Separation and recovery process method, process equipment and control equipment for mixture
By layering the mixture containing silicone oil and metal lithium and reacting metal lithium with water, lithium recovery and multiple recycling of silicon oil are achieved, solving the problems of active lithium consumption and safety risks in lithium-ion batteries, and improving the risk of increased active lithium Battery performance and resource utilization.
Patent Information
- Application Number
- CN202411057628.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-31
- Publication Date
- 2024-11-19
AI Technical Summary
During the formation of lithium-ion batteries, the formation of the negative electrode SEI film consumes a large amount of active lithium, especially when high-capacity silicon-based negative electrode materials are used, resulting in low coulomb efficiency and battery capacity in the first week of the battery. The existing lithium supplementation method poses safety risks. and the issue of waste of lithium resources.
Using a mixture separation and recovery process, the silicone oil layer is separated from the lithium-containing layer by layering the mixture containing silicone oil and lithium metal, and the reaction between metal lithium and water is used to generate lithium hydroxide to achieve lithium recovery and multiple recycling of silicone oil reduces waste of lithium resources and safety risks.
Effective recycling of lithium resources reduces the waste of lithium resources, improves the recovery rate of lithium, and reduces the cost during the lithium chip collection process through multiple recycles of silicone oil, and improves the first week of the battery's coulomb efficiency and battery capacity.
Smart Images

Figure CN118979159A_ABST
Abstract
Description
[0001] This application is a divisional application of the Chinese application with application number 202211362117.5, application date October 31, 2022, and invention name “Separation and recovery process method, process equipment and control equipment for mixture”. Technical Field
[0002] The present invention relates to the technical field of chemical material separation and recovery, and in particular to a separation and recovery process method, process equipment and control equipment for a mixture. Background Art
[0003] During the formation process of lithium-ion batteries, the formation of the negative electrode SEI film consumes a large amount of active lithium, especially when some high-capacity silicon-based negative electrode materials are added, resulting in low coulombic efficiency and battery capacity in the first week of the battery. Supplementing active lithium is an effective means to solve this problem. Currently, many ways of supplementing active lithium have been reported, mainly two categories: negative electrode lithium supplementation and positive electrode lithium supplementation. For example, negative electrode lithium supplementation includes physical mixed lithiation of metallic lithium, such as adding metallic lithium powder to the negative electrode or rolling metallic lithium foil on the surface of the electrode.
[0004] Metallic lithium chips will be generated in the lithium replenishment process. Metallic lithium is active and needs to be collected. Collecting them separately has great safety risks. In the prior art, silicone oil infiltration and passivation methods can greatly reduce the risk of lithium chip collection. However, the metallic lithium chips infiltrated with silicone oil need to be further separated and recovered to save lithium resources. Summary of the invention
[0005] The main purpose of the present invention is to provide a separation and recovery process method for a mixture, aiming to separate silicone oil and metallic lithium and recover lithium to save lithium resources.
[0006] To achieve the above object, the present invention provides a separation and recovery process for a mixture, characterized in that the separation and recovery process for the mixture comprises the following steps:
[0007] The mixture containing silicone oil and metallic lithium is treated in layers to separate the silicone oil layer and the lithium-containing layer;
[0008] The silicone oil layer is separated from the lithium-containing layer, and the metallic lithium is collected from the separated lithium-containing layer.
[0009] Optionally, in the step of separating the silicone oil layer from the lithium-containing layer and collecting the metallic lithium from the separated lithium-containing layer, the following steps are included:
[0010] The silicone oil layer is separated from the lithium-containing layer, the metallic lithium is collected from the separated lithium-containing layer, and the separated silicone oil layer is used for passivation collection of metallic lithium.
[0011] Taking into account that the mixture containing silicone oil and metallic lithium in the present application is derived from the mixture produced in the process of collecting lithium chips during the lithium replenishment process, the separation and recovery process method of the present application is adopted to separate the silicone oil layer from the lithium-containing layer, collect the metallic lithium from the separated lithium-containing layer, and apply the separated silicone oil layer to the passivation collection step of metallic lithium. Not only can lithium be recovered to save lithium resources, and the recovered lithium can be used in the lithium replenishment process, but the separated silicone oil layer can also be used for the passivation collection of metallic lithium. That is, the recovered silicone oil can be recycled for many times, greatly reducing the cost of silicone oil used in the process of collecting metallic lithium chips.
[0012] Optionally, in the step of treating the mixture containing silicone oil and metallic lithium in layers to separate the silicone oil layer and the lithium-containing layer, the following steps are included:
[0013] A mixture containing silicone oil and metallic lithium and water are put into a reaction device to make the metallic lithium react with the water, so that the silicone oil layer and the lithium-containing layer are separated into layers.
[0014] A simple solid-liquid separation method cannot completely remove the silicone oil on the surface of metallic lithium. In order to achieve effective separation, metallic lithium is reacted with water to generate lithium hydroxide. The lithium hydroxide exists in the water phase, and the water phase is separated from the silicone oil layer to achieve the separation of lithium compounds and silicone oil.
[0015] Optionally, the step of adding a mixture containing silicone oil and metallic lithium and water into a reaction device to allow the metallic lithium to react with the water to separate the silicone oil layer and the lithium-containing layer includes the following steps:
[0016] Water is added to the reaction device, and a mixture containing silicone oil and metallic lithium is put into the reaction device in batches, so that the metallic lithium reacts with the water, and the silicone oil layer and the lithium-containing layer are separated into layers.
[0017] Considering that the reaction between lithium metal and water is an exothermic reaction and produces hydrogen, for safety reasons, the mixture containing silicone oil and lithium metal is added to the reaction device in small amounts and multiple times to avoid the risk of combustion caused by violent reactions. The specific number of times of addition is not limited and is allocated according to the amount of the mixture.
[0018] Optionally, the weight of the mixture containing silicone oil and metallic lithium added in each batch is 1g-10g.
[0019] A smaller amount of a mixture containing silicone oil and metallic lithium is used to react with water to avoid an overly violent reaction, thereby ensuring that the reaction process does not cause a risk of combustion due to excessive intensity.
[0020] Optionally, the weight of the mixture containing silicone oil and metallic lithium added in each batch is 1g-5g;
[0021] And / or, the content of metallic lithium in the mixture containing silicone oil and metallic lithium is 10%-80%.
[0022] In order to further ensure that the reaction process does not cause the risk of combustion due to excessive intensity, the weight of the mixture containing silicone oil and metallic lithium added in each batch is 1g-5g.
[0023] In order to further ensure that the reaction process will not cause the risk of combustion due to excessive intensity, the content of metallic lithium in the mixture of silicone oil and metallic lithium is 10%-80%, and the content of metallic lithium in the mixture of silicone oil and metallic lithium can be 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80%.
[0024] Optionally, the ratio of the weight of the mixture containing silicone oil and metallic lithium put into the reaction device in each batch to the weight of the water is (1:100)-(1:2000).
[0025] The amount of water should not be too much, as it will lead to waste. At the same time, the amount of water should not be too little, as too little water will lead to too high concentration of reaction products in the later stage of the reaction, slowing down the reaction rate and prolonging the operation time. Therefore, the weight ratio of the mixture containing silicone oil and metal lithium put into the reaction device in each batch to the weight ratio of water is (1:100)-(1:2000).
[0026] Optionally, the ratio of the weight of the mixture containing silicone oil and metallic lithium put into the reaction device in each batch to the weight of the water is: (1:1000)-(1:2000);
[0027] And / or, the content of metallic lithium in the mixture containing silicone oil and metallic lithium is 10%-80%.
[0028] Under the premise of ensuring a complete and rapid reaction, the less water there is, the higher the concentration of lithium hydroxide generated by the reaction is, which can slow down the subsequent reaction speed and avoid the risk of combustion caused by violent reactions. The weight ratio of the mixture of silicone oil and metallic lithium put into the reaction device in each batch to the weight of water is (1:1000)-(1:2000). In order to ensure a full reaction, the content of metallic lithium in the mixture of silicone oil and metallic lithium is 10%-80%, and the content of metallic lithium in the mixture of silicone oil and metallic lithium can be 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80%.
[0029] Optionally, water is added to the reaction device, and the mixture containing silicone oil and metallic lithium is added to the reaction device in batches, so that the metallic lithium reacts with the water, and in the step of separating the silicone oil layer and the lithium-containing layer, the interval time between batches is 5s-10s.
[0030] In order to ensure that the metallic lithium in the mixture containing silicone oil and metallic lithium added each time can react completely, the interval time between batches is 5s-10s, for example, the interval time can be 5s, 6s, 7s, 8s, 9s, 10s.
[0031] Optionally, the interval time is 7-10s.
[0032] In order to avoid the situation where the metallic lithium in the previous batch of the mixture of silicone oil and metallic lithium has not yet reacted completely, and the next batch of the mixture of silicone oil and metallic lithium is added, resulting in the superposition of multiple batches of reactions, too fast a feeding speed, too much unreacted metallic lithium in the water, and the risk of combustion due to violent reaction, the feeding time is controlled within the range of 7-10s. For example, the interval time can be 7s, 8s, 9s, or 10s.
[0033] Optionally, the step of separating the silicone oil layer from the lithium-containing layer and collecting the metallic lithium from the separated lithium-containing layer includes the following steps:
[0034] The silicone oil layer is separated from the lithium-containing layer, and carbon dioxide is introduced into the separated lithium-containing layer to make the lithium-containing compound in the lithium-containing layer react with the carbon dioxide to obtain a reactant.
[0035] In order to extract metallic lithium from lithium hydroxide aqueous solution, lithium hydroxide is converted into lithium carbonate, and lithium carbonate solution has the value of extracting metallic lithium. Therefore, the silicone oil layer is separated from the lithium-containing layer, and carbon dioxide is introduced into the separated lithium-containing layer to make the lithium-containing compound in the lithium-containing layer react with carbon dioxide to obtain a reactant, which is lithium carbonate.
[0036] Optionally, the carbon dioxide is introduced at a rate of 1 L / min-20 L / min.
[0037] For the convenience of operation, the carbon dioxide introduction rate is 1L / min-20L / min, and the carbon dioxide introduction rate can be 1L / min, 5L / min, 10L / min, 15L / min, and 20L / min.
[0038] Optionally, the carbon dioxide is introduced at a rate of 5 L / min-10 L / min.
[0039] In order to take into account both reaction rate and ease of operation, the amount of carbon dioxide introduced is 5L / min-10L / min, and the amount of carbon dioxide introduced can be 5L / min, 7L / min, 9L / min, and 10L / min.
[0040] Optionally, in the step of treating the mixture containing silicone oil and metallic lithium in layers to separate the silicone oil layer and the lithium-containing layer, the following steps are included:
[0041] A mixture containing silicone oil and metallic lithium is put into a reaction device, and the reaction device is heated to melt the metallic lithium, so that the silicone oil layer and the lithium-containing layer are separated into layers.
[0042] In order to separate the silicone oil from the metallic lithium, the mixture containing the silicone oil and the metallic lithium in the reaction device is heated to melt the metallic lithium. The metallic lithium melt and the silicone oil produced after melting are separated into layers due to their different densities, and the separated silicone oil and the molten metallic lithium can be separated. For example, the density of the silicone oil is greater than that of the metallic lithium, and the silicone oil will be present in the lower layer of the melt, and the silicone oil can flow out from the opening at the lower end of the reaction device.
[0043] Optionally, the heating temperature of the reaction device is 200°C-300°C.
[0044] The melting point of metallic lithium is 180°C. The metallic lithium can be melted by heating at 200°C for a long time, or by increasing the temperature to 300°C and heating rapidly to melt the metallic lithium. There is no specific limitation. For example, the heating temperature of the reaction device can be 200°C, 250°C, or 300°C.
[0045] Optionally, the heating time of the reaction device is 1h-2h.
[0046] According to actual operation, the heating time can be selected to be 1h-2h, for example, 1h, 1.5h, 2h. A high heating temperature can shorten the heating time, and a low heating temperature can extend the heating time.
[0047] Optionally, the step of separating the silicone oil layer from the lithium-containing layer and collecting the metallic lithium from the separated lithium-containing layer includes the following steps:
[0048] The silicone oil layer is separated from the lithium-containing layer, and the separated lithium-containing layer is put into a distillation tank to purify the metallic lithium by distillation.
[0049] After the silicone oil and the molten metallic lithium are separated, some silicone oil impurities may still exist in the molten metallic lithium. Therefore, the metallic lithium is purified by distillation. Specifically, the metallic lithium is purified by distillation by utilizing the large difference in boiling points between the metallic lithium (boiling point of about 1340°C) and the silicone oil in the mixture of molten metallic lithium and silicone oil.
[0050] Optionally, during the distillation and purification process, the distillation temperature is 100°C-500°C.
[0051] By setting the distillation temperature to the boiling point of the silicone oil or above the boiling point, the silicone oil can be separated from the molten metallic lithium. The distillation temperature can be 100°C, 200°C, 300°C, 400°C, or 500°C.
[0052] Optionally, during the distillation and purification process, the distillation temperature is 100°C-200°C;
[0053] And / or, during the distillation and purification process, the distillation heating time is 2h-3h.
[0054] In order to avoid the loss of metallic lithium due to the carrying of metallic lithium during the silicone oil separation process caused by the distillation temperature being too high and the distillation rate being too fast, the distillation temperature can be controlled at 100°C, 150°C, or 200°C.
[0055] The distillation heating time can be adjusted accordingly according to the selection of the distillation temperature to ensure the effective separation of silicone oil and metallic lithium. The distillation time can be 2h, 2.5h, or 3h.
[0056] The present application provides a separation and recovery process equipment for a mixture, and the separation and recovery process equipment for the mixture comprises:
[0057] A reaction device, wherein the reaction device is used to load a mixture containing silicone oil and metallic lithium;
[0058] A lithium-containing layer recovery device, the lithium-containing layer recovery device is connected to the reaction device and is used to recover the lithium-containing layer;
[0059] A silicone oil recovery device is connected to the reaction device to recover silicone oil.
[0060] In the process of reacting metallic lithium with water, the reaction device is used to add a mixture containing silicone oil and metallic lithium and water, so that the metallic lithium reacts with water to generate a lithium hydroxide aqueous solution. The lithium hydroxide aqueous solution is separated from the silicone oil and the silicone oil, with the silicone oil located in the upper layer and the silicone oil located in the lower layer. The lithium-containing layer recovery device is connected to the lower part of the reaction device, and the silicone oil recovery device is connected to the upper part of the reaction device, so that the lithium hydroxide aqueous solution is recovered from the lower part of the reaction device to the lithium-containing layer recovery device, and the silicone oil is recovered from the upper part of the reaction device to the silicone oil recovery device. The recovered silicone oil is further used for lithium chips collection.
[0061] In the process of heating and melting the metallic lithium in the mixture containing silicone oil and metallic lithium to achieve separation of metallic lithium and silicone oil, a reaction device is used to add the mixture containing silicone oil and metallic lithium, and the reaction device has a heating structure. The reaction device is heated to make the metallic lithium molten. The molten metallic lithium is located on the upper layer of the silicone oil. The lithium-containing layer recovery device is connected to the upper part of the reaction device, and the silicone oil recovery device is connected to the lower part of the reaction device. The molten metallic lithium is recovered from the upper part of the reaction device to the lithium-containing layer recovery device, and the silicone oil is recovered from the lower part of the reaction device to the silicone oil recovery device. The recovered silicone oil is further used for lithium chips collection.
[0062] Optionally, the separation and recovery process equipment of the mixture further comprises:
[0063] An air supply device is used to introduce carbon dioxide into the lithium-containing layer in the lithium-containing layer recovery device.
[0064] In order to facilitate the reaction of carbon dioxide and lithium hydroxide aqueous solution, the separation and recovery process equipment of the mixture is also provided with a gas supply device, through which carbon dioxide is introduced into the lithium hydroxide aqueous solution in the lithium-containing layer recovery device to convert the lithium hydroxide into lithium carbonate for the subsequent extraction of metallic lithium.
[0065] Optionally, the separation and recovery process equipment of the mixture further comprises:
[0066] A distillation device is connected to the lithium-containing layer recovery device, and the distillation device is used to distill and purify the lithium-containing layer in the lithium-containing layer recovery device.
[0067] In order to purify the molten metallic lithium, the separation and recovery process equipment of the mixture also includes a distillation device, which is connected to the lithium-containing layer recovery device, and is used to distill and purify the molten metallic lithium in the lithium-containing layer recovery device.
[0068] The present application also provides a control device, including: a memory, a processor, and a control program for a mixture separation and recovery process device stored in the memory and capable of running on the processor, wherein the described method is implemented when the processor executes the control program for the mixture separation and recovery process device.
[0069] The separation and recovery process method of the mixture of the present application can not only be manually operated by an operator, but also the method can be stored in a memory, and the control program of the method can be run by a processor, so that the corresponding separation and recovery process equipment of the mixture can implement the set operating steps, realize intelligent processing, reduce labor costs, and improve work efficiency.
[0070] The separation and recovery process of the mixture of the present application comprises the following steps: treating the mixture containing silicone oil and metallic lithium in layers to separate the silicone oil layer and the lithium-containing layer; separating the silicone oil layer from the lithium-containing layer, and collecting metallic lithium from the separated lithium-containing layer. The separation and recovery process of the present application can separate silicone oil and metallic lithium to recover lithium and save lithium resources. BRIEF DESCRIPTION OF THE DRAWINGS
[0071] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.
[0072] Figure 1 Schematic diagram of the separation and recovery process of the mixture of the present invention;
[0073] Figure 2 It is a structural schematic diagram of an embodiment of a separation and recovery process equipment for a mixture of the present invention;
[0074] Figure 3 The figure is a schematic structural diagram of another embodiment of the separation and recovery process equipment of the mixture of the present invention. DETAILED DESCRIPTION
[0075] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0076] It should be noted that all directional indications in the embodiments of the present invention (such as up, down, left, right, front, back, etc.) are only used to explain the relative position relationship, movement status, etc. between the components under a certain specific posture (as shown in the accompanying drawings). If the specific posture changes, the directional indication will also change accordingly.
[0077] In the present invention, unless otherwise clearly specified and limited, the terms "connection", "fixation", etc. should be understood in a broad sense. For example, "fixation" can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0078] In addition, in the present invention, descriptions such as "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the meaning of "and / or" appearing in the full text is to include three parallel solutions. Taking "A and / or B as an example", it includes solution A, or solution B, or solutions that satisfy both A and B. In addition, the technical solutions between the various embodiments can be combined with each other, but it must be based on the ability of ordinary technicians in this field to implement. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by the present invention.
[0079] Lithium metal is a silvery white metal element, soft and the metal with the lowest density. It is used in atomic reactors, light alloys and batteries. The melting point of lithium metal is about 180℃, the boiling point is about 1342℃, and the density is 0.534g / cm 3 , hardness is 0.6. Lithium metal is a metal with strong metal activity. Unlike other alkali metals, lithium reacts slowly with water at room temperature. The reaction equation is 2Li+2H2O=2LiOH+H2.
[0080] Silicone oil is a polysiloxane with chain structure of different polymerization degrees. It has a boiling point of about 300℃ and a density of 0.963g / cm3. It is a colorless, odorless, non-toxic and non-volatile liquid. Silicone oil can be used for high-grade lubricating oil, shockproof oil, insulating oil, defoaming agent, release agent, etc.
[0081] Silicone oil passivation of lithium metal refers to immersing lithium metal in silicone oil. The surface of lithium metal is covered with silicone oil, which isolates lithium metal from air and water to protect lithium metal and prevent it from coming into contact with active substances and reacting.
[0082] During the formation process of lithium-ion batteries, the formation of the negative electrode SEI film consumes a large amount of active lithium, especially when some high-capacity silicon-based negative electrode materials are added, resulting in low coulombic efficiency and battery capacity in the first week of the battery. Supplementing active lithium is an effective means to solve this problem. Currently, many ways of supplementing active lithium have been reported, mainly two categories: negative electrode lithium supplementation and positive electrode lithium supplementation. For example, negative electrode lithium supplementation includes physical mixed lithiation of metallic lithium, such as adding metallic lithium powder to the negative electrode or rolling metallic lithium foil on the surface of the electrode.
[0083] Metallic lithium chips will be generated in the lithium replenishment process. Metallic lithium is active and needs to be collected. Collecting them separately has great safety risks. In the prior art, silicone oil infiltration and passivation methods can greatly reduce the risk of lithium chip collection. However, the metallic lithium chips infiltrated with silicone oil need to be further separated and recovered to save lithium resources.
[0084] In order to separate lithium from silicone oil and recycle lithium to save lithium resources, the present application provides a separation and recovery process method for a mixture, which comprises the following steps: treating the mixture containing silicone oil and metallic lithium in layers to separate the silicone oil layer and the lithium-containing layer; separating the silicone oil layer from the lithium-containing layer, and collecting metallic lithium from the separated lithium-containing layer.
[0085] By utilizing the immiscible characteristics of the silicone oil layer and the lithium-containing layer to separate the silicone oil layer and the lithium-containing layer, the silicone oil and metallic lithium can be separated to recover lithium and save lithium resources.
[0086] Furthermore, in the step of separating the silicone oil layer from the lithium-containing layer and collecting metallic lithium from the separated lithium-containing layer, the following steps are included: separating the silicone oil layer from the lithium-containing layer, collecting metallic lithium from the separated lithium-containing layer, and applying the separated silicone oil layer to the passivation collection of metallic lithium.
[0087] Taking into account that the mixture containing silicone oil and metallic lithium in the present application is derived from the mixture produced in the process of collecting lithium chips during the lithium replenishment process, the separation and recovery process method of the present application is adopted to separate the silicone oil layer from the lithium-containing layer, collect the metallic lithium from the separated lithium-containing layer, and apply the separated silicone oil layer to the passivation collection step of metallic lithium. Not only can lithium be recovered to save lithium resources, and the recovered lithium can be used in the lithium replenishment process, but the separated silicone oil layer can also be used for the passivation collection of metallic lithium. That is, the recovered silicone oil can be recycled for many times, greatly reducing the cost of silicone oil used in the process of collecting metallic lithium chips.
[0088] Furthermore, in the step of stratifying the mixture containing silicone oil and metallic lithium to separate the silicone oil layer and the lithium-containing layer, the following steps are included: putting the mixture containing silicone oil and metallic lithium and water into a reaction device to allow the metallic lithium to react with the water to separate the silicone oil layer and the lithium-containing layer.
[0089] At room temperature, metallic lithium is solid and silicone oil is liquid, so they can be separated directly by solid-liquid separation. However, due to the adhesiveness of silicone oil, it is easy to adhere to the surface of metallic lithium. The simple solid-liquid separation method cannot completely remove the silicone oil on the surface of metallic lithium. In order to achieve effective separation, metallic lithium is reacted with water to generate lithium hydroxide. The lithium hydroxide exists in the water phase, and the water phase is separated from the silicone oil layer to achieve the separation of lithium compounds and silicone oil.
[0090] It can be understood that when the mixture containing silicone oil and metallic lithium and water are put into the reaction device, the mixture containing silicone oil and metallic lithium can be put into the reaction device first, and then the water; or the water can be put into the reaction device first, and then the mixture containing silicone oil and metallic lithium can be put into the reaction device; or the mixture containing silicone oil and metallic lithium and water can be put into the reaction device at the same time. The specific steps are not limited, and the operation can be performed according to the convenience of actual operation.
[0091] Furthermore, the step of introducing a mixture containing silicone oil and metallic lithium and water into a reaction device to allow the metallic lithium to react with water and separate the silicone oil layer and the lithium-containing layer includes the following steps: adding water to the reaction device, introducing the mixture containing silicone oil and metallic lithium into the reaction device in batches, allowing the metallic lithium to react with water and separate the silicone oil layer and the lithium-containing layer.
[0092] Batches means that the mixture containing silicone oil and metallic lithium is not put into the reaction device all at once, but the mixture containing silicone oil and metallic lithium is divided into multiple portions, and the multiple portions of the mixture containing silicone oil and metallic lithium are put into the reaction device multiple times at intervals. For example, the mixture containing silicone oil and metallic lithium is divided into 10 portions, and the mixture containing silicone oil and metallic lithium is put into the reaction device in 10 times.
[0093] It can be understood that the content of metallic lithium in the mixture containing silicone oil and metallic lithium can be 1%, 10%, 30%, 50%, 80%, 90%, etc., without specific limitation. The amount of each batch input can be determined according to the content of metallic lithium in the mixture containing silicone oil and metallic lithium during actual operation. For example, when the content of metallic lithium is increased, the amount of each batch input can be reduced to ensure a smooth reaction. When the content of metallic lithium is low, the amount of each batch input can be increased to speed up the entire operation process and save time. The entire operation process is balanced according to the safety of the reaction and the duration of the process.
[0094] Considering that the reaction between metallic lithium and water is an exothermic reaction and produces hydrogen, for safety reasons, the mixture containing silicone oil and metallic lithium is added to the reaction device in small amounts and multiple times to avoid the risk of combustion caused by violent reactions.
[0095] Furthermore, the weight of the mixture containing silicone oil and metallic lithium added in each batch is 1g-10g.
[0096] A smaller amount of a mixture containing silicone oil and metallic lithium is used to react with water to avoid an overly violent reaction, thereby ensuring that the reaction process does not cause a risk of combustion due to excessive intensity.
[0097] Further, the weight of the mixture containing silicone oil and metallic lithium added in each batch is 1g-5g; and / or the content of metallic lithium in the mixture containing silicone oil and metallic lithium is 10%-80%.
[0098] In order to further ensure that the reaction process does not cause the risk of combustion due to excessive intensity, the weight of the mixture containing silicone oil and metallic lithium added in each batch is 1g-5g.
[0099] In order to further ensure that the reaction process does not cause the risk of combustion due to excessive intensity, the content of metallic lithium in the mixture containing silicone oil and metallic lithium is 10%-80%, and the content of metallic lithium in the mixture containing silicone oil and metallic lithium can be 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80%. Of course, it can also be lower, for example, it can be 1%, 5%, etc., and there is no specific limitation.
[0100] Furthermore, the weight ratio of the mixture containing silicone oil and metallic lithium put into the reaction device in each batch to the weight ratio of water is (1:100)-(1:2000).
[0101] The amount of water should not be too much, as too much water will lead to waste. At the same time, the amount of water should not be too little, as too little water will lead to too high concentration of reaction products in the later stage of the reaction, slowing down the reaction rate and prolonging the operation time. Therefore, the weight ratio of the mixture containing silicone oil and metallic lithium in each batch put into the reaction device to the weight ratio of water is (1:100)-(1:2000), for example, it can be 1:100, 1:200, 1:300, 1:400, 1:500, 1:600, 1:700, 1:800, 1:900, 1:1000, 1:1100, 1:1200, 1:1300, 1:1400, 1:1500, 1:1600, 1:1700, 1:1800, 1:1900, 1:2000, without specific limitation.
[0102] Furthermore, the weight ratio of the mixture containing silicone oil and metallic lithium to the weight of water in each batch of the reaction device is: (1:1000)-(1:2000); and / or the content of metallic lithium in the mixture containing silicone oil and metallic lithium is 10%-80%.
[0103] On the premise of ensuring a complete and rapid reaction, the less the amount of water, the higher the concentration of lithium hydroxide generated by the reaction, which can slow down the subsequent reaction rate and avoid the risk of combustion caused by violent reactions. The ratio of the weight of the mixture containing silicone oil and metallic lithium put into the reaction device in each batch to the weight of water is (1:1000)-(1:2000). For example, it can be 1:1000, 1:1100, 1:1200, 1:1300, 1:1400, 1:1500, 1:1600, 1:1700, 1:1800, 1:1900, 1:2000, without specific limitation.
[0104] In order to ensure sufficient reaction, the content of metallic lithium in the mixture containing silicone oil and metallic lithium is 10%-80%, and the content of metallic lithium in the mixture containing silicone oil and metallic lithium can be 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80%. Of course, it can also be lower, for example, it can be 1%, 5%, etc., and there is no specific limitation.
[0105] Furthermore, water is added to the reaction device, and the mixture containing silicone oil and metallic lithium is put into the reaction device in batches to allow the metallic lithium to react with water, and in the step of separating the silicone oil layer and the lithium-containing layer, the interval time between batches is 5s-10s.
[0106] In order to ensure that the metallic lithium in the mixture containing silicone oil and metallic lithium added each time can react completely, the interval time between batches is 5s-10s, for example, the interval time can be 5s, 6s, 7s, 8s, 9s, 10s.
[0107] Furthermore, the interval time is 7-10s.
[0108] In order to avoid the situation where the metallic lithium in the previous batch of the mixture of silicone oil and metallic lithium has not yet reacted completely, and the next batch of the mixture of silicone oil and metallic lithium is added, resulting in the superposition of multiple batches of reactions, too fast a feeding speed, too much unreacted metallic lithium in the water, and the risk of combustion due to violent reaction, the feeding time is controlled within the range of 7-10s. For example, the interval time can be 7s, 8s, 9s, or 10s.
[0109] Furthermore, in the step of separating the silicone oil layer from the lithium-containing layer and collecting metallic lithium from the separated lithium-containing layer, the following steps are included: separating the silicone oil layer from the lithium-containing layer, introducing carbon dioxide into the separated lithium-containing layer, causing the lithium-containing compound in the lithium-containing layer to react with the carbon dioxide to obtain a reactant.
[0110] In order to extract metallic lithium from lithium hydroxide aqueous solution, lithium hydroxide is converted into lithium carbonate, and lithium carbonate solution has the value of extracting metallic lithium. Therefore, the silicone oil layer is separated from the lithium-containing layer, and carbon dioxide is introduced into the separated lithium-containing layer to make the lithium-containing compound in the lithium-containing layer react with carbon dioxide to obtain a reactant, which is lithium carbonate.
[0111] It is understandable that the reaction of the mixture containing silicone oil and metallic lithium with water produces a mixture of silicone oil and lithium hydroxide solution. The silicone oil in the mixture is in the upper layer. The silicone oil can be separated out by gravity separation using an oil-water separator. The separated silicone oil can be reused in the collection of lithium chips. The lithium hydroxide solution in the mixture is in the lower layer. The lithium hydroxide solution can be separated out by gravity separation using an oil-water separator. Carbon dioxide is introduced into the separated lithium hydroxide solution to generate a lithium carbonate solution, which is used in the subsequent metallic lithium extraction step.
[0112] Furthermore, the amount of carbon dioxide introduced is 1 L / min-20 L / min.
[0113] For the convenience of operation, the carbon dioxide introduction rate is 1L / min-20L / min, and the carbon dioxide introduction rate can be 1L / min, 5L / min, 10L / min, 15L / min, and 20L / min.
[0114] Furthermore, the amount of carbon dioxide introduced is 5L / min-10L / min.
[0115] In order to take into account both reaction rate and ease of operation, the amount of carbon dioxide introduced is 5L / min-10L / min, and the amount of carbon dioxide introduced can be 5L / min, 7L / min, 9L / min, and 10L / min.
[0116] Furthermore, in the step of stratifying the mixture containing silicone oil and metallic lithium to separate the silicone oil layer and the lithium-containing layer, the following steps are included: putting the mixture containing silicone oil and metallic lithium into a reaction device, heating the reaction device to melt the metallic lithium, and separating the silicone oil layer and the lithium-containing layer.
[0117] In order to separate the silicone oil from the metallic lithium, the mixture containing the silicone oil and the metallic lithium in the reaction device is heated to melt the metallic lithium. The metallic lithium melt and the silicone oil produced after melting are separated into layers due to their different densities, and the separated silicone oil and the molten metallic lithium can be separated. For example, the density of the silicone oil is greater than that of the metallic lithium, and the silicone oil will be present in the lower layer of the melt, and the silicone oil can flow out from the opening at the lower end of the reaction device.
[0118] Furthermore, the heating temperature of the reaction device is 200°C-300°C.
[0119] The melting point of metallic lithium is about 180°C. The metallic lithium can be melted by heating at 200°C for a long time, or by rapidly heating at 300°C. The specific conditions are not limited. For example, the heating temperature of the reaction device can be 200°C, 250°C, or 300°C. It can be understood that the heating temperature is mainly ensured to be higher than the melting point of metallic lithium and lower than the decomposition temperature of silicone oil. If the decomposition temperature of silicone oil is high enough, the heating temperature can be further increased. The specific conditions are not limited. The heating temperature is set below 300°C. On the one hand, it is applicable to most silicone oils, that is, conventional and cheap silicone oils can be used to process lithium chips. On the other hand, it saves heat energy, reduces the load of heating equipment, and saves costs.
[0120] Furthermore, the heating time of the reaction device is 1h-2h.
[0121] According to actual operation, the heating time can be selected to be 1h-2h, for example, 1h, 1.5h, 2h. A high heating temperature can shorten the heating time, and a low heating temperature can extend the heating time.
[0122] Furthermore, in the step of separating the silicone oil layer from the lithium-containing layer and collecting metallic lithium from the separated lithium-containing layer, the following steps are included: separating the silicone oil layer from the lithium-containing layer, placing the separated lithium-containing layer into a distillation tank, and distilling and purifying the metallic lithium.
[0123] After the silicone oil and the molten metallic lithium are separated, there may still be some silicone oil impurities in the molten metallic lithium. Therefore, the metallic lithium is purified by distillation. Specifically, the metallic lithium (boiling point is about 1340°C) and silicone oil (silicone oil has different components and structures, and its boiling point is different. For example, its boiling point can be 100°C or about 300°C, depending on the silicone oil used) in the mixture of molten metallic lithium and silicone oil are greatly different, and the metallic lithium is purified by distillation.
[0124] The specific operation steps are: separating the silicone oil layer from the lithium-containing layer, putting the separated lithium-containing layer into a distillation tank, and distilling and purifying the metallic lithium. For example, the molten metallic lithium in the reaction device is located on the upper layer of the silicone oil, and the molten metallic lithium can be transported to the distillation tank through the upper pipeline of the reaction device for purification.
[0125] Furthermore, during the distillation and purification process, the distillation temperature is 100°C-500°C.
[0126] By setting the distillation temperature to the boiling point of the silicone oil or above the boiling point, the silicone oil can be separated from the molten metallic lithium. The distillation temperature can be 100°C, 200°C, 300°C, 400°C, or 500°C.
[0127] Furthermore, during the distillation and purification process, the distillation temperature is 100° C.-200° C.; and / or, during the distillation and purification process, the distillation heating time is 2 h-3 h.
[0128] In order to avoid the loss of metallic lithium due to the carrying of metallic lithium during the silicone oil separation process caused by the distillation temperature being too high and the distillation rate being too fast, the distillation temperature can be controlled at 100°C, 150°C, or 200°C.
[0129] The distillation heating time can be adjusted accordingly according to the selection of the distillation temperature to ensure the effective separation of silicone oil and metallic lithium. The distillation time can be 2h, 2.5h, or 3h.
[0130] The present application also provides a separation and recovery process equipment for the mixture, which includes a reaction device, a lithium-containing layer recovery device and a silicone oil recovery device. The reaction device is used to load a mixture containing silicone oil and metallic lithium. The lithium-containing layer recovery device is connected to the reaction device to recover the lithium-containing layer. The silicone oil recovery device is connected to the reaction device to recover the silicone oil.
[0131] like Figure 2As shown, in the process of reacting metallic lithium with water, the reaction device is used to add a mixture containing silicone oil and metallic lithium and water, so that the metallic lithium reacts with water to generate a lithium hydroxide aqueous solution, and the lithium hydroxide aqueous solution is separated from the silicone oil and water, with the silicone oil located in the upper layer and the silicone oil located in the lower layer. The lithium-containing layer recovery device is connected to the lower part of the reaction device, and the silicone oil recovery device is connected to the upper part of the reaction device, so that the lithium hydroxide aqueous solution is recovered from the lower part of the reaction device to the lithium-containing layer recovery device, and the silicone oil is recovered from the upper part of the reaction device to the silicone oil recovery device, and the recovered silicone oil is continuously used for lithium chips collection.
[0132] Furthermore, the separation and recovery process equipment for the mixture also includes a gas supply device, which is used to introduce carbon dioxide into the lithium-containing layer in the lithium-containing layer recovery device.
[0133] like Figure 2 As shown, in order to facilitate the reaction of carbon dioxide and lithium hydroxide aqueous solution, the separation and recovery process equipment of the mixture is also provided with a gas supply device, through which carbon dioxide is introduced into the lithium hydroxide aqueous solution in the lithium-containing layer recovery device to convert the lithium hydroxide into lithium carbonate for the subsequent extraction of metallic lithium.
[0134] like Figure 3 As shown, in the process of heating and melting the metallic lithium in the mixture containing silicone oil and metallic lithium to achieve separation of metallic lithium and silicone oil, the reaction device is used to put the mixture containing silicone oil and metallic lithium, and the reaction device has a heating structure, the reaction device is heated to make the metallic lithium molten, the molten metallic lithium is located on the upper layer of the silicone oil, the lithium-containing layer recovery device is connected to the upper part of the reaction device, and the silicone oil recovery device is connected to the lower part of the reaction device, so that the molten metallic lithium is recovered from the upper part of the reaction device to the lithium-containing layer recovery device, and the silicone oil is recovered from the lower part of the reaction device to the silicone oil recovery device, and the recovered silicone oil is continuously used for lithium chips collection.
[0135] Furthermore, the separation and recovery process equipment of the mixture also includes a distillation device, which is connected to the lithium-containing layer recovery device, and the distillation device is used to distill and purify the lithium-containing layer in the lithium-containing layer recovery device.
[0136] like Figure 3 As shown, in order to purify the molten metallic lithium, the separation and recovery process equipment of the mixture also includes a distillation device, which is connected to the lithium-containing layer recovery device, and the distillation device is used to distill and purify the molten metallic lithium in the lithium-containing layer recovery device.
[0137] Furthermore, the present application also provides a control device, which includes a memory, a processor, and a control program for a mixture separation and recovery process equipment that is stored in the memory and can run on the processor. When the processor executes the control program for the mixture separation and recovery process equipment, the above-mentioned mixture separation and recovery process method is implemented.
[0138] The separation and recovery process method of the mixture of the present application can not only be manually operated by an operator, but also the method can be stored in a memory, and the control program of the method can be run by a processor, so that the corresponding separation and recovery process equipment of the mixture can implement the set operating steps, realize intelligent processing, reduce labor costs, and improve work efficiency.
[0139] Those skilled in the art will appreciate that embodiments of the present invention may be provided as methods, systems, or computer program products. Therefore, the present invention may take the form of a complete hardware embodiment, a complete software embodiment, or an embodiment combining software and hardware. Moreover, the present invention may take the form of a computer program product implemented on one or more computer-usable storage media (including but not limited to disk storage, CD-ROM, optical storage, etc.) containing computer-usable program code.
[0140] The present invention is described with reference to flowcharts and / or block diagrams of methods, devices (systems), and computer program products according to embodiments of the present invention. It should be understood that each process and / or block in the flowchart and / or block diagram, as well as the combination of processes and / or blocks in the flowchart and / or block diagram, can be implemented by computer program instructions. These computer program instructions can be provided to a processor of a general-purpose computer, a special-purpose computer, an embedded processor, or other programmable data processing device to produce a machine, so that the instructions executed by the processor of the computer or other programmable data processing device generate instructions for implementing the processes in the flowchart and / or block diagram. Figure 1 A process or multiple processes and / or boxes Figure 1 A device that provides the functions specified in a block or multiple blocks.
[0141] These computer program instructions may also be stored in a computer-readable memory capable of directing a computer or other programmable data processing device to operate in a specific manner, so that the instructions stored in the computer-readable memory produce an article of manufacture comprising an instruction device, which implements the process Figure 1 A process or multiple processes and / or boxes Figure 1 A function specified in one or more boxes.
[0142] These computer program instructions can also be loaded onto a computer or other programmable data processing device so that a series of operating steps are executed on the computer or other programmable device to produce a computer-implemented process, thereby providing instructions for implementing the process. Figure 1 A process or multiple processes and / or boxes Figure 1 The steps for the functions specified in one or more boxes.
[0143] Example
[0144] Example 1
[0145] The invention adopts a process of reaction of metallic lithium with water to recover lithium from a mixture containing silicone oil and metallic lithium.
[0146] An opening is provided at the lower end of the reaction device, which is closed during the reaction process. 1L of water is added to the reaction device, and 5g of a mixture containing silicone oil and metallic lithium is added to the 5L of water. Every 7s, 5g of the mixture containing silicone oil and metallic lithium is continuously added to the water. After lithium chips are continuously added 5,000 times, the reaction is completed, the lithium hydroxide aqueous solution layer and the silicone oil layer are separated, the opening at the lower end of the reaction device is opened, and the lithium hydroxide solution and the silicone oil are separated by gravity. Carbon dioxide gas is introduced into the separated lithium hydroxide solution at a rate of 10L / min. After a period of reaction, lithium carbonate with metallic lithium recovery value is finally obtained, and the recovered silicone oil can be used for the passivation collection of metallic lithium.
[0147] The mass content of metallic lithium in the mixture containing silicone oil and metallic lithium is 10%. After the above process steps, the recovery rate of lithium in the obtained lithium carbonate is 85% of the metallic lithium in the mixture containing silicone oil and metallic lithium.
[0148] Example 2-Example 11
[0149] On the basis of Example 1, various parameters were adjusted to obtain Examples 2 to 10.
[0150] As shown in Table 1 and Table 2 below:
[0151] Based on Example 1, Example 2 and Example 3 change the amount of the mixture containing silicone oil and metallic lithium added to the reaction device each time while keeping other conditions unchanged.
[0152] Based on Example 1, Example 4 and Example 5 change the proportion of metallic lithium in the mixture containing silicone oil and metallic lithium, and change the ratio of the weight of the mixture containing silicone oil and metallic lithium to the weight of water in each batch put into the reaction device, while keeping other conditions unchanged.
[0153] Based on Example 1, Example 6 and Example 7 change the proportion of metallic lithium in the mixture containing silicone oil and metallic lithium and change the interval time between batches while keeping other conditions unchanged.
[0154] Based on Example 1, Example 8 and Example 10 change the proportion of metallic lithium in the mixture containing silicone oil and metallic lithium and change the introduction rate of carbon dioxide gas while keeping other conditions unchanged.
[0155] Example 11 is based on Example 10, with other conditions unchanged, the proportion of metallic lithium in the mixture containing silicone oil and metallic lithium is changed.
[0156] Table 1 Separation and recovery parameters of a mixture containing silicone oil and metallic lithium
[0157]
[0158]
[0159] Table 2 Separation and recovery parameters of a mixture containing silicone oil and metallic lithium
[0160]
[0161] As can be seen from the data of Table 1 and Table 2, the data of Example 1 to Example 3 show that, under the same conditions, the lower the amount of the mixture of silicone oil and metallic lithium put into the reaction device each time, the better the recovery rate of lithium. The data of Example 4 and Example 5 show that, under the same conditions, in the weight ratio of the weight of the mixture of silicone oil and metallic lithium put into the reaction device in each batch to the weight ratio of water, the more water, the better the recovery rate of lithium. The data of Example 6 and Example 7 show that, under the same conditions, the longer the interval between batches, the better the recovery rate of lithium. The data of Example 1 and Example 8 show that, under the same conditions, the faster the speed of carbon dioxide gas introduction, the better the recovery rate of lithium.
[0162] Example 12
[0163] A process for separating the metallic lithium from the silicone oil by heating the metallic lithium in a mixture containing the silicone oil and the metallic lithium to melt the metallic lithium.
[0164] An opening is provided at the lower end of the reaction device, which is closed during the reaction process. 1 kg of a mixture containing silicone oil and metallic lithium is placed in the reaction device, which is heated to 200°C. After heating for 1 hour, the metallic lithium is heated to a molten state. The opening is opened, and the silicone oil is separated from the opening. The molten metallic lithium is input into a distillation tank and heated at a distillation temperature of 150°C for 3 hours to separate a small amount of silicone oil impurities in the metallic lithium melt, thereby finally obtaining metallic lithium with a higher purity.
[0165] The mass content of metallic lithium in the mixture containing silicone oil and metallic lithium is 10%. After the above process steps, the recovery rate of lithium in the obtained lithium carbonate is 60% of the metallic lithium in the mixture containing silicone oil and metallic lithium.
[0166] Example 13-Example 21
[0167] On the basis of Example 12, various parameters were adjusted to obtain Examples 13 to 21.
[0168] As shown in Table 3 and Table 4 below:
[0169] Example 13-Example 14 Based on Example 1, the heating temperature of the reaction device is changed while other conditions remain unchanged.
[0170] Example 15 is based on Example 1, with other conditions unchanged, the proportion of metallic lithium in the mixture containing silicone oil and metallic lithium is changed, and the heating temperature of the reaction device is changed.
[0171] Example 16-Example 18 Based on Example 1, with other conditions unchanged, the proportion of metallic lithium in the mixture containing silicone oil and metallic lithium is changed, and the distillation heating temperature is changed.
[0172] Example 19 is based on Example 1, with other conditions unchanged, the proportion of metallic lithium in the mixture containing silicone oil and metallic lithium is changed, and the distillation heating temperature is changed.
[0173] Example 20 is based on Example 1, with other conditions unchanged, the heating time of the reaction device is changed.
[0174] Example 21 is based on Example 1, with other conditions unchanged, the proportion of metallic lithium in the mixture containing silicone oil and metallic lithium is changed, and the distillation heating time is changed.
[0175] Table 3 Separation and recovery parameters of a mixture containing silicone oil and metallic lithium
[0176]
[0177]
[0178] Table 4 Separation and recovery parameters of a mixture containing silicone oil and metallic lithium
[0179]
[0180] As can be seen from the data in Tables 3 and 4, the data in Examples 12 to 14 show that under the same conditions, the change in the heating temperature of the reaction device does not change the recovery rate of lithium much. The data in Examples 16 to 18 show that under the same conditions, the higher the distillation heating temperature, the higher the recovery rate of lithium. The data in Examples 1 and 20 show that under the same conditions, the shorter the heating time of the reaction device, the higher the recovery rate of lithium.
[0181] The above are only preferred embodiments of the present invention, and are not intended to limit the patent scope of the present invention. All equivalent structural changes made using the contents of the present invention's specification and drawings, or directly / indirectly applied in other related technical fields, are included in the patent protection scope of the present invention.
Claims
1. A separation and recovery process for a mixture, characterized in that: The separation and recovery process of the mixture comprises the following steps: Putting a mixture containing silicone oil and metallic lithium into a reaction device, heating the reaction device to melt the metallic lithium, and separating the silicone oil layer and the lithium-containing layer; The silicone oil layer is separated from the lithium-containing layer, and the separated lithium-containing layer is put into a distillation tank to purify the metallic lithium by distillation.
2. The separation and recovery process of the mixture as claimed in claim 1, characterized in that: The step of separating the silicone oil layer from the lithium-containing layer, placing the separated lithium-containing layer into a distillation tank, and distilling and purifying the metallic lithium comprises the following steps: The silicone oil layer is separated from the lithium-containing layer, the separated lithium-containing layer is put into a distillation tank, the metallic lithium is distilled and purified, and the separated silicone oil layer is used for the passivation collection of metallic lithium.
3. The separation and recovery process of the mixture as claimed in claim 1, characterized in that: The heating temperature of the reaction device is 200°C-300°C.
4. The separation and recovery process of the mixture as claimed in claim 3, characterized in that: The heating time of the reaction device is 1h-2h.
5. The separation and recovery process of the mixture as claimed in claim 1, characterized in that: During the distillation and purification process, the distillation temperature is 100°C-500°C.
6. The separation and recovery process of the mixture as claimed in claim 5, characterized in that: During the distillation and purification process, the distillation temperature is 100°C-200°C; And / or, during the distillation and purification process, the distillation heating time is 2h-3h.
7. A separation and recovery process equipment for a mixture, characterized in that: The separation and recovery process equipment of the mixture includes: A reaction device, wherein the reaction device is used to load a mixture containing silicone oil and metallic lithium; A lithium-containing layer recovery device, the lithium-containing layer recovery device is connected to the reaction device and is used to recover the lithium-containing layer; a silicone oil recovery device, the silicone oil recovery device being connected to the reaction device and used for recovering silicone oil; and A distillation device is connected to the lithium-containing layer recovery device, and the distillation device is used to distill and purify the lithium-containing layer in the lithium-containing layer recovery device.
8. A control device, characterized in that: include: A memory, a processor, and a control program for a separation and recovery process equipment for a mixture stored in the memory and capable of running on the processor, wherein the processor implements the method described in any one of claims 1 to 6 when executing the control program for the separation and recovery process equipment for the mixture.