Multi-principal-element alloy as well as preparation method and application thereof

By adjusting the proportions of Y, Zr, Hf, Ta, and W elements and employing hot-pressing sintering and laser remelting processes, the problems of low hardness and uneven microstructure in multi-principal alloy materials have been solved, enabling the preparation of high-quality multi-principal alloys suitable for high-end equipment in the aerospace and nuclear industries.

CN118979184APending Publication Date: 2024-11-19GANJIANG INNOVATION ACAD CHINESE ACAD OF SCI +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411083579.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Existing multi-principal-element alloy materials suffer from problems such as low hardness, uneven internal structure, and numerous surface pores. Furthermore, their preparation process is cumbersome and costly, making it difficult to meet the needs of large-scale industrial production.

Method used

Using Y, Zr, Hf, Ta and W as main elements, multi-principal element alloys are prepared by controlling the content ratio of each element and combining hot pressing sintering and laser remelting processes to form a uniform internal structure and a smooth surface.

Benefits of technology

It significantly improves the hardness and surface quality of multi-principal element alloys, enhances high-temperature stability and density, simplifies the preparation process, reduces production costs, and is suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979184A_ABST
    Figure CN118979184A_ABST
Patent Text Reader

Abstract

The invention relates to a multi-principal-element alloy and a preparation method and application thereof, the multi-principal-element alloy comprises the following components: 0-20 at% of Y, 0-40 at% of Zr, 0-25 at% of Hf, 0-40 at% of Ta and 0-25 at% of W, and except the element Y, the atom percentage content of the other elements is not 0; according to the multi-principal-element alloy, Y, Zr, Hf, Ta and W elements are selected as principal elements, the content ratio of all the elements is controlled, all the elements are synergistically compounded, the hardness value, compactness and surface forming quality of the obtained multi-principal-element alloy are obviously improved, the preparation process is short, the production cost is low, and large-scale industrial production can be achieved; the multi-principal-element alloy can be used as a hot-end component of high-end equipment, and development of the fields of aerospace or nuclear industry and the like is promoted.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of alloy materials, and in particular to a multi-principal-component alloy and a preparation method and application thereof. Background Art

[0002] As a new type of alloy material, multi-principal alloy expands the design scope of alloy from a single principal element to multiple principal elements, with the main components reaching 5 or more, so that the composition of the alloy has more room for adjustment, thereby producing different properties to meet the requirements of different service environments for materials; more importantly, multi-principal alloy materials can combine the advantages of each principal element, and show higher hardness, excellent wear resistance and corrosion resistance compared to traditional metals and their alloys. Therefore, the study of multi-principal alloys will enrich the research in the field of materials science and broaden the application field of such materials.

[0003] As we all know, metallic tungsten has the characteristics of high hardness, high density and high strength, good electrical and thermal conductivity, low thermal expansion coefficient, strong radiation absorption ability, high pressure resistance and excellent electrical corrosion resistance. It plays an irreplaceable role in aerospace, mechanical processing and nuclear industry. However, pure tungsten is difficult to process, has a high ductile-brittle transition temperature and a low recrystallization temperature, which limits its development. Therefore, researchers began to improve the defects of pure tungsten by doping other metal elements, such as doping Ta elements. Tantalum has a high melting point (2996℃), an extremely low ductile-brittle transition temperature (-196℃) and good plastic processing ability, which can improve the brittleness and processing performance of W; Hf elements can also be doped so that the other impurity elements form stable compounds to improve the grain boundaries, increase the toughness of the material, and achieve the purpose of strengthening the material; however, the tungsten-tantalum-hafnium alloy material currently obtained by doping with multiple metal elements and combining traditional forging and sintering processes has the defects of poor ablation resistance, low hardness, coarse grains and uneven structure, which still cannot meet the use requirements, and its preparation process is cumbersome and the production cost is high, so it cannot be mass-produced industrially.

[0004] CN109778042A discloses a high-strength tungsten-based alloy and a preparation method thereof. The tungsten-based alloy is composed of tungsten and FeNiCoCrMn x Al y The multi-principal alloy composition is prepared by high temperature melting and high pressure gas atomization method to prepare FeNiCoCrMn x Al y Multi-principal alloy powder is then bonded to a tungsten matrix through a hot pressing and sintering process to form a high-strength tungsten-based alloy component with multi-phase reinforcement and better comprehensive performance. However, its Vickers hardness is only 540HV~625HV, and there is still much room for improvement. In addition, the bonding phase is easy to fall off, resulting in a low production qualification rate, and it is not suitable for large-scale production.

[0005] CN112063907A discloses a multi-principal high-temperature alloy and a preparation method thereof. The molecular formula of the multi-principal high-temperature alloy is (NbMoTaW) 18 (Ti 18 Al 5 Zr 5 ), which is prepared by mechanical alloying and low impurity influence process, has a microhardness of 688-710HV, which also has a large room for improvement. However, its preparation consumes a lot of raw materials and has a high preparation cost.

[0006] Based on this, how to provide a new type of multi-principal component alloy and its preparation method to meet the demand for multi-principal component alloy materials with high hardness and smoothness without holes has become a problem that needs to be solved urgently and has great research significance for the development of the alloy material field. Summary of the invention

[0007] In order to solve the above technical problems, the present invention provides a multi-principal component alloy and a preparation method and application thereof. By using Y, Zr, Hf, Ta and W elements as the main elements and controlling the content ratio of each element, the elements are synergistically compounded, so that the hardness and surface forming quality of the obtained multi-principal component alloy are significantly improved, the high-temperature stability is strong and the internal structure is uniform, which promotes the development of the field of multi-principal component alloy materials. The preparation process is short, the production cost is low, and it can be mass-produced industrially.

[0008] To achieve this object, the present invention adopts the following technical solutions:

[0009] In the first aspect, the present invention provides a multi-principal component alloy, which includes the following components in terms of atomic percentage: Y: 0-20at%, Zr: 0-40at%, Hf: 0-25at%, Ta: 0-40at% and W: 0-25at%, and except for element Y, the atomic percentages of the remaining elements are not 0.

[0010] Wherein, Y: 0-20at%, for example, it can be 0at%, 0.2at%, 0.5at%, 1at%, 1.5at%, 2at%, 2.5at%, 3at%, 3.5at%, 4at%, 4.5at%, 5at%, 6at%, 8at%, 10at%, 12at%, 15at%, 18at% or 20at%; Zr: 0-40at%, for example, it can be 0.5at%, 1at%, 3at%, 5at%, 8at%, 10at%, 15at%, 20at%, 25at%, 30at%, 35at% or 40at%; Hf: 0-25at%, For example, it may be 0.5at%, 1at%, 3at%, 5at%, 7at%, 10at%, 13at%, 15at%, 17at%, 20at%, 23at% or 25at%, etc.; Ta: 0-40at%, for example, it may be 0.2at%, 0.4at%, 0.7at%, 0.9at%, 1at%, 5at%, 10at%, 15at%, 20at%, 25at%, 30at%, 35at% or 40at%, etc.; W: 0-25at%, for example, it may be 0.5at%, 1at%, 5at%, 10at%, 15at%, 20at% or 25at%, etc.

[0011] The multi-principal component alloy of the present invention uses five elements, Y, Zr, Hf, Ta and W, as the main elements. By adjusting the content ratio between the elements, the elements are compounded and work synergistically, so that the hardness, internal structure uniformity and surface quality of the obtained multi-principal component alloy are improved, thereby solving the problems of low hardness, uneven internal structure and many surface holes in existing alloy materials.

[0012] Preferably, the multi-principal alloy comprises the following components in atomic percentage: Y: 0-20 at %, Zr: 20-25 at %, Hf: 20-25 at %, Ta: 20-25 at % and W: 20-25 at %.

[0013] The present invention further prefers Y: 0-20at%, Zr: 20-25at%, Hf: 20-25at%, Ta: 20-25at% and W: 20-25at%, so that each element can better play its own advantages and work together to further improve the hardness of the multi-principal component alloy, reduce surface hole defects, and effectively improve the overall quality of the obtained multi-principal component alloy.

[0014] Preferably, in terms of atomic percentage, the content of Y element in the multi-principal component alloy is 0.5-10 at %.

[0015] The present invention further prefers that the content of Y element in the multi-principal component alloy is 0.5-10at%, which can ensure its ablation resistance while having a higher hardness; if the content of Y element is lower, the ablation resistance of the obtained multi-principal component alloy is poor; if the content of Y element is higher, the hardness of the multi-principal component alloy will be poor.

[0016] In a second aspect, the present invention provides a method for preparing the multi-principal component alloy according to the first aspect, the preparation method comprising the following steps:

[0017] (1) mixing Y powder, Zr powder, Hf powder, Ta powder and W powder according to atomic percentage to obtain a mixed raw material;

[0018] (2) hot pressing and sintering the mixed raw material described in step (1) to obtain a sintered matrix;

[0019] (3) The sintered matrix of step (2) is subjected to laser remelting treatment to obtain the multi-principal component alloy.

[0020] The multi-principal component alloy described in the present invention is prepared by a method combining hot pressing sintering and laser remelting. The remelting layer can be prepared in situ on the surface of the sintered substrate, which significantly improves the surface hardness of the obtained multi-principal component alloy. The grain size of the remelting layer is small and the distribution of the principal component elements is uniform, so that the surface molding quality of the obtained multi-principal component alloy is excellent, the high-temperature stability is good, and the strength is high. The preparation method does not require powder spraying or prefabricated powder coating process, is easy to operate, and has low production cost.

[0021] Preferably, the mixing in step (1) is carried out in a first protective gas atmosphere.

[0022] Preferably, the first protective gas comprises argon and / or argon. .

[0023] The present invention preferably performs the mixing in a protective gas atmosphere in order to prevent the air from affecting the purity of the powder raw materials, thereby affecting the purity of the obtained multi-principal element alloy.

[0024] Preferably, the mixing method includes ball milling mixing.

[0025] Preferably, the material-ball ratio of the ball milling mixture is (1-15):1, for example, it can be 1:1, 3:1, 5:1, 8:1, 10:1, 12:1 or 15:1.

[0026] Preferably, the ball milling speed of the ball milling mixing is 100 to 400 r / min, for example, 100 r / min, 200 r / min, 300 r / min or 400 r / min.

[0027] Preferably, the ball milling time of the ball milling mixing is 3 to 48 hours, for example, it can be 3 hours, 6 hours, 9 hours, 18 hours, 24 hours, 36 hours or 48 hours.

[0028] Preferably, the purity of the W powder, Ta powder, Hf powder, Zr powder and Y powder in step (1) is ≥99.95%, for example, it can be 99.95%, 99.96%, 99.97%, 99.98% or 99.99%.

[0029] Preferably, the average particle size of the mixed raw material in step (1) is 1 to 10 μm, for example, it can be 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm or 10 μm.

[0030] The present invention further preferably has an average particle size of 1 to 10 μm, which is conducive to hot pressing sintering densification, can improve the comprehensive performance of the multi-principal component alloy and reduce the introduction of oxygen and impurities during its forming process; if the average particle size of the mixed raw material is too small, it will lead to an increase in its specific surface area, and the oxygen content and impurity content of the initial mixed raw material will be too high; if the average particle size of the mixed raw material is too large, it will be unfavorable for alloy densification sintering.

[0031] Preferably, before the hot pressing and sintering in step (2), the mixed raw material is compacted to obtain a pre-pressed embryo.

[0032] Preferably, the hot pressing sintering in step (2) is carried out in a vacuum environment.

[0033] Preferably, the vacuum degree of the vacuum environment is 1.0×10 -4 ~1.0×10 -3 Pa, for example, can be 1.0×10 - 4 Pa, 3.0×10 -4 Pa, 5.0×10 -4 Pa, 7.0×10 -4 Pa or 1.0×10 -3 Pa et al.

[0034] The present invention further preferably performs the hot pressing sintering in step (2) at a vacuum degree of 1.0×10 -4 ~1.0×10 -3 Pa in a vacuum environment to avoid the generation of impurities that may affect the performance of the multi-principal alloy.

[0035] Preferably, the hot pressing sintering in step (2) includes a first temperature rising treatment, a first heat preservation treatment, a pressurization treatment, a second temperature rising treatment, a second heat preservation and pressure preservation treatment, and a temperature falling treatment performed in sequence.

[0036] Preferably, the first temperature increase treatment comprises: increasing the temperature to 1000-1300° C. at a temperature increase rate of 10-20° C. / min.

[0037] Wherein, the heating rate is 10-20°C / min, for example, it can be 10°C / min, 12°C / min, 15°C / min, 18°C / min or 20°C / min.

[0038] The terminal temperature of the heating is 1000-1300°C, for example, it can be 1000°C, 1050°C, 1100°C, 1150°C, 1200°C, 1250°C or 1300°C.

[0039] The present invention further prefers that the heating rate of the first heating is 10-20°C / min and the terminal temperature is 1000-1300°C, which is conducive to the orderly growth of grains and the discharge of pores, thereby improving the density and surface quality of the obtained multi-principal component alloy material; if the heating rate is too fast, it will lead to an increase in internal pores, thereby affecting the density of the obtained multi-principal component alloy; if the heating rate is too slow, it will cause the hot pressing sintering effect to deteriorate, affecting the product quality; similarly, if the terminal temperature of the first heating is too low, the sintering reaction will not be triggered; if the terminal temperature of the first heating is too high, the density of the obtained multi-principal component alloy will deteriorate.

[0040] Preferably, the first heat preservation treatment lasts for 10 to 20 minutes, for example, 10 minutes, 12 minutes, 15 minutes, 18 minutes or 20 minutes.

[0041] Preferably, the pressure treatment includes: pressurizing to 30-45 MPa within 1-2 hours.

[0042] The time of the pressure treatment is 1 to 2 hours, for example, 1 hour, 1.2 hours, 1.5 hours, 1.8 hours or 2 hours.

[0043] The terminal pressure of the pressurization treatment is 30-45 MPa, for example, 30 MPa, 32 MPa, 35 MPa, 38 MPa, 40 MPa, 42 MPa or 45 MPa.

[0044] The present invention further prefers that the endpoint pressure of the pressurization treatment is 30-45 MPa. This is because under the action of pressure, the contact area between the particles increases, which is beneficial to the densification sintering of the raw materials, reduces pores and gaps, thereby eliminating holes and improving the bonding strength between grains; thereby improving the density, hardness, bending strength and fracture toughness of the obtained multi-principal component alloy; if the endpoint pressure of the pressurization treatment is too low, it will lead to an increase in the number of holes in the obtained multi-principal component alloy, thereby causing its hardness and surface quality to deteriorate; if the endpoint pressure of the pressurization treatment is too high, it will lead to an increase in grain size, which will also affect the comprehensive performance of the obtained multi-principal component alloy.

[0045] Preferably, the second temperature increase treatment comprises: increasing the temperature to 1500-2000° C. at a temperature increase rate of 5-15° C. / min.

[0046] The heating rate of the second heating treatment is 5 to 15°C / min, for example, 5°C / min, 8°C / min, 10°C / min, 12°C / min or 15°C / min.

[0047] The terminal temperature of the second temperature rising treatment is 1500-2000°C, for example, 1500°C, 1600°C, 1700°C, 1800°C, 1900°C or 2000°C.

[0048] The present invention further prefers that the heating rate of the second heating is 5-15°C / min and the endpoint temperature is 1500-2000°C, which can further improve the density, hardness and surface quality of the obtained multi-principal component alloy; if the heating rate of the second heating is too low or the endpoint temperature is too low, it will lead to insufficient hot pressing sintering, thereby affecting the product quality; if the heating rate of the second heating is too high or the endpoint temperature is too high, it will lead to an increase in the number of pores in the obtained multi-principal component alloy and a decrease in hardness.

[0049] Preferably, the second heat-insulating and pressure-insulating treatment lasts for 1 to 3 hours, for example, 1 hour, 1.5 hours, 2 hours, 2.5 hours or 3 hours.

[0050] Preferably, the cooling treatment comprises: cooling to 700-900° C. at a cooling rate of 10-20° C. / min.

[0051] The cooling rate of the cooling treatment is 10-20°C / min, for example, 10°C / min, 12°C / min, 15°C / min, 18°C / min or 20°C / min.

[0052] The terminal temperature of the cooling treatment is 700-900°C, for example, 700°C, 750°C, 800°C, 850°C or 900°C.

[0053] The present invention further prefers that the cooling rate of the cooling treatment is 10-20°C / min and the cooling end point is 700-900°C, followed by furnace cooling; this is beneficial to releasing some thermal stress inside the material, facilitating the migration and discharge of pores inside the material, thereby reducing the pores in the obtained multi-principal element alloy and improving its density; if the cooling rate is too fast, it will lead to greater thermal stress, thereby causing residual stress in the material or generating micro cracks.

[0054] Preferably, the cooling process also includes a pressure relief process, and the pressure relief process is performed 10 to 30 minutes after the cooling process begins, for example, 10 minutes, 15 minutes, 20 minutes, 25 minutes or 30 minutes.

[0055] Preferably, the temperature reduction treatment further includes cooling.

[0056] Preferably, the cooling comprises: cooling with the furnace to 20-25°C, for example, 20°C, 22°C, 24°C or 25°C.

[0057] Preferably, the laser power of the laser remelting treatment in step (3) is 100-500 W, for example, it can be 100 W, 150 W, 200 W, 250 W, 300 W, 350 W, 400 W, 450 W or 500 W, etc., preferably 300-350 W.

[0058] Preferably, the laser scanning speed of the laser remelting treatment in step (3) is 100 to 1000 mm / s, for example, it can be 100 mm / s, 200 mm / s, 300 mm / s, 400 mm / s, 500 mm / s, 600 mm / s, 700 mm / s, 800 mm / s, 900 mm / s or 1000 mm / s, etc., preferably 100 to 200 mm / s.

[0059] The present invention further prefers that the power of the laser remelting treatment is 100-500W and the laser scanning speed is 100-1000mm / s; the two work together to effectively control the forming quality of the multi-principal component alloy, ensure that its surface is flat and free of cracks and holes, and can ensure that the bonding measure between the sintered matrix and the remelted layer is good; if the laser power is too large or the laser scanning speed is too low, it will cause the energy received by the surface of the multi-principal component alloy to be too high, thereby causing the formation of surface holes, which is not conducive to the bonding between the remelted layer and the sintered matrix, resulting in poor quality of the obtained multi-principal component alloy; if the laser power is too small or the laser scanning speed is too high, it will cause the energy received by the surface of the multi-principal component alloy to be too low, resulting in too low thickness of the remelted layer, resulting in poor strengthening effect of laser remelting.

[0060] Preferably, the spot diameter of the laser remelting treatment in step (3) is 0.05-0.5 mm, for example, it can be 0.05 mm, 0.1 mm, 0.15 mm, 0.2 mm, 0.25 mm, 0.3 mm, 0.35 mm, 0.4 mm, 0.45 mm or 0.5 mm.

[0061] Preferably, the wind speed of the fan in the laser remelting process in step (3) is 20 to 60 mm / s, for example, it can be 20 mm / s, 30 mm / s, 40 mm / s, 50 mm / s or 60 mm / s.

[0062] It is worth noting that in the laser remelting process of the present invention, the fan speed of the laser remelting treatment is preferably 20-60 mm / s, and it is necessary to observe in real time whether there is smoke in the forming chamber. If there is smoke, the fan speed needs to be increased, otherwise it may affect the forming quality of the multi-principal element alloy.

[0063] Preferably, the number of laser remelting times in the laser remelting treatment in step (3) is 5 to 25 times, for example, 5 times, 10 times, 15 times, 20 times or 25 times, etc., preferably 10 to 20 times.

[0064] The present invention further prefers that the number of laser remelting times of the laser remelting treatment is 5 to 25 times, which can ensure the formation of the remelting layer and the remelting depth, thereby improving the performance of the multi-principal component alloy; if the number of remelting times is less, the strengthening effect of the remelting layer becomes worse, resulting in the deterioration of the quality of the multi-principal component alloy; if the number of remelting times is more, the strengthening effect is not significantly improved, but the energy consumption increases.

[0065] Preferably, the laser remelting treatment in step (3) is carried out in a protective gas atmosphere.

[0066] Preferably, the protective gas comprises argon and / or nitrogen.

[0067] Preferably, the gas flow rate of the protective gas is 4 to 45 L / min, for example, it can be 4 L / min, 4.5 L / min, 5 L / min, 10 L / min, 12.5 L / min, 15 L / min, 40 L / min, 42.5 L / min or 45 L / min.

[0068] As a preferred technical solution of the preparation method described in the second aspect of the present invention, the preparation method comprises the following steps:

[0069] (1) In a first protective gas atmosphere, Y powder, Zr powder, Hf powder, Ta powder and W powder with a purity of ≥99.95% by atomic percentage are ball milled for 3 to 48 hours at a material-to-ball ratio of (1 to 15):1 and a ball milling speed of 100 to 400 r / min to obtain a mixed raw material with an average particle size of 1 to 10 μm;

[0070] (2) The mixed raw materials described in step (1) are placed in a vacuum of 1.0×10 -4 ~1.0×10 -3 Hot pressing sintering is performed in a vacuum environment of 1.5 Pa to obtain a sintered matrix;

[0071] The hot pressing sintering comprises: firstly heating the temperature to 1000-1300°C at a heating rate of 10-20°C / min, then performing a first heat preservation treatment for 10-20min; then pressurizing to 30-45MPa within 1-2h, and heating to 1500-2000°C at a heating rate of 5-15°C / min; then performing a second heat preservation and pressure preservation treatment for 1-3h, then cooling the temperature to 700-900°C at a cooling rate of 10-20°C / min, and performing a pressure relief treatment 10-30min after the start of the cooling treatment, and finally cooling to 20-25°C with the furnace;

[0072] (3) subjecting the sintered substrate of step (2) to laser remelting treatment, wherein the laser remelting treatment comprises: performing laser remelting 5 to 25 times in a second protective gas atmosphere with a gas flow rate of 4 to 45 L / min, with a laser power of 100 to 500 W, a laser scanning speed of 100 to 1000 mm / s, a spot diameter of 0.05 to 0.5 mm, and a fan speed of 20 to 60 mm / s, to obtain the multi-principal alloy.

[0073] In a third aspect, the present invention provides an application of the multi-principal component alloy described in the first aspect, wherein the multi-principal component alloy is used as a hot end component material.

[0074] The multi-principal element alloy described in the present invention has a wide range of applications, and is mainly used as hot end component materials for high-end equipment in the fields of aerospace or nuclear industry, such as nose cones and wing leading edge materials for hypersonic aircraft or first wall materials for nuclear fusion, etc., which is of great significance to the development of the field of high-temperature alloys.

[0075] Compared with the prior art, the present invention has at least the following beneficial effects:

[0076] (1) The multi-principal component alloy provided by the present invention uses Y, Zr, Hf, Ta and W elements as the main components, regulates the content ratio of each main component element, effectively utilizes the respective advantages of Y, Zr, Hf, Ta and W elements, and works synergistically to make the internal structure uniform, the surface smooth and almost free of holes. The overall molding quality of the obtained main component alloy is excellent, and it has greater application potential in the field of alloy materials.

[0077] (2) The preparation method of the multi-principal component alloy provided by the present invention combines hot pressing sintering and remelting treatment to form a remelting layer on the surface of the sintered matrix to improve the surface hardness of the obtained multi-principal component alloy. The preparation method does not require pre-fabricated powder coating, and the preparation process is simple and low in cost. The parameters of the heating, cooling and pressurizing process of hot pressing sintering are further regulated, as well as the parameters such as laser power and laser scanning speed during the remelting process, so as to further improve the bonding force between the remelting layer and the matrix, and the quality of the remelting layer. As a result, the hardness value of the sintered matrix of the multi-principal component alloy is preferably as high as 515HV 0.2 The hardness of the remelted layer after laser remelting is preferably as high as 840HV 0.2 The above is more than 1.56 times higher than that of the sintered matrix, and the remelted layer is well bonded to the sintered matrix; the density of the multi-principal alloy is preferably as high as 99.874% or more, and its surface element distribution is uniform, the grain size is reduced, and the surface molding quality is excellent.

[0078] (3) Application of the multi-principal component alloy provided by the present invention. The multi-principal component alloy can be widely used in hot end component materials of high-end equipment in the fields of aerospace or nuclear industry, such as nose cone and wing leading edge materials of hypersonic aircraft or first wall materials of nuclear fusion, etc., which promotes the development of multi-principal component alloy materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0079] Figure 1 is a hardness distribution diagram from the remelting layer to the sintered matrix of the multi-principal alloy provided in Example 1 of the present invention;

[0080] Figure 2 are surface morphology images of the multi-principal element alloys provided in Examples 1 and 6-7 of the present invention, wherein a-c are surface morphology images of the multi-principal element alloy provided in Example 7 at 400 μm, 40 μm and 2 μm, respectively, d-f are surface morphology images of the multi-principal element alloy provided in Example 1 at 400 μm, 40 μm and 2 μm, respectively, and g-i are surface morphology images of the multi-principal element alloy provided in Example 6 at scales of 400 μm, 40 μm and 2 μm, respectively;

[0081] Figure 3are cross-sectional morphology diagrams of the multi-principal alloys provided in Examples 1 and 6-7 of the present invention, wherein a-c are cross-sectional morphology diagrams of the multi-principal alloys provided in Examples 7, 1 and 6 at a scale of 400 μm, and d-f are cross-sectional morphology diagrams of the multi-principal alloys provided in Examples 7, 1 and 6 at a scale of 40 μm;

[0082] Figure 4 are surface morphology images of the multi-principal alloys provided in Examples 1 and 8 to 10 of the present invention, wherein a to d are surface morphology images of the multi-principal alloys provided in Examples 10, 9, 8 and 1 at a scale of 400 μm, e to h are surface morphology images of the multi-principal alloys provided in Examples 10, 9, 8 and 1 at a scale of 40 μm, and i to l are surface morphology images of the multi-principal alloys provided in Examples 10, 9, 8 and 1 at a scale of 2 μm;

[0083] Figure 5 are cross-sectional morphology diagrams of the multi-principal alloys provided in Example 1 and Examples 8 to 10 of the present invention, wherein a to d are cross-sectional morphology diagrams of the multi-principal alloys provided in Example 10, Example 9, Example 8 and Example 1 at a scale of 300 μm, e to h are cross-sectional morphology diagrams of the multi-principal alloys provided in Example 10, Example 9, Example 8 and Example 1 at a scale of 40 μm, i is a cross-sectional morphology diagram of the multi-principal alloy provided in Example 10 at a scale of 2 μm, j is a cross-sectional morphology diagram of the multi-principal alloy provided in Example 9 at a scale of 4 μm, k and l are cross-sectional morphology diagrams of the multi-principal alloys provided in Example 8 and Example 1 at a scale of 6 μm, respectively;

[0084] Figure 6 It is a trend chart showing the hardness values ​​of the sintered matrix and the remelted layer of the multi-principal component alloys provided in Example 1 and Examples 11 to 14 of the present invention as the Y element content changes. DETAILED DESCRIPTION

[0085] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and through specific implementation methods. However, the following examples are only simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.

[0086] Example 1

[0087] This embodiment provides a multi-principal alloy and a preparation method thereof, wherein the multi-principal alloy includes the following components: Y: 5at%, Zr: 23.75at%, Hf: 23.75at%, Ta: 23.75at% and W: 23.75at%;

[0088] The preparation method comprises the following steps:

[0089] (1) In an argon atmosphere, Y powder with a purity of 99.97%, Zr powder with a purity of 99.99%, Hf powder with a purity of 99.95%, Ta powder with a purity of 99.96%, and W powder with a purity of 99.95% were ball-milled according to the above atomic percentages at a material-to-ball ratio of 5:1 and a ball milling speed of 350 r / min for 24 h to obtain a mixed raw material with an average particle size of 5 μm;

[0090] (2) The mixed raw materials described in step (1) are placed in a vacuum of 5.0×10 -4 Hot pressing sintering is performed in a vacuum environment of 1.5 Pa to obtain a sintered matrix;

[0091] The hot pressing sintering includes: first heating to 1200°C at a heating rate of 15°C / min, then performing a first heat preservation treatment for 15 minutes; then pressurizing to 30MPa within 1 hour, and heating to 1500°C at a heating rate of 10°C / min; then performing a second heat preservation and pressure preservation treatment for 2 hours, then cooling to 800°C at a cooling rate of 15°C / min, and performing a pressure relief treatment to 0MPa 20 minutes after the start of the cooling treatment, and finally cooling to 25°C with the furnace;

[0092] (3) subjecting the sintered substrate of step (2) to laser remelting treatment, wherein the laser remelting treatment comprises: performing laser remelting 15 times in an argon atmosphere with a gas flow rate of 35 L / min, with a laser power of 325 W, a laser scanning speed of 100 mm / s, a spot diameter of 0.1 mm, and a fan speed of 40 mm / s; and obtaining the multi-principal element alloy.

[0093] like Figure 1 As shown, it is a hardness distribution diagram from the remelting layer to the sintered matrix of the multi-principal alloy provided in this embodiment. It can be seen that the remelting layer has the highest hardness, which can reach 865HV 0.2 The sintered matrix hardness is only 553HV 0.2 The hardness of the remelted layer can reach 1.56 times that of the sintered matrix, and the surface hardness increases from the sintered matrix to the remelted layer, indicating that laser remelting can significantly improve the surface hardness of the sintered matrix, thereby achieving the effect of surface strengthening of the multi-principal alloy.

[0094] Example 2

[0095] This embodiment provides a multi-principal alloy and a preparation method thereof, wherein the multi-principal alloy includes the following components: Y: 0.5 at %, Zr: 24.82 at %, Hf: 24.28 at %, Ta: 24.65 at % and W: 24.25 at %;

[0096] The preparation method comprises the following steps:

[0097] (1) In an argon atmosphere, Y powder with a purity of 99.95%, Zr powder with a purity of 99.98%, Hf powder with a purity of 99.97%, Ta powder with a purity of 99.96% and W powder with a purity of 99.95% were ball-milled according to the above atomic percentages at a material-to-ball ratio of 3:1 and a ball milling speed of 100 r / min for 48 hours to obtain a mixed raw material with an average particle size of 1 μm;

[0098] (2) The mixed raw materials described in step (1) are placed in a vacuum of 1.0×10 -4 Hot pressing sintering is performed in a vacuum environment of 1.5 Pa to obtain a sintered matrix;

[0099] The hot pressing sintering includes: first heating to 1000°C at a heating rate of 10°C / min, then performing a first heat preservation treatment for 20 minutes; then pressurizing to 35MPa within 1.5 hours, and heating to 1800°C at a heating rate of 5°C / min; then performing a second heat preservation and pressure preservation treatment for 1 hour, then cooling to 900°C at a cooling rate of 10°C / min, and performing a pressure relief treatment to 0MPa 10 minutes after the start of the cooling treatment, and finally cooling to 22°C with the furnace;

[0100] (3) subjecting the sintered substrate of step (2) to laser remelting treatment, wherein the laser remelting treatment comprises: performing laser remelting 10 times in an argon atmosphere with a gas flow rate of 4 L / min, with a laser power of 300 W, a laser scanning speed of 120 mm / s, a spot diameter of 0.05 mm and a fan speed of 20 mm / s; and obtaining the multi-principal element alloy.

[0101] Example 3

[0102] This embodiment provides a multi-principal alloy and a preparation method thereof, wherein the multi-principal alloy includes the following components: Y: 8at%, Zr: 22.32at%, Hf: 23.17at%, Ta: 24.02at% and W: 24.49at%;

[0103] The preparation method comprises the following steps:

[0104] (1) In an argon atmosphere, Y powder with a purity of 99.98%, Zr powder with a purity of 99.95%, Hf powder with a purity of 99.97%, Ta powder with a purity of 99.98% and W powder with a purity of 99.96% were ball-milled according to the above atomic percentages at a material-to-ball ratio of 15:1 and a ball milling speed of 400 r / min for 12 h to obtain a mixed raw material with an average particle size of 10 μm;

[0105] (2) The mixed raw materials described in step (1) are placed in a vacuum of 1.0×10 -3 Hot pressing sintering is performed in a vacuum environment of 1.5 Pa to obtain a sintered matrix;

[0106] The hot pressing sintering includes: first heating to 1300°C at a heating rate of 20°C / min, then performing a first heat preservation treatment for 10 minutes; then pressurizing to 45MPa within 2 hours, and heating to 2000°C at a heating rate of 15°C / min; then performing a second heat preservation and pressure preservation treatment for 3 hours, then cooling to 700°C at a cooling rate of 20°C / min, and performing a pressure relief treatment to 0MPa 30 minutes after the start of the cooling treatment, and finally cooling to 20°C with the furnace;

[0107] (3) subjecting the sintered substrate of step (2) to laser remelting treatment, wherein the laser remelting treatment comprises: performing laser remelting 20 times in an argon atmosphere with a gas flow rate of 45 L / min, with a laser power of 350 W, a laser scanning speed of 150 mm / s, a spot diameter of 0.5 mm, and a fan speed of 60 mm / s; and obtaining the multi-principal element alloy.

[0108] Example 4

[0109] This embodiment provides a multi-principal component alloy and a preparation method thereof, which is the same as that of Embodiment 1 except that the pressure after the pressurization treatment during the hot pressing sintering process in step (2) of the preparation method is 25 MPa.

[0110] Example 5

[0111] This embodiment provides a multi-principal component alloy and a preparation method thereof, which is the same as that of Embodiment 1 except that the terminal temperature of the second heating treatment during the hot pressing sintering process in step (2) of the preparation method is 1400°C.

[0112] Embodiment 6-7

[0113] Examples 6 to 7 are the same as Example 1 except that the laser power of the laser remelting process in step (3) of the preparation method is 300 W and 350 W.

[0114] Embodiments 8 to 10

[0115] Examples 8 to 10 are the same as Example 1 except that the laser scanning speeds of the laser remelting treatment in step (3) of the preparation method are 200 mm / s, 300 mm / s and 400 mm / s respectively.

[0116] Examples 11 to 14

[0117] Examples 11 to 14 are the same as Example 1 except that the atomic percentage of the Y element in the multi-principal alloy is 0at%, 10at%, 15at% and 20at% respectively, and the amounts of the other four elements are adaptively increased or decreased on average according to the reduction or increase of the Y element to ensure that the total content is 100at%.

[0118] 2. Comparison

[0119] Comparative Example 1

[0120] This comparative example provides a multi-principal alloy, which is the same as Example 1 except that the content of Y element is 24at%, and the other four elements are each 19at%.

[0121] Comparative Example 2

[0122] This comparative example provides a multi-principal-component alloy, which is the same as Example 1 except that the Y element is replaced by Yb.

[0123] 3. Test and its results

[0124] ① Test the surface morphology and cross-sectional morphology of the multi-principal alloys provided in the above-mentioned Examples 1 and 6-7. The results are as follows: Figure 2 and Figure 3 As shown, it can be seen that: at a laser scanning speed of 100 mm / s, when the laser powers are 300 W (Example 6), 325 W (Example 1) and 350 W (Example 7) respectively, the surface of the multi-principal element alloy is relatively uniform and smooth, and there are no holes on the surface. At laser powers of 300 W and 350 W, there are only a few holes in the cross section of the multi-principal element alloy, and there are no holes in the cross section at 325 W, and the effect is best.

[0125] ② The surface morphology and cross-sectional morphology of the multi-principal alloys provided in the above-mentioned Examples 1 and 8 to 10 were tested. The results are as follows: Figure 4 and Figure 5 As shown, it can be seen that: under a laser power of 325 W, at 100 mm / s (Example 1) and 200 mm / s (Example 8), the surface is very smooth, with almost no cracks on the surface and almost no holes in the cross section. At 300 mm / s (Example 9) and 400 mm / s (Example 10), the surface becomes slightly rough, with a small amount of cracks appearing, and the number of holes in the cross section also increases. It can be seen that under a laser power of 325 W, as the laser scanning speed increases, the surface quality of the multi-principal element alloy deteriorates slightly, and the best effect is achieved at 100-200 mm / s.

[0126] ③ Test the hardness values ​​(HV) of the sintered matrix and remelted layer of the multi-principal alloy obtained in the above embodiments and comparative examples. 0.2, hardness test was performed under a load of 200g), and the density of the principal alloy; the results are shown in Table 1; and a variation trend diagram of the hardness values ​​of the sintered matrix and the remelted layer of the multi-principal alloy provided in Example 1 and Examples 11 to 14 as the Y element content changes is drawn, as shown in Figure 6 As shown;

[0127] Depend on Figure 6 It can be seen that the present invention forms a remelting layer on the surface of the sintered substrate by adjusting the content of the Y element and adopting a method of combining hot pressing sintering and laser remelting. The hardness of the remelting layer is significantly higher than the temperature of the sintered substrate. The hardness of the remelting layer is preferably as high as 730HV. 0.2 The hardness of the remelted layer is about 1.5 times that of the sintered matrix. That is, the surface hardness of the multi-principal alloy is significantly improved. When the content of the Y element is 0-10 at%, the hardness of the remelted layer is higher. As the content of the Y element continues to increase, the hardness decreases, but remains at 550 HV. 0.2 above.

[0128] Table 1

[0129]

[0130]

[0131] From Table 1 we can see that:

[0132] (1) It can be seen from Examples 1 to 3 that the present invention uses five elements, Y, Zr, Hf, Ta and W, as main elements, controls the content ratio of each element, and combines hot pressing sintering with laser remelting to strengthen the multi-main element alloy, and the hardness of the remelted layer is as high as 840 HV 0.2 Above, the density is as high as 99.874%.

[0133] (2) It can be seen from Examples 1 and 4 that the hardness of the sintered matrix is ​​only 419 HV due to the pressure of 25 MPa after the pressurization treatment in step (2) of the preparation method of Example 4, which is too low. 0.2 , and the hardness of the remelted layer after laser remelting is only 604HV 0.2 ; It can be seen that the present invention further improves the hardness of the obtained multi-principal element alloy by further optimizing the pressure after the pressurization treatment to 30-45MPa.

[0134] (3) It can be seen from Examples 1 and 5 that since the temperature of the second heating treatment in Example 5 is too low, the hardness of the sintered matrix is ​​reduced, thereby affecting the hardness of the remelted layer and the density is also reduced; therefore, it can be seen that the present invention further prefers that the terminal temperature of the second heating treatment is 1500-2000°C, which further improves the hardness of the obtained multi-principal component alloy.

[0135] (4) It can be seen from Examples 1 and 6 to 10 that, due to the low or high laser power or laser scanning speed in Examples 6 to 10, the energy received by the sintered substrate is too large or too small, resulting in the hardness of the remelted layer being reduced to 800 HV. 0.2 Below, the density drops to below 98.852%.

[0136] (5) It can be seen from Example 1 and Examples 11 to 14 and Comparative Example 1 that since the content of Y element in Example 11 is 0at%, and the hardness of Y element itself is relatively low, when Y element is not doped, the hardness of the sintered matrix and the remelted layer of the obtained multi-principal component alloy are relatively high, but its ablation resistance is relatively poor; in addition, since the hardness of Y element itself is relatively low in Examples 12 to 14 and Comparative Example 1, the hardness of the multi-principal component alloy decreases with the gradual increase of the content of Y element, and the density also decreases; it can be seen that the present invention further prefers that the Y content in the multi-principal component alloy is 0.5 to 10at%, which further improves the hardness of the obtained multi-principal component alloy and ensures the ablation resistance.

[0137] (6) It can be seen from Example 1 and Comparative Example 2 that since the Y element is replaced by the Yb element in Comparative Example 2, the hardness is not as high as when Y is added, and the molding quality after hot pressing sintering and laser remelting is poor. This shows that the present invention selects to dope the Y element and use Y, Zr, Hf, Ta and W elements as multi-principal element elements. The hardness of the obtained multi-principal element alloy is significantly improved while ensuring corrosion resistance.

[0138] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A multi-principal alloy, It is characterized in that In terms of atomic percentage, the multi-principal alloy includes the following components: Y: 0-20at%, Zr: 0-40at%, Hf: 0-25at%, Ta: 0-40at% and W: 0-25at%, and except for the Y element, the atomic percentages of the remaining elements are not 0.

2. The multi-principal alloy according to claim 1, It is characterized in that The multi-principal alloy comprises the following components in terms of atomic percentage: Y: 0-20 at %, Zr: 20-25 at %, Hf: 20-25 at %, Ta: 20-25 at % and W: 20-25 at %; Preferably, in terms of atomic percentage, the content of the Y element in the multi-principal component alloy is 0.5-10 at %.

3. A method for preparing the multi-principal alloy according to claim 1 or 2, It is characterized in that The preparation method comprises the following steps: (1) mixing Y powder, Zr powder, Hf powder, Ta powder and W powder according to atomic percentage to obtain a mixed raw material; (2) hot pressing and sintering the mixed raw material described in step (1) to obtain a sintered matrix; (3) The sintered matrix of step (2) is subjected to laser remelting treatment to obtain the multi-principal alloy.

4. The preparation method according to claim 3, It is characterized in that The mixing in step (1) is carried out in a first protective gas atmosphere; Preferably, the first protective gas comprises argon and / or nitrogen; Preferably, the mixing method includes ball milling; Preferably, the material-ball ratio of the ball milling mixture is (1-15):1; Preferably, the ball milling speed of the ball milling mixing is 100 to 400 r / min; Preferably, the ball milling time of the ball milling mixing is 3 to 48 hours; Preferably, the purity of the W powder, Ta powder, Hf powder, Zr powder and Y powder in step (1) is ≥ 99.95%; Preferably, the average particle size of the mixed raw materials in step (1) is 1 to 10 μm.

5. The preparation method according to claim 3 or 4, It is characterized in that The hot pressing sintering in step (2) is carried out in a vacuum environment; Preferably, the vacuum degree of the vacuum environment is 1.0×10 -4 ~1.0×10 -3 Pa.

6. The preparation method according to any one of claims 3 to 5, It is characterized in that The hot pressing sintering in step (2) includes a first heating treatment, a first heat preservation treatment, a pressurization treatment, a second heating treatment, a second heat preservation and pressure preservation treatment, and a cooling treatment performed in sequence; Preferably, the first temperature increase treatment comprises: increasing the temperature to 1000-1300° C. at a temperature increase rate of 10-20° C. / min; Preferably, the first heat preservation treatment time is 10 to 20 minutes; Preferably, the pressure treatment comprises: pressurizing to 30-45 MPa within 1-2 hours; Preferably, the second temperature increase treatment comprises: increasing the temperature to 1500-2000° C. at a temperature increase rate of 5-15° C. / min; Preferably, the second heat preservation and pressure preservation treatment time is 1 to 3 hours; Preferably, the cooling treatment comprises: cooling to 700-900° C. at a cooling rate of 10-20° C. / min.

7. The preparation method according to claim 6, It is characterized in that The temperature reduction process also includes a pressure relief process, and the pressure relief process is performed 10 to 30 minutes after the temperature reduction process begins; Preferably, the temperature reduction treatment further includes cooling; Preferably, the cooling comprises: cooling to 20-25°C with the furnace.

8. The preparation method according to any one of claims 3 to 7, It is characterized in that The laser power of the laser remelting treatment in step (3) is 100 to 500 W, preferably 300 to 350 W; Preferably, the laser scanning speed of the laser remelting treatment in step (3) is 100 to 1000 mm / s, preferably 100 to 200 mm / s; Preferably, the spot diameter of the laser remelting treatment in step (3) is 0.05 to 0.5 mm; Preferably, the fan speed of the laser remelting process in step (3) is 20 to 60 mm / s; Preferably, the laser remelting process in step (3) is performed 5 to 25 times, preferably 10 to 20 times; Preferably, the laser remelting treatment in step (3) is performed in a second protective gas atmosphere; Preferably, the second protective gas comprises argon and / or nitrogen; Preferably, the gas flow rate of the protective gas is 4 to 45 L / min.

9. The preparation method according to any one of claims 3 to 8, It is characterized in that The preparation method comprises the following steps: (1) In a first protective gas atmosphere, Y powder, Zr powder, Hf powder, Ta powder and W powder with a purity of ≥99.95% by atomic percentage are ball milled for 3 to 48 hours at a material-to-ball ratio of (1 to 15):1 and a ball milling speed of 100 to 400 r / min to obtain a mixed raw material with an average particle size of 1 to 10 μm; (2) The mixed raw materials described in step (1) are placed in a vacuum of 1.0×10 -4 ~1.0×10 -3 Hot pressing sintering is performed in a vacuum environment of 1.5 Pa to obtain a sintered matrix; The hot pressing sintering comprises: firstly heating the temperature to 1000-1300°C at a heating rate of 10-20°C / min, then performing a first heat preservation treatment for 10-20min; then pressurizing to 30-45MPa within 1-2h, and heating to 1500-2000°C at a heating rate of 5-15°C / min; then performing a second heat preservation and pressure preservation treatment for 1-3h, then cooling the temperature to 700-900°C at a cooling rate of 10-20°C / min, and performing a pressure relief treatment 10-30min after the start of the cooling treatment, and finally cooling to 20-25°C with the furnace; (3) subjecting the sintered substrate of step (2) to laser remelting treatment, wherein the laser remelting treatment comprises: performing laser remelting 5 to 25 times in a second protective gas atmosphere with a gas flow rate of 4 to 45 L / min, with a laser power of 100 to 500 W, a laser scanning speed of 100 to 1000 mm / s, a spot diameter of 0.05 to 0.5 mm, and a fan speed of 20 to 60 mm / s, to obtain the multi-principal alloy.

10. A use of the multi-principal alloy according to claim 1 or 2, It is characterized in that The multi-principal alloy is used as a hot end component material.