermore, the polyols include propylene glycol, butanediol, hexanediol, polypropylene glycol, polyethylene glycol, polytetrahydrofuranol, polycaprolactone, hydroxyl-terminated polyester, polycarbonate diol, polyether polyol, modified castor oil diol, diethylene glycol, etc.
[0025] Furthermore, the filler is mainly white or black, with the white filler being titanium dioxide and the black filler being carbon black.
[0026] Furthermore, the coupling agent is one or more of the following: epoxy phosphate coupling agents, silane coupling agents, titanate coupling agents, aluminate coupling agents, and aluminum-titanium composite coupling agents.
[0027] Furthermore, the additives include wetting and leveling agents, defoamers, thixotropic agents, pigments, ultraviolet absorbers, etc.
[0028] Furthermore, the latent thermal cation initiator is one or more of the following: hexafluoroantimonic acid blocked ammonium salt, hexafluorophosphate blocked ammonium salt, hexafluorophosphate blocked thioonium salt, hexafluoroantimonic acid blocked thioonium salt, trifluorosulfonic acid blocked ammonium salt, and pentafluorophenylboronic acid blocked ammonium salt.
[0029] Furthermore, the initiator diluent is one or more of propylene carbonate, butyrolactone, alcohols, and hydroxyl-terminated diluents.
[0030] A second objective of this invention is to provide a method for preparing the above-mentioned cationic thermosetting ink composition, comprising the following steps:
[0031] (1) Heat and mix the epoxy resin, diluent, toughening agent, coupling agent and additives in component A until homogeneous;
[0032] (2) Add the uniformly mixed material from step (1) to the filler and grind it thoroughly on a grinder until the fineness is less than 5μm for later use;
[0033] (3) At room temperature, the latent cationic initiator of component B is stirred and dissolved in the diluent until it is colorless and transparent to obtain a mixed solution;
[0034] (4) Mix the material ground in step (2) and the mixed solution in step (3) evenly to obtain a cationic thermosetting ink composition.
[0035] The beneficial effects of this invention are as follows:
[0036] The cationic thermosetting ink composition of this invention differs from the commonly used epoxy amine solvent system or acrylate photothermal curing system. It adopts a thermosetting method, which results in a high degree of resin reaction and full release of reaction stress, leading to superior mechanical properties and adhesion, without cracking or blistering. Furthermore, thermosetting is not limited by film thickness or light exposure, and can be used for deep curing of irregular structures and high pigment and filler systems, greatly expanding its application fields.
[0037] The main component of the cationic thermosetting ink composition of the present invention is an alicyclic epoxy resin without benzene ring structure, which has the advantages of low color, excellent yellowing resistance, high crosslinking density, and high mechanical strength. Furthermore, the epoxy resin curing agent is a highly active latent thermocation initiator, which has good compatibility with alicyclic epoxy resin, requires a small amount, reacts quickly, has excellent comprehensive performance, and has high production line efficiency.
[0038] The cationic thermosetting ink composition of the present invention, through formulation combination, enables the coating to form a denser and high-performance cross-linked network, with excellent properties such as high opacity, high hardness, high adhesion, water resistance, and yellowing resistance. Attached Figure Description
[0039] Figure 1 The image shows the water resistance test results of the cured composition of Example 1 of the present invention.
[0040] Left: Adhesion of cured white ink after boiling is 5B; Right: Adhesion of cured black ink after boiling is 5B.
[0041] Figure 2 The figures show the cured composition of Example 1 and the results of the temperature resistance yellowing test of Comparative Example 1.
[0042] Left: Example 1; Right: Comparative Example 1;
[0043] Figure 3 The images show the cured composition of Example 1 and the UV yellowing resistance test results of Comparative Example 1.
[0044] Left: Example 1, Right: Comparative Example 1. Detailed Implementation
[0045] The principles and features of the present invention are described below with reference to embodiments. The examples given are only for explaining the present invention and are not intended to limit the scope of the present invention.
[0046] Example 1:
[0047] A cationic thermosetting ink, comprising component A and component B:
[0048] Component A: 60 parts of 3,4-epoxycyclohexylcarboxylic acid-3',4'-epoxycyclohexylmethyl ester modified epoxy resin (Yantai Donghua New Material Co., Ltd., DE1701), 10 parts of hydrogenated bisphenol A type epoxy resin, 10 parts of polyether polyol HM210, 10 parts of toughening agent B1 epoxidized soybean oil, 5 parts of toughening agent B2 nano-core-shell rubber Zhongyuan MX154, 5 parts of diluent polytetrahydrofuran alcohol, 2 parts of silane coupling agent KH-560, 1.3 parts of additives (0.5 parts of defoamer BYK A530, 0.3 parts of leveling agent BYK333, 0.5 parts of wetting and dispersing agent BYK W903); 60 parts of titanium dioxide filler;
[0049] Heat the epoxy resin, diluent, toughening agent, coupling agent and additives in component A to 80°C and mix them evenly. Then add the filler and grind them thoroughly on a ceramic three-roll mill until the fineness is less than 5μm for later use.
[0050] Component B: 1 part of latent cationic initiator blocked ammonium hexafluoroantimony salt (Yantai Donghua New Materials Co., Ltd., DH081), 9 parts of initiator diluent propylene carbonate;
[0051] At room temperature, the latent cationic initiator of component B is dissolved in initiator diluent by stirring until it becomes colorless and transparent, thus obtaining a mixed solution;
[0052] The ground components A and B were mixed evenly in a mass ratio of 100:10 to obtain a cationic thermosetting ink composition, which was then cured in an oven at 180°C for 8 minutes to obtain cured white ink.
[0053] In addition, the titanium dioxide filler in Example 1 was replaced with 15.5 parts of carbon black, and cured to obtain cured black ink.
[0054] Example 2:
[0055] A cationic thermosetting ink, comprising component A and component B:
[0056] Component A: 40 parts of 3,4-epoxycyclohexylcarboxylic acid-3',4'-epoxycyclohexylmethyl ester modified epoxy resin (Yantai Donghua New Materials Co., Ltd., DE021E), 20 parts of 3,4-epoxycyclohexylcarboxylic acid-3',4'-epoxycyclohexylmethyl ester modified epoxy resin (Yantai Donghua New Materials Co., Ltd., DE1701), 10 parts of solid bisphenol A epoxy resin E20, 5 parts of poly[(2-epoxyethylene)-1,2-cyclohexanediol]2-ethyl-2-(hydroxymethyl)-1,3-propanediol ether epoxy resin (structural formula 2, Nantong Xinnaxi S-51), 5 parts of polypropylene glycol diglycidyl ether, 5 parts of diluent diethylene glycol, 5 parts of diluent polypropylene glycol, 3 parts of silane coupling agent KH-560, 1.3 parts of additives (0.5 parts of defoamer BYK). A530, 0.3 parts leveling agent BYK333, 0.5 parts wetting and dispersing agent BYK W903, 55 parts titanium dioxide filler;
[0057] Heat the epoxy resin, diluent, toughening agent, coupling agent and additives in component A to 80°C and mix them evenly. Then add the filler and grind them thoroughly on a ceramic three-roll mill until the fineness is less than 5μm for later use.
[0058] Component B: 1 part of latent cationic initiator blocked ammonium hexafluoroantimony salt (Yantai Donghua New Materials Co., Ltd., DH080), 4 parts of initiator diluent propylene carbonate;
[0059] At room temperature, the latent cationic initiator of component B is dissolved in initiator diluent by stirring until it becomes colorless and transparent, thus obtaining a mixed solution;
[0060] The ground components A and B were mixed evenly in a mass ratio of 100:5 to obtain a cationic thermosetting ink composition, which was then cured in an oven at 180°C for 8 minutes to obtain cured white ink.
[0061] Comparative Example 1:
[0062] A commercially available thermosetting ink, comprising agent A and agent B:
[0063] Agent A Model: DK-105G
[0064] Agent B, Model: DK-08
[0065] Manufacturer: Dick Printing Materials (Jiangmen) Co., Ltd.;
[0066] Mix agent A and agent B in a mass ratio of 100:10 and cure in an oven at 180℃ for 8 minutes to obtain cured white ink.
[0067] Comparative Example 2:
[0068] Component A: 75 parts 3,4-epoxycyclohexylcarboxylic acid-3',4'-epoxycyclohexylmethyl ester (Yantai Donghua New Material Co., Ltd., DE021E), 15 parts oxetane (Nantong Xinnaxi S-101), 10 parts nano-core-shell rubber Zhongyuan MX154, 0.5 parts BYK A530, 0.3 parts BYK333, 60 parts titanium dioxide filler;
[0069] Grind the above component A thoroughly on a ceramic three-roll mill until the fineness is less than 5μm for later use;
[0070] Component B: 1 part blocked ammonium hexafluoroantimony salt (Yantai Donghua New Materials Co., Ltd., DH080), 9 parts propylene carbonate;
[0071] Mix component A and component B in a mass ratio of 100:10 and cure in an oven at 180°C for 8 minutes to obtain cured white ink.
[0072] Performance testing
[0073] Adhesion test: cross-cut adhesion test, substrate: glass sheet, test standard GB / T 9286-2021;
[0074] Acid resistance test: Adhesion is tested after soaking in 5% NaOH at 25℃ for 24 hours, according to the test standard GB / T9286-2021;
[0075] Alkali resistance test: Adhesion is tested after soaking in 5% HCl at 25℃ for 24 hours, according to the test standard GB / T9286-2021.
[0076] Water resistance: Adhesion was tested after boiling water at 100℃ for 2 hours, according to the test standard GB / T 9286-2021;
[0077] Moisture and heat resistance: Adhesion was tested after treatment at 85℃ / 85%RH for 500 hours, according to test standard GB / T9286-2021;
[0078] UV aging resistance test: QUV, ASTM G154 Cycle1, perform colorimetric Lab test, and calculate Δb;
[0079] Heat resistance aging test: Oven temperature 180℃ for 1 hour, colorimetric Lab test was performed, and Δb was calculated;
[0080] Colorimetric testing: Testing equipment: HunterLab Ultrascan VIS; Testing method: Reflectance method;
[0081] Hardness test: Pencil hardness tester, test standard GB / T 6730-2006.
[0082] The performance test results of the cured white inks obtained in Examples 1-2 and Comparative Examples 1-2 are shown in Table 1.
[0083] Table 1. Performance test results of cured white ink obtained from the examples and comparative examples.
[0084]
[0085] The experimental results show that, after curing, the white ink prepared by adding titanium dioxide filler in Example 1 and the black ink prepared by replacing titanium dioxide filler with carbon black are as follows: Figure 1 As shown, it exhibits excellent glass adhesion and water resistance; after boiling in water for 2 hours, there is no color change, no bubbling, and no peeling. Furthermore, its adhesion in the cross-cut adhesion test is 5B. The thermosetting white ink prepared according to Example 1 demonstrates excellent resistance to yellowing; after baking at 180 degrees Celsius for 1 hour, there is no color change, while Comparative Example 1 (commercially available product) shows obvious yellowing visible to the naked eye. Figure 2 As shown; after 400 hours of QUV aging, Comparative Example 1 (commercially available product) exhibited significant yellowing, while the thermosetting white ink prepared in Example 1 showed virtually no color change, demonstrating excellent resistance to UV yellowing. Figure 3 As shown.
[0086] Compared to the conventional thermosetting ink of Comparative Example 1 (commercially available product), the cationic system inks of Examples and Comparative Example 2 have excellent heat resistance and UV resistance to yellowing, and the formulation is all-solid and environmentally friendly. At the same time, through the combination of different resins, toughening agents and diluents, Examples have adhesion and water resistance, acid and alkali resistance comparable to Comparative Example 1 (commercially available product) compared to Comparative Example 2.
[0087] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A cationic thermosetting ink composition, It is characterized in that It includes component A and component B. Component A includes the following components in parts by weight: Epoxy resin 40-80 parts, toughening agent 10-30 parts, diluent 10-30 parts, filler 10-70 parts, coupling agent 0.5-5 parts, auxiliary agent 0-5 parts; Component B includes the following components in parts by weight: 0.2-5 parts of latent cationic initiator, 0.2-100 parts of initiator diluent; The mass ratio of component A to component B is 100:5-20.
2. The cationic thermosetting ink composition according to claim 1, It is characterized in that The epoxy resin is two or more of alicyclic epoxy resin, modified alicyclic epoxy resin, hydrogenated bisphenol A epoxy resin, bisphenol A epoxy resin and bisphenol F epoxy resin.
3. The cationic heat curable ink composition according to claim 2, It is characterized in that The alicyclic epoxy resin is one or more of the following resins:
4. The cationic heat curable ink composition according to claim 2, It is characterized in that The modified alicyclic epoxy resin is a divalent fatty alcohol modified alicyclic epoxy resin or a fatty acid modified alicyclic epoxy resin.
5. The cationic thermosetting ink composition according to claim 1, It is characterized in that The toughening agent comprises a toughening agent B1 and a toughening agent B2. In parts by weight, the toughening agent B1 is 5-30 parts, and the toughening agent B2 is 0-15 parts. The epoxy toughening agent B1 is a glycidyl ether or glycidyl ester toughening agent. The toughening agent B2 is a nano core-shell rubber.
6. The cationic thermosetting ink composition according to claim 1, It is characterized in that The diluent is one or more of polyols, terminal hydroxyl acrylates, terminal hydroxyl vinyl ethers or oxetanes.
7. The cationic thermosetting ink composition according to claim 1, It is characterized in that The filler is mainly a white filler or a black filler; the coupling agent is one or more of an epoxy phosphate coupling agent, a silane coupling agent, a titanate coupling agent, an aluminate coupling agent and an aluminum-titanium composite coupling agent.
8. The cationic thermosetting ink composition according to claim 1, It is characterized in that The latent cationic initiator is one or more of hexafluoroantimonate blocked ammonium salt, hexafluorophosphate blocked ammonium salt, hexafluorophosphate blocked sulfonium salt, hexafluoroantimonate blocked sulfonium salt, trifluorosulfonic acid blocked ammonium salt, and pentafluorophenylboric acid blocked ammonium salt.
9. The cationic thermosetting ink composition according to claim 1, It is characterized in that The initiator diluent is one or more of propylene carbonate, butyrolactone, alcohols and terminal hydroxyl structure diluents.
10. A method for preparing the cationic thermosetting ink composition according to any one of claims 1 to 9, It is characterized in that The steps include: (1) heating and mixing the epoxy resin, diluent, toughening agent, coupling agent and auxiliary agent in component A and stirring them uniformly; (2) adding fillers to the uniformly mixed materials in step (1), and grinding them on a grinder until the fineness is less than 5 μm for later use; (3) At room temperature, the latent cationic initiator of component B is dissolved in the initiator diluent by stirring until it becomes colorless and transparent to obtain a mixed solution; (4) The ground material of step (2) and the mixed solution of step (3) are mixed evenly to obtain a cationic thermosetting ink composition.
Citation Information
Cited By
Alicyclic epoxy resin system full-solid-content white codine, and preparation method and application of alicyclic epoxy resin system full-solid-content white codine
CN121045511A