Heat treatment method suitable for thin-wall single crystal alloy

By performing a stepped heating and gas-cooled solution treatment on thin-walled single-crystal alloys, the problem of microstructure control in thin-walled single-crystal alloys was solved, the high-temperature mechanical properties and the uniformity of the γ′ phase were improved, and the defects caused by traditional heat treatment were avoided.

CN118979210APending Publication Date: 2024-11-19BEIHANG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411059799.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Existing technologies cannot effectively control the microstructure of thin-walled single-crystal alloys, leading to a decrease in their high-temperature performance, and traditional heat treatment processes are prone to introducing microstructural defects.

Method used

A solution treatment method with stepped heating and air cooling is used to heat treat thin-walled single-crystal alloys, controlling the cooling rate at 90–300 °C/min, preferably 200–300 °C/min, and adjusting the heat treatment regime to adapt to the non-traditional structural characteristics of thin-walled single-crystal alloys.

Benefits of technology

This study achieved effective control of the microstructure of thin-walled single-crystal alloys, avoided microstructural defects, improved high-temperature mechanical properties, and ensured the uniformity of the γ′ phase and the high-temperature creep life of the alloy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979210A_ABST
    Figure CN118979210A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of single-crystal alloys, and particularly relates to a heat treatment method suitable for a thin-wall single-crystal alloy. The thin-wall single crystal alloy is subjected to solution treatment, the wall thickness of the thin-wall single crystal alloy is smaller than or equal to 0.5 mm, and the solution treatment comprises stepped heating treatment and cooling treatment; the cooling treatment mode is air cooling, and the cooling rate of the air cooling is 90-300 DEG C / min. According to the heat treatment method for the single crystal thin-wall sample, the structure of the thin-wall sample can be effectively regulated and controlled, so that the thin-wall sample has a better structure size, and meanwhile, the structure defect caused by a traditional heat treatment system is avoided. Theoretical and technical guidance can be provided for the structure regulation and control technology and unconventional structure regulation and control of the single-crystal alloy in application, and help is provided for application of the single-crystal alloy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of single crystal alloys, and in particular relates to a heat treatment method suitable for thin-walled single crystal alloys. Background Art

[0002] The excellent high-temperature mechanical properties of Ni-based single crystal alloys and Ni3Al-based single crystal alloys make them widely used as aero-engine blades. The above two single crystal alloys are mainly composed of γ / γ′ phases. The γ phase is a face-centered cubic crystal structure, and the γ′ phase is an L12 structure. The number and morphology of the γ and γ′ phases will directly determine the mechanical properties of the high-temperature alloy. Current research believes that the high-temperature strength of Ni-based single crystal high-temperature alloys depends on the γ′ phase. There is an elastic repulsion between adjacent γ′ phases, which are separated by γ channels. This phase structure maintains the high-temperature stability of the alloy. When high temperature and stress act on the alloy at the same time, it will have a complex effect on the internal structure of the alloy. The plastic activity caused by the diffusion of elements and dislocation sliding inside the alloy will cause the organization to evolve, breaking the original stable structure, thereby changing the creep behavior of the alloy.

[0003] The size of the γ / γ′ phases of a single crystal alloy is controlled by its heat treatment system. The heat treatment system is usually divided into solution treatment and aging treatment. The purpose of solution treatment is to eliminate the element segregation in the cast structure by step-by-step temperature increase. This segregation will increase the size difference of the γ′ phase in the dendrite trunk and interdendritic region, making the overall γ′ phase size uniformity inside the alloy poor. Solution treatment can make the elements inside the alloy more uniform by eliminating segregation at high temperature, and at the same time re-precipitate the γ′ phase with uniform size through a certain cooling rate, thereby improving the uniformity of the γ′ phase size of the alloy. Aging treatment can adjust the morphology of the γ′ phase, etc., so that the alloy structure reaches a state with optimal performance.

[0004] At present, the heat treatment system for single crystal alloys only considers round bars or thicker plate samples, and one alloy usually has only one standard heat treatment system. As the blade structure prepared by single crystal alloy changes, the single crystal thin plate part of the casting is getting thinner and thinner, and the thinnest part is even less than 0.5mm. The smaller wall thickness speeds up the cooling rate during the heat treatment of the alloy, that is, under the same heat treatment conditions, the thin wall will have a higher cooling rate. Too high a cooling rate will significantly affect the organizational size and segregation of the alloy, thereby affecting the high temperature performance of the alloy. Summary of the invention

[0005] The purpose of the present invention is to provide a heat treatment method suitable for thin-walled single crystal alloys. The heat treatment method provided by the present invention is suitable for thin-walled single crystal alloy specimens, and can effectively regulate the structure of the thin-walled specimens so that they have a more optimal structure size. At the same time, it avoids the structural defects caused by traditional heat treatment systems, thereby making the thin-walled specimens have better high-temperature mechanical properties.

[0006] In order to achieve the above object, the present invention provides the following technical solutions:

[0007] The present invention provides a heat treatment method suitable for thin-walled single crystal alloy, comprising the following steps:

[0008] The thin-walled single crystal alloy is subjected to solid solution treatment, wherein the wall thickness of the thin-walled single crystal alloy is ≤0.5 mm, and the solid solution treatment includes step-by-step heating treatment and cooling treatment; the cooling treatment is performed by air cooling, and the air cooling rate is 90-300°C / min.

[0009] Preferably, the air cooling rate is 200-300°C / min.

[0010] Preferably, the step-wise temperature increase treatment comprises: heating the thin-walled single crystal alloy to a first temperature for a first heat preservation, heating from the first temperature to a second temperature for a second heat preservation, heating from the second temperature to a third temperature for a third heat preservation, heating from the third temperature to a fourth temperature for a fourth heat preservation, heating from the fourth temperature to a fifth temperature for a fifth heat preservation, and heating from the fifth temperature to a sixth temperature for a sixth heat preservation;

[0011] The first temperature is 1305±2°C, and the first insulation time is 2h;

[0012] The second temperature is 1310±2°C, and the second insulation time is 2h;

[0013] The third temperature is 1315±2°C, and the third insulation time is 2h;

[0014] The fourth temperature is 1320±2° C., and the fourth insulation time is 2 hours;

[0015] The fifth temperature is 1325±2°C, and the fifth insulation time is 4h;

[0016] The sixth temperature is 1330±2° C., and the sixth insulation time is 4 hours.

[0017] Preferably, the thin-walled single crystal alloy includes a Ni-based single crystal alloy or a Ni3Al-based single crystal alloy.

[0018] Preferably, the thin-walled single crystal alloy comprises the following elements in percentage by mass: 7.6-9.8% Al, 2.2-3.6% Cr, 8-9.4% Mo, 1.2-3.2% Re, 2.6-4.5% Ta, and the remainder Ni.

[0019] The present invention provides a heat-treated thin-walled single crystal alloy obtained by the heat treatment method described in the above technical solution.

[0020] Preferably, the size of the γ′ phase in the thin-walled single crystal alloy after the heat treatment is 0.49-0.69 μm.

[0021] Preferably, the thin-walled single crystal alloy does not contain carbides after the heat treatment.

[0022] The present invention provides a heat treatment method suitable for thin-walled single crystal alloys, comprising the following steps: subjecting the thin-walled single crystal alloy to solid solution treatment, wherein the wall thickness of the thin-walled single crystal alloy is ≤0.5 mm, and the solid solution treatment includes a step-by-step heating treatment and a cooling treatment; the cooling treatment is performed by air cooling, and the cooling rate of the air cooling is 90-300°C / min. The present invention combines solidification theory with the non-traditional structural characteristics of thin-walled single crystal alloys, improves the traditional heat treatment system of single crystal alloys, and enables it to adapt to the organizational regulation needs of unconventional casting structure samples, fills the gap in organizational regulation of unconventional structure single crystal alloy samples that have not yet received widespread attention, and provides valuable guidance for the future application of complex unconventional casting structures of single crystal alloys. The heat treatment method for single crystal thin-walled samples provided by the present invention can effectively regulate the organization of thin-walled samples, so that they have a better organizational size, while avoiding the organizational defects caused by traditional heat treatment systems. In terms of application, it can provide theoretical and technical guidance for the organizational regulation technology of single crystal alloys and the organizational regulation of unconventional structures, and provide help for the application of single crystal alloys. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 Heat treatment structure and γ′ phase size of thin-walled and thick-walled samples when the standard heat treatment system is adopted; Figure 1 (a) and (c) are the heat-treated microstructure and γ′ phase size of the thin-walled specimen; Figure 1 (b) and (d) are the heat-treated structures and γ′ phase sizes of thick-walled samples;

[0024] Figure 2 This is a characterization diagram of carbides in thin-walled specimens using a standard heat treatment regime. DETAILED DESCRIPTION

[0025] The present invention provides a heat treatment method suitable for thin-walled single crystal alloy, comprising the following steps:

[0026] The thin-walled single crystal alloy is subjected to solid solution treatment, wherein the wall thickness of the thin-walled single crystal alloy is ≤0.5 mm, and the solid solution treatment includes step-by-step heating treatment and cooling treatment; the cooling treatment is performed by air cooling, and the air cooling rate is 90-300°C / min.

[0027] In the present invention, unless otherwise specified, all preparation raw materials / components are commercially available products well known to those skilled in the art.

[0028] In the present invention, the thin-walled single crystal alloy preferably includes a Ni-based single crystal alloy or a Ni3Al-based single crystal alloy.

[0029] In a specific embodiment of the present invention, the thin-walled single crystal alloy preferably includes the following elements in percentage by mass: Al element 7.6-9.8%, Cr element 2.2-3.6%, Mo element 8-9.4%, Re element 1.2-3.2%, Ta element 2.6-4.5%, and the balance Ni element.

[0030] In a specific embodiment of the present invention, the thin-walled single crystal alloy is in a cast structure before being subjected to solution treatment.

[0031] In a specific embodiment of the present invention, the wall thickness of the thin-walled single crystal alloy is 0.5 mm.

[0032] In the present invention, the step-wise temperature increase treatment preferably includes: heating the thin-walled single crystal alloy to a first temperature for a first heat preservation, heating from the first temperature to a second temperature for a second heat preservation, heating from the second temperature to a third temperature for a third heat preservation, heating from the third temperature to a fourth temperature for a fourth heat preservation, heating from the fourth temperature to a fifth temperature for a fifth heat preservation, and heating from the fifth temperature to a sixth temperature for a sixth heat preservation. The first temperature is preferably 1305±2°C, and the first heat preservation time is preferably 2h; the second temperature is preferably 1310±2°C, and the second heat preservation time is preferably 2h; the third temperature is preferably 1315±2°C, and the third heat preservation time is preferably 2h; the fourth temperature is preferably 1320±2°C, and the fourth heat preservation time is preferably 2h; the fifth temperature is preferably 1325±2°C, and the fifth heat preservation time is preferably 4h; the sixth temperature is preferably 1330±2°C, and the sixth heat preservation time is preferably 4h.

[0033] In the present invention, the air cooling is air cooling, and the cooling rate of the air cooling is preferably 200-300°C / min.

[0034] The present invention provides a heat-treated thin-walled single crystal alloy obtained by the heat treatment method described in the above technical solution.

[0035] In the present invention, the size of the γ′ phase in the heat-treated thin-walled single crystal alloy is 0.49 to 0.69 μm, preferably 0.49 to 0.61 μm. The heat-treated thin-walled single crystal alloy does not contain carbides.

[0036] The present invention provides a heat treatment system suitable for single crystal alloys with a wall thickness of less than 0.5 mm. The heat treatment system provided by the present invention is different from the conventional heat treatment system for single crystal alloys. The temperature and cooling rate of the heat treatment system are adjusted. Compared with the conventional heat treatment system, the present invention enables thin-walled single crystal alloy samples (with a wall thickness of less than 0.5 mm) to have a more optimal organizational size through the adjusted heat treatment system, and solves the organizational segregation defects caused by the mismatch of conventional heat treatment, thereby providing an effective heat treatment method for thin-walled samples with a more optimal organization.

[0037] In the present invention, the γ′ phase is an important strengthening phase in the single crystal alloy, which precipitates from the γ matrix during the cooling process, and its morphology and size are related to the precipitation and growth process. According to the classical nucleation theory, the critical nucleation entropy of the γ′ phase precipitated from the matrix is ​​shown in Formula 1:

[0038]

[0039] In formula 1: ΔG is the critical nucleation energy, ΔG v is the change in volume free energy per unit volume, ΔG S is the change in surface free energy per unit volume, and σ is the specific surface energy of the interface between the γ phase and the γ' phase.

[0040] From formula 1, it can be seen that under the same heat treatment conditions, the cooling rate of the thin-walled sample is higher, which increases the undercooling of the γ′ phase nucleation, resulting in a larger ΔG v With a smaller ΔG, the amount of nucleation increases and the growth process is shortened, so the number of γ′ phases formed is large and the size is fine. As the wall thickness increases, the cooling rate decreases, the number of γ′ phase nuclei is small, the growth time becomes longer, and the size of the γ′ phase will be larger. When the standard heat treatment system is used for thin-walled specimens, the size of the γ′ phase will be small due to the excessive cooling rate.

[0041] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0042] In the following embodiments and comparative examples: the model alloy composition (mass percentage) is: Al: 9.8%, Cr: 2.5%, Mo: 8.1%, Re: 2.2%, Ta: 2.8%, Ni: balance.

[0043] Comparative Example 1

[0044] In this comparative example: the solid solution system (i.e. standard heat treatment system) of the model alloy is:

[0045] 1305℃ / 2h+1310℃ / 2h+1315℃ / 2h+1320℃ / 2h+1325℃ / 4h+1330℃ / 4h+air cooling (≈600℃ / min);

[0046] This system was used to heat treat single crystal alloy sheets with a wall thickness of 5 mm and a wall thickness of 0.5 mm, respectively, and the microstructures were as follows: Figure 1 shown.

[0047] Figure 1 are the heat-treated structures and γ′ phase sizes of thin-wall and thick-wall in Comparative Example 1, where Figure 1 (a) and (c) are the characterization results of thin-walled specimens. Figure 1 (b) and (d) in the figure are the characterization results of thick-walled specimens. Figure 1 It can be seen that for the standard heat treatment system, the size of the γ′ phase of the thin-walled sample is smaller than that of the thick-walled sample. The size of the γ′ phase of the thick-walled sample is mostly 0.6-0.9 μm, and the size of the γ′ phase of the thin-walled sample is mostly 0.4-0.5 μm. At the same time, it is found in the thin-walled sample that Figure 2 The white carbide shown is usually caused by too fast cooling rate, and the C element between the dendrites has no time to diffuse, which is not good for high temperature mechanical properties.

[0048] It can be seen from this that the standard heat treatment system suitable for thick walls cannot meet the requirements of thin-wall heat treatment. Therefore, in the following Example 1 of the present invention, a cooling rate different from the standard heat treatment system in Comparative Example 1 is designed for thin-walled samples.

[0049] Example 1

[0050] In this embodiment: the solid solution system of the model alloy is:

[0051] 1305℃ / 2h+1310℃ / 2h+1315℃ / 2h+1320℃ / 2h+1325℃ / 4h+1330℃ / 4h+air cooling; the cooling rate of air cooling is shown in Table 1.

[0052] The heat treatment system of this embodiment is used to heat treat a single crystal alloy sheet with a wall thickness of 0.5 mm. The γ′ phase size and high temperature rupture life of the 0.5 mm thin-walled sample after heat treatment under different cooling rates are shown in Table 1. Table 1 shows the γ′ phase size and high temperature rupture life of the 0.5 mm thin-walled sample after heat treatment under different cooling rates.

[0053] Table 1 γ′ phase size and high temperature rupture life of thin-walled samples at different cooling rates

[0054] serial number Cooling speed γ′ phase size / μm carbide 1100℃ / 140MPa 1 300-600℃ / min 0.43-0.54 have 10.2-36.1h 2 200-300℃ / min 0.49-0.61 none 48.6-62.7h 3 90-200℃ / min 0.58-0.69 none 31.5-50.2h

[0055] exist Figure 1In numbers 1, 2 and 3, the cooling rate within a range means that the influence on the alloy structure within this range is the same and there is no major change, so the range is used in numbers 1, 2 and 3 to represent different cooling rates.

[0056] It can be seen from Table 1 that in this embodiment, when the cooling rate after solution treatment is 300-600℃ / min, the size of the γ′ phase is small, carbides are precipitated in the structure, and the high-temperature endurance life of the alloy is also the shortest; when the cooling rate is reduced to 300-200℃ / min, the size of the γ′ phase increases, no carbides are precipitated, and the high-temperature endurance life of the alloy is optimal; when the cooling rate is reduced to 90-200℃ / min, the size of the γ′ phase is 0.58-0.69μm, no carbides are precipitated in the structure, and the high-temperature endurance life of the alloy is 31.5-50.2h, which is less than the alloy when the cooling rate is 200-300℃ / min. Therefore, the solution cooling rate for the optimal mechanical properties of the thin-walled sample is 200-300℃ / min.

[0057] Through the above verification, the present invention improves the solution cooling rate of the alloy thin-walled sample. In the thin-walled sample, appropriately reducing the cooling rate can effectively inhibit the precipitation of carbides and increase the size of the γ′ phase. The present invention changes the heat treatment system of the model alloy thin-walled sample to:

[0058] 1305℃ / 2h+1310℃ / 2h+1315℃ / 2h+1320℃ / 2h+1325℃ / 4h+1330℃ / 4h+air cooling, where the air cooling rate is 200-300℃ / min.

[0059] It can be seen from the above embodiments that the present invention combines solidification theory with non-traditional structural characteristics to improve the traditional heat treatment system so that it can adapt to the organizational control needs of unconventional casting structure samples, making up for the gap in organizational control of unconventional structure single crystal alloy samples that have not yet received widespread attention, and providing valuable guidance for the future application of complex unconventional casting structures of single crystal alloys. The heat treatment method of the single crystal thin-walled sample of the present invention can effectively control the organization of the thin-walled sample so that it has a more optimal organizational size, while avoiding the organizational defects caused by the traditional heat treatment system. In terms of application, it can provide theoretical and technical guidance for the organizational control technology of single crystal alloys and the organizational control of unconventional structures, and provide help for the application of single crystal alloys.

[0060] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A heat treatment method suitable for thin-walled single crystal alloys, characterized in that: The following steps are involved: The thin-walled single crystal alloy is subjected to solid solution treatment, wherein the wall thickness of the thin-walled single crystal alloy is ≤0.5 mm, and the solid solution treatment includes step-by-step heating treatment and cooling treatment; the cooling treatment is performed by air cooling, and the air cooling rate is 90-300°C / min.

2. The heat treatment method according to claim 1, characterized in that The air cooling temperature reduction rate is 200-300°C / min.

3. The heat treatment method according to claim 1 or 2, characterized in that: The step-wise temperature-raising treatment comprises: heating the thin-walled single crystal alloy to a first temperature for a first heat preservation, heating from the first temperature to a second temperature for a second heat preservation, heating from the second temperature to a third temperature for a third heat preservation, heating from the third temperature to a fourth temperature for a fourth heat preservation, heating from the fourth temperature to a fifth temperature for a fifth heat preservation, and heating from the fifth temperature to a sixth temperature for a sixth heat preservation; The first temperature is 1305±2°C, and the first insulation time is 2h; The second temperature is 1310±2°C, and the second insulation time is 2h; The third temperature is 1315±2°C, and the third insulation time is 2h; The fourth temperature is 1320±2° C., and the fourth insulation time is 2 hours; The fifth temperature is 1325±2°C, and the fifth insulation time is 4h; The sixth temperature is 1330±2° C., and the sixth insulation time is 4 hours. 4 . The heat treatment method according to claim 1 , wherein the thin-walled single crystal alloy comprises a Ni-based single crystal alloy or a Ni 3 Al-based single crystal alloy.

5. The heat treatment method according to claim 1, characterized in that: The thin-walled single crystal alloy comprises the following elements in percentage by mass: 7.6-9.8% Al element, 2.2-3.6% Cr element, 8-9.4% Mo element, 1.2-3.2% Re element, 2.6-4.5% Ta element, and the balance Ni element.

6. The heat-treated thin-walled single crystal alloy obtained by the heat treatment method according to any one of claims 1 to 5.

7. The heat-treated thin-walled single crystal alloy according to claim 6, characterized in that: The size of the γ′ phase in the thin-walled single crystal alloy after the heat treatment is 0.49-0.69 μm.

8. The heat-treated thin-walled single crystal alloy according to claim 6 or 7, characterized in that: The thin-walled single crystal alloy does not contain carbides after the heat treatment.