Blank for hot stamping, method for producing same, hot-stamped component, and method for producing same
By heating the aluminum-silicon plating layer and multi-stage heating treatment on the steel plate in the hot stamping process, the alloying layer is formed, which solves the problems of hydrogen-induced delayed fracture and mold sintering in the hot stamping parts, and improves the hydrogen embrittlement of the parts and Resistance to peel.
Patent Information
- Application Number
- CN202411063677.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2020-09-29
- Filing Date
- 2020-11-18
- Publication Date
- 2024-11-19
AI Technical Summary
In the hot stamping process, the hot stamping parts are prone to hydrogen-induced delayed fracture and mold sintering, and the prior art is difficult to effectively solve these problems.
By immersing the steel plate in a plating bath including aluminum and silicon, forming a plating layer, and heating at a certain temperature to form an alloying layer, followed by manufacturing the hot stamping parts by a multi-stage heating and homogenizing heating process, preventing or minimizing the delay caused by hydrogen. Breakage and mold sintering.
It effectively improves the hydrogen embrittlement and peel resistance of hot stamping parts, reduces the occurrence of hydrogen-induced delayed damage and mold sintering, and improves the overall performance of the parts.
Smart Images

Figure CN118979213A_ABST
Abstract
Description
[0001] This application is a divisional application of the Chinese patent application with application number 202080041211.3, application date November 18, 2020, and invention name “Blank for hot stamping and its manufacturing method, hot stamping parts and its manufacturing method”. Technical Field
[0002] The invention relates to a hot stamping blank and a manufacturing method thereof, a hot stamping component and a manufacturing method thereof. Background Art
[0003] As the world's environmental and fuel consumption regulations are increasingly tightened, the demand for lighter vehicle materials is also increasing. As a result, research and development of ultra-high strength steel and hot stamping steel is very active. Among them, the hot stamping process usually consists of heating / forming / cooling / trimming, and the phase change and microstructural changes of the material are utilized in the process.
[0004] In recent years, research on preventing delayed fracture and improving corrosion resistance and weldability in hot stamping parts manufactured by hot stamping processes has been very active. Related technologies include Korean Patent Publication No. 10-2018-0095757 (Invention Title: Method for Manufacturing Hot Stamping Parts). Summary of the invention
[0005] Technical issues
[0006] Embodiments of the present invention provide a hot stamping blank and a method for manufacturing the same, and a hot stamping component and a method for manufacturing the same, which can prevent or minimize the problems of hydrogen-induced delayed fracture and die sintering during a hot stamping process.
[0007] Technical Solution
[0008] An embodiment of the present invention provides a method for manufacturing a blank for hot stamping, the method comprising: immersing a steel plate in a plating bath including aluminum and silicon to form a plating layer on the steel plate; and heating the steel plate on which the plating layer is formed at a first temperature for a first time, wherein the first temperature is 540°C to 600°C.
[0009] According to this embodiment, when the first temperature is 540° C., the first time may be greater than or equal to 60 minutes.
[0010] According to this embodiment, when the first temperature is 600° C., the first time may be greater than or equal to 10 minutes.
[0011] According to the present embodiment, forming the plating layer on the steel sheet may be forming an Al—Si plating layer on the steel sheet.
[0012] According to this embodiment, the coating weight of the coating layer may be 40 g / m 2Up to 200g / m 2 .
[0013] According to the present embodiment, in heating the steel sheet on which the plating layer has been formed, at least a portion of the steel sheet and the plating layer may diffuse into each other, thereby forming an alloyed layer.
[0014] According to this embodiment, the alloying layer may be provided as a single layer.
[0015] According to the present embodiment, the method may further include forming a blank by cutting the steel plate on which the alloying layer is formed.
[0016] Another embodiment of the present invention provides a hot stamping blank, which includes a steel plate and an alloying layer, wherein the alloying layer is located on the steel plate and is provided as a single layer.
[0017] According to the present embodiment, the steel plate may include 0.19wt% to 0.38wt% of carbon (C), 0.1wt% to 1wt% of silicon (Si), 1wt% to 2wt% of manganese (Mn), greater than 0 and less than or equal to 0.03wt% of phosphorus (P), greater than 0 and less than or equal to 0.01wt% of sulfur (S), 0.1wt% to 0.6wt% of chromium (Cr), 0.01wt% to 0.05wt% of titanium (Ti), 0.001wt% to 0.005wt% of boron (B), the remainder of iron (Fe) and inevitable impurities.
[0018] According to this embodiment, the alloying layer may be provided with a FeAlSi alloy.
[0019] Another embodiment of the present invention provides a method for manufacturing a hot stamping part, which includes: heating a steel plate on which a coating layer has been formed at a first temperature for a first time; cutting the heated steel plate to form a blank; multi-stage heating of the blank in stages; and uniform heating of the blank heated in multiple stages at a temperature of Ac3 to 1000°C; wherein the first temperature is 540°C to 600°C.
[0020] According to this embodiment, when the first temperature is 540° C., the first time may be greater than or equal to 60 minutes.
[0021] According to this embodiment, when the first temperature is 600° C., the first time may be greater than or equal to 10 minutes.
[0022] According to the present embodiment, multi-stage heating and uniform heating can be performed in a heating furnace provided with a plurality of zones having temperature ranges different from each other.
[0023] According to this embodiment, in the plurality of intervals, the ratio of the length of the interval in which the blank is heated in multiple stages to the length of the interval in which the blank is uniformly heated may satisfy a range of 1:1 to 4:1.
[0024] According to this embodiment, the temperatures of the plurality of zones may increase from the inlet of the heating furnace to the outlet of the heating furnace.
[0025] According to the present embodiment, in the section where the blank is heated in multiple stages, the temperature difference between two adjacent sections may be greater than 0°C and less than or equal to 100°C.
[0026] According to the present embodiment, among the plurality of zones, the temperature of the zone in which the blank is uniformly heated may be higher than the temperature of the zone in which the blank is multi-stage heated.
[0027] According to the present embodiment, after the soaking heating, the method may further include: transferring the soaked and heated blank from the heating furnace to a die; hot stamping the transferred blank to form a molded body; and cooling the formed molded body.
[0028] Another embodiment of the present invention provides a hot stamping component, which includes a steel plate and an alloyed layer arranged on the steel plate, wherein the alloyed layer is equipped with a first layer, a second layer and a third layer laminated in sequence, wherein the area fraction of the second layer to the alloyed layer is greater than 0 and less than or equal to 33%.
[0029] According to the present embodiment, the first layer may include α-Fe, the second layer may include Fe2Al5, and the third layer may include FeAl.
[0030] According to the present embodiment, the first layer may have a hardness of 200 Hv to 800 Hv, the second layer may have a hardness of 700 Hv to 1200 Hv, and the third layer may have a hardness of 200 Hv to 800 Hv.
[0031] Beneficial Effects
[0032] According to an embodiment of the present invention, before the hot stamping process, the steel sheet having an aluminum-silicon (Al-Si) coating layer formed thereon is heated at a first temperature for a first time to form an integral alloyed layer provided as a single layer on the steel sheet.
[0033] In addition, by multi-stage heating and uniform heating of the blank on which the alloy layer has been formed on the steel plate to produce hot stamping parts, the hydrogen embrittlement and peeling resistance of the manufactured parts can be improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 is a cross-sectional view showing a cross section of a blank for hot stamping according to an embodiment.
[0035] Figure 2 1 is a flowchart schematically showing a method for manufacturing a blank for hot stamping according to an embodiment.
[0036] Figure 3 It is schematically shown Figure 2Flow chart of the steel plate manufacturing process.
[0037] Figure 4 1 is a diagram showing a zone in which a steel sheet and a plating layer are alloyed in a method for producing a hot stamping blank according to an embodiment.
[0038] Figure 5 : is a cross-sectional view showing the cross section of the blank for hot stamping manufactured by the method for manufacturing the blank for hot stamping in which the heating step S120 is omitted.
[0039] Figure 6 is a cross-sectional view showing a cross section of a hot stamping part according to an embodiment.
[0040] Figure 7 FIG. 1 is a flow chart schematically showing a method for manufacturing a hot stamping component according to an embodiment.
[0041] Figure 8 FIG. 1 is a diagram showing a heating furnace equipped with a plurality of zones for describing a multi-stage heating step and a soaking heating step in a method for manufacturing a hot stamped component according to an embodiment.
[0042] Fig. 9 3 is a diagram showing a cross section of a component manufactured by the hot stamping component manufacturing method in which the heating step S310 is omitted.
[0043] Fig.10 is a diagram showing an iron (Fe)-aluminum (Al) phase diagram. DETAILED DESCRIPTION
[0044] The present invention is susceptible to various changes and embodiments, so specific embodiments are shown in the drawings and described in detail in the detailed description. Figure 1 The effects and features of the present invention and methods of implementing the present invention will become apparent from the embodiments described in detail. However, the present invention is not limited to the embodiments disclosed below and can be implemented in various forms.
[0045] In the following embodiments, terms such as first, second, etc. are used to distinguish one constituent element from another constituent element and do not have limiting meanings.
[0046] In the following embodiments, an expression in the singular includes an expression in the plural unless there is a clear distinction in the context.
[0047] In the following embodiments, terms such as including or having mean that the features or constituent elements recorded in the specification exist, and do not preclude the possibility of adding one or more other features or constituent elements.
[0048] In the following embodiments, when it is mentioned that part of a film, region, component, etc. is located above other parts, it includes not only the case where it is directly located above other parts, but also the case where other films, regions, components, etc. are sandwiched therebetween.
[0049] For the convenience of description, the size of the components in the drawings may be enlarged or reduced. For example, for the convenience of description, the size and thickness of each component shown in the drawings are arbitrarily shown, and therefore the present invention is not necessarily limited to the contents shown in the drawings.
[0050] When some embodiments can be implemented in other ways, a specific process sequence different from the described sequence can be implemented. For example, two processes described in succession can actually be performed at the same time, or can be performed in a reverse order to the described sequence.
[0051] Hereinafter, embodiments of the present invention will be described in detail with reference to the accompanying drawings. When describing with reference to the accompanying drawings, the same or corresponding components are given the same reference numerals.
[0052] Figure 1 is a cross-sectional view showing a cross section of a blank for hot stamping according to an embodiment.
[0053] refer to Figure 1 According to an embodiment, a hot stamping blank may include a steel plate 100 and a first alloyed layer 200 , wherein the first alloyed layer 200 is disposed on the steel plate 100 .
[0054] The steel plate 100 may be a steel plate manufactured by performing a hot rolling process and / or a cold rolling process on a steel billet, which is cast to include a predetermined alloy element at a predetermined content. For example, the steel plate 100 may include carbon (C), silicon (Si), manganese (Mn), phosphorus (P), sulfur (S), titanium (Ti), boron (B), a balance of iron (Fe), and other inevitable impurities. In addition, the steel plate 100 may further include one or more components of niobium (Nb), molybdenum (Mo), and aluminum (Al).
[0055] Carbon (C) is a main element that determines the strength and hardness of the steel plate 100, and is added for the purpose of ensuring the tensile strength and hardenability characteristics of the steel plate 100 after the hot stamping process. For example, carbon (C) may be included in the steel plate in an amount of 0.19wt% to 0.38wt% based on the total weight of the steel plate 100. When the content of carbon is less than 0.19wt%, it may be difficult to ensure the mechanical strength of the steel plate 100. On the contrary, when the content of carbon is greater than 0.38wt%, a decrease in toughness or a brittleness control problem of the steel plate 100 may be caused.
[0056] Silicon (Si) is a solid solution strengthening element, which can improve the strength and ductility of the steel sheet 100. In addition, silicon can play a role in inhibiting the formation of cementite, which is the initiation of cracking caused by hydrogen embrittlement. The silicon can be included in the steel sheet in an amount of 0.1wt% to 1wt% based on the total weight of the steel sheet 100. When the content of silicon is less than 0.1wt%, it is difficult to obtain the above-mentioned effect. On the contrary, when the content of silicon is greater than 1wt%, the plating characteristics of the steel sheet 100 are likely to decrease.
[0057] Manganese (Mn) is added for the purpose of increasing hardenability and strength during heat treatment. Manganese may be included in the steel sheet in an amount of 1wt% to 2wt% based on the total weight of the steel sheet 100. When the manganese content is less than 1wt%, the hard phase fraction of the hot stamping part may not meet the standard due to insufficient grain refinement effect. In contrast, when the manganese content is greater than 2wt%, ductility and toughness may be reduced due to manganese segregation or pearlite bands, which becomes a cause of reduced bending performance, and an uneven microstructure may occur.
[0058] Phosphorus (P) is added for the purpose of preventing the toughness of the steel sheet 100 from decreasing. Phosphorus may be included in the steel sheet in an amount greater than 0 and less than or equal to 0.03 wt % based on the total weight of the steel sheet 100. When the content of phosphorus is greater than 0.03 wt %, iron phosphide compounds are generated, thereby decreasing the toughness and causing cracks in the steel sheet 100 during the manufacturing process.
[0059] Sulfur (S) may be included in the steel plate in an amount greater than 0 and less than or equal to 0.01 wt % based on the total weight of the steel plate 100. When the sulfur content is greater than 0.01 wt %, hot working properties may be reduced and surface defects such as cracks may occur due to the generation of giant inclusions.
[0060] Chromium (Cr) is added for the purpose of improving the hardenability and strength of the steel plate 100. Chromium may be included in the steel plate in an amount of 0.1wt% to 0.6wt% based on the total weight of the steel plate 100. When the content of chromium is less than 0.1wt%, the effect of improving the hardenability and strength may be insufficient. On the contrary, when the content of chromium is greater than 0.6wt%, it may cause an increase in production cost and a decrease in toughness of the steel plate 100.
[0061] Titanium (Ti) is added for the purpose of improving the hardenability and material quality caused by the formation of precipitates after hot stamping heat treatment. In addition, titanium can effectively contribute to the refinement of austenite grains by forming precipitate phases such as Ti (C, N) at high temperatures. Titanium can be included in the steel plate in an amount of 0.01wt% to 0.05wt% based on the total weight of the steel plate 100. When the titanium content is less than 0.01wt%, the formation of precipitates may not be obvious and the grain refinement effect may not be sufficient. In contrast, when the titanium content is greater than 0.05wt%, a decrease in elongation and a decrease in toughness may occur.
[0062] Boron (B) is added for the purpose of ensuring the hardenability and strength of the steel sheet 100 by ensuring a martensitic structure, and a grain refinement effect is obtained by increasing the austenite grain growth temperature. Boron may be included in the steel sheet in an amount of 0.001wt% to 0.005wt% based on the total weight of the steel sheet 100. When the content of boron is less than 0.001wt%, the hardenability improvement effect may not be sufficient. On the contrary, when the content of boron is greater than 0.005wt%, the risk of brittleness and the risk of poor elongation may increase.
[0063] For example, the first alloyed layer 200 may be formed on at least one side of the steel plate 100 and may be provided as a single layer. For example, the first alloyed layer 200 may be provided as a FeAlSi alloy.
[0064] As described below, the steel sheet 100 and the aluminum-silicon (Al-Si) coating layer formed on the steel sheet 100 may be heated at a first temperature for a first time so that the steel sheet 100 and the aluminum-silicon (Al-Si) coating layer are alloyed to form the first alloyed layer 200. At this time, the aluminum-silicon (Al-Si) coating layer does not remain on the steel sheet 100, and at least a portion of the steel sheet 100 and the entire aluminum-silicon (Al-Si) coating layer may be alloyed.
[0065] Figure 2 is a flow chart schematically showing a method for manufacturing a blank for hot stamping according to an embodiment, Figure 3 It is schematically shown Figure 2 The following is a flow chart of the steel plate manufacturing process. Figure 2 and Figure 3 A method for manufacturing a blank for hot stamping is described.
[0066] refer to Figure 2 According to an embodiment, the method for manufacturing a blank for hot stamping may include a plating layer forming step S110 and a heating step S120 .
[0067] The plating layer forming step S110 is as follows Figure 3As shown, the steel billet may include a hot rolling step S210, a cooling / coiling step S220, a cold rolling step S230, an annealing heat treatment step S240, and a molten plating step S250. First, a steel billet in a semi-finished state as a target of a steel plate forming process is prepared. At this time, the steel billet may include 0.19wt% to 0.38wt% of carbon (C), 0.1wt% to 1wt% of silicon (Si), 1wt% to 2wt% of manganese (Mn), greater than 0 and less than or equal to 0.03wt% of phosphorus (P), greater than 0 and less than or equal to 0.01wt% of sulfur (S), 0.1wt% to 0.6wt% of chromium (Cr), 0.01wt% to 0.05wt% of titanium (Ti), 0.001wt% to 0.005wt% of boron (B), the remainder of iron (Fe) and unavoidable impurities.
[0068] In order to perform hot rolling, the reheating step of the steel slab is performed. In the steel slab reheating step, by reheating the steel slab secured by the continuous casting process at a predetermined temperature, the components segregated during casting can be re-solidified. For example, the slab reheating temperature (SRT) can be 1200°C to 1400°C. When the slab reheating temperature (SRT) is lower than 1200°C, the components segregated during casting cannot be fully re-solidified, so it may be difficult to obtain the homogenization effect of the alloy elements, and it is difficult to obtain the solid solution effect of titanium (Ti). The higher the slab reheating temperature (SRT), the more beneficial it is to homogenization, but when the slab reheating temperature (SRT) is higher than 1400°C, it is not only difficult to ensure the strength due to the increase in the grain size of the austenite crystal, but the excessive heating process may also increase the manufacturing cost of the steel plate.
[0069] In the hot rolling step S210 of the steel billet, the reheated steel billet is hot rolled at a predetermined finishing temperature. For example, the finishing delivery temperature (Finishing Delivery Temperature: FDT) can be 880°C to 950°C. At this time, when the finishing temperature (FDT) is lower than 880°C, a mixed crystal structure is generated due to rolling in abnormal areas, making it difficult to ensure the workability of the steel plate. Not only is there a problem of decreased workability due to microstructural inhomogeneity, but also problems with plate passability may occur during the hot rolling process due to rapid phase changes. When the finishing temperature (FDT) is higher than 950°C, the austenite grains may coarsen. In addition, due to the coarsening of TiC precipitates, the performance of hot stamping parts may be reduced.
[0070] In the cooling / coiling step S220, the hot-rolled steel plate is cooled to a predetermined coiling temperature (CoilingTemperature: CT) and coiled. For example, the coiling temperature may be 550°C to 800°C. The coiling temperature affects the redistribution of carbon (C). When the coiling temperature is lower than 550°C, the low-temperature phase fraction caused by overcooling increases, thereby increasing the strength, and there is a risk of increased rolling load during cold rolling, and the ductility may drop suddenly. In contrast, when the coiling temperature is higher than 800°C, formability and strength degradation may occur due to abnormal grain growth or excessive grain growth.
[0071] In the cold rolling step S230, the coiled steel sheet is uncoiled and pickled before cold rolling. At this time, the pickling is performed to remove the coiled steel sheet, that is, the hot rolled coil manufactured by the hot rolling process.
[0072] The annealing heat treatment step S240 is to perform annealing heat treatment on the cold-rolled steel sheet at a temperature higher than or equal to 700° C. For example, the annealing heat treatment includes heating the cold-rolled sheet and then cooling the heated cold-rolled sheet at a predetermined cooling rate.
[0073] The molten metal coating step S250 is to form a coating layer on the annealed heat treated steel sheet. For example, in the molten metal coating step S250, an aluminum-silicon (Al-Si) coating layer may be formed on the annealed heat treated steel sheet.
[0074] Specifically, in the molten plating step S250, the steel sheet may be immersed in a molten plating bath including 8wt% to 12wt% silicon (Si) and the remainder aluminum (Al). At this time, the molten plating bath may maintain a temperature of 400° C. to 700° C. The plating layer may be based on 40 g / m 2 Up to 200g / m 2 is formed by plating of an amount.
[0075] The heating step S120 heats the steel sheet on which the aluminum-silicon (Al-Si) plating layer has been formed. More specifically, the heating step S120 heats the steel sheet on which the aluminum-silicon (Al-Si) plating layer has been formed, thereby forming a first alloying layer.
[0076] In the heating step S120, the heating time and the heating temperature for heating the steel sheet on which the aluminum-silicon (Al-Si) plating layer has been formed may satisfy the following mathematical formula.
[0077] [Mathematical formula]
[0078] In(t)=α+(β / (R×T))
[0079] Here, t is heating time, α is a correction coefficient according to the plating amount, β is a correction coefficient according to the silicon (Si) content included in the plating layer, R is a gas constant, and T is a heating temperature. In the mathematical formula, the heating temperature (T) refers to an absolute temperature.
[0080] In the method for manufacturing a hot stamping blank according to one embodiment, the coating weight of the aluminum-silicon (Al-Si) coating layer formed on the steel plate may be 40 g / m 2 Up to 200g / m 2 , therefore the correction coefficient α according to the plating amount can have a value of -31.09 to -10.36.
[0081] In addition, considering the content of silicon (Si) included in the aluminum-silicon (Al—Si) coating layer and activation energy of silicon (Si), β may have a value of 84752.2 J / mol to 254256.5 J / mol.
[0082] For example, in the heating step S120, the steel plate on which an aluminum-silicon (Al-Si) coating layer has been formed can be heated at a heating temperature (T). For example, in the heating step S120, the steel plate on which an aluminum-silicon (Al-Si) coating layer has been formed can be heated at a first temperature. At this time, the first temperature can be 540°C to 600°C. When the first temperature is lower than 540°C, the time required for at least a portion of the steel plate to alloy with the aluminum-silicon (Al-Si) coating layer increases, so process loss (Loss) may occur. In contrast, when the first temperature is higher than 600°C, in the manufacturing process of the hot stamping part described later, a liquid phase may be formed on the surface of the blank, thereby causing problems with mold sintering.
[0083] For example, in the heating step S120, the steel plate on which the aluminum-silicon (Al-Si) coating layer has been formed may be heated during the heating time (t). For example, in the heating step S120, the steel plate on which the aluminum-silicon (Al-Si) coating layer has been formed may be heated for a first time. At this time, the first time may be 10 minutes to 120 minutes. Specifically, when the first temperature is 540°C, the first time may be greater than 60 minutes and less than 120 minutes, and when the first temperature is 600°C, the first time may be greater than or equal to 10 minutes and less than 60 minutes. When the first time is less than 10 minutes, the steel plate and the aluminum-silicon (Al-Si) coating layer may not be fully alloyed. In contrast, when the first time is greater than 120 minutes, the productivity of the hot stamping part may decrease due to the excessively long heating time.
[0084] According to the heating step S120, when the first temperature is 540°C, the shortest time required for the overall alloying of the aluminum-silicon (Al-Si) coating layer may be about 60 minutes. That is, according to the heating step S120, the overall alloyed layer can only be formed by heating the steel plate on which the aluminum-silicon (Al-Si) coating layer is formed at 540°C for about 60 minutes or more. Therefore, when the first temperature is higher than 540°C, the shortest time that the overall alloyed layer can be formed may be less than 60 minutes, and the shortest time may be between 10 minutes and 60 minutes.
[0085] In addition, according to the heating step S120, when the first temperature is 600° C., the shortest time required for the overall alloying of the aluminum-silicon (Al-Si) coating layer may be about 10 minutes. That is, according to the heating step S120, the overall alloying layer can only be formed by heating the steel plate on which the aluminum-silicon (Al-Si) coating layer is formed at 600° C. for about 10 minutes or more. Therefore, when the first temperature is lower than 600° C., the shortest time that the overall alloying layer can be formed may be greater than 10 minutes, and the shortest time may be between 10 minutes and 60 minutes.
[0086] Figure 4 : is a diagram showing the alloying range of the steel sheet and the coating layer in the method for manufacturing a hot stamping blank according to one embodiment. More specifically, Figure 4 This is a diagram showing the range of alloying of the plating layer in a graph of heating time according to the heating temperature that satisfies the mathematical formula.
[0087] As described above, in the heating step S120, the steel plate on which the aluminum-silicon (Al-Si) coating layer is formed may be heated at a first temperature for a first time so that at least a portion of the steel plate and the aluminum-silicon (Al-Si) coating layer are alloyed to form an entire alloyed layer.
[0088] Therefore, in the Figure 4 In the A interval, at least a portion of the steel plate and the aluminum-silicon (Al-Si) coating layer can diffuse with each other to form a first alloyed layer. At this time, the formed first alloyed layer can be configured as a single layer. For example, the first alloyed layer can be configured as a FeAlSi alloy. For example, no aluminum-silicon (Al-Si) coating layer remains on the steel plate, and at least a portion of the steel plate and the entire aluminum-silicon (Al-Si) coating layer can be alloyed.
[0089] Then, a blank forming step may be performed. The blank forming step may be to form a blank by cutting the steel plate on which the first alloyed layer has been formed. In the blank forming step, the steel plate on which the first alloyed layer has been formed may be cut into a desired shape according to the purpose to form the blank.
[0090] For example, the blank forming step may be performed before the heating step S120. For example, after the blank is formed by cutting a steel plate on which an aluminum-silicon (Al-Si) plating layer is formed, the heating step S120 of heating the formed blank may be performed.
[0091] Figure 5 This is a cross-sectional view showing a cross section of a blank for hot stamping manufactured by the method for manufacturing a blank for hot stamping in which the heating step S120 is omitted.
[0092] refer to Figure 1 and Figure 5 , the hot stamping blank manufactured by the hot stamping blank manufacturing method including the heating step S120 can be equipped with a steel plate 100 and a first alloyed layer 200 arranged on the steel plate 100. The first alloyed layer 200 can be formed by alloying the steel plate 100 and the aluminum-silicon (Al-Si) coating layer formed on the steel plate 100. Specifically, the steel plate 100 and the aluminum-silicon (Al-Si) coating layer formed on the steel plate 100 can be heated at a first temperature for a first time so that the steel plate 100 and the aluminum-silicon (Al-Si) coating layer are alloyed to form the first alloyed layer 200. At this time, no aluminum-silicon (Al-Si) coating layer remains on the steel plate 100, and at least a portion of the steel plate 100 and the aluminum-silicon (Al-Si) coating layer can be alloyed as a whole.
[0093] The hot stamping blank manufactured by the hot stamping blank manufacturing method in which the heating step S120 is omitted may include a steel plate 100 , a first alloyed layer 200 ′ disposed on the steel plate, and an aluminum-silicon (Al—Si) plating layer 250 ′ disposed on the first alloyed layer 200 ′.
[0094] Therefore, it can be seen that in the hot stamping blank in which the heating step S120 is performed, the aluminum-silicon (Al-Si) plating layer formed on the steel plate 100 is alloyed into the first alloying layer 200, but in the hot stamping blank in which the heating step S120 is omitted, part of the aluminum-silicon (Al-Si) plating layer remains on the steel plate 100.
[0095] Therefore, thanks to the fact that the aluminum-silicon (Al-Si) coating layers formed on the hot stamping blank during the heating step S120 are alloyed into the first alloying layer 200, the hydrogen inflow and mold sintering problems caused by the formation of an aluminum-silicon (Al-Si) liquid phase on the surface can be prevented or minimized during the austenitization process subjected to high-temperature heat treatment.
[0096] Figure 6 is a cross-sectional view showing a cross section of a hot stamping part according to an embodiment.
[0097] refer to Figure 6According to an embodiment, a hot stamping component may include a steel plate 100 and a second alloyed layer 300 , wherein the second alloyed layer 300 is located on the steel plate 100 and includes a first layer 310 , a second layer 320 , and a third layer 330 stacked in sequence.
[0098] The second alloyed layer 300 is formed on at least one side of the steel plate 100 and may include aluminum (Al). The second alloyed layer 300 may include a first layer 310, a second layer 320, and a third layer 330 sequentially laminated on the steel plate 100. The third layer 330 may include a FeAl phase.
[0099] The first layer 310 may include alloyed iron (Fe), aluminum (Al), and silicon (Si). For example, the first layer 310 may have an α-Fe phase.
[0100] The second layer 320 may include a Fe2Al5 phase. For example, the area fraction of the second layer 320 to the alloyed layer 300 may be greater than 0% and less than or equal to 33%. When the area fraction of the second layer 320 to the alloyed layer 300 is greater than 33%, the peeling resistance and hydrogen embrittlement resistance of the hot stamping component manufactured by the hot stamping component manufacturing method may be reduced.
[0101] On the other hand, the first layer 310 may have a hardness of 200 Hv to 800 Hv, the second layer 320 may have a hardness of 700 Hv to 1200 Hv, and the third layer 330 may have a hardness of 200 Hv to 800 Hv.
[0102] For example, the hot stamping part may further include a surface layer disposed on the second alloying layer 300. The surface layer is a layer including 80 wt % or more of aluminum (Al), which may prevent oxidation of the steel sheet 100. For example, the average thickness of the surface layer disposed on the steel sheet may be 100 nm to 200 nm.
[0103] Figure 7 FIG. 1 is a flow chart schematically showing a method for manufacturing a hot stamping component according to an embodiment.
[0104] refer to Figure 7 According to an embodiment, the method for manufacturing a hot stamping component may include a heating step S310, a blank forming step S320, a multi-stage heating step S330, a uniform heating step S340, a transfer step S350, a forming step S360, and a cooling step S370.
[0105] The heating step S310 is to heat the steel sheet on which the aluminum-silicon (Al-Si) coating layer has been formed. More specifically, the heating step S310 is to heat the steel sheet on which the aluminum-silicon (Al-Si) coating layer has been formed, thereby forming a first alloying layer. At this time, the steel sheet on which the aluminum-silicon (Al-Si) coating layer has been formed can be heated by Figure 3 The steel slab shown is manufactured through a hot rolling step S210, a cooling / coiling step S220, a cold rolling step S230, an annealing heat treatment step S240, and a hot-dip coating step S250.
[0106] In the heating step S310, the heating time and the heating temperature for heating the steel plate on which the aluminum-silicon (Al-Si) plating layer is formed may satisfy the following mathematical formula.
[0107] [Mathematical formula]
[0108] In(t)=α+(β / (R×T))
[0109] Here, t is heating time, α is a correction coefficient according to the plating amount, β is a correction coefficient according to the silicon (Si) content included in the plating layer, R is a gas constant, and T is a heating temperature. In the mathematical formula, the heating temperature (T) refers to an absolute temperature.
[0110] In the method for manufacturing a hot stamping component according to one embodiment, the coating weight of the aluminum-silicon (Al-Si) coating layer formed on the steel plate may be 40 g / m 2 Up to 200g / m 2 , therefore the correction coefficient α according to the plating amount can have a value of -31.09 to -10.36.
[0111] In addition, considering the content of silicon (Si) included in the aluminum-silicon (Al—Si) coating layer and activation energy of silicon (Si), β may have a value of 84752.2 J / mol to 254256.5 J / mol.
[0112] For example, in the heating step S310, the steel plate on which an aluminum-silicon (Al-Si) coating layer has been formed can be heated at a heating temperature (T). For example, in the heating step S120, the steel plate on which an aluminum-silicon (Al-Si) coating layer has been formed can be heated at a first temperature. At this time, the first temperature can be 540°C to 600°C. When the first temperature is lower than 540°C, the time required for at least a portion of the steel plate to alloy with the aluminum-silicon (Al-Si) coating layer increases, so process loss (Loss) may occur. In contrast, when the first temperature is higher than 600°C, during the manufacturing process of the hot stamping part, a liquid phase may be formed on the surface of the blank, causing problems with mold sintering.
[0113] For example, in the heating step S310, the steel plate on which the aluminum-silicon (Al-Si) coating layer has been formed may be heated during the heating time (t). For example, in the heating step S120, the steel plate on which the aluminum-silicon (Al-Si) coating layer has been formed may be heated for a first time. At this time, the first time may be 10 minutes to 120 minutes. Specifically, when the first temperature is 540°C, the first time may be greater than 60 minutes and less than 120 minutes, and when the first temperature is 600°C, the first time may be greater than or equal to 10 minutes and less than 60 minutes. When the first time is less than 10 minutes, the steel plate and the aluminum-silicon (Al-Si) coating layer may not be fully alloyed. In contrast, when the first time is greater than 120 minutes, the productivity of the hot stamping part may decrease due to the excessively long heating time.
[0114] According to the heating step S310, when the first temperature is 540°C, the shortest time required for the overall alloying of the aluminum-silicon (Al-Si) coating layer may be about 60 minutes. That is, according to the heating step S310, the overall alloyed layer can only be formed by heating the steel plate on which the aluminum-silicon (Al-Si) coating layer is formed at 540°C for about 60 minutes or more. Therefore, when the first temperature is higher than 540°C, the shortest time that the overall alloyed layer can be formed may be less than 60 minutes, and the shortest time may be between 10 minutes and 60 minutes.
[0115] In addition, according to the heating step S310, when the first temperature is 600° C., the shortest time required for the overall alloying of the aluminum-silicon (Al-Si) coating layer may be about 10 minutes. That is, according to the heating step S120, the overall alloying layer can only be formed by heating the steel plate on which the aluminum-silicon (Al-Si) coating layer is formed at 600° C. for about 10 minutes or more. Therefore, when the first temperature is lower than 600° C., the shortest time for forming the overall alloying layer may be greater than 10 minutes, and the shortest time may be between 10 minutes and 60 minutes.
[0116] The blank forming step S320 may be formed by cutting the steel plate on which the first alloyed layer is formed. In the blank forming step S320, the steel plate on which the first alloyed layer is formed may be cut into a desired shape according to the purpose to form the blank.
[0117] For example, the blank forming step S320 may also be performed before the heating step S310. For example, after the blank is formed by cutting a steel plate on which an aluminum-silicon (Al-Si) plating layer is formed, the heating step S120 of heating the formed blank may be performed.
[0118] The multi-stage heating step S330 may be heating the billet in stages, and the uniform heating step S340 may be heating the billet heated in multiple stages at a uniform temperature. In the multi-stage heating step S330, the billet can be heated in stages when passing through multiple sections equipped in the heating furnace. There may be multiple sections in the multiple sections equipped in the heating furnace for performing the multi-stage heating step S330, and the temperature of each section is set to rise from the entrance of the heating furnace where the billet is placed to the exit of the heating furnace where the billet is taken out, so that the billet can be heated in stages. The uniform heating step S340 may be performed after the multi-stage heating step S330. In the uniform heating step S340, the billet heated in multiple stages can be heat treated when passing through the section of the heating furnace with the temperature set to Ac3 to 1000°C. Preferably, in the uniform heating step S340, the billet heated in multiple stages can be uniformly heated at a temperature of 930°C to 1000°C. More preferably, in the uniform heating step S340 , the multi-stage heated billet may be uniformly heated at a temperature of 950° C. to 1000° C. In addition, the uniform heating step S340 may be performed in one or more of the plurality of zones provided in the heating furnace.
[0119] Figure 8 FIG. 1 is a diagram showing a heating furnace equipped with a plurality of zones for describing a multi-stage heating step and a soaking heating step in a method for manufacturing a hot stamped component according to an embodiment.
[0120] refer to Figure 8 According to an embodiment, the heating furnace may be equipped with a plurality of zones having different temperature ranges. More specifically, the heating furnace may be equipped with a first zone P1 having a first temperature range T1, a second zone P2 having a second temperature range T2, a third zone P3 having a third temperature range T3, a fourth zone P4 having a fourth temperature range T4, a fifth zone P5 having a fifth temperature range T5, a sixth zone P6 having a sixth temperature range T6, and a seventh zone P7 having a seventh temperature range T7.
[0121] For example, in the multi-stage heating step S330, the blank can be heated in stages when passing through a plurality of defined zones (e.g., the first zone P1 to the fourth zone P4) in the heating furnace. In addition, in the uniform heating step S340, the blank that has been multi-stage heated in the first zone P1 to the fourth zone P4 can be uniformly heated in the fifth zone P5 to the seventh zone P7.
[0122] The first section P1 to the seventh section P7 may be arranged in sequence in the heating furnace. The first section P1 having the first temperature range T1 may be adjacent to the entrance of the heating furnace where the blank is placed, and the seventh section P7 having the seventh temperature range T7 may be adjacent to the exit of the heating furnace where the blank is discharged. Therefore, the first section P1 having the first temperature range T1 may be the first section of the heating furnace, and the seventh section P7 having the seventh temperature range T7 may be the last section of the heating furnace. Among the multiple sections of the heating furnace, the fifth section P5, the sixth section P6, and the seventh section P7 may be sections for performing uniform heating, rather than sections for performing multi-stage heating.
[0123] The temperature of the plurality of zones provided in the heating furnace, for example, the temperature of the first zone P1 to the seventh zone P7, may increase from the entrance of the heating furnace where the billet is placed to the exit of the heating furnace where the billet is taken out. However, the temperatures of the fifth zone P5, the sixth zone P6, and the seventh zone P7 may be the same. In addition, among the plurality of zones provided in the heating furnace, the temperature difference between two adjacent zones may be greater than 0°C and less than or equal to 100°C. For example, the temperature difference between the first zone P1 and the second zone P2 may be greater than 0°C and less than or equal to 100°C.
[0124] For example, the first temperature range T1 of the first interval P1 may be 840°C to 860°C, 835°C to 865°C. The second temperature range T2 of the second interval P2 may be 870°C to 890°C, 865°C to 895°C. The third temperature range T3 of the third interval P3 may be 900°C to 920°C, 895°C to 925°C. The fourth temperature range T4 of the fourth interval P4 may be 920°C to 940°C, 915°C to 945°C. The fifth temperature range T5 of the fifth interval P5 may be Ac3 to 1000°C. Preferably, the fifth temperature range T5 of the fifth interval P5 may be greater than or equal to 930°C and less than or equal to 1000°C. Further preferably, the fifth temperature range T5 of the fifth interval P5 may be greater than or equal to 950°C and less than or equal to 1000°C. The sixth temperature range T6 of the sixth interval P6 and the seventh temperature range T7 of the seventh interval P7 may be the same as the fifth temperature range T5 of the fifth interval P5.
[0125] Figure 8 2 shows that the heating furnace according to one embodiment is equipped with seven zones with different temperature ranges, but the present invention is not limited thereto. The heating furnace may be equipped with five, six or eight zones with different temperature ranges.
[0126] The soaking heating step S340 can be performed in the last part of the plurality of sections of the heating furnace. For example, the soaking heating step can be performed in the fifth section P5, the sixth section P6, and the seventh section P7 of the heating furnace. When the heating furnace is equipped with a plurality of sections, if the length of one section is long, there may be problems such as temperature changes in the section. Therefore, while the sections for performing the soaking heating step are divided into the fifth section P5, the sixth section P6, and the seventh section P7, the fifth section P5, the sixth section P6, and the seventh section P7 can have the same temperature range in the heating furnace.
[0127] In the uniform heating step S340, the billet heated in multiple stages may be uniformly heated at a temperature of Ac3 to 1000° C. Preferably, in the uniform heating step S340, the billet heated in multiple stages may be uniformly heated at a temperature of 930° C. to 1000° C. More preferably, in the uniform heating step S340, the billet heated in multiple stages may be uniformly heated at a temperature of 950° C. to 1000° C.
[0128] For example, the ratio of the length D1 of the section where the billet is heated in multiple stages to the length D2 of the section where the billet is heated uniformly may be 1:1 to 4:1. More specifically, the ratio of the sum of the lengths of the first section P1 to the fourth section P4 as the section where the billet is heated in multiple stages to the sum of the lengths of the fifth section P5 to the seventh section P7 as the section where the billet is heated uniformly may satisfy 1:1 to 4:1. When the length of the section where the billet is heated uniformly increases, so that the ratio of the length D1 of the section where the billet is heated in multiple stages to the length D2 of the section where the billet is heated uniformly is greater than 1:1, an austenite (FCC) structure is generated in the uniform heating section, and the amount of hydrogen infiltrated into the billet increases, so that the delayed fracture may increase. In addition, when the length of the interval in which the blank is uniformly heated is reduced, so that the ratio of the length D1 of the interval in which the blank is heated in multiple stages to the length D2 of the interval in which the blank is uniformly heated is less than 4:1, since the uniform heating interval (time) is not fully ensured, the strength of the parts manufactured by the hot stamping part manufacturing process may be uneven.
[0129] For example, among the plurality of zones provided in the heating furnace, the length of the zone for performing the soaking heating step S340 may be 20% to 50% of the total length of the heating furnace. In addition, in the multi-stage heating step S330 and the soaking heating step S340, at least two blanks having different thicknesses may be transferred to the heating furnace at the same time.
[0130] For example, the blank may stay in the heating furnace for 180 seconds to 360 seconds. That is, the time for the blank to be heated in multiple stages and soaked may be 180 seconds to 360 seconds. When the time the blank stays in the heating furnace is shorter than 180 seconds, it may be difficult to fully soak at the required soaking temperature. In addition, when the time the blank stays in the heating furnace is longer than 360 seconds, the amount of hydrogen that penetrates into the blank may increase, the risk of delayed fracture may increase, and the corrosion resistance after hot stamping may decrease.
[0131] The transfer step S350 is to transfer the heated blank from the heating furnace to the die. In the transfer step S350, the heated blank may be air-cooled for 10 to 15 seconds.
[0132] The forming step S360 is to hot stamp the transferred blank to form a molded body, and the cooling step S370 is to cool the formed molded body.
[0133] The final product can be formed by cooling the formed body while being formed into the final part shape in the die. The die may be equipped with a cooling channel for refrigerant circulation inside. The heated blank can be quickly cooled by the circulation of the refrigerant supplied through the cooling channel equipped with the die. At this time, in order to prevent the spring back phenomenon of the sheet and maintain the desired shape, pressurization and rapid cooling can be performed in the state of closing the die. When the heated blank is formed and cooled, it can be cooled at an average cooling rate of at least greater than or equal to 10°C / s until the martensite final temperature. The blank can be kept in the die for 3 seconds to 20 seconds. When the holding time in the die is shorter than 3 seconds, the cooling of the material is not fully carried out, and the temperature deviation of each part caused by the residual heat may affect the embrittlement quality. In addition, since a sufficient amount of martensite is not generated, it is possible that the mechanical properties cannot be ensured. In contrast, when the holding time in the die is longer than 20 seconds, the productivity may decrease due to the longer holding time in the die.
[0134] Fig. 9 3 is a diagram showing a cross section of a component manufactured by the hot stamping component manufacturing method in which the heating step S310 is omitted.
[0135] refer to Figure 6 and Fig. 9 The hot stamping component manufactured by the hot stamping component manufacturing method including the heating step S310 includes a second alloyed layer 300, and the second alloyed layer 300 may include a first layer 310, a second layer 320, and a third layer 330 stacked in sequence. At this time, the first layer 310 may include α-Fe, the second layer 320 may include Fe2Al5, and the third layer 330 may include FeAl.
[0136] The hot stamping component manufactured by the manufacturing method in which the heating step S310 is omitted may also include a second alloyed layer 300'. The second alloyed layer 300' of the hot stamping component manufactured by the manufacturing method in which the heating step S310 is omitted may include a first layer 310', a second layer 320', a third layer 330' and a fourth layer 340' stacked in sequence. At this time, the first layer 310' may include α-Fe, the second layer 320' may include Fe2Al5, the third layer 330' may include FeAl, and the fourth layer 340' may include Fe2Al5.
[0137] It can be seen that the outermost layer of the second alloyed layer 300 included in the hot stamping component manufactured by the manufacturing method including the heating step S310 is FeAl phase, but the outermost layer of the second alloyed layer 300 ′ included in the hot stamping component manufactured by the manufacturing method in which the heating step S310 is omitted is Fe2Al5 phase.
[0138] Therefore, it can be seen that when the blank is preheated (heating step S310 ) before the multi-stage heating step S330 and the soaking heating step S340 , the final hot stamped part includes a second alloyed layer 300 in which no Fe 2 Al 5 phase is formed.
[0139] It is known that Fe2Al5 has a higher crack occurrence frequency and a higher crack extension degree than FeAl phase. When a component is manufactured by a manufacturing method of a hot stamping component according to an embodiment, the Fe2Al5 phase present in the outermost layer of the second alloying layer 300 disappears, so the frequency of crack occurrence decreases, crack extension is suppressed, and the peeling resistance of the manufactured component can be improved.
[0140] When a blank having an aluminum-silicon (Al-Si) coating formed on a steel plate is heated at the hot stamping process temperature, at least a portion of the aluminum-silicon (Al-Si) coating may remain without forming an alloying layer, thereby forming a liquid aluminum-silicon (Al-Si) layer. At this time, the hydrogen diffusion rate of the liquid aluminum-silicon (Al-Si) layer is faster than that of the alloying layer, and the surface hydrogen absorption capacity is stronger. Therefore, there is a problem of hydrogen being introduced into the steel plate through the liquid aluminum-silicon (Al-Si) layer, causing hydrogen-induced delayed damage. In addition, there is a problem of reduced productivity due to the sintering of the liquid aluminum-silicon (Al-Si) layer to the mold.
[0141] Fig.10 is a diagram showing an iron (Fe)-aluminum (Al) phase diagram.
[0142] refer to Fig.10, it can be seen that in the iron (Fe)-aluminum (Al) phase diagram, the melting point of FeAl3 is about 1160° C., and the melting point of Fe2Al5 is about 1169° C. Therefore, when forming a FeAl alloy, the alloy may have a higher melting point than the melting point of aluminum-silicon (Al-Si) (about 660° C.).
[0143] For example, before heating (multi-stage heating and soaking heating) a steel plate on which an aluminum-silicon (Al-Si) coating layer has been formed, the steel plate on which an aluminum-silicon (Al-Si) coating layer has been formed can be heated at a first temperature for a first time to alloy at least a portion of the steel plate with the aluminum-silicon (Al-Si) coating layer to form a first alloyed layer. Then, by heating (multi-stage heating and soaking heating) the steel plate on which the first alloyed layer has been formed to manufacture a hot stamping part, hydrogen-induced delayed damage of the manufactured part can be prevented or minimized, and the occurrence of a mold sintering phenomenon can be prevented or minimized during the process.
[0144] Below, the present invention will be further described in detail by examples. However, the following examples are used to specifically describe the present invention, and the scope of the present invention is not limited by the following examples. Those skilled in the art can appropriately modify and change the following examples within the scope of the present invention.
[0145] [Table 1]
[0146]
[0147] [Table 2]
[0148] Heating temperature Heating time Example 1 540℃ 60 minutes Example 2 600℃ 10 minutes Comparative Example 1 - - Comparative Example 2 540℃ 55 minutes Comparative Example 3 600℃ 8 minutes Comparative Example 4 480℃ 9 hours Comparative Example 5 520℃ 130 minutes Comparative Example 6 500℃ 270 minutes Comparative Example 7 540℃ 145 minutes Comparative Example 8 570℃ 280 minutes Comparative Example 9 600℃ 10 hours
[0149] [Table 3]
[0150] Heating furnace section First interval Second interval The third section The fourth section Fifth section The sixth section Seventh section Heating furnace length 1600mm 2800mm 3200mm 4400mm 4000mm 4000mm 2000mm
[0151] [Table 4]
[0152]
[0153] Table 1 shows the composition of the steel plate, Table 2 shows the heating temperature and heating time of Example 1, Example 2, and Comparative Examples 1 to 9, Table 3 shows the length of each zone of the heating furnace, and Table 4 shows the heating furnace set temperature and heating furnace residence time of each zone.
[0154] A blank having an aluminum-silicon (Al-Si) coating layer formed on a steel plate having the composition in Table 1 was heated according to the conditions in Table 2, and then the heated blank was heated in a heating furnace satisfying the conditions in Tables 3 and 4 by multi-stage heating and uniform heating to produce a hot stamping part.
[0155] According to Table 2, Examples 1 and 2 are examples that satisfy the heating temperature and heating time of heating steps S120 and S310, Comparative Example 1 is an example in which heating steps S120 and S310 are not performed, Comparative Examples 2 and 3 are examples in which the heating time of heating steps S120 and S310 is not satisfied, and Comparative Examples 4 to 6 are examples in which the heating temperature of heating steps S120 and S310 is not satisfied.
[0156] As in Example 1 and Example 2, when the heating temperature and heating time of heating steps S120 and S310 are met, at least a portion of the steel plate is alloyed with the aluminum-silicon (Al-Si) coating layer formed on the steel plate, thereby forming an overall alloyed layer.
[0157] However, as in Comparative Examples 1 to 6, when the heating steps S120 and S310 are omitted or the heating temperature and / or heating time of the heating steps S120 and S310 are not met, an aluminum-silicon (Al—Si) coating layer may remain on the steel plate.
[0158] In addition, Comparative Examples 7 to 9 correspond to the case where the heating time exceeds the heating step S120, S310. Taking Comparative Examples 7 to 9 as an example, at least a portion of the steel plate is alloyed with the aluminum-silicon (Al-Si) coating layer formed on the steel plate, thereby forming an overall alloyed layer. However, due to the excessively long heating time in Comparative Examples 7 to 9, the productivity of the hot stamping parts may decrease.
[0159] <Diffusible Hydrogen Content and Hydrogen-Induced Delayed Failure Evaluation>
[0160] Thermal desorption spectroscopy was performed on Example 1, Example 2, and Comparative Examples 1 to 9. More specifically, the temperature was raised from room temperature to 500°C at a heating rate of 20°C / min, and the content of diffused hydrogen released by the hot stamping parts at a temperature less than or equal to 350°C was measured. The hydrogen-induced delayed damage evaluation was performed by a four-point bending test. The four-point bending test is a test method in which a stress less than or equal to the elastic limit level is applied to a specific point of a specimen manufactured by reproducing a state exposed to a corrosive environment to confirm whether stress corrosion cracking occurs. At this time, stress corrosion cracking refers to cracking caused by the simultaneous action of corrosion and continuous tensile stress.
[0161] [Table 5]
[0162] Diffusible hydrogen content (wppm) Hydrogen-induced delayed damage Example 1 0.376 Unbroken Example 2 0.364 Unbroken Comparative Example 1 0.923 fracture Comparative Example 2 0.759 fracture Comparative Example 3 0.702 fracture Comparative Example 4 0.816 fracture Comparative Example 5 0.768 fracture Comparative Example 6 0.769 fracture Comparative Example 7 0.391 Unbroken Comparative Example 8 0.403 Unbroken Comparative Example 9 0.401 Unbroken
[0163] Table 5 shows the content of diffused hydrogen released from Example 1, Example 2, and Comparative Examples 1 to 9 and the results of the evaluation of hydrogen-induced delayed damage.
[0164] Referring to Table 5, it can be seen that the amount of diffusible hydrogen released from Comparative Example 1 is greater than that released from Examples 1 and 2. This shows that when the heating steps S120 and S310 are performed before the hot stamping process, the amount of hydrogen flowing in from the outside is reduced.
[0165] In addition, it can be seen that the amount of diffusible hydrogen released from Comparative Examples 2 and 3 (when the heating time is not satisfied) is greater than that from Examples 1 and 2.
[0166] Furthermore, it can be seen that the diffusible hydrogen content released from Comparative Examples 4, 5, and 6 (when the heating temperature is not satisfied) is greater than that released from Examples 1 and 2.
[0167] However, it can be seen that although the diffusible hydrogen content released from Comparative Examples 7, 8 and 9 (when the heating temperature is met but the heating time is longer than 60 minutes) is greater than that released from Examples 1 and 2, it is less than that released from Comparative Examples 1 to 6.
[0168] As can be seen from this, when the heating steps S120 and S310 are performed before the hot stamping process, the amount of diffusible hydrogen released from the manufactured hot stamped component is reduced, and thus the amount of hydrogen flowing in from the outside is reduced.
[0169] However, when the steel plate on which aluminum-silicon (Al-Si) is formed is heated at a first temperature for 120 minutes or more before performing the hot stamping process, although the amount of diffusible hydrogen released from the manufactured hot stamped part is reduced, when the heating time is longer than 120 minutes, the productivity of the hot stamped part may decrease due to the excessively long heating time.
[0170] The results of the hydrogen-induced delayed fracture evaluation showed that Example 1, Example 2, and Comparative Examples 7 to 9 did not break, but Comparative Examples 1 to 6 broke.
[0171] It can be seen that when the heating steps S120 and S310 are performed before the hot stamping process, the amount of hydrogen flowing in from the outside is reduced, and thus a better resistance to delayed hydrogen damage is shown. Therefore, before the hot stamping process is performed, when the steel sheet on which aluminum-silicon (Al-Si) is formed is heated at a first temperature for a first time, the hydrogen embrittlement of the manufactured hot stamping part can be improved.
[0172] <Evaluation of Peeling Resistance>
[0173] In order to evaluate the peeling resistance of Example 1, Example 2 and Comparative Examples 1 to Comparative Examples 6, the adhesion of the alloyed layer was measured by a dolly test. The adhesion was measured under the conditions of a speed of 0.6 MPa / s, a peeling area of 20 pi, a maximum load of 24 MPa, a curing temperature of 120°C, and a curing time of 20 minutes.
[0174] [Table 6]
[0175] Adhesion strength Example 1 6.29MPa Example 2 6.44MPa Comparative Example 1 3.44MPa Comparative Example 2 4.08MPa Comparative Example 3 3.34MPa Comparative Example 4 3.52MPa Comparative Example 5 3.79MPa Comparative Example 6 3.12MPa
[0176] Table 6 shows the dolly test results of Example 1, Example 2, and Comparative Examples 1 to 6.
[0177] Referring to Table 6, it can be seen that the bonding strengths of Example 1 and Example 2 are higher than the bonding strengths of Comparative Examples 1 to 6.
[0178] It can be seen that the peeling resistance of the hot stamping part that performs the heating steps S120 and S310 before the hot stamping process is higher than the peeling resistance of the hot stamping part that omits the heating steps S120 and S310 or performs a heating step that does not meet the heating conditions.
[0179] Therefore, when the heating steps S120 and S310 are performed before the hot stamping process is performed, the peeling resistance of the manufactured hot stamping part can be improved.
[0180] As described above, the present invention is described with reference to an embodiment shown in the accompanying drawings, but this is only exemplary, and those skilled in the art will understand that various changes and variations of the embodiments can be made based on the embodiments. Therefore, the true technical protection scope of the present invention should be determined by the technical concept of the attached claims.
Claims
1. A method for manufacturing a hot stamping blank, the method comprising: immersing the steel sheet in a plating bath including aluminum and silicon, thereby forming a plating layer on the steel sheet; as well as heating the steel sheet having the coating layer formed thereon at a first temperature for a first time, The first temperature is 540°C to 600°C, and When the first temperature is 600° C., the first time is 10 minutes to 60 minutes.
2. The method for manufacturing a hot stamping blank according to claim 1, wherein: When the first temperature is 540° C., the first time is greater than or equal to 60 minutes.
3. The method for manufacturing a hot stamping blank according to claim 1, wherein: Forming the plating layer on the steel sheet is forming an Al—Si plating layer on the steel sheet.
4. The method for manufacturing a hot stamping blank according to claim 3, wherein: The coating weight of the coating layer is 40g / m 2 Up to 200g / m 2 .
5. The method for manufacturing a hot stamping blank according to claim 3, wherein: In heating the steel sheet on which the plating layer has been formed, at least a portion of the steel sheet and the plating layer diffuse into each other, thereby forming an alloyed layer.
6. The method for manufacturing a hot stamping blank according to claim 5, wherein: The alloying layer is provided as a single layer.
7. The method for manufacturing a hot stamping blank according to claim 5, further comprising: The blank is formed by cutting the steel plate on which the alloyed layer is formed.
Citation Information
Patent Citations
Hot press-formed member with excellent powdering resistance at time of press forming, and method for manufacturing same
CN106164317A
Hpf member having excellent delamination resistance, and preparation method therefor
CN107614733A
Aluminum-iron alloy-coated steel sheet for hot press forming, having excellent hydrogen delayed fracture resistance, peeling resistance, and weldability and hot-formed member using same
CN108474096A
High-toughness hot stamping aluminum-silicon coated steel plate and preparing method thereof
CN110484820A
Fe-Al PLATED HOT-STAMPED MEMBER AND METHOD FOR PRODUCING Fe-Al PLATED HOT-STAMPED MEMBER
CN110573644A