Anti-flooding and anti-floating two-component gray coating and preparation method thereof

By using specific dispersant and leveling agent systems in the paint, the floating color and flowering problem in gray paint is solved, and the effective solution to the static floating color, paint film floating color and paint film flowering in the can is achieved, ensuring the coating is carried out. Color uniformity and stability of the layer.

CN118978850AInactive Publication Date: 2024-11-19HUNAN AEROSPACE SANFENG SCI & TECH CO LTD

Patent Information

Application Number
CN202411011075.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Gray acrylic polyurethane coatings are prone to floating color and flowering during application. The existing technology is difficult to solve the problems of static floating color, paint film floating color and paint film flowering in the can at the same time.

Method used

Using two-component gray coatings, including components A and B, polyurethane polymer dispersants, high molecular weight unsaturated carboxylic acid dispersants, fluorocarbon modified polymer leveling agents and organics Modify the silicone leveling agent to control the mass ratio of the dispersant and the leveling agent to form an effective dispersion system to solve the problem of floating color and flowering.

Benefits of technology

It effectively solves the problems of static floating color, floating color of paint film and flowering in the can, ensuring the color uniformity and stability of the coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004964371030000061
    Figure BDA0004964371030000061
  • Figure BDA0004964371030000071
    Figure BDA0004964371030000071
  • Figure BDA0004964371030000072
    Figure BDA0004964371030000072
Patent Text Reader

Abstract

The invention discloses an anti-flooding and anti-floating two-component gray coating and a preparation method thereof, and belongs to the technical field of coatings, the anti-flooding and anti-floating two-component gray coating comprises a component A and a component B, the component A is prepared from the following components in parts by mass: 40 to 70 parts of hydroxy acrylic resin, 0.4 to 3.5 parts of dispersing agent, 0.3 to 1.2 parts of organic modified bentonite, 5 to 25 parts of barium sulfate, 5 to 25 parts of titanium dioxide, 0.2 to 2 parts of carbon black, 3 to 15 parts of xylene, 3 to 15 parts of butyl acetate, 3 to 15 parts of propylene glycol methyl ether acetate, 0.01 to 0.08 part of drier, 0.1 to 1 part of defoaming agent and 0.2 to 3 parts of flatting agent; by adopting the polyurethane high polymer dispersing agent, the high molecular weight unsaturated carboxylic acid dispersing agent, the specific fluorocarbon modified polymer leveling agent and the organic modified organic silicon leveling agent system, the problems of static flooding in a tank, flooding of a paint film and floating of the paint film are effectively solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coatings, and in particular to a two-component grey coating capable of preventing floating color and blurring, and a preparation method thereof. Background Art

[0002] Among industrial coatings, acrylic polyurethane coatings are widely used due to their excellent weather resistance, chemical resistance and mechanical properties. However, gray acrylic polyurethane coatings are prone to floating color and floating during application, that is, the surface color of the coating is uneven after drying, and stripes, spots or color differences appear, which affects the appearance of the coating and the stability of production. In the prior art, although the floating color and floating can be reduced to a certain extent by adjusting the type and amount of pigments and optimizing the coating formula, it is still difficult to completely solve this problem.

[0003] There are two main types of floating color: 1. Static floating color in the can: The paint is evenly dispersed and left in the storage tank for a period of time. One or more pigments in the paint can separate and float on the surface. This phenomenon is called static floating color in the can; 2. Dynamic floating color in the coating film: The phenomenon of pigment particles separating during the drying process of the coating film is called dynamic floating color. There are two types of pigment separation in dynamic floating color: Floating color in the coating film: The surface color of the coating film is uniform, but there is a difference between the surface and the bottom layer. Use fingers to rub and spread to identify the floating color. Floating in the coating film: The surface color of the coating film is uneven. In the existing paint production, many ways to prevent floating color and floating are to adjust the color-to-base ratio, the type of pigment, and the use of dispersants, but it is difficult to effectively solve static floating color in the can, floating color in the paint film, and floating in the paint film at the same time.

[0004] In view of this, this application is filed. Summary of the invention

[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a two-component gray paint with anti-floating color and floating, which solves the problems of static floating color in the can, paint film floating color and paint film floating.

[0006] To achieve the above object, the technical solution adopted by the present invention is:

[0007] A two-component grey paint for preventing floating and blooming, comprising component A and component B;

[0008] The component A comprises the following components in parts by weight: 40 to 70 parts of hydroxy acrylic resin, 0.4 to 3.5 parts of dispersant, 0.3 to 1.2 parts of organic modified bentonite, 5 to 25 parts of barium sulfate, 5 to 25 parts of titanium dioxide, 0.2 to 2 parts of carbon black, 3 to 15 parts of xylene, 3 to 15 parts of butyl acetate, 3 to 15 parts of propylene glycol methyl ether acetate, 0.01 to 0.08 parts of drying agent, 0.1 to 1 parts of defoaming agent, and 0.2 to 3 parts of leveling agent;

[0009] The B component includes the following components in parts by weight: 40 to 80 parts of isocyanate, 10 to 20 parts of xylene, and 10 to 20 parts of butyl acetate;

[0010] The dispersant comprises a polyurethane polymer dispersant and a high molecular weight unsaturated carboxylic acid dispersant, and the mass ratio of the polyurethane polymer dispersant to the high molecular weight unsaturated carboxylic acid dispersant is (0.3-1.5): (0.1-2).

[0011] The present invention combines the above-mentioned various raw materials in a specific ratio, and solves the floating color and floating problem from three aspects of static floating color in the can, floating color of the paint film, and floating color of the paint film through the interaction of the various raw materials under the specific gray paint system.

[0012] The inventors of the present invention have found that, in the specific system of the gray coating, hydroxyl acrylic resin and pigment filler of the present invention, the dispersant is the key to solving the problem of floating color and floating. The present invention adopts a polyurethane polymer dispersant and a high molecular weight unsaturated carboxylic acid dispersant and a specific fluorocarbon modified polymer leveling agent and an organic modified silicone leveling agent system, and controls the mass ratio of the dispersant and the leveling agent to meet the scope of the present invention, thereby effectively solving the problems of static floating color in the tank, floating color of the paint film and floating of the paint film.

[0013] As a preferred embodiment of the present invention, the mass ratio of the polyurethane polymer dispersant to the high molecular weight unsaturated carboxylic acid dispersant is (0.8-1.2):(0.5-0.7).

[0014] As a preferred embodiment of the present invention, the polyurethane polymer dispersant includes at least one of BYK-163, EFKA-4010, BYK-161, EFKA-4310, Disponer 9850, and AFCONE-4071.

[0015] As a preferred embodiment of the present invention, the high molecular weight unsaturated carboxylic acid dispersant includes at least one of BYK-104, EFKA-5066, and Disponer 904S.

[0016] As a preferred embodiment of the present invention, the hydroxy acrylic resin includes at least one of Nupes Setalux 1753, Sanwang SWU3625, Dongsheng ESB-2050, Sanwang 6167, and Tongde 1011.

[0017] As a preferred embodiment of the present invention, the leveling agent includes a fluorocarbon modified polymer leveling agent and an organic modified silicone leveling agent; the mass ratio of the fluorocarbon modified polymer leveling agent to the organic modified silicone leveling agent is (0.1-1): (0.1-2).

[0018] As a preferred embodiment of the present invention, the fluorocarbon modified polymer leveling agent includes at least one of Sago-3882 leveling agent, VOK-FLOW 376S leveling agent, and EFKA-3777 leveling agent; and / or

[0019] The organic modified silicone leveling agent includes at least one of BYK-333, BYK-310, TEGO-435, Levaslip836, and Coatosil 2820.

[0020] As a preferred embodiment of the present invention, the organic modified bentonite includes at least one of Bentone 27, Bentone 38, and BYK-CLAYTONE-APA;

[0021] The particle size of the barium sulfate is 1000-1500 meshes.

[0022] As a preferred embodiment of the present invention, the titanium dioxide is at least one of Ishihara R930 titanium dioxide, DuPont 902 titanium dioxide, and DuPont 706 titanium dioxide;

[0023] The carbon black is at least one of Mitsubishi MA-100 carbon black, Orion FW-200 carbon black, and Orion U carbon black.

[0024] The present invention also provides a method for preparing the two-component gray paint for preventing floating color, comprising the following steps:

[0025] (1) Preparation of component A:

[0026] Step 1. Weigh each component by weight, add butyl acetate, propylene glycol methyl ether acetate, and xylene into a stirring kettle, and stir at a speed of 200 to 500 rpm for 2 to 10 minutes;

[0027] Step 2. Add the dispersant and defoamer into the stirring tank and stir at 200-500 rpm for 2-10 minutes;

[0028] Step 3. Add the hydroxy acrylic resin into the stirring kettle and stir at a speed of 200 to 500 rpm for 2 to 10 minutes;

[0029] Step 4. Add titanium dioxide, carbon black powder, anti-settling agent and barium sulfate into a stirring kettle, and stir at a speed of 1000 to 1500 rpm for 10 to 30 minutes to obtain a mixed material;

[0030] Step 5. The mixed material in step 4 is transferred to a sand mill, the sand milling medium is zirconium beads, and the mixture is sand milled until the particle size is 10 μm. The mixture is then sand milled and transferred to a stirring kettle. A leveling agent and a drying agent are added, and the mixture is stirred at a speed of 400 to 800 rpm for 5 to 15 minutes to obtain component A.

[0031] (2) Preparation of component B:

[0032] Step 1. Weigh each component by weight, add butyl acetate and propylene glycol methyl ether acetate into a stirring kettle, and stir at a speed of 200 to 500 rpm for 2 to 10 minutes;

[0033] Step 2. Add isocyanate into a stirring kettle and stir at a speed of 400 to 800 rpm for 10 to 20 minutes to obtain component B;

[0034] (3) Component A and component B are mixed evenly to obtain a two-component gray paint that is resistant to floating and blurring.

[0035] The beneficial effects of the present invention are as follows: the present invention adopts a polyurethane polymer dispersant and a high molecular weight unsaturated carboxylic acid dispersant and a specific fluorocarbon modified polymer leveling agent and an organic modified silicone leveling agent system, and controls the mass ratio of the dispersant and the leveling agent to meet the scope of the present invention, thereby effectively solving the problems of static floating color in the tank, floating color of the paint film, and blooming of the paint film. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical solutions and advantages of the embodiments of the present application clearer, the technical solutions in the embodiments of the present application are described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.

[0037] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0038] In this application, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values ​​of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0039] The raw materials used in the embodiments and comparative examples are described as follows:

[0040] Hydroxylated acrylic resin-1: Nupec Setalux 1753.

[0041] Hydroxylated acrylic resin-2: Dongsheng ESB-2050.

[0042] Dispersant-1: Polyurethane polymer dispersant, EFKA, EFKA-4310.

[0043] Dispersant-2: Polyurethane polymer dispersant, Deqian, Disponer 9850.

[0044] Dispersant-3: polyurethane polymer dispersant, AFCONE-4071.

[0045] Dispersant-4: High molecular weight unsaturated carboxylic acid dispersant, EFKA, EFKA-5066.

[0046] Dispersant-5: High molecular weight unsaturated carboxylic acid dispersant, BYK, BYK-104.

[0047] Dispersant-6: High molecular weight unsaturated carboxylic acid dispersant, Deqian, Disponer 904S.

[0048] Dispersant-7: Polyphosphate dispersant: BYK, BYK-110.

[0049] Dispersant-8: Structured acrylic copolymer containing pigment-affinity groups Dispersant: BYK-2001

[0050] Leveling agent-1: Fluorocarbon modified polymer leveling agent, Sago, Sago-3882 leveling agent.

[0051] Leveling agent-2: Fluorocarbon modified polymer leveling agent, VOK-FLOW 376S leveling agent.

[0052] Leveling agent-3: organic modified silicone leveling agent, BYK, BYK-333.

[0053] Leveling agent-4: organic modified silicone leveling agent, Deqian, Levaslip 836.

[0054] Leveling agent-5: polyacrylate leveling agent, BYK, BYK-385N.

[0055] Leveling agent-6: polyacrylate leveling agent, Digo, TEGO FLOW370.

[0056] Defoamer: Polysiloxane defoamer: Efka, Efka SI 2722.

[0057] Barium sulfate: 1250 mesh.

[0058] Titanium dioxide: DuPont 706.

[0059] Carbon black: Mitsubishi MA-100 carbon black.

[0060] Drier: American gas Dabco T-12.

[0061] Unless otherwise specified, the components and raw materials used in the embodiments and comparative examples of the present invention are all commercially available raw materials, and the components and raw materials used in each parallel experiment are all of the same kind.

[0062] The following examples are provided to facilitate understanding of the present invention. These examples are not provided to limit the scope of the claims.

[0063] Examples 1 to 11, Comparative Examples 1 to 10

[0064] The component A in the formula of the two-component gray coating for preventing floating and floating of Examples 1 to 11 and Comparative Examples 1 to 10 is shown in Table 1 and Table 2 (all in the tables are parts by weight).

[0065] The B components of Examples 1 to 11 and Comparative Examples 1 to 10 are the same, and all include: 70 parts of isocyanate, 15 parts of xylene, and 15 parts of butyl acetate.

[0066] The preparation methods of the two-component gray coatings for preventing floating and floating of Examples 1 to 11 and Comparative Examples 1 to 10 all include the following steps:

[0067] (1) Preparation of component A:

[0068] Step 1. Weigh each component by weight, add butyl acetate, propylene glycol methyl ether acetate, and xylene into a stirring kettle, and stir at 400 rpm for 4 minutes;

[0069] Step 2. Add the dispersant and defoamer into the stirring kettle and stir at 400 rpm for 4 minutes;

[0070] Step 3. Add the hydroxylated acrylic resin into the stirred tank and stir at 400 rpm for 4 minutes;

[0071] Step 4. Add titanium dioxide, carbon black powder, anti-settling agent and barium sulfate into a stirring kettle, and stir at 1400 rpm for 20 minutes to obtain a mixed material;

[0072] Step 5. The mixed material in step 4 is transferred to a sand mill with zirconium beads as the sand milling medium until the material is sand milled to 10 μm, then the sand milling is stopped and the material is transferred to a stirring kettle, a leveling agent and a drying agent are added, and the material is stirred at a speed of 500 rpm for 10 minutes to obtain component A;

[0073] (2) Preparation of component B:

[0074] Step 1. Weigh each component by weight, add butyl acetate and propylene glycol methyl ether acetate into a stirring kettle, and stir at 400 rpm for 5 minutes;

[0075] Step 2. Add isocyanate into a stirring kettle and stir at 500 rpm for 15 minutes to obtain component B;

[0076] (3) Component A and component B are mixed evenly to obtain a two-component gray paint that is resistant to floating and blurring.

[0077] Table 1

[0078]

[0079]

[0080] Table 2

[0081]

[0082] Performance Testing

[0083] 1. Static floating color in the can: Put the prepared paint into a 50℃ hot storage box, take it out for observation after 10 days, and evaluate the surface state of the paint after opening the cover. (1-5 levels, 1. Uniform state, 2. Careful observation, slight floating white or floating black, 3. Visible floating white or floating black, 4. Obvious floating white or floating black, 5. Very serious floating white or floating black).

[0084] 2. Paint film blooming: After the paint film is completely dry, observe the surface of the paint film and make an assessment. (Grade 1-5: 1. Uniform state, 2. Careful observation, slight white spots or black spots, 3. Visible white spots or black spots, 4. Obvious white spots or black spots, 5. Severe white spots and black spots).

[0085] 3. Paint film floating color: Use the finger rubbing method. When the paint film is half dry, rub your fingers until the paint film begins to become viscous and the pigment particles no longer migrate and separate. After the paint film is completely dry, test the color difference between the unrubbed area and the rubbed area. The smaller the color difference, the better.

[0086] Table 3

[0087]

[0088]

[0089] As can be seen from Table 3, the present invention effectively solves the problems of static floating color in the tank, floating color of the paint film, and blooming of the paint film by adopting a polyurethane polymer dispersant and a high molecular weight unsaturated carboxylic acid dispersant and a specific fluorocarbon modified polymer leveling agent and an organic modified silicone leveling agent system, and controlling the mass ratio of the dispersant and the leveling agent to meet the scope of the present invention.

[0090] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A two-component gray paint for preventing floating color, characterized in that: It includes component A and component B; The component A comprises the following components in parts by weight: 40 to 70 parts of hydroxy acrylic resin, 0.4 to 3.5 parts of dispersant, 0.3 to 1.2 parts of organic modified bentonite, 5 to 25 parts of barium sulfate, 5 to 25 parts of titanium dioxide, 0.2 to 2 parts of carbon black, 3 to 15 parts of xylene, 3 to 15 parts of butyl acetate, 3 to 15 parts of propylene glycol methyl ether acetate, 0.01 to 0.08 parts of drying agent, 0.1 to 1 parts of defoaming agent, and 0.2 to 3 parts of leveling agent; The B component includes the following components in parts by weight: 40 to 80 parts of isocyanate, 10 to 20 parts of xylene, and 10 to 20 parts of butyl acetate; The dispersant comprises a polyurethane polymer dispersant and a high molecular weight unsaturated carboxylic acid dispersant, and the mass ratio of the polyurethane polymer dispersant to the high molecular weight unsaturated carboxylic acid dispersant is (0.3-1.5): (0.1-2).

2. The two-component gray paint for preventing floating color and floating according to claim 1, characterized in that: The mass ratio of the polyurethane polymer dispersant to the high molecular weight unsaturated carboxylic acid dispersant is (0.8-1.2): (0.5-0.7).

3. The two-component gray paint for preventing floating color and floating according to claim 1, characterized in that: The polyurethane polymer dispersant includes at least one of BYK-163, EFKA-4010, BYK-161, EFKA-4310, Disponer 9850, and AFCONE-4071.

4. The two-component gray paint for preventing floating color and floating according to claim 1, characterized in that: The high molecular weight unsaturated carboxylic acid dispersant includes at least one of BYK-104, EFKA-5066, and Disponer 904S.

5. The two-component gray paint for preventing floating color and floating according to claim 1, characterized in that: The hydroxy acrylic resin includes at least one of Nupes Setalux 1753, Sanwang SWU3625, Dongsheng ESB-2050, Sanwang 6167, and Tongde 1011.

6. The two-component gray paint for preventing floating color and floating according to claim 1, characterized in that: The leveling agent comprises a fluorocarbon modified polymer leveling agent and an organic modified silicone leveling agent; the mass ratio of the fluorocarbon modified polymer leveling agent to the organic modified silicone leveling agent is (0.1-1): (0.1-2).

7. The two-component gray paint for preventing floating color and floating according to claim 6, characterized in that: The fluorocarbon modified polymer leveling agent includes at least one of Sago-3882 leveling agent, VOK-FLOW 376S leveling agent, and EFKA-3777 leveling agent; and / or The organic modified silicone leveling agent includes at least one of BYK-333, BYK-310, TEGO-435, Levaslip836, and Coatosil2820.

8. The two-component gray paint for preventing floating color and floating according to claim 1, characterized in that: The organic modified bentonite includes at least one of Bentone 27, Bentone 38, and BYK-CLAYTONE-APA; The particle size of the barium sulfate is 1000-1500 meshes.

9. The two-component gray paint for preventing floating color and floating according to claim 1, characterized in that: The titanium dioxide is at least one of Ishihara R930 titanium dioxide, DuPont 902 titanium dioxide, and DuPont 706 titanium dioxide; The carbon black is at least one of Mitsubishi MA-100 carbon black, Orion FW-200 carbon black, and Orion U carbon black.

10. The method for preparing the two-component gray paint with anti-floating and floating properties according to any one of claims 1 to 9, characterized in that: The following steps are involved: (1) Preparation of component A: Step 1. Weigh each component by weight, add butyl acetate, propylene glycol methyl ether acetate, and xylene into a stirring kettle, and stir at a speed of 200 to 500 rpm for 2 to 10 minutes; Step 2. Add the dispersant and defoamer into the stirring tank and stir at 200-500 rpm for 2-10 minutes; Step 3. Add the hydroxy acrylic resin into the stirring kettle and stir at a speed of 200 to 500 rpm for 2 to 10 minutes; Step 4. Add titanium dioxide, carbon black powder, anti-settling agent and barium sulfate into a stirring kettle, and stir at a speed of 1000 to 1500 rpm for 10 to 30 minutes to obtain a mixed material; Step 5. The mixed material in step 4 is transferred to a sand mill, the sand milling medium is zirconium beads, and the mixture is sand milled until the particle size is 10 μm. The mixture is then sand milled and transferred to a stirring kettle. A leveling agent and a drying agent are added, and the mixture is stirred at a speed of 400 to 800 rpm for 5 to 15 minutes to obtain component A. (2) Preparation of component B: Step 1. Weigh each component by weight, add butyl acetate and propylene glycol methyl ether acetate into a stirring kettle, and stir at a speed of 200 to 500 rpm for 2 to 10 minutes; Step 2. Add isocyanate into a stirring kettle and stir at a speed of 400 to 800 rpm for 10 to 20 minutes to obtain component B; (3) Component A and component B are mixed evenly to obtain a two-component gray paint that is resistant to floating and blurring.

Citation Information

Patent Citations

  • Weather-resistant finish matching with low-modulus high-displacement polyurethane sealant and preparation method thereof

    CN107586509A

  • Water-based two-component polyurethane coating as well as preparation method and application thereof

    CN115710454A

Cited By

  • ABA block type polyacrylate dispersant as well as preparation method and application thereof