Roller type pulse electroplating equipment and method and electroplating film
By using roller pulse electroplating equipment and methods, the problems of uneven current distribution and coating accumulation in electroplating equipment are solved by applying alternating positive and negative pulse currents. This achieves uniformity and density gradient changes in the electroplated coating of the substrate, thereby improving production efficiency and product quality.
Patent Information
- Application Number
- CN202411053419.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-19
AI Technical Summary
In existing electroplating equipment, edge electroplating leads to uneven current distribution on the substrate, and the accumulation of coating on the conductive roller causes scratches or perforations. Electroplating on the conductive roller also results in uneven coating and oxidation problems, affecting production efficiency and product quality.
A roller pulse electroplating equipment is used. Through the conductive roller assembly and the pulse power supply assembly, positive and reverse pulse currents are applied alternately to control the current density and coating thickness, ensuring uniform electroplating of the substrate and preventing coating accumulation on the conductive roller.
It achieves a gradient change in the thickness and density of the electroplated layer on the substrate, avoids the accumulation of plating layer on the conductive roller, improves production efficiency and product quality, and prevents scratches or perforations.
Smart Images

Figure CN118979296A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electroplating, and in particular to a roller pulse electroplating device, method and electroplating film. Background Art
[0002] At present, the production process of composite copper current collectors mostly adopts magnetron plus electroplating. Magnetron makes the substrate conductive, and electroplating is used to quickly thicken the coating. Electroplating equipment is divided into two types based on the way of powering, one is clamping electroplating, and the other is conductive roller electroplating. Both of the above methods use DC power supply.
[0003] Disadvantages / deficiencies of existing technologies:
[0004] At present, in the clamped edge electroplating, the electrode (cathode) is clamped on the two edges of the substrate. In the TD direction, the current distribution on the substrate is uneven, the current density on both sides is high, and the current density in the middle is low, resulting in uneven thickness of the coating in the TD direction. At present, it can only be adjusted by adjusting the arrangement (density) of the anode plate. However, there is no way to adjust it after the equipment is formed. Because of the uneven current distribution, the width of the substrate cannot be too large, which reduces the production efficiency of the equipment.
[0005] At present, the conductive roller is used for electrification, that is, the electrode (cathode) is added to the conductive roller, and the conductive roller contacts the substrate over the entire width. In theory, the current distribution is uniform in the TD direction and uneven in the MD direction, but the substrate moves along the MD direction. Generally speaking, the current loaded on the substrate during the entire electroplating process is still uniform. However, since there is also current on the conductive roller, the plating solution contacts the conductive roller and also plates the conductive roller. As time goes by, the coating on the conductive roller will become thicker and thicker, which will cause scratches on the contacted substrate. At present, the conductive roller is placed outside the plating tank, and a squeezing roller is added at the front end of the conductive roller to prevent too much plating solution from being brought to the conductive roller. The conductive roller is sprayed or immersed in dilute sulfuric acid for deplating. However, this method brings new problems. The substrate (with the plated copper layer) after the liquid is discharged is very easy to oxidize, and an oxide layer will be formed on the substrate. When passing through multiple plating tanks, multiple oxide layers will be formed, which cannot meet the product requirements. In addition, due to the volatilization of water on the squeezing roller, copper sulfate crystals will be formed, which will also cause scratches or perforations to the substrate. Summary of the invention
[0006] The object of the present invention is to provide a roller pulse electroplating device, method and electroplating film to solve the problems raised in the above background technology.
[0007] In order to solve the above technical problems, the present invention provides the following technical solutions: a roller pulse electroplating device, comprising an aqueduct mechanism and a power supply assembly, a unwinding mechanism is installed on one side of the aqueduct mechanism, the aqueduct mechanism comprises a plating trough, when the aqueduct is in use, the aqueduct is filled with plating solution, a conductive roller assembly is installed in the aqueduct, when the conductive roller assembly is in use, the conductive roller assembly is immersed in the plating solution, the unwinding mechanism sends out the substrate, and passes it around the conductive roller assembly, the substrate is electrically connected to the conductive roller, the power supply assembly applies current to the conductive roller assembly, the forward cycle time of the current is greater than the reverse cycle time, and / or the forward cycle current amplitude of the current is greater than the reverse cycle current amplitude.
[0008] The conductive roller assembly consists of a conductive roller A and a conductive roller B, wherein the conductive roller A is located on one side of the conductive roller B, and the conductive roller A and the conductive roller B are respectively used to contact and conduct with the opposite sides of the substrate, a group of rollers are installed on one side of the conductive roller B, an insoluble anode A is arranged between the conductive roller B and the roller, a tension roller A is installed on one side of the roller, and an insoluble anode B is arranged between the tension roller A and the roller, the conductive roller A, the conductive roller B, the roller, the insoluble anode A, the tension roller A and the insoluble anode B form an electroplating unit, a plurality of the electroplating units are arranged in the aqueduct, and the substrate passes through the plurality of electroplating units in sequence.
[0009] A washing mechanism, a drying mechanism and a winding mechanism are sequentially installed on one side of the aqueduct mechanism. The substrate is sequentially connected to a conductive roller A, a conductive roller B, an insoluble anode A, a passing roller, an insoluble anode B and a tension roller A. After the substrate passes through the aqueduct mechanism, it is sequentially connected to the washing mechanism, the drying mechanism and the winding mechanism. The conductive roller A and the conductive roller B are both made of titanium anode material. One end of the conductive roller A and the conductive roller B are both provided with a brush. The plating solution is a copper sulfate solution. The tension roller A is made of L stainless steel. The insoluble anode A and the insoluble anode B are both made of titanium anode material. The insoluble anode A and the insoluble anode B are both electrically connected to the power supply component.
[0010] The power supply component consists of a pulse power supply A and a pulse power supply B. Both the pulse power supply A and the pulse power supply B output unidirectional pulse currents, and the output current pulse periods of the pulse power supply A and the pulse power supply B do not overlap at all. The pulse currents output by the pulse power supply A and the pulse power supply B are in opposite directions.
[0011] The power supply component is a pulse power supply, which is a bidirectional pulse power supply. The pulse power supply outputs a bidirectional pulse current, the forward cycle time of the bidirectional pulse current is greater than the reverse cycle time, and / or the forward cycle current amplitude of the pulse current is greater than the reverse cycle current amplitude.
[0012] The pulse power supply A and the pulse power supply B are both constant current pulse power supplies. The pulse power supply A and the pulse power supply B sputter a conductive copper layer on the surface of the substrate through the conductive roller A and the conductive roller B respectively according to the electroplating principle.
[0013] A roller pulse electroplating method comprises the following steps: in the roller pulse electroplating equipment, placing a substrate in a plating solution, performing a pulse electroplating process to obtain a plating layer; thereby obtaining an electroplated film.
[0014] In the pulse electroplating process, the forward pulse time is longer than the reverse pulse time; and the current amplitudes of the forward and reverse pulses are the same.
[0015] A plated film is obtained by electroplating according to a roller pulse electroplating method.
[0016] The electroplated film comprises a substrate and a plating layer, wherein the plating layer is a metal layer, and in the direction from the surface of the metal layer to the surface of the substrate, the density of the metal layer presents a gradient rising trend.
[0017] Compared with the prior art, the beneficial effects achieved by the present invention are: positive pulse plating, reverse pulse copper removal. When the positive pulse is applied, the copper layer on the substrate becomes thicker and thicker until the required thickness is reached. After that, when the reverse pulse is applied, the copper layer on the conductive roller A will be dissolved in each cycle due to the effect of the reverse pulse current, so that the copper layer will not accumulate, achieving the purpose of "no plating" on the conductive roller A. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:
[0019] Figure 1 It is a schematic diagram of the overall structure of the present invention;
[0020] Figure 2 It is a structural diagram of the aqueduct mechanism and a waveform diagram of the pulse power supply;
[0021] Figure 3 It is the waveform diagram of unidirectional pulse current;
[0022] Figure 4 It is the waveform diagram of bidirectional pulse current.
[0023] In the figure: 1. unwinding mechanism; 2. aqueduct mechanism; 21. plating solution; 22. conductive roller A; 23. conductive roller B; 24. insoluble anode A; 241. insoluble anode B; 25. over roller; 26. tension roller A; 27. pulse power supply A; 28. pulse power supply B; 29. substrate; 3. washing mechanism; 4. drying mechanism; 5. winding mechanism. DETAILED DESCRIPTION
[0024] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] See also Figure 1-Figure 4 The present invention provides a technical solution: a roller pulse electroplating device, including an aqueduct mechanism 2 and a power supply assembly, a unwinding mechanism 1 is installed on one side of the aqueduct mechanism 2, the aqueduct mechanism 2 includes a plating tank, when the aqueduct is in use, the aqueduct is filled with a plating solution 21, a conductive roller assembly is installed in the aqueduct, when the conductive roller assembly is in use, the conductive roller assembly is immersed in the plating solution 21, the unwinding mechanism 1 sends out a substrate 29, and passes it after it is wrapped around the conductive roller assembly, the substrate is electrically connected to the conductive roller, the power supply assembly applies current to the conductive roller assembly, the positive cycle time of the current is greater than the reverse cycle time, and / or the positive cycle current amplitude of the current is greater than the reverse cycle current amplitude.
[0026] The conductive roller assembly consists of a conductive roller A22 and a conductive roller B23. The conductive roller A22 is located on one side of the conductive roller B23. The conductive roller A22 and the conductive roller B23 are respectively used to contact and conduct with the opposite sides of the substrate. A group of rollers 25 are installed on one side of the conductive roller B23. An insoluble anode A24 is arranged between the conductive roller B23 and the roller 25. A tension roller A26 is installed on one side of the roller 25. An insoluble anode B241 is arranged between the tension roller A26 and the roller 25. The conductive roller A22, the conductive roller B23, the roller 25, the insoluble anode A24, the tension roller A26 and the insoluble anode B241 form an electroplating unit. A plurality of electroplating units are arranged in the aqueduct, and the substrate 29 passes through the plurality of electroplating units in sequence.
[0027] A washing mechanism 3, a drying mechanism 4 and a winding mechanism 5 are sequentially installed on one side of the aqueduct mechanism 2. The substrate 29 is sequentially connected to the conductive roller A22, the conductive roller B23, the insoluble anode A24, the passing roller 25, the insoluble anode B241 and the tension roller A26. After the substrate 29 passes through the aqueduct mechanism 2, it is sequentially connected to the washing mechanism 3, the drying mechanism 4 and the winding mechanism 5. The conductive roller A22 and the conductive roller B23 are both made of titanium anode material. Brushes are provided at one end of the conductive roller A22 and the conductive roller B23. The plating solution 21 is copper sulfate solution. The tension roller A26 is made of 304L stainless steel. The insoluble anode A24 and the insoluble anode B241 are both made of titanium anode material. The insoluble anode A24 and the insoluble anode B241 are both electrically connected to the power supply assembly.
[0028] A roller pulse electroplating method includes the following steps: in a roller pulse electroplating device, a substrate 29 is placed in a plating solution 21, and a pulse electroplating process is performed to obtain a coating; thereby, an electroplated film is obtained.
[0029] In the pulse electroplating process, the forward pulse time is greater than the reverse pulse time; the current amplitudes of the forward and reverse pulses are the same.
[0030] A plated film is obtained by electroplating according to a roller pulse electroplating method.
[0031] Embodiment 1:
[0032] The power supply component is composed of a pulse power supply A27 and a pulse power supply B28. Both the pulse power supply A27 and the pulse power supply B28 output unidirectional pulse currents, and the output current pulse cycles of the pulse power supply A27 and the pulse power supply B28 do not overlap at all. The pulse currents output by the pulse power supply A27 and the pulse power supply B28 are in opposite directions.
[0033] The pulse power supply A27 and the pulse power supply B28 are both constant current pulse power supplies. According to the electroplating principle, the pulse power supply A27 and the pulse power supply B28 sputter a conductive copper layer on the surface of the substrate 29 through the conductive roller A22 and the conductive roller B23 respectively.
[0034] Embodiment 2:
[0035] The power supply component is a pulse power supply, which is a bidirectional pulse power supply. The pulse power supply outputs a bidirectional pulse current, the forward cycle time of the bidirectional pulse current is greater than the reverse cycle time, and / or the forward cycle current amplitude of the pulse current is greater than the reverse cycle current amplitude.
[0036] The bidirectional pulse power supply sputters a conductive copper layer on the surface of the substrate 29 through the conductive roller A22 and the conductive roller B23 according to the electroplating principle.
[0037] The working principle of the present invention is as follows: when the pulse power supply A27 is loaded with a positive pulse current, the conductive roller A22 acts as a cathode, and thus the substrate 29 also acts as a cathode, and the insoluble anode A24 acts as an anode. According to the electroplating principle, copper will be deposited at the cathode, so that the copper layer of the substrate 29 is thickened, and a copper layer will also be plated on the conductive roller A22. According to the conductivity principle of the material, the current density on the conductive roller A22 is much smaller than the current density on the substrate 29, and there is no anode function under the conductive roller A22, so the copper layer deposited on the conductive roller A22 will be much lower than the copper layer deposited on the substrate 29.
[0038] When the pulse power supply A27 loads a reverse pulse current, the conductive roller A22 acts as the anode, and thus the substrate 29 also acts as the anode, and the insoluble anode A24 acts as the cathode. According to the electroplating principle, the copper on the anode will be redissolved into the plating solution 21. Since the reverse pulse time is short and the copper layer on the conductive roller A22 is thin, when the copper layer on the conductive roller A22 is completely dissolved, only a small part of the copper on the substrate 29 is dissolved.
[0039] In a conventional electroplating process, metal ions will be deposited layer by layer on the surface of the base film, and the density will gradually decrease from the bottom layer to the surface layer; in this scheme, the electroplating-electrolysis cycle is carried out, and each electrolysis will electrolyze the metal with the lowest surface density of the metal layer electroplated in the previous electroplating, and then deposit again. Each cycle will form a layer of plating with a certain trend of density change, and there will also be a certain trend of change between multiple layers.
[0040] Under continuous operation, the copper layer on the substrate 29 becomes thicker and thicker until the required thickness is reached. Due to the reverse pulse current, the copper layer on the conductive roller A22 is dissolved in each cycle, so no copper layer is accumulated, thus achieving the purpose of "no plating" on the conductive roller A22.
[0041] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0042] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A roller pulse plating equipment, Features: The invention comprises an aqueduct mechanism (2) and a power supply component, wherein a reeling mechanism (1) is installed on one side of the aqueduct mechanism (2), wherein the aqueduct mechanism (2) comprises a plating tank, wherein when the aqueduct is in use, the aqueduct is filled with a plating solution (21), wherein a conductive roller component is installed in the aqueduct, wherein when the conductive roller component is in use, the conductive roller component is immersed in the plating solution (21), wherein the reeling mechanism (1) delivers a substrate (29) and passes it behind the conductive roller component, wherein the substrate is electrically connected to the conductive roller component, wherein the power supply component applies a current to the conductive roller component, wherein the positive cycle time of the current is greater than the reverse cycle time, and / or the positive cycle current amplitude of the current is greater than the reverse cycle current amplitude.
2. A roller pulse plating device according to claim 1, Features: The conductive roller assembly is composed of a conductive roller A (22) and a conductive roller B (23). The conductive roller A (22) is located on one side of the conductive roller B (23). The conductive roller A (22) and the conductive roller B (23) are respectively used to contact and conduct with two opposite sides of the substrate. A group of rollers (25) are installed on one side of the conductive roller B (23). An insoluble anode A (24) is arranged between the conductive roller B (23) and the roller (25). A tension roller A (26) is installed on one side of the roller (25). An insoluble anode B (241) is arranged between the tension roller A (26) and the roller (25). The conductive roller A (22), the conductive roller B (23), the roller (25), the insoluble anode A (24), the tension roller A (26) and the insoluble anode B (241) form an electroplating unit. A plurality of electroplating units are arranged in the aqueduct. The substrate (29) passes through the plurality of electroplating units in sequence.
3. A roller pulse plating device according to claim 2, Features: A washing mechanism (3), a drying mechanism (4) and a winding mechanism (5) are sequentially installed on one side of the aqueduct mechanism (2); the substrate (29) is sequentially connected to a conductive roller A (22), a conductive roller B (23), an insoluble anode A (24), a passing roller (25), an insoluble anode B (241) and a tension roller A (26); after the substrate (29) passes through the aqueduct mechanism (2), it is sequentially connected to the washing mechanism (3), the drying mechanism (4) and the winding mechanism (5); The conductive roller A (22) and the conductive roller B (23) are both made of titanium anode material, and one end of the conductive roller A (22) and the conductive roller B (23) are both provided with a brush, the plating solution (21) is a copper sulfate solution, the tension roller A (26) is made of 304L stainless steel, the insoluble anode A (24) and the insoluble anode B (241) are both made of titanium anode material, and the insoluble anode A (24) and the insoluble anode B (241) are both electrically connected to a power supply component.
4. A roller pulse plating device according to claim 3, Features: The power supply assembly is composed of a pulse power supply A (27) and a pulse power supply B (28). Both the pulse power supply A (27) and the pulse power supply B (28) output unidirectional pulse currents, and the output current pulse cycles of the pulse power supply A (27) and the pulse power supply B (28) do not overlap at all. The pulse currents output by the pulse power supply A (27) and the pulse power supply B (28) are in opposite directions.
5. A roller pulse plating device according to claim 3, Features: The power supply component is a pulse power supply, which is a bidirectional pulse power supply. The pulse power supply outputs a bidirectional pulse current, the forward cycle time of the bidirectional pulse current is greater than the reverse cycle time, and / or the forward cycle current amplitude of the pulse current is greater than the reverse cycle current amplitude.
6. A roller pulse plating device according to claim 4, Features: The pulse power source A (27) and the pulse power source B (28) are both constant current pulse power sources. The pulse power source A (27) and the pulse power source B (28) respectively sputter a conductive copper layer on the surface of the substrate (29) through the conductive roller A (22) and the conductive roller B (23) according to the electroplating principle.
7. A roller pulse plating method, Features: The roller pulse electroplating method comprises the following steps: in a roller pulse electroplating device as described in any one of claims 1 to 6, placing a substrate (29) in a plating solution (21), performing a pulse electroplating process to obtain a coating; thereby obtaining an electroplated film.
8. A roller pulse plating method according to claim 7, Features: In the pulse electroplating process, the forward pulse time is greater than the reverse pulse time; The current amplitude of the forward and reverse pulses is the same.
9. An electroplated film, Features: The electroplated film obtained by roller pulse plating method according to claim 7.
10. The electroplated film according to claim 9, Features: The electroplated film comprises a substrate (29) and a plating layer, wherein the plating layer is a metal layer, and in the direction from the surface of the metal layer to the surface of the substrate (29), the density of the metal layer presents a gradient upward trend.
Citation Information
Cited By
A low-damage scratch-preventing metal particle-preventing roll-to-roll electroplating cathode conductive roller shaft, a manufacturing method thereof, an electroplating method, and an electroplating apparatus
CN123043602A