Double-sided adhesive tape

By using a multi-layer foam resin layer with a multi-layer structure and adjusting the energy storage modulus of the adhesive layer in the adhesive tape, the problem of insufficient retaining force under shear and inclined loads is solved, and the reprocessing ability is improved and paste performance.

CN118978871APending Publication Date: 2024-11-19SEKISUI CHEMICAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411048081.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2020-09-23
Filing Date
2021-09-22
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing adhesive tapes are insufficient in holding force under shear and inclined loads, and it is difficult to effectively peel off residues during reprocessing of electronic equipment, affecting the handling properties and adhesion properties.

Method used

Designed with a double-sided adhesive tape, in which the foamed base material consists of a multi-layer structure foamed resin layer, including a first foamed resin layer with a higher foamed magnification and a second foamed magnification with a lower foamed magnification. 2. The energy storage modulus of the foam resin layer and the adhesive layer are adjusted to above 11,000 Pa to improve the following properties of the height difference and the retention force of shear and inclined loads, and optimize the reprocessing properties.

Benefits of technology

High retention forces under shear and inclined loads are achieved, adhesion handling is improved, and residues are effectively peeled off during reprocessing, improving performance during adhesion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978871A_ABST
    Figure CN118978871A_ABST
Patent Text Reader

Abstract

The purpose of the present invention is to provide a double-sided pressure-sensitive adhesive tape which has high following properties for the height difference between both pressure-sensitive adhesive surfaces, can exhibit high holding power against shear loads and inclined loads, has excellent reworkability for at least one pressure-sensitive adhesive surface, and also has excellent handling properties during adhesion. The present invention relates to a double-sided pressure-sensitive adhesive tape having a foam base material and pressure-sensitive adhesive layers laminated on both surfaces of the foam base material, the foam base material having a first foamed resin layer and a second foamed resin layer laminated on at least one surface of the first foamed resin layer, the foaming ratio of the second foamed resin layer is lower than that of the first foamed resin layer, and the storage modulus of at least one of the adhesive layers at 180 DEG C is 11000 Pa or more.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional of the application with national application number 202180028783.2 (international application number PCT / JP202I / 034884) which entered the Chinese national stage on October 14, 2022 and whose invention name is “Double-sided Adhesive Tape”. Technical Field

[0002] The present invention relates to a double-sided adhesive tape having high conformability to height differences on both adhesive surfaces, being able to exert high holding power against shear loads and tilt loads, having excellent reworkability on at least one adhesive surface, and also having excellent handling properties during lamination. Background Art

[0003] Adhesive tapes are widely used for fixing electronic components. Specifically, in display devices such as televisions and monitors, adhesive tapes are used to fix a cover plate on a surface to a housing. Such adhesive tapes are used in a manner such as being arranged around a display screen in a frame-like shape.

[0004] In recent years, the pursuit of design and functionality has led to the development of narrow frame display devices such as televisions and monitors, and expectations for frameless display devices are also increasing. In the manufacture of existing display devices, the cover is sometimes fixed to the housing by embedding or screwing, but embedding and screwing are difficult in display devices with narrow frames, so there is an increasing demand for fixing with adhesive tape, and the thinning and narrowing of adhesive tapes are also being promoted.

[0005] As an adhesive tape that can be used in such a display device, for example, Patent Documents 1 and 2 describe an impact-absorbing tape that is a cross-linked polyolefin resin foam sheet in which an acrylic adhesive layer is laminated and integrated on at least one side of a substrate layer, and the substrate layer has a specific cross-linking degree and aspect ratio of bubbles.

[0006] The foam substrate has appropriate flexibility and can relax stress. Therefore, by using the foam substrate as the substrate of the pressure-sensitive adhesive tape, there are advantages such as being able to improve step tracking performance, improving impact resistance, and reducing display unevenness generated in a display device.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Application Publication No. 2009-242541

[0010] Patent Document 2: Japanese Patent Application Publication No. 2009-258274 Summary of the invention

[0011] Problems to be solved by the invention

[0012] However, as display devices such as televisions and monitors continue to grow in size, the weight of fixed components such as covers and housings has also increased. Therefore, a very large load is applied to adhesive tapes, especially adhesive tapes that have been thinned and narrowed, which is greater than ever before. Among them, a very large load is applied in the shear direction, and a high holding force is required for the shear load. In addition, in applications such as wall-mounted televisions, the display device is set in a state of being tilted forward relative to the vertical direction, for example, about 20 to 45 degrees, and a high holding force is also required against the inclined load.

[0013] In addition, electronic components have tended to become more expensive in recent years, and therefore, when a defect occurs during the fixing of a component, for example, it is required that the component can be reprocessed. As one of the methods for reprocessing a component, for example, the following method is used: tearing the foam substrate of the adhesive tape with a cutting knife to break the interlayers and remove the component, and peeling off a portion of the adhesive tape remaining on the component. In such a case, the adhesive tape is required to have excellent reprocessability that allows it to be peeled off without leaving residue (for example, a portion of the foam substrate remaining due to rupture) on the component.

[0014] An object of the present invention is to provide a double-sided adhesive tape having high level-adjustability on both adhesive surfaces, capable of exerting high holding power against shear loads and tilt loads, excellent reworkability on at least one adhesive surface, and excellent handling properties during lamination.

[0015] Means used to solve problems

[0016] The present invention relates to a double-sided adhesive tape comprising a foam substrate and adhesive layers laminated on both sides of the foam substrate, wherein the foam substrate comprises a first foamed resin layer and a second foamed resin layer laminated on at least one side of the first foamed resin layer, the foaming ratio of the second foamed resin layer is lower than that of the first foamed resin layer, and at least one of the adhesive layers has a storage modulus of 11000 Pa or more at 180°C.

[0017] Hereinafter, the present invention will be described in detail.

[0018] The inventors of the present invention have studied the use of a multilayer substrate reinforced by laminating a resin layer on at least one side of a foamed resin layer as a foam substrate in a double-sided adhesive tape having a foam substrate and adhesive layers laminated on both sides of the foam substrate in order to improve the holding force against shear loads and tilt loads and to improve the reprocessability of at least one adhesive surface.

[0019] However, for example, when the resin layer on one or both sides is too hard, the height difference followability of the side laminated with the resin layer is reduced, and peeling is likely to occur. In recent years, there has been an increase in the number of cases where the adhesive tape partially overlaps with the polarizing plate in the display device, or partially overlaps with the guide formed on the housing in order to indicate the adhesive tape's pasting position. For the adhesive tape, when it is used in a thin and narrow width, it is also required to fully follow the height difference of such polarizing plates, guides, etc. On the other hand, in the case where the resin layer is too soft on both sides in order to improve the height difference followability (for example, in the case of using styrene-acrylic block copolymers in the resin layers on both sides), it is impossible to fully obtain the holding force for the shear load and the tilt load, and the adhesive tape stretches during pasting, resulting in poor handling.

[0020] In view of these problems, the present inventors have studied: using a foamed resin layer (outermost layer) as a resin layer laminated on a foamed resin layer (foamed resin layer in the center), and adjusting the foaming ratio of the outermost layer to be lower than the foaming ratio of the foamed resin layer in the center. The present inventors have found that by using such a multilayer substrate as a foam substrate, it is possible to take into account the height difference tracking of the two adhesive surfaces, the holding power for shear loads and tilting loads, and the reprocessability of at least one adhesive surface, and also to obtain excellent handling properties. The present inventors have further found that by adjusting the storage modulus of at least one of the adhesive layers at 180°C to a specific range, the holding power for shear loads and tilting loads can be further improved, thereby completing the present invention.

[0021] The double-sided adhesive tape of the present invention comprises a foam substrate and adhesive layers laminated on both sides of the foam substrate. By comprising the foam substrate, the double-sided adhesive tape of the present invention has improved step-following property and can exhibit excellent stress relaxation property.

[0022] The foam substrate includes a first foamed resin layer and a second foamed resin layer laminated on at least one surface of the first foamed resin layer, and the second foamed resin layer has a lower expansion ratio than the first foamed resin layer.

[0023] By laminating the second foamed resin layer on the first foamed resin layer, the deformation stress of the first foamed resin layer caused by the application of shear load or tilting load can be alleviated and not easily transferred to the adhesive layer, and the peeling of the adhesive layer can be suppressed. In addition, by laminating the second foamed resin layer on the first foamed resin layer, the double-sided adhesive tape of the present invention can be peeled off and removed during reprocessing without leaving residue (for example, a part of the first foamed resin layer that is broken and remains) on the adherend on the side where the second foamed resin layer is laminated, and excellent reprocessability can be exerted.

[0024] In addition, when a too hard resin layer is stacked on the first foamed resin layer, the height difference followability of the side stacked with the resin layer is reduced. In contrast, in the double-sided adhesive tape of the present invention, by stacking the second foamed resin layer on the first foamed resin layer, the reduction of the height difference followability of the two adhesive surfaces can be suppressed. On the other hand, in the case of stacking too soft resin layers on both sides of the first foamed resin layer to improve the height difference followability (for example, in the case of using styrene-acrylic acid block copolymers in the resin layers on both sides), it is impossible to fully obtain the holding force for shear load and tilt load, and the problem of poor handling during pasting occurs. In contrast, the double-sided adhesive tape of the present invention can exert high holding force for shear load and tilt load by stacking the second foamed resin layer on the first foamed resin layer, and the handling during pasting is also excellent.

[0025] The foam substrate may have the second foam resin layer only on one side of the first foam resin layer, or may have the second foam resin layer on both sides of the first foam resin layer. In order to further improve the holding power of the double-sided adhesive tape for shear load and tilt load and to achieve excellent reprocessability on both adhesive surfaces, it is preferred to have the second foam resin layer on both sides of the first foam resin layer. It should be noted that, in this case, the resin composition, physical properties, thickness, etc. of the second foam resin layers on both sides may be the same or different.

[0026] In addition, usually, the adhesive tape is provided in the state of being wound into a roll, extracted from this roll and used. And, under the situation that the two sides of above-mentioned 1st foamed resin layer are laminated with too hard resin layer, if the diameter of core becomes the size more than certain, then wrinkles and breaks are produced when winding. On the contrary, in double-sided adhesive tape of the present invention, by laminating the above-mentioned 2nd foamed resin layer on the above-mentioned 1st foamed resin layer, even under the situation that the two sides are laminated with the above-mentioned 2nd foamed resin layer, the overall flexibility of the double-sided adhesive tape can be guaranteed. Thus, easily the double-sided adhesive tape is wound into a roll, and the handling property significantly improves, and wrinkles and breaks can be suppressed when winding.

[0027] The foam substrate may have other layers such as an adhesive layer in addition to the first foamed resin layer and the second foamed resin layer. However, from the viewpoint of preventing the complication of the manufacturing process, it is preferred that no other layers are provided between the first foamed resin layer and the second foamed resin layer.

[0028] exist Figure 3 A cross-sectional view schematically showing an example of the double-sided pressure-sensitive adhesive tape of the present invention is shown in FIG. Figure 3The double-sided adhesive tape 7 shown has a foam substrate 8 and adhesive layers 91, 92 laminated on both sides of the foam substrate 8. The foam substrate 8 has a first foam resin layer 10 and second foam resin layers 11, 12 laminated on both sides of the first foam resin layer 10. Figure 3 In the double-sided adhesive tape shown, the second foamed resin layer is laminated on both surfaces of the first foamed resin layer, but the present invention is not limited to such an embodiment.

[0029] The first foamed resin layer may have a continuous cell structure or a closed cell structure, preferably a closed cell structure. The closed cell structure improves the strength of the first foamed resin layer, thereby suppressing deformation and interlayer damage of the first foamed resin layer when a shear load and an inclined load are applied, and further improving the holding power of the double-sided adhesive tape against the shear load and the inclined load.

[0030] The first foamed resin layer may have a single-layer structure or a multi-layer structure.

[0031] The first foamed resin layer is not particularly limited, and examples thereof include a polyurethane foamed resin layer, a polyolefin foamed resin layer, a rubber foamed resin layer, an acrylic foamed resin layer, etc. Among them, from the perspective of being able to exert excellent stress relaxation and strength, a polyurethane foamed resin layer or a polyolefin foamed resin layer is preferred, and a polyolefin foamed resin layer is more preferred.

[0032] The polyurethane foam resin layer is not particularly limited, and examples thereof include a polyurethane foam resin layer formed from a urethane resin composition containing polyisocyanate and polyol. Such a polyurethane foam resin layer can be produced by heat-curing the urethane resin composition.

[0033] The polyolefin foamed resin layer is not particularly limited, and examples thereof include a foamed resin layer formed of a polyethylene resin, a polypropylene resin, a polybutadiene resin, etc. Among them, a foamed resin layer formed of a polyethylene resin is preferred from the perspective of easily obtaining a soft polyolefin foamed resin layer.

[0034] The polyethylene resin is not particularly limited, and examples thereof include polyethylene resins obtained by polymerization using polymerization catalysts such as Ziegler-Natta compounds, metallocene compounds, and chromium oxide compounds. In addition, from the perspective of increasing the flexibility of the first foamed resin layer, a linear low-density polyethylene is preferred as the polyethylene resin. The linear low-density polyethylene is preferably a linear low-density polyethylene obtained by copolymerizing ethylene with a small amount of α-olefin used as required, and examples of the α-olefin include propylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene, 1-octene, etc. Among them, α-olefins having 4 to 10 carbon atoms are preferred.

[0035] The expansion ratio of the first foamed resin layer is not particularly limited as long as it is higher than the expansion ratio of the second foamed resin layer.

[0036] When the first foamed resin layer is a polyolefin foamed resin layer, the preferred lower limit of the foaming ratio of the first foamed resin layer is 5 cm 3 / g, the preferred upper limit is 30cm 3 / g. If the above expansion ratio is 5cm 3 / g or more, the first foamed resin layer can have appropriate softness, and the height difference followability and stress relaxation of the two adhesive surfaces of the double-sided adhesive tape are further improved. 3 / g or less, the strength of the first foamed resin layer is sufficiently improved, and the holding power of the double-sided adhesive tape against shear load and tilt load is further improved. The more preferred lower limit of the foaming ratio is 8 cm 3 / g, and the more preferred upper limit is 25cm 3 / g, and a further preferred lower limit is 10 cm 3 / g, and a further preferred upper limit is 20 cm 3 / g, and a further preferred upper limit is 18 cm 3 / g.

[0037] In addition, the expansion ratio can be calculated|required based on JIS K 7222 (when polyethylene is used). In addition, the expansion ratio can be calculated|required as the reciprocal of an apparent density.

[0038] The thickness of the first foamed resin layer is not particularly limited, and the preferred lower limit is 100 μm, and the preferred upper limit is 2000 μm. If the thickness is above 100 μm, the first foamed resin layer can have appropriate flexibility, and the height difference followability and stress relaxation of the two adhesive surfaces of the double-sided adhesive tape are further improved. If the thickness is below 2000 μm, the deformation of the first foamed resin layer when a shear load and an inclined load are applied can be suppressed, and the holding force of the double-sided adhesive tape for a shear load and an inclined load is further improved. The more preferred lower limit of the thickness is 300 μm, the more preferred upper limit is 1500 μm, the further preferred lower limit is 500 μm, and the further preferred upper limit is 1000 μm.

[0039] The thickness of the foamed resin layer can be measured using a dial thickness gauge (for example, “ABSDIGIMATIC INDICATOR” manufactured by Mitutoyo Corporation).

[0040] The second foamed resin layer is not particularly limited as long as it has a lower foaming ratio than the first foamed resin layer. It may be a foamed resin layer having the same bubble structure, layer structure, resin composition, physical properties, etc. as the first foamed resin layer, or it may be a foamed resin layer having a different bubble structure, layer structure, resin composition, physical properties, etc. from the first foamed resin layer.

[0041] The second foamed resin layer may have a continuous cell structure or a closed cell structure, preferably a closed cell structure. By having a closed cell structure, the strength of the second foamed resin layer is improved, so that the double-sided adhesive tape can be peeled off and removed during reprocessing without further residue (e.g., a portion of the first foamed resin layer that is broken and remains) on the adherend on the side where the second foamed resin layer is laminated, thereby achieving better reprocessability.

[0042] The second foamed resin layer may have a single-layer structure or a multi-layer structure.

[0043] The second foamed resin layer is not particularly limited, and examples thereof include a polyurethane foamed resin layer, a polyolefin foamed resin layer, a rubber foamed resin layer, an acrylic foamed resin layer, etc. Among them, from the perspective of being able to exert excellent stress relaxation and strength, a polyurethane foamed resin layer or a polyolefin foamed resin layer is preferred, and a polyolefin foamed resin layer is more preferred.

[0044] The polyurethane foam resin layer is not particularly limited and may be the same as the polyurethane foam resin layer in the first foam resin layer. The polyolefin foam resin layer is also not particularly limited and may be the same as the polyolefin foam resin layer in the first foam resin layer.

[0045] The expansion ratio of the second foamed resin layer is not particularly limited as long as it is lower than the expansion ratio of the first foamed resin layer, and a preferred lower limit is 1.1 cm 3 / g, the preferred upper limit is 7cm 3 / g. If the above expansion ratio is 1.1cm 3 / g or more, the second foamed resin layer can have appropriate softness, and the height difference followability and stress relaxation of the two adhesive surfaces of the double-sided adhesive tape are further improved. 3 / g or less, the strength of the second foamed resin layer is sufficiently improved, the holding power of the double-sided adhesive tape against shear load and tilt load is further improved, and the handling property during pasting is also further improved. The more preferred lower limit of the foaming ratio is 1.3 cm 3 / g, and the more preferred upper limit is 5cm 3 / g, and a further preferred lower limit is 1.4 cm 3 / g, and a further preferred upper limit is 2 cm 3 / g, and a further preferred lower limit is 1.5 cm 3 / g, and a further preferred upper limit is 1.9 cm 3 / g.

[0046] The thickness of the second foamed resin layer is not particularly limited, and the preferred lower limit is 5 μm, and the preferred upper limit is 100 μm. If the thickness is more than 5 μm, the holding force of the double-sided adhesive tape for shear load and tilt load is further improved. If the thickness is below 100 μm, the height difference followability and stress relaxation of the two adhesive surfaces of the double-sided adhesive tape are further improved. The more preferred lower limit of the thickness is 10 μm, the more preferred upper limit is 80 μm, the further preferred lower limit is 30 μm, and the further preferred upper limit is 60 μm.

[0047] The 25% compressive strength of the foam substrate (the entire foam substrate) is not particularly limited, and the preferred lower limit is 1kPa, and the preferred upper limit is 200kPa. If the 25% compressive strength is above 1kPa, the strength of the foam substrate is sufficiently improved, and the holding power of the double-sided adhesive tape for shear load and tilt load is further improved. If the 25% compressive strength is below 200kPa, the foam substrate can have moderate softness, and the height difference followability and stress relaxation of the two adhesive surfaces of the double-sided adhesive tape are further improved. The more preferred lower limit of the 25% compressive strength is 10kPa, the more preferred upper limit is 100kPa, the further preferred lower limit is 20kPa, and the further preferred upper limit is 40kPa.

[0048] For example, the 25% compressive strength of the foam substrate (the entire foam substrate) can be adjusted to be within the above range by adjusting the expansion ratio of the first foamed resin layer.

[0049] The 25% compressive strength can be determined by the following measurement based on JIS K 6254:2016 using, for example, “Autograph AGS-X” manufactured by Shimadzu Corporation.

[0050] The foam substrate is cut into 20mm×20mm pieces and overlapped to make a sample with a thickness of about 5mm×20mm×20mm. The sample is crushed along the compression direction at a speed of 10mm / min, and the pressure (N) when it is compressed by 25% is confirmed. The 25% compression strength is calculated based on the obtained pressure and the following formula (2). It should be noted that the case where the thickness of the sample is set to 100 and it is compressed by 25% (the thickness of the sample becomes 75) is considered to be compressed by 25%.

[0051] Compression strength (kPa) = pressure (N) / 0.4 (2)

[0052] The thickness of the foam substrate (foam substrate as a whole) is not particularly limited, and the preferred lower limit is 105 μm, and the preferred upper limit is 2100 μm. If the thickness is within the above range, the holding force of the double-sided adhesive tape for shear load and tilt load is further improved, and the height difference followability and stress relaxation of the two adhesive surfaces are also further improved. The more preferred lower limit of the thickness is 310 μm, the more preferred upper limit is 1580 μm, the further preferred lower limit is 530 μm, and the further preferred upper limit is 1060 μm.

[0053] In the above-mentioned foam substrate, the ratio of the thickness of the above-mentioned first foamed resin layer to the thickness of the above-mentioned second foamed resin layer (the value of the thickness of the above-mentioned first foamed resin layer / the thickness of the above-mentioned second foamed resin layer) is not particularly limited, and a preferred lower limit is 1.0, and a preferred upper limit is 400. If the ratio of the above-mentioned thickness is within the above-mentioned range, the holding force of the double-sided adhesive tape for shear load and tilt load is further improved, and the height difference followability and stress relaxation of the two adhesive surfaces are also further improved. The more preferred lower limit of the ratio of the above-mentioned thickness is 3, and the more preferred upper limit is 150, and the further preferred lower limit is 5, and the further preferred upper limit is 40.

[0054] In the above-mentioned foam substrate, the ratio of the expansion ratio of the above-mentioned first foamed resin layer to the expansion ratio of the above-mentioned second foamed resin layer (the value of the expansion ratio of the above-mentioned first foamed resin layer / the expansion ratio of the above-mentioned second foamed resin layer) is not particularly limited, and the preferred lower limit is 1.3, and the preferred upper limit is 100. If the ratio of the above-mentioned expansion ratio is within the above-mentioned range, the holding force of the double-sided adhesive tape for shear load and tilt load is further improved, and the height difference followability and stress relaxation of the two adhesive surfaces are also further improved. The more preferred lower limit of the ratio of the above-mentioned expansion ratio is 3, the more preferred upper limit is 50, the further preferred lower limit is 8, and the further preferred upper limit is 20.

[0055] The method for manufacturing the foam substrate is not particularly limited, and may be a method in which the first foamed resin layer and the second foamed resin layer are separately produced and then pressed or bonded together with the aid of an adhesive layer or the like, and preferably a method in which a foamable composition for forming the first foamed resin layer and a foamable composition for forming the second foamed resin layer are subjected to multi-layer extrusion. If the multi-layer extrusion method is used, the first foamed resin layer and the second foamed resin layer can be laminated without the aid of an adhesive layer or the like, which is preferred from the viewpoint of preventing complication of the manufacturing process.

[0056] The method for performing the multi-layer extrusion is not particularly limited. For example, first, the foamable composition forming the first foamed resin layer and the foamable composition forming the second foamed resin layer are extruded separately, and the foamable compositions extruded separately are merged into a layer in a mold in a molten state to obtain a laminated sheet in which a plurality of layers formed by the foamable compositions are stacked. The foamable composition forming the first foamed resin layer and the foamable composition forming the second foamed resin layer are, for example, compositions containing the polyethylene resin and a thermally decomposable foaming agent as described above. By changing the type and amount of the thermally decomposable foaming agent, the foaming ratio of the obtained foamed resin layer can be adjusted.

[0057] Next, at least one surface of the obtained laminated sheet is irradiated with ionizing radiation to crosslink the polyethylene resin. The expansion ratio of the obtained foamed resin layer can be adjusted by changing the crosslinking degree of the polyethylene resin.

[0058] Furthermore, the laminated sheet after foaming and crosslinking by heating etc. can be obtained as a foam substrate having the first foamed resin layer and the second foamed resin layer. The laminated sheet after crosslinking by heating etc. can also be stretched during and / or after foaming.

[0059] The adhesive layer is laminated on both sides of the foam substrate. It should be noted that the resin composition, physical properties, thickness, etc. of the adhesive layers on both sides may be the same or may be the same.

[0060] The lower limit of the storage modulus of at least one of the above-mentioned adhesive layers at 180°C is 11,000 Pa. It should be noted that in this case, the storage modulus of both sides of the above-mentioned adhesive layer at 180°C can be within this range, or only the storage modulus of one side at 180°C can be within this range. If the storage modulus at 180°C is 11,000 Pa or more, the bulk strength (Japanese: バルク強度) of the above-mentioned adhesive layer is improved, and peeling of the above-mentioned adhesive layer when a shear load or an inclined load is applied can be suppressed. The preferred lower limit of the storage modulus at 180°C is 13,000 Pa, the more preferred lower limit is 15,000 Pa, and the further preferred lower limit is 20,000 Pa.

[0061] There is no particular limitation on the upper limit of the storage modulus at 180°C, and the preferred upper limit is 50,000 Pa. If the storage modulus at 180°C is 50,000 Pa or less, interfacial peeling when a shear load or an inclined load is applied can be suppressed due to insufficient wettability at the interface of the above-mentioned adhesive layer. The more preferred upper limit of the storage modulus at 180°C is 40,000 Pa, and the further preferred upper limit is 32,000 Pa.

[0062] The storage modulus of the above-mentioned adhesive layer at 180°C can be adjusted to the above range, for example, by adjusting the composition, weight average molecular weight, molecular weight distribution (weight average molecular weight / number average molecular weight), etc. of the acrylic copolymer contained in the above-mentioned adhesive layer; adjusting the types and amounts of the crosslinking agent and tackifying resin contained in the above-mentioned adhesive layer; adjusting the gel fraction of the above-mentioned adhesive layer, etc.

[0063] It should be noted that the storage modulus at 180°C can be obtained using a viscoelasticity measuring device (for example, "Rheometrics Dynamic Analyze RDA-700" manufactured by Rheometrics) under the conditions of a measurement temperature of -40 to 200°C, a heating rate of 3°C / min, and a frequency of 10 Hz.

[0064] The above-mentioned adhesive layer is not particularly limited, and examples thereof include: an acrylic adhesive layer, a rubber-based adhesive layer, a urethane adhesive layer, a silicone-based adhesive layer, etc. Among them, from the viewpoint of being relatively stable to light, heat, moisture, etc. and being able to adhere to various adherends (low selectivity of adherends), at least one of the above-mentioned adhesive layers is preferably an acrylic adhesive layer. That is, at least one of the above-mentioned adhesive layers preferably contains an acrylic copolymer. It should be noted that in this case, the above-mentioned adhesive layer can contain an acrylic copolymer on both sides, or only on one side.

[0065] From the viewpoint that the ease of pasting at low temperature becomes good due to the improvement of initial viscosity, the acrylic copolymer is preferably obtained by copolymerizing a monomer mixture containing butyl acrylate and / or 2-ethylhexyl acrylate. More preferably, the acrylic copolymer is obtained by copolymerizing a monomer mixture containing butyl acrylate and 2-ethylhexyl acrylate.

[0066] The preferred lower limit of the content of the butyl acrylate in the total monomer mixture is 30% by weight, and the preferred upper limit is 80% by weight. When the content of the butyl acrylate is within this range, both high adhesive force and tack can be achieved.

[0067] The preferred lower limit of the content of the 2-ethylhexyl acrylate in the total monomer mixture is 10% by weight, the preferred upper limit is 100% by weight, the more preferred lower limit is 30% by weight, the more preferred upper limit is 80% by weight, the further preferred lower limit is 50% by weight, and the further preferred upper limit is 60% by weight. When the content of the 2-ethylhexyl acrylate is within this range, high adhesive force can be exerted.

[0068] The monomer mixture may contain other copolymerizable monomers other than butyl acrylate and 2-ethylhexyl acrylate as required. Examples of the other copolymerizable monomers include (meth)acrylic acid alkyl esters having 1 to 3 carbon atoms in the alkyl group, (meth)acrylic acid alkyl esters having 13 to 18 carbon atoms in the alkyl group, and functional monomers.

[0069] Examples of the alkyl (meth)acrylates in which the alkyl group has 1 to 3 carbon atoms include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, and the like. Examples of the alkyl (meth)acrylates in which the alkyl group has 13 to 18 carbon atoms include tridecyl methacrylate, stearyl (meth)acrylate, and the like. Examples of the functional monomers include hydroxyalkyl (meth)acrylates, glyceryl dimethacrylate, glycidyl (meth)acrylate, 2-methacryloyloxyethyl isocyanate, (meth)acrylic acid, itaconic acid, maleic anhydride, crotonic acid, maleic acid, and fumaric acid, and the like.

[0070] Among them, from the viewpoint of improving the storage modulus and volume strength of the above-mentioned adhesive layer at 180°C, hydroxyl-containing monomers such as hydroxyalkyl (meth)acrylates and glycerol dimethacrylate are preferred. That is, the above-mentioned acrylic copolymer preferably has a structural unit derived from a hydroxyl-containing monomer. The above-mentioned hydroxyalkyl (meth)acrylate is not particularly limited, and more specifically, for example, 2-hydroxyethyl (meth)acrylate and the like can be cited.

[0071] In order to copolymerize the above-mentioned monomer mixture to obtain the above-mentioned acrylic copolymer, it is sufficient to subject the above-mentioned monomer mixture to a free radical reaction in the presence of a polymerization initiator. As a method for subjecting the above-mentioned monomer mixture to a free radical reaction, i.e., a polymerization method, a conventionally known method can be used, for example, solution polymerization (boiling point polymerization or constant temperature polymerization), emulsion polymerization, suspension polymerization, bulk polymerization, etc.

[0072] The preferred lower limit of the weight average molecular weight (Mw) of the acrylic copolymer is 500,000. If the weight average molecular weight of the acrylic copolymer is 500,000 or more, the storage modulus and volume strength of the adhesive layer at 180° C. are improved, and peeling of the adhesive layer when a shear load or an inclined load is applied can be suppressed. The more preferred lower limit of the weight average molecular weight is 600,000, the further preferred lower limit is 800,000, and the further preferred lower limit is 1,000,000.

[0073] The upper limit of the weight average molecular weight of the acrylic copolymer is not particularly limited, and the preferred upper limit is 2,000,000. If the weight average molecular weight of the acrylic copolymer is below 2,000,000, it is possible to suppress the interfacial peeling caused by the insufficient wettability of the interface of the adhesive layer when a shear load or an inclined load is applied. The more preferred upper limit of the weight average molecular weight of the acrylic copolymer is 1,900,000, the further preferred upper limit is 1,800,000, and the further preferred upper limit is 1,750,000.

[0074] In addition, the weight average molecular weight (Mw) means the weight average molecular weight converted into standard polystyrene based on GPC (Gel Permeation Chromatography).

[0075] The preferred lower limit of the ratio (Mw / Mn) of the weight average molecular weight (Mw) of the acrylic copolymer to the number average molecular weight (Mn) is 1.05, and the preferred upper limit is 5.0. If Mw / Mn is 5.0 or less, the proportion of low molecular weight components is suppressed, the storage modulus and volume strength of the adhesive layer at 180°C are improved, and the peeling of the adhesive layer when a shear load or an inclined load is applied can be suppressed. The more preferred upper limit of Mw / Mn is 4.5, the further preferred upper limit is 4, and the further preferred upper limit is 3.5.

[0076] From the viewpoint of exerting high adhesive force, at least one of the adhesive layers preferably contains a tackifier resin. In this case, the adhesive layer may contain a tackifier resin on both sides or only on one side.

[0077] Examples of the tackifying resin include rosin resins, rosin ester resins, hydrogenated rosin resins, terpene resins, terpene phenol resins, coumarone indene resins, alicyclic saturated hydrocarbon resins, C5 petroleum resins, C9 petroleum resins, C5-C9 copolymerized petroleum resins, etc. These tackifying resins may be used alone or in combination of two or more. Among them, rosin resins or terpene resins are preferred, and rosin resins or terpene resins having hydroxyl groups are more preferred.

[0078] The preferred lower limit of the softening temperature of the tackifying resin is 70°C, and the preferred upper limit is 170°C. If the softening temperature is 70°C or higher, it is possible to prevent the adhesive layer from becoming too soft and reducing the holding power for shear loads and tilt loads. If the softening temperature is 170°C or lower, it is possible to prevent the interface peeling from occurring when a shear load or tilt load is applied due to insufficient wettability of the interface of the adhesive layer. A more preferred lower limit of the softening temperature is 120°C.

[0079] In addition, the softening temperature is the softening temperature measured by the JIS K2207 ring and ball method.

[0080] The preferred lower limit of the hydroxyl value of the tackifying resin is 25. By making the hydroxyl value above the above value, it is possible to suppress the occurrence of interface peeling when a shear load or an oblique load is applied due to insufficient interaction at the interface of the adhesive layer. The more preferred lower limit of the hydroxyl value is 30. The upper limit of the hydroxyl value is not particularly limited.

[0081] In addition, the hydroxyl value can be measured according to JIS K1557 (phthalic anhydride method).

[0082] The content of the above-mentioned tackifying resin is not particularly limited, and the preferred lower limit relative to 100 parts by weight of the above-mentioned acrylic copolymer is 10 parts by weight, and the preferred upper limit is 40 parts by weight. If the content of the above-mentioned tackifying resin is more than 10 parts by weight, the adhesive force of the above-mentioned adhesive layer is improved. If the content of the above-mentioned tackifying resin is less than 40 parts by weight, it is possible to suppress the above-mentioned adhesive layer from becoming too hard and reducing the adhesive force.

[0083] For at least one of the above-mentioned adhesive layers, it is preferred that a cross-linking structure is formed between the main chains of the resin constituting the above-mentioned adhesive layer (e.g., the above-mentioned acrylic copolymer, the above-mentioned tackifying resin, etc.) by a cross-linking agent. It should be noted that, in this case, the above-mentioned adhesive layer may be added with a cross-linking agent on both sides, or may be added with a cross-linking agent only on one side. By adjusting the type and amount of the above-mentioned cross-linking agent, it is easy to adjust the storage modulus and gel fraction of the above-mentioned adhesive layer at 180°C.

[0084] The crosslinking agent is not particularly limited, and examples thereof include isocyanate crosslinking agents, aziridine crosslinking agents, epoxy crosslinking agents, metal chelate crosslinking agents, etc. Among them, isocyanate crosslinking agents are preferred.

[0085] The amount of the crosslinking agent added is preferably 0.01 parts by weight, and the upper limit is preferably 10 parts by weight, with a more preferred lower limit being 0.1 parts by weight and the upper limit being more preferably 3 parts by weight, based on 100 parts by weight of the acrylic copolymer.

[0086] The adhesive layer may contain a silane coupling agent for the purpose of improving adhesion. The silane coupling agent is not particularly limited, and examples thereof include epoxy silanes, acrylic silanes, methacrylic silanes, amino silanes, and isocyanate silanes.

[0087] The adhesive layer may contain a coloring material for the purpose of imparting light-shielding properties. The coloring material is not particularly limited, and examples thereof include carbon black, aniline black, titanium oxide, etc. Among them, carbon black is preferred because it is relatively inexpensive and chemically stable.

[0088] The adhesive layer may contain conventionally known fine particles and additives such as inorganic fine particles, conductive fine particles, an antioxidant, a foaming agent, an organic filler, and an inorganic filler, as required.

[0089] The preferred lower limit of the gel fraction of at least one of the above-mentioned adhesive layers is 15% by weight. It should be noted that, in this case, the gel fraction of both sides of the above-mentioned adhesive layer can be within this range, or the gel fraction of only one side can be within this range. If the above-mentioned gel fraction is 15% by weight or more, the storage modulus and volume strength of the above-mentioned adhesive layer at 180°C are improved, and the peeling of the above-mentioned adhesive layer when a shear load or an inclined load is applied can be suppressed. The more preferred lower limit of the above-mentioned gel fraction is 30% by weight, and the further preferred lower limit is 40% by weight.

[0090] The upper limit of the gel fraction is not particularly limited, and the preferred upper limit is 80% by weight. If the gel fraction is below 80% by weight, it is possible to suppress the interfacial peeling caused by insufficient wettability of the interface of the adhesive layer when a shear load or an inclined load is applied. The more preferred upper limit of the gel fraction is 75% by weight, the further preferred upper limit is 70% by weight, and the further preferred upper limit is 65% by weight.

[0091] In addition, the gel fraction of the pressure-sensitive adhesive layer can be measured by the following method.

[0092] The double-sided adhesive tape was cut into a flat rectangular shape of 50 mm × 100 mm to prepare a test piece. After the test piece was immersed in ethyl acetate at 23°C for 24 hours, it was taken out from ethyl acetate and dried at 110°C for 1 hour. The weight of the test piece after drying was measured, and the gel fraction was calculated using the following formula (1). It should be noted that no release film for protecting the adhesive layer was laminated on the test piece.

[0093] Gel fraction (wt%) = 100 × (W 2 -W 0 ) / (W 1 -W 0 )(1)

[0094] (W 0 : Weight of foam substrate, W 1 : Weight of the test piece before immersion, W 2 : Weight of the test piece after immersion and drying)

[0095] The thickness of the adhesive layer is not particularly limited, and the preferred lower limit of the thickness of the adhesive layer on one side is 20 μm, and the preferred upper limit is 100 μm. If the thickness of the adhesive layer is 20 μm or more, the adhesive force of the adhesive layer is sufficient. If the thickness of the adhesive layer is 100 μm or less, the stress relaxation of the foam substrate can also fully contribute to the stress relaxation of the double-sided adhesive tape as a whole. The more preferred lower limit of the thickness of the adhesive layer is 25 μm, the more preferred upper limit is 80 μm, the further preferred lower limit is 30 μm, the further preferred upper limit is 70 μm, the further preferred lower limit is 35 μm, and the further preferred upper limit is 65 μm.

[0096] The thickness of the pressure-sensitive adhesive layer can be measured using a dial thickness gauge (for example, “ABSDIGIMATIC INDICATOR” manufactured by Mitutoyo Corporation).

[0097] The double-sided pressure-sensitive adhesive tape of the present invention may include other layers in addition to the foam substrate and the pressure-sensitive adhesive layer as required.

[0098] The preferred lower limit of the strength of the double-sided adhesive tape of the present invention when it is extended by 5 mm from the initial distance between the clamping fixtures in the tensile test is 1.5 N. If the above strength is 1.5 N or more, the holding force of the double-sided adhesive tape for shear load and tilt load is further improved, and the handling property during pasting is also further improved. The more preferred lower limit of the above strength is 1.7 N, and the further preferred lower limit is 2.2 N.

[0099] For example, the strength of the second foamed resin layer can be adjusted to be within the above range by adjusting the expansion ratio of the second foamed resin layer to be within an appropriate range to increase the strength of the second foamed resin layer.

[0100] It should be noted that in the tensile test, the strength when the initial distance between the clamping fixtures is extended by 5 mm can be measured by a method based on JIS K 7161. Specifically, for example, a double-sided adhesive tape is punched into a dumbbell shape using a punching blade "Stretching No. 3 Dumbbell" manufactured by Polymer Meter Co., Ltd., etc., to prepare a test piece. For example, using "Autograph AGS-X" manufactured by Shimadzu Corporation, the obtained test piece is stretched at a tension rate of 50 mm / min at 25°C and a relative humidity of 50%. At this time, the initial distance between the clamping fixtures is set to 60 mm, and the strength when the distance is extended by 5 mm (the distance between the clamping fixtures is 65 mm) is read.

[0101] The 25% compressive strength of the double-sided adhesive tape of the present invention is not particularly limited, and the preferred lower limit is 20kPa, and the preferred upper limit is 70kPa. If the above-mentioned 25% compressive strength is more than 20kPa, the holding force of the double-sided adhesive tape for shear load and tilt load is further improved. If the above-mentioned 25% compressive strength is less than 70kPa, the height difference followability and stress relaxation of the two adhesive surfaces of the double-sided adhesive tape are further improved. The more preferred lower limit of the above-mentioned 25% compressive strength is 25kPa, the further preferred lower limit is 27kPa, and the particularly preferred lower limit is 30kPa. The more preferred upper limit of the above-mentioned 25% compressive strength is 65kPa, the further preferred upper limit is 60kPa, and the particularly preferred upper limit is 40kPa.

[0102] The 25% compressive strength of the double-sided pressure-sensitive adhesive tape of the present invention can be measured in accordance with JIS K 6254:2016, similar to the 25% compressive strength of the foam substrate.

[0103] The double-sided adhesive tape of the present invention preferably has a tensile strength of 2N or more when a sample obtained by slicing the first foamed resin layer is subjected to a tensile test at 23°C. If the tensile strength is 2N or more, the double-sided adhesive tape can exhibit better reprocessability at room temperature. The tensile strength is more preferably 3N or more, and further preferably 4N or more.

[0104] The upper limit of the tensile strength at break is not particularly limited, but is preferably 20N, and more preferably 15N, from the viewpoint of step followability and stress relaxation properties.

[0105] The double-sided adhesive tape of the present invention preferably has a tensile elongation at break of 30 mm or more when a sample obtained by slicing the first foamed resin layer is subjected to a tensile test at 23°C. If the tensile elongation at break is 30 mm or more, the double-sided adhesive tape can exhibit better reprocessability at room temperature. The tensile elongation at break is more preferably 50 mm or more, and further preferably 70 mm or more.

[0106] The upper limit of the tensile elongation at break is not particularly limited, but is preferably 200 mm from the viewpoint of exerting a holding force against a shear load and an inclined load.

[0107] The method of conducting a 23° C. tensile test on a sample obtained by slicing the first foamed resin layer is as follows.

[0108] The double-sided adhesive tape was cut into dumbbell No. 3 size (center width 5 mm), and the first foamed resin layer (center portion) was sliced ​​with a feather blade. Thus, a sample of adhesive layer / second foamed resin layer / first foamed resin layer (about half the thickness) was obtained.

[0109] Each sample was subjected to a tensile test using "Autograph AGS-X" manufactured by Shimadzu Corporation at a tensile speed of 100 mm / min, a temperature of 23°C, and a distance between clamps of 45 mm. The strength at which the sample broke was taken as the tensile breaking strength, and the elongation at which the sample broke was taken as the tensile breaking elongation.

[0110] In the double-sided adhesive tape of the present invention, the tensile strength at break when a sample obtained by slicing the first foamed resin layer is subjected to a tensile test at 80°C is preferably 1 N or more. If the tensile strength at break is 1 N or more, the double-sided adhesive tape can exhibit better reprocessability at high temperatures. The tensile strength at break is more preferably 1.5 N or more.

[0111] The upper limit of the tensile strength at break is not particularly limited, but is preferably 10 N from the viewpoint of step followability and stress relaxation properties.

[0112] In the double-sided adhesive tape of the present invention, the tensile strength reduction rate when a sample obtained by slicing the first foamed resin layer is subjected to a tensile test at 80° C. is preferably 70% or less. If the tensile strength reduction rate is 70% or less, the double-sided adhesive tape can exhibit better reprocessability at high temperatures. The tensile strength reduction rate is more preferably 60% or less.

[0113] The lower limit of the reduction rate of tensile strength at break is not particularly limited, and the lower the better. The actual lower limit is about 10%.

[0114] The method of conducting a tensile test at 80° C. on a sample obtained by slicing the first foamed resin layer is as follows.

[0115] The double-sided adhesive tape was cut into strips of 5 mm in size, and the first foamed resin layer (center portion) was sliced ​​with a feather blade to obtain a sample of adhesive layer / second foamed resin layer / first foamed resin layer (about half the thickness).

[0116] Using the "Autograph AGS-X" manufactured by Shimadzu Corporation, each sample was subjected to a tensile test under the conditions of a tensile speed of 100 mm / min, a temperature of 80°C, and a distance between the clamps of 10 mm. It should be noted that after setting the sample at a distance between the clamps of 10 mm, the measurement was started after being placed in an environment of 80°C for 5 minutes. The strength when the sample broke was taken as the tensile breaking strength. In addition, the value of 1-(tensile breaking strength at 80°C / tensile breaking strength at 23°C) was calculated as the tensile breaking strength reduction rate.

[0117] The thickness of the double-sided adhesive tape of the present invention is not particularly limited, and the preferred lower limit is 100 μm, and the preferred upper limit is 3000 μm. If the above thickness is 100 μm or more, the adhesive force of the double-sided adhesive tape becomes sufficient, and the stress relaxation property also becomes sufficient. If the above thickness is 3000 μm or less, the double-sided adhesive tape can be used to achieve sufficient bonding and fixing, and the height difference tracking property of the two adhesive surfaces also becomes sufficient. The more preferred lower limit of the above thickness is 250 μm, the more preferred upper limit is 1600 μm, the further preferred lower limit is 350 μm, the further preferred upper limit is 1500 μm, the further preferred lower limit is 500 μm, and the further preferred upper limit is 1300 μm.

[0118] The method for producing the double-sided pressure-sensitive adhesive tape of the present invention may be, for example, the following method.

[0119] First, in acrylic copolymer, tackifier, crosslinking agent etc., add solvent and make the solution of adhesive A. Apply the solution of adhesive A to the demoulding treatment surface of release film, dry the solvent in the solution and remove it, thus forming adhesive layer. Utilize rubber roller etc. to pressurize and adhere the adhesive layer to the surface of foam substrate. Adhesive layer is also adhered to the other single side of foam substrate in the same way, and the double-sided adhesive tape having adhesive layer on both sides of foam substrate and the surface of adhesive layer covered by release film can be obtained.

[0120] The double-sided adhesive tape of the present invention can be used for any purpose, for example, to fix components in electronic devices. The electronic devices are not particularly limited, and examples thereof include televisions, monitors, portable electronic devices, and vehicle-mounted electronic devices.

[0121] Wherein, the double-sided adhesive tape of the present invention is suitable for display devices such as televisions and monitors, and is especially used for fixing components in relatively large display devices, specifically, for example, in the above-mentioned display device, the cover plate on the surface is fixed to the housing. The double-sided adhesive tape of the present invention can exert high holding power to shear load and tilt load, so it is also suitable for use even when the double-sided adhesive tape of narrow width is used to fix components in relatively large display devices. The double-sided adhesive tape of the present invention can be narrow width, and its width is not particularly limited, and the preferred lower limit is 0.5mm, and the preferred upper limit is 20mm, and the more preferred lower limit is 1mm, and the more preferred upper limit is 5mm. The shape of the double-sided adhesive tape of the present invention in these uses is not particularly limited, and rectangle, frame shape, circle, ellipse, annular shape etc. can be cited.

[0122] The double-sided pressure-sensitive adhesive tape of the present invention can also be used for interior decoration of vehicles, interior decoration of household appliances (eg, TVs, monitors, air conditioners, refrigerators, etc.), and the like.

[0123] Effects of the Invention

[0124] According to the present invention, a double-sided pressure-sensitive adhesive tape can be provided which has high step-adjustability on both pressure-sensitive adhesive surfaces, can exert high holding power against shear loads and tilt loads, has excellent reworkability on at least one pressure-sensitive adhesive surface, and is also excellent in handling properties during lamination. BRIEF DESCRIPTION OF THE DRAWINGS

[0125] Figure 1 Schematic diagram showing a 45° tilt holding force test of a double-sided adhesive tape.

[0126] Figure 2 Schematic diagram showing a shear holding force test of a double-sided adhesive tape.

[0127] Figure 3 This is a cross-sectional view schematically showing an example of the double-sided pressure-sensitive adhesive tape of the present invention. DETAILED DESCRIPTION

[0128] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0129] (Preparation of acrylic copolymer A)

[0130] In a reactor equipped with a thermometer, a stirrer, and a cooling tube, 159 parts by weight of ethyl acetate, 75 parts by weight of butyl acrylate (BA), 25 parts by weight of 2-ethylhexyl acrylate (2EHA), 0.1 parts by weight of 2-hydroxyethyl acrylate (HEA), and 5 parts by weight of acrylic acid (AAc) were added as solvents. After nitrogen substitution, the reactor was set in a water bath set at 60°C, and the reactor was heated to start reflux. 30 minutes after the start of reflux, 0.050 parts by weight of azobisisobutyronitrile as a polymerization initiator was added to the reactor and reacted for 6 hours. Then, ethyl acetate was added to the reactor to dilute and cool it, thereby obtaining a solution of acrylic copolymer A.

[0131] The obtained solution of acrylic copolymer A was diluted 50 times with tetrahydrofuran (THF), and the obtained dilution was filtered with a filter (material: polytetrafluoroethylene, pore size: 0.2 μm). The obtained filtrate was supplied to a gel permeation chromatograph (manufactured by Waters, 2690Separations Model), and GPC was performed under the conditions of a sample flow rate of 1 ml / min and a column temperature of 40°C to measure the polystyrene-converted molecular weight of acrylic copolymer A and obtain the weight average molecular weight (Mw). The weight average molecular weight (Mw) was 1.4 million. As a column, GPCKF-806L (manufactured by Showa Denko K.K.) was used, and as a detector, a differential refractometer was used.

[0132] (Preparation of acrylic copolymer B)

[0133] A solution of acrylic copolymer B was obtained in the same manner as acrylic copolymer A except that the solvent was changed to 100 parts by weight of ethyl acetate and 50 parts by weight of toluene and the polymerization initiator was changed to 0.14 parts by weight of azobisisobutyronitrile. The weight average molecular weight of the obtained acrylic copolymer B was 800,000.

[0134] (Preparation of acrylic copolymer C)

[0135] A solution of acrylic copolymer C was obtained in the same manner as acrylic copolymer A except that the polymerization initiator was changed to 0.04 parts by weight of azobisisobutyronitrile. The weight average molecular weight of the obtained acrylic copolymer C was 1,600,000.

[0136] (Preparation of acrylic copolymer D)

[0137] A solution of acrylic copolymer D was obtained in the same manner as acrylic copolymer A except that the blending amount of acrylic acid was changed to 3 parts by weight. The weight average molecular weight of the obtained acrylic copolymer D was 1,400,000.

[0138] (Preparation of acrylic copolymer E)

[0139] 50 parts by weight of ethyl acetate as a solvent was added to a reactor equipped with a thermometer, a stirrer, and a cooling tube. After nitrogen substitution, the reactor was heated and refluxed. 30 minutes after ethyl acetate was boiled, 0.20 parts by weight of azobisisobutyronitrile as a polymerization initiator was added. A monomer mixture consisting of 75 parts by weight of butyl acrylate, 25 parts by weight of 2-ethylhexyl acrylate, 0.1 parts by weight of 2-hydroxyethyl acrylate, and 3 parts by weight of acrylic acid was evenly and slowly added thereto over 1 hour and 30 minutes to react. 0.15 parts by weight of azobisisobutyronitrile was added 30 minutes after the addition was completed, and a polymerization reaction was further performed for 5 hours. Ethyl acetate was added to the reactor, and the mixture was cooled while being diluted to obtain a solution of acrylic copolymer E. The weight average molecular weight of the obtained acrylic copolymer E was 400,000.

[0140] (Styrene-acrylic block copolymer A)

[0141] A styrene-acrylic block copolymer A having the physical properties and composition shown in Table 1 was prepared.

[0142] [Table 1]

[0143]

[0144] (Example 1)

[0145] (1) Preparation of foam substrate

[0146] As the foamable composition for forming the first foamed resin layer (central foamed resin layer), a composition consisting of 100 parts by weight of a polyethylene resin (UBE polyethylene F420), 8.5 parts by weight of azodicarbonamide as a thermal decomposition type foaming agent, 1 part by weight of zinc oxide as a decomposition temperature regulator, and 0.5 parts by weight of 2,6-di-tert-butyl-p-cresol as an antioxidant was used.

[0147] As the foamable composition forming the second foamed resin layer (outermost layer), a composition consisting of 100 parts by weight of a polyethylene resin (UBE polyethylene F420), 1.1 parts by weight of azodicarbonamide as a thermal decomposition type foaming agent, 1 part by weight of zinc oxide as a decomposition temperature regulator, and 0.5 parts by weight of 2,6-di-tert-butyl-p-cresol as an antioxidant was used.

[0148] It should be noted that UBE polyethylene F420 refers to "UBEPOLYETHYLENE F420" (density: 0.920 g / cm 3 ).

[0149] The foamable composition forming the first foamed resin layer (the central foamed resin layer) and the foamable composition forming the second foamed resin layer (the outermost layer) were supplied to an extruder for multilayer extrusion molding and melt-kneaded at 130° C. After melt-kneading, a foam roll in the form of a long sheet having a thickness of about 1.0 mm and layers formed by the foamable composition forming the second foamed resin layer (the outermost layer) laminated on both sides of the layer formed by the foamable composition forming the first foamed resin layer (the central foamed resin layer) was extruded.

[0150] Next, the two sides of the long sheet-shaped foam roll were irradiated with an electron beam of 4.0 Mrad at an accelerating voltage of 500 kV to perform crosslinking. The crosslinked foam roll was continuously fed into a foaming furnace maintained at 250° C. by hot air and infrared heaters to heat and foam it, and the stretching ratio of MD was set to 3.5 times and the stretching ratio of TD was set to 3.5 times to stretch it. Thus, a foam substrate was obtained in which the second foamed resin layer (outermost layer)-1 and the second foamed resin layer (outermost layer)-2 were laminated on both sides of the first foamed resin layer (the central foamed resin layer). The thickness of each foamed resin layer and the foaming ratio based on JIS K 7222, as well as the thickness of the foam substrate and the 25% compressive strength based on JIS K 6254:2016 were measured. The measurement results are shown in Table 2.

[0151] (2) Production of double-sided adhesive tape

[0152] 15 parts by weight of polymerized rosin ester resin (Pensel D-135 manufactured by Arakawa Chemical Industries, Ltd., softening point 135°C, hydroxyl value 45) and 15 parts by weight of terpene phenolic resin (YS POLYSTAR G150 manufactured by Yasuhara Chemical Co., Ltd., softening point 150°C, hydroxyl value 135) were added to 100 parts by weight of the solid content of acrylic copolymer A. 30 parts by weight of ethyl acetate (manufactured by Fuji Chemicals Co., Ltd.) and 1.3 parts by weight of isocyanate crosslinking agent (manufactured by Nippon Polyurethane Co., Ltd., trade name "Coronate L45") as a solid content were further added and stirred to obtain an adhesive solution.

[0153] Prepare a release film with a thickness of 75 μm, apply an adhesive solution to the release treatment surface of the release film, and dry it at 110°C for 5 minutes to form an adhesive layer with a thickness of 50 μm. The adhesive layer is laminated to the surface of the foam substrate obtained above. Next, the same adhesive layer as above is laminated to the surface opposite to the foam substrate after peeling off the PET separator in the same manner. Then, heat at 40°C for 48 hours to mature. Thus, a double-sided adhesive tape covered with a release film is obtained.

[0154] (3) Determination of gel fraction

[0155] The double-sided adhesive tape was cut into a flat rectangular shape of 50 mm × 100 mm to prepare a test piece. After the test piece was immersed in ethyl acetate at 23°C for 24 hours, it was taken out from ethyl acetate and dried at 110°C for 1 hour. The weight of the test piece after drying was measured, and the gel fraction was calculated using the following formula (1). It should be noted that the release film for protecting the adhesive layer was not laminated on the test piece.

[0156] Gel fraction (wt%) = 100 × (W 2 -W 0 ) / (W 1 -W 0 )(1)

[0157] (W 0 : Weight of foam substrate, W 2 : Weight of the test piece before immersion, W 2 : Weight of the test piece after immersion and drying)

[0158] (4) Determination of storage modulus at 180°C

[0159] The storage modulus of the adhesive layer at 180° C. was determined using a viscoelasticity measuring device (Rheometrics Dynamic Analyze RDA-700 manufactured by Rheometrics) at a measuring temperature of −40 to 200° C., a heating rate of 3° C. / min, and a frequency of 10 Hz.

[0160] (5) Determination of strength when the extension is 5 mm from the initial distance between the clamps (tensile test)

[0161] Based on JIS K 7161, the strength at the time of elongation of 5 mm from the initial distance between clamping jigs was measured as follows.

[0162] The double-sided adhesive tape was punched into a dumbbell shape using a punching blade "Stretching No. 3 Dumbbell Shape" manufactured by Polymer Meter Co., Ltd. to prepare a test piece. The obtained test piece was stretched at a stretching speed of 50 mm / min at 25°C and a relative humidity of 50% using "Autograph AGS-X" manufactured by Shimadzu Corporation. At this time, the initial distance between the clamping fixtures was set to 60 mm, and the strength was read when the distance was extended by 5 mm (the distance between the clamping fixtures was 65 mm).

[0163] (6) Determination of 25% compressive strength

[0164] The 25% compressive strength of the double-sided pressure-sensitive adhesive tape was measured in accordance with JIS K 6254:2016 in the same manner as the 25% compressive strength of the foam substrate.

[0165] (7) 23℃ tensile test

[0166] The double-sided adhesive tape was cut into the size of dumbbell No. 3 (center width 5 mm), and the first foamed resin layer (center portion) was sliced ​​with a feather blade. Thus, the samples were divided into adhesive layer / second foamed resin layer (outermost layer)-1 / first foamed resin layer (about half the thickness) (referred to as "samples on the second foamed resin layer (outermost layer)-1 side") and first foamed resin layer (about half the thickness) / second foamed resin layer (outermost layer)-2 / adhesive layer (referred to as "samples on the second foamed resin layer (outermost layer)-2 side").

[0167] Each sample was subjected to a tensile test using "Autograph AGS-X" manufactured by Shimadzu Corporation at a tensile speed of 100 mm / min, a temperature of 23°C, and a distance between clamps of 45 mm. The strength at which the sample broke was taken as the tensile breaking strength, and the elongation at which the sample broke was taken as the tensile breaking elongation.

[0168] (8) 80℃ tensile test

[0169] The double-sided adhesive tape was cut into strips of 5 mm in size, and the first foamed resin layer (center portion) was sliced ​​with a feather blade. Thus, the samples were divided into adhesive layer / second foamed resin layer (outermost layer)-1 / first foamed resin layer (about half the thickness) (referred to as "samples on the second foamed resin layer (outermost layer)-1 side"), and first foamed resin layer (about half the thickness) / second foamed resin layer (outermost layer)-2 / adhesive layer (referred to as "samples on the second foamed resin layer (outermost layer)-2 side").

[0170] Using the "Autograph AGS-X" manufactured by Shimadzu Corporation, each sample was subjected to a tensile test under the conditions of a tensile speed of 100 mm / min, a temperature of 80°C, and a distance between the clamps of 10 mm. It should be noted that after setting the sample at a distance between the clamps of 10 mm, the measurement was started after being placed in an environment of 80°C for 5 minutes. The strength when the sample broke was taken as the tensile breaking strength. In addition, the value of 1-(tensile breaking strength at 80°C / tensile breaking strength at 23°C) was calculated as the tensile breaking strength reduction rate.

[0171] (Examples 2 to 6, 11 to 14)

[0172] A double-sided adhesive tape was obtained in the same manner as in Example 1 except that the foam substrate was changed as shown in Table 2. It should be noted that the thickness of the foamed resin layer was adjusted by adjusting the thickness during multi-layer extrusion and the stretching ratio in MD and TD, and the foaming ratio of the foamed resin layer was adjusted by adjusting the amount of the thermal decomposition type foaming agent.

[0173] (Examples 7 to 10)

[0174] The double-sided adhesive tape was obtained in the same manner as in Example 1 except that the adhesive layer was changed as shown in Table 2. It should be noted that in Example 6, acrylic copolymer B was used and the amount of the crosslinking agent was set to 1.9 parts by weight of the solid content. In Example 7, acrylic copolymer C was used and the amount of the crosslinking agent was set to 1.1 parts by weight of the solid content. In both Examples 8 and 9, acrylic copolymer D was used, but the gel fraction was changed by setting the amount of the crosslinking agent to 1.4 parts by weight of the solid content in Example 8 and 1.1 parts by weight of the solid content in Example 9.

[0175] (Comparative Example 1)

[0176] In "(1) Preparation of foam substrate", the foamable composition for forming the second foamed resin layer (outermost layer) was not used, but only the foamable composition for forming the first foamed resin layer (central foamed resin layer) was used. A double-sided adhesive tape was obtained in the same manner as in Example 1 except that a polyethylene terephthalate (PET) sheet and a styrene-acrylic copolymer sheet were laminated on both sides of the obtained first foamed resin layer (central foamed resin layer).

[0177] Specifically, in "(1) Preparation of foam substrate", first, only the first foamed resin layer (foamed resin layer in the center) is formed. Next, an adhesive solution containing acrylic copolymer A is applied to the surface of a polyethylene terephthalate (PET) sheet (manufactured by Toray Industries, Inc., X30) having a thickness of 50 μm, and dried at 110°C for 5 minutes, thereby forming an adhesive layer having a thickness of 20 μm. The obtained first foamed resin layer (foamed resin layer in the center) is laminated on the adhesive layer to obtain a laminate consisting of polyethylene terephthalate (PET) sheet / adhesive layer / first foamed resin layer (foamed resin layer in the center).

[0178] Further, 5 parts by weight of a crosslinking agent was added to the ethyl acetate solution of the styrene-acrylic block copolymer A relative to 100 parts by weight of the styrene-acrylic block copolymer A, and the mixture was applied to a 50 μm thick polyethylene terephthalate (PET) sheet with a demoulding treatment applied to the surface, and dried to obtain a non-crosslinked resin film with a thickness of 40 μm. As a crosslinking agent, a product name "Coronate L45" manufactured by Japan Polyurethane Co., Ltd. was used. The non-crosslinked resin film was laminated on the first foamed resin layer (foamed resin layer in the center) side of a laminate composed of a polyethylene terephthalate (PET) sheet / adhesive layer / first foamed resin layer (foamed resin layer in the center), to obtain a laminate composed of a polyethylene terephthalate (PET) sheet / adhesive layer / first foamed resin layer (foamed resin layer in the center) / non-crosslinked resin film. Next, the uncrosslinked resin film was thermally crosslinked by heating at 40°C for 48 hours, thereby obtaining a foam substrate consisting of polyethylene terephthalate (PET) sheet / adhesive layer / first foamed resin layer (center foamed resin layer) / styrene-acrylic copolymer sheet.

[0179] (Comparative Example 2)

[0180] In "(1) Preparation of foam substrate", a double-sided adhesive tape is obtained in the same manner as in Example 1 except that a foamable composition for forming the second foamed resin layer (outermost layer) is not used, but only a foamable composition for forming the first foamed resin layer (central foamed resin layer) is used, and styrene-acrylic copolymer sheets are laminated on both sides of the obtained first foamed resin layer (central foamed resin layer).

[0181] Specifically, in "(1) Preparation of foam substrate", first, only the first foamed resin layer (central foamed resin layer) is formed. Next, 5 parts by weight of a crosslinking agent is added to an ethyl acetate solution of a styrene-acrylic acid block copolymer A relative to 100 parts by weight of the styrene-acrylic acid block copolymer A, and the mixture is applied to a 50 μm thick polyethylene terephthalate (PET) sheet with a surface subjected to a demolding treatment, and dried to obtain a 40 μm thick uncrosslinked resin film. As a crosslinking agent, a product of Japan Polyurethane Co., Ltd., trade name "Coronate L45", is used.

[0182] An uncrosslinked resin film was laminated on the first foamed resin layer (the central foamed resin layer) to obtain a laminate consisting of uncrosslinked resin film / first foamed resin layer (the central foamed resin layer). Next, the uncrosslinked resin film was thermally crosslinked by heating at 40° C. for 48 hours to obtain a laminate consisting of styrene-acrylic copolymer sheet / first foamed resin layer (the central foamed resin layer).

[0183] Furthermore, the uncrosslinked resin film prepared in the same manner was laminated on the first foamed resin layer (the central foamed resin layer) side of the laminate composed of the styrene-acrylic copolymer sheet / the first foamed resin layer (the central foamed resin layer) to obtain a laminate composed of the styrene-acrylic copolymer sheet / the first foamed resin layer (the central foamed resin layer) / uncrosslinked resin film. Next, the uncrosslinked resin film was thermally crosslinked by heating at 40° C. for 48 hours to obtain a foam substrate composed of the styrene-acrylic copolymer sheet / the first foamed resin layer (the central foamed resin layer) / styrene-acrylic copolymer sheet.

[0184] (Comparative Example 3)

[0185] In "(1) Preparation of foam substrate", a double-sided adhesive tape was obtained in the same manner as in Example 1, except that a foamable composition for forming the second foamed resin layer (outermost layer) was not used, and only a foamable composition for forming the first foamed resin layer (central foamed resin layer) was used, and polyethylene (PE) sheets were laminated on both sides of the obtained first foamed resin layer (central foamed resin layer).

[0186] Specifically, in "(1) Preparation of foam substrate", first, only the first foamed resin layer (foamed resin layer in the center) is formed. A release film with a thickness of 75 μm is prepared, and an adhesive solution containing acrylic copolymer A is applied to the release-treated surface of the release film, and dried at 110°C for 5 minutes to form an adhesive layer with a thickness of 6 μm. Next, the adhesive layer is bonded to the surface of a low-density polyethylene (PE) sheet with a thickness of 40 μm to obtain a laminate consisting of an adhesive layer / low-density polyethylene (PE) sheet. The release film of the adhesive layer in the laminate consisting of an adhesive layer / low-density polyethylene (PE) sheet is peeled off and bonded to the first foamed resin layer (foamed resin layer in the center). Next, in the same manner, an adhesive layer / low-density polyethylene (PE) sheet is also bonded to the surface opposite to the first foamed resin layer (foamed resin layer in the center). Then, it is heated at 40°C for 48 hours to be cured. A foam substrate consisting of polyethylene (PE) sheet / adhesive layer / first foamed resin layer (central foamed resin layer) / adhesive layer / polyethylene (PE) sheet was obtained.

[0187] (Comparative Example 4)

[0188] In "(1) Preparation of foam substrate", a double-sided adhesive tape was obtained in the same manner as in Example 2, except that a foamable composition for forming the second foamed resin layer (outermost layer) was not used, and only a foamable composition for forming the first foamed resin layer (central foamed resin layer) was used, and a polyethylene terephthalate (PET) sheet was laminated on one side of the obtained first foamed resin layer (central foamed resin layer).

[0189] Specifically, in "(1) Preparation of foam substrate", first, only the first foamed resin layer (foamed resin layer in the center) is formed. Next, an adhesive solution containing acrylic copolymer A is applied to the surface of a polyethylene terephthalate (PET) sheet (manufactured by Toray Industries, Inc., X30) having a thickness of 50 μm, and dried at 110°C for 5 minutes, thereby forming an adhesive layer having a thickness of 20 μm. The obtained first foamed resin layer (foamed resin layer in the center) is laminated on the adhesive layer to obtain a foam substrate consisting of polyethylene terephthalate (PET) sheet / adhesive layer / first foamed resin layer (foamed resin layer in the center).

[0190] (Comparative Example 5)

[0191] In “(1) Preparation of foam substrate”, a double-sided adhesive tape was obtained in the same manner as in Example 2, except that a foaming composition for forming the second foaming resin layer (outermost layer) was not used, but only a foaming composition for forming the first foaming resin layer (center foaming resin layer).

[0192] (Comparative Examples 6 to 8)

[0193] A double-sided adhesive tape was obtained in the same manner as in Example 1 except that the adhesive layer was changed as shown in Table 3. In Comparative Example 6, acrylic copolymer E was used, but the gel fraction was changed by setting the amount of the crosslinking agent to 2.5 parts by weight of the solid content. In Comparative Example 7, acrylic copolymer D was used in the same manner as in Examples 8 and 9, but the gel fraction was changed by setting the amount of the crosslinking agent to 0.7 parts by weight of the solid content.

[0194] (Comparative Example 9)

[0195] In "(1) Preparation of Foam Base Material", only the foamable composition for forming the first foamable resin layer (the central foamable resin layer) was used instead of the foamable composition for forming the second foamable resin layer (the outermost layer). A double-sided adhesive tape was obtained in the same manner as in Example 1 except that acrylic copolymer sheets were laminated on both sides of the obtained first foamable resin layer (the central foamable resin layer).

[0196] Specifically, in "(1) Preparation of foam substrate", first, only the first foamed resin layer (the central foamed resin layer) is formed. Next, 100 parts by weight of ethyl acetate is added to 45 parts by weight of LA2270 manufactured by Kuraray Co., Ltd. and stirred to obtain a solution. The obtained solution is applied to a 50 μm thick polyethylene terephthalate (PET) sheet with a surface release treatment, and dried at 110°C for 5 minutes to obtain a resin film with a thickness of 40 μm. The exposed side of the resin film is bonded to one side of the first foamed resin layer (the central foamed resin layer). A resin film with a thickness of 40 μm is again prepared by the same operation as above, and the exposed side of the resin film is bonded to the side opposite to the first foamed resin layer (the central foamed resin layer) to obtain a foam substrate.

[0197] <Evaluation>

[0198] The double-sided pressure-sensitive adhesive tapes obtained in Examples and Comparative Examples were evaluated as follows. The results are shown in Tables 4 and 5.

[0199] (1) Evaluation of high and low difference tracking

[0200] A single-sided adhesive tape (125mm×20mm, 300μm thick) was pasted on a glass plate (125mm×50mm, 1.5mm thick) to create a height difference of 300μm. The double-sided adhesive tape was cut into a size of 25mm×50mm, and one side was lined with a polyethylene terephthalate (PET) sheet with a thickness of 23μm. The other side of the double-sided adhesive tape was pasted on the side of the glass plate where the height difference was created, and a 2kg rubber roller was reciprocated once from the glass plate side to perform pressure bonding. The air bite distance from the height difference portion was measured and evaluated according to the following criteria.

[0201] A: The air penetration distance is less than 700μm

[0202] B: The air penetration distance is 700 μm or more and less than 800 μm

[0203] C: The air penetration distance is 800 μm or more and less than 900 μm

[0204] D: The air penetration distance is 900 μm or more and less than 1000 μm

[0205] E: Air penetration distance is 1000 μm or more

[0206] (2) Evaluation of retention

[0207] (2-1) 45° tilt holding force test

[0208] exist Figure 1Schematic diagram showing a 45° tilt holding force test of a double-sided adhesive tape is shown in FIG.

[0209] The obtained double-sided adhesive tape 18 was cut into a size of 25 mm×25 mm, and the adhesive layer on the second foamed resin layer (outermost layer)-2 side was attached to the glass plate 17, and a 2 kg rubber roller was reciprocated once at a speed of 300 mm / min on the double-sided adhesive tape 18. Next, the adhesive layer on the second foamed resin layer (outermost layer)-1 side of the double-sided adhesive tape 18 was attached to the SUS plate 16, and after being pressed from the SUS plate 16 side with a 5 kg weight for 10 seconds, it was placed in an environment of 23° C. and a relative humidity of 50% for 24 hours to prepare a test sample.

[0210] The test sample was placed at 60°C and 90% relative humidity with a 1 kg weight 15 installed at the center of the SUS plate 16 to apply a load to the double-sided adhesive tape 18 and the SUS plate 16. The sample was maintained at an inclination of 45° and the time until the weight 15 fell (falling time) was measured. Evaluation was performed according to the following criteria.

[0211] ○: Falling time is more than 250 hours

[0212] △: Drop time is more than 50 hours and less than 250 hours

[0213] ×: Drop time is less than 50 hours

[0214] (2-2) Shear holding force test

[0215] exist Figure 2 Schematic diagram showing the shear holding force test of a double-sided adhesive tape is shown in FIG. Figure 2 (a) Main view, Figure 2 (b) is a side view.

[0216] like Figure 2 As shown in (a) and (b), the adhesive layer on the second foamed resin layer (outermost layer)-2 side of the double-sided adhesive tape 3 was backed by a PET film (#50) 4. The adhesive layer on the second foamed resin layer (outermost layer)-1 side of the double-sided adhesive tape 3 was adhered to the SUS plate 1 and the SUS plate 2 to prepare a test sample with a bonding area of ​​25 mm×25 mm between the SUS plate 1 and the double-sided adhesive tape 3. The test sample was prepared as follows.

[0217] First, prepare SUS plate 1 (thickness 2mm×50mm×70mm, the surface of the SUS304 steel plate specified in JIS-G-4305 was evenly polished with water-resistant polishing paper No. 360) and SUS plate 2 (thickness 1mm×30mm×50mm, not polished). After cleaning SUS plate 1 and SUS plate 2 with ethanol, dry them thoroughly. Cut the double-sided adhesive tape 3 into a width of 25mm×length of 140mm, peel off the release film on one side, and stick a PET film (#50) 4 on the exposed adhesive layer. Next, peel off the release film on the other side, and stick the end of the exposed adhesive layer to the SUS plate 1 in a way that bubbles cannot enter, and crimp with a 2kg rubber roller reciprocating once at a speed of 10mm / second. At this time, the SUS plate 1 and the double-sided adhesive tape 3 are pasted in a way that overlaps 30mm. Furthermore, the end of the adhesive layer on the opposite side to the end attached to the SUS plate 1 was attached to the SUS plate 2, and a 2 kg rubber roller was reciprocated once at a speed of 10 mm / second to perform pressure bonding. At this time, the double-sided adhesive tape 3 was arranged in a manner covering the front and back sides of the SUS plate 2. Then, the through hole 5 was provided in the double-sided adhesive tape 3 together with the SUS plate 2, and the double-sided adhesive tape 3 was cut in a manner that the attachment area of ​​the SUS plate 1 and the double-sided adhesive tape 3 became 25 mm×25 mm.

[0218] After the test sample prepared as described above was placed in a thermostatic chamber at 50°C and 80%RH for 24 hours, a 2kg weight 6 was installed on the through hole 5 under the same environment, and the offset after 200 hours was measured and evaluated according to the following criteria. In addition, the shear holding power of the adhesive layer on the second foamed resin layer (outermost layer)-2 side of the double-sided adhesive tape 3 was also evaluated in the same manner.

[0219] ○: The deviation after 200 hours is less than 2 mm

[0220] △: The deviation after 200 hours is 2 mm or more and less than 10 mm

[0221] ×: Displacement after 200 hours is 10 mm or more

[0222] (3) Evaluation of reprocessability at 23°C and 80°C

[0223] Cut the double-sided adhesive tape into a size of 5mm×100mm, and stick one side to the glass plate. Stick the other side of the double-sided adhesive tape to the glass plate to make a laminate of glass plate / double-sided adhesive tape / glass plate, and press it with a weight of 5kg for 10 seconds. Slice the first foamed resin layer (central part) of the obtained laminate with a feather blade. Thus, it is divided into a sample of glass plate / adhesive layer / second foamed resin layer (outermost layer)-1 / first foamed resin layer (about half the thickness) (set as "sample on the side of the second foamed resin layer (outermost layer)-1"), and a sample of the first foamed resin layer (about half the thickness) / second foamed resin layer (outermost layer)-2 / adhesive layer / glass plate (set as "sample on the side of the second foamed resin layer (outermost layer)-2").

[0224] In the evaluation of the reworkability at 23° C., each sample was left to stand at 23° C. for 4 days, and then the double-sided adhesive tape portion was peeled off from the glass plate at high speed by hand.

[0225] In the evaluation of the reworkability at 80° C., each sample was left at 80° C. for 1 day, and immediately after being taken out, the double-sided adhesive tape portion was peeled off from the glass plate by hand at high speed.

[0226] ◎: No adhesive residue, the double-sided adhesive tape is not broken, and the glass plate can be reprocessed ○: There is adhesive residue, but the double-sided adhesive tape is not broken, and the glass plate can be reprocessed

[0227] ×: The double-sided adhesive tape is broken and the glass plate cannot be reprocessed

[0228] Based on the evaluation results of the samples on the second foamed resin layer (outermost layer)-1 side and the samples on the second foamed resin layer (outermost layer)-2 side, comprehensive evaluation of reprocessability was performed on 23°C reprocessability and 80°C reprocessability according to the following criteria.

[0229] ◎: The evaluation results of the sample on the second foamed resin layer (outermost layer)-1 side and the sample on the second foamed resin layer (outermost layer)-2 side were both ◎

[0230] ○: At least one of the evaluation results of the sample on the second foamed resin layer (outermost layer)-1 side and the sample on the second foamed resin layer (outermost layer)-2 side is ◎, or both are ○

[0231] △: At least one of the evaluation results of the sample on the second foamed resin layer (outermost layer)-1 side and the sample on the second foamed resin layer (outermost layer)-2 side is ○

[0232] ×: The evaluation results of the sample on the second foamed resin layer (outermost layer)-1 side and the sample on the second foamed resin layer (outermost layer)-2 side were both ×

[0233] (4) Evaluation of processability

[0234] The obtained double-sided adhesive tape was cut into a size of 3 mm in width × 10 mm in length, and stretched at 1 N for 10 seconds using Autograph AGS-X (manufactured by Shimadzu Corporation) at 25°C and a relative humidity of 50%, and the elongation (mm) was measured. Evaluation was performed according to the following criteria. The initial load change was set to 1 N / sec.

[0235] ○: Elongation is less than 10 mm.

[0236] ×: The elongation is 10 mm or more.

[0237] (5) Evaluation of whether there is breakage

[0238] The obtained double-sided adhesive tape was cut into a size of 100 mm×300 mm and was wound around a paper core having a diameter of 3 inches so that the second foamed resin layer (outermost layer)-2 side was on the inner side to obtain a roll.

[0239] The double-sided pressure-sensitive adhesive tape was unwound from the obtained roll, and then visually observed and evaluated based on the following criteria.

[0240] ○: No breakage was observed.

[0241] ×: The breakage was confirmed.

[0242] [Table 2]

[0243]

[0244] [Table 3]

[0245]

[0246] [Table 4]

[0247]

[0248] [Table 5]

[0249]

[0250] Industrial Applicability

[0251] According to the present invention, a double-sided pressure-sensitive adhesive tape can be provided which has high step-adjustability on both pressure-sensitive adhesive surfaces, can exert high holding power against shear loads and tilt loads, has excellent reworkability on at least one pressure-sensitive adhesive surface, and is also excellent in handling properties during lamination.

[0252] Description of Reference Numerals

[0253] 1.2 SUS board

[0254] 3 Test piece (double-sided adhesive tape)

[0255] 4 PET film (#50)

[0256] 5 Through holes

[0257] 6 weights (3kg)

[0258] 7 Double-sided adhesive tape

[0259] 8 Foam substrate

[0260] 91, 92 Adhesive layer

[0261] 10 1st foamed resin layer

[0262] 11, 12 Second foamed resin layer

[0263] 15 weights (1kg)

[0264] 16 SUS plate

[0265] 17 Glass Plate

[0266] 18 Double-sided adhesive tape

Claims

1. A double-sided adhesive tape, characterized in that: A foam substrate and adhesive layers laminated on both sides of the foam substrate. The foam substrate comprises a first foamed resin layer and a second foamed resin layer laminated on at least one side of the first foamed resin layer, wherein the second foamed resin layer has a lower foaming ratio than the first foamed resin layer. At least one of the adhesive layers has a storage modulus of 11000 Pa or more at 180°C.

2. The double-sided adhesive tape according to claim 1, characterized in that The foam substrate has no other layer between the first foamed resin layer and the second foamed resin layer.

3. The double-sided adhesive tape according to claim 1 or 2, characterized in that: The double-sided adhesive tape has a strength of 1.5 N or more when stretched 5 mm from an initial distance between clamps in a tensile test.

4. The double-sided adhesive tape according to claim 1 or 2, characterized in that: The 25% compressive strength of the foam substrate is 200 kPa or less.

5. The double-sided adhesive tape according to claim 1 or 2, characterized in that: The double-sided adhesive tape has a tensile breaking strength of 2N or more when a sample formed by slicing the first foamed resin layer is subjected to a 23°C tensile test, and a tensile breaking strength of 2N or more when a sample formed by slicing the first foamed resin layer is subjected to an 80°C tensile test, and the tensile breaking strength reduction rate is less than 70%.

6. The double-sided adhesive tape according to claim 1 or 2, characterized in that: The double-sided adhesive tape has a tensile breaking elongation of 30 mm or more when a sample obtained by slicing the first foamed resin layer is subjected to a 23° C. tensile test.

7. The double-sided adhesive tape according to claim 1 or 2, characterized in that: The first foamed resin layer is a polyolefin foamed resin layer with a foaming ratio of 5 cm 3 / g or more and 30cm 3 / g or less.

8. The double-sided adhesive tape according to claim 1 or 2, characterized in that: The foam substrate has the second foamed resin layer on both surfaces of the first foamed resin layer.

9. The double-sided adhesive tape according to claim 8, characterized in that The second foamed resin layer on both sides of the first foamed resin layer has the same expansion ratio.

10. The double-sided adhesive tape according to claim 1 or 2, characterized in that: At least one of the pressure-sensitive adhesive layers contains an acrylic copolymer having a weight average molecular weight of 500,000 or more, and has a gel fraction of 15% by weight or more.

11. The double-sided adhesive tape according to claim 1 or 2, characterized in that: The second foamed resin layer is a polyolefin foamed resin layer.

12. The double-sided adhesive tape according to claim 1 or 2, characterized in that: The double-sided adhesive tape has a width of 20 mm or less.

13. The double-sided adhesive tape according to claim 1 or 2, characterized in that: The double-sided adhesive tape has a thickness of 100 μm or more and 3000 μm or less.

14. The double-sided adhesive tape according to claim 1 or 2, characterized in that: The double-sided adhesive tape has a 25% compressive strength of 20 kPa or more and 70 kPa or less.

15. The double-sided adhesive tape according to claim 1 or 2, characterized in that: The second foamed resin layer has a thickness of 100 μm or less.

16. The double-sided adhesive tape according to claim 1 or 2, characterized in that: In the foam substrate, a ratio of the thickness of the first foamed resin layer to the thickness of the second foamed resin layer, that is, a value of the thickness of the first foamed resin layer / the thickness of the second foamed resin layer is 1.0 or more and 400 or less.

17. The double-sided adhesive tape according to claim 1 or 2, characterized in that: In the foam substrate, a ratio of the expansion ratio of the first foamed resin layer to the expansion ratio of the second foamed resin layer, that is, a value of the expansion ratio of the first foamed resin layer / the expansion ratio of the second foamed resin layer is 1.3 or more and 100 or less.

18. A double-sided adhesive tape, characterized in that: A foam substrate and adhesive layers laminated on both sides of the foam substrate. The foam substrate comprises a first polyolefin foamed resin layer and a second polyolefin foamed resin layer laminated on at least one side of the first polyolefin foamed resin layer, wherein the second polyolefin foamed resin layer has a lower foaming ratio than the first polyolefin foamed resin layer. The 25% compressive strength of the foam substrate as a whole is 200 kPa or less. At least one of the adhesive layers has a storage modulus of 11000 Pa or more at 180°C.