Flexible nylon 11 piezoelectric separation fiber membrane with adjustable structure as well as preparation method and application of flexible nylon 11 piezoelectric separation fiber membrane
Through cosolvent-induced crystallization and coaxial electrospinning technology, a flexible nylon 11 piezoelectric separation fiber membrane with adjustable structure was prepared, which solved the problem of difficult to form a high-dimensional structure of nylon 11 material, and improved its piezoelectric output performance. In energy storage equipment and self-rechargeable batteries.
Patent Information
- Application Number
- CN202411072403.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-06
AI Technical Summary
In the prior art, it is difficult for nylon 11 materials to form a high-dimensional structure, which limits its piezoelectric output performance, and is not used in flexible self-rechargeable batteries.
Through cosolvent-induced crystallization and coaxial electrospinning technology, flexible nylon 11 piezoelectric separation fiber membrane with adjustable structure is prepared, combined with in-situ pore-making phase, regulating the composition and morphology of the fibers, and generating high-voltage electroactive phases, improving the Piezoelectric output performance of fibers.
It realizes the high power output performance of the flexible nylon 11 piezoelectric separation fiber membrane, which is suitable for energy storage equipment and micro-sized intelligent wearable energy systems, and provides potential applications of self-rechargeable batteries.
Smart Images

Figure CN118979339A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of energy-capturing materials and energy storage battery devices, and specifically relates to a structurally adjustable flexible nylon 11 piezoelectric separation fiber membrane and a preparation method and application thereof, which are mainly used in the fields of energy-capturing devices, energy storage batteries, emergency energy supply, and micro-intelligent wearable energy systems. Background Art
[0002] As the most studied member of the odd-numbered nylon family, nylon 11 is a promising functional material for future electronic devices or energy storage systems. However, nylon 11 prepared by conventional methods such as coating, casting, and unidirectional / bidirectional stretching is mostly a two-dimensional structure such as a planar film or block, which cannot exert its effective piezoelectric output performance. Therefore, it is crucial to optimize the structure or design higher-dimensional structural materials.
[0003] Electrospinning technology can be used to prepare one-, two- and three-dimensional structure devices, with the advantages of simple operation, controllable conditions and low cost. In addition, the fiber structure, such as porous and hollow structures, can be adjusted by precisely controlling the spinning conditions and post-electrospinning treatment to optimize the fiber performance and achieve customized applications. However, the most stable non-piezoelectric / ferroelectric α phase will inevitably be formed in the process of spinning nylon 11 fibers by electrospinning.
[0004] The development of flexible power sources is a promising strategy to solve the problem of wearable electronic devices working without a power source or charging base. Flexible self-rechargeable batteries are energy storage devices that simultaneously collect and store energy through force-to-electric conversion with piezoelectric effect. Among them, the piezoelectric diaphragm has a dual function. On the one hand, it acts as a battery diaphragm to prevent battery short circuit. On the other hand, it can act as a piezoelectric electrolyte to provide piezoelectric potential in the internal circuit to drive ion migration and achieve the effect of self-charging. At present, there is no research report on the use of nylon 11 in flexible self-rechargeable batteries. Summary of the invention
[0005] In view of the above-mentioned deficiencies in the prior art, the present invention provides a structurally adjustable flexible nylon 11 piezoelectric separation fiber membrane and a preparation method and application thereof. The present invention has the advantages of simple technology, flexibility and lightness, variable and controllable structure, controllable piezoelectric active crystal phase, high electromechanical output performance and portable self-powered. The prepared flexible self-rechargeable battery has huge potential application prospects in energy storage equipment, emergency energy supply and micro-intelligent wearable energy systems.
[0006] To achieve the above purpose, the technical solution adopted by the present invention to solve the technical problem is:
[0007] A method for preparing a structurally adjustable flexible nylon 11 piezoelectric separation fiber membrane comprises the following steps:
[0008] (1) adding nylon 11 particles and inorganic nanofillers into a co-solvent system for reaction to prepare a homogeneous matrix solution A;
[0009] (2) adding nylon 11 particles and polyethylene glycol into a co-solvent system for reaction to prepare a homogeneous matrix solution B;
[0010] (3) The homogeneous matrix solutions A and B were defoamed and then formed into membranes by coaxial electrospinning to obtain structurally adjustable flexible nylon 11 piezoelectric separation fiber membranes.
[0011] Furthermore, the nylon 11 particles are commercially available products, such as RTP nylon 11, French Arkema nylon 11 BESMOTL, etc.
[0012] Furthermore, in step (1), the mass ratio of nylon 11 particles to the co-solvent system is 1:1-5; the mass ratio of nylon 11 particles to the inorganic nanofiller is 1-2:0-0.5.
[0013] Furthermore, in step (2), the mass ratio of nylon 11 particles, polyethylene glycol and co-solvent system is 0-2.5:5-20:5-15.
[0014] Furthermore, the co-solvent system includes an organic protonic acid solvent and a benign solvent in a volume ratio of 1:1 to 10.
[0015] Further, the organic protonic acid solvent is at least one of formic acid, acetic acid, propionic acid, oxalic acid, benzoic acid, malonic acid, trichloroacetic acid and trifluoroacetic acid;
[0016] The benign solvent is at least one of hexafluoroisopropanol, acetone and dichloromethane.
[0017] Furthermore, the inorganic nanofiller is at least one of nano-barium titanate, nano-zinc oxide, lead zirconate titanate, carbon nanotubes and graphene nanosheets.
[0018] Furthermore, the reaction temperature in step (1) and step (2) is 25 to 70° C., and the stirring speed is 200 to 600 rpm.
[0019] Furthermore, the polyethylene glycol is at least one of PEG300, PEG600 and PEG4000.
[0020] Furthermore, the coaxial electrospinning process in step (3) is:
[0021] The solution in A is a homogenous matrix solution B, and the rate is 1.0-2.5 mL / h;
[0022] The solution in the bolus B is the homogeneous matrix solution A, and the rate is 2.0-7.5 mL / h;
[0023] The distance between the needle and the roller is 5-15 cm;
[0024] The receiver drum has a rotation speed of 30-500rpm;
[0025] The positive voltage is 12-18V and the negative voltage is -1.0~-1.5V.
[0026] Furthermore, the defoaming time is 1 to 5 minutes.
[0027] Furthermore, after electrospinning, vacuum annealing, pure water immersion ultrasonic replacement and drying treatment are also included, wherein the vacuum annealing temperature is 40-120°C, the annealing time is 2-6h, the pure water immersion ultrasonic replacement time is 0.5-2.5h, the drying treatment method is vacuum drying or freeze drying, the vacuum drying temperature is 40-80°C, and the drying time is 8-24h.
[0028] A flexible nylon 11 piezoelectric separation fiber membrane with adjustable structure is prepared by adopting the method.
[0029] The above-mentioned flexible nylon 11 piezoelectric separation fiber membrane is used in the preparation of flexible energy capture devices and energy storage devices.
[0030] A lithium-ion battery uses the above-mentioned flexible nylon 11 piezoelectric separation fiber membrane as a separator between a positive electrode material and a negative electrode material.
[0031] Furthermore, the lithium-ion battery is a self-charging lithium-ion battery.
[0032] Furthermore, the assembly method of the self-charging lithium-ion battery is as follows: align the positive electrode tab, positive electrode sheet, separator, negative electrode sheet, and negative electrode tab in order and wrap them in an aluminum-plastic film, heat seal three sides, and leave one side to inject electrolyte; then, place the preliminarily assembled soft-pack lithium-ion battery in a vacuum oven to dry for a certain period of time, then transfer it to a glove box filled with argon atmosphere, inject a quantitative electrolyte, and use a vacuum heat sealer to completely seal it, and finally obtain a self-charging flexible lithium-ion battery.
[0033] Furthermore, the positive electrode tab is an aluminum tab, the positive electrode material is lithium iron phosphate (LiFePO4), the diaphragm is a flexible hollow nylon 11 piezoelectric fiber membrane, the negative electrode tab is a nickel tab, the negative electrode material is graphite, the vacuum drying temperature is 60°C, the vacuum drying time is 12h, and the injected electrolyte is lithium hexafluorophosphate electrolyte (1M LiPF6in EC:DMC=1:1vol%).
[0034] Beneficial effects of the present invention:
[0035] 1. The present invention effectively regulates the composition, macroscopic morphology and piezoelectric output performance of the piezoelectric fiber membrane by combining co-solvent induced crystallization, coaxial electrospinning and in-situ pore formation. The piezoelectric fiber membrane prepared by the present invention can effectively regulate the size of the fiber by adjusting the concentration of the spinning solution, and increase the piezoelectric active phase component by inducing the formation of the polar crystal phase (δ' phase) in nylon 11 by the co-solvent. The piezoelectric output capacity is regulated by adjusting the wheelbase between the needle and the roller and the rotation speed of the roller, and the tightness of the overlap between the fibers is improved, thereby greatly improving the electromechanical output performance of the piezoelectric fiber membrane.
[0036] 2. The present invention can effectively adjust the structural morphology of the obtained flexible nylon 11 piezoelectric separation fiber membrane by the concentration of the AB axis solvent, the distance from the needle to the roller, the rotation speed of the roller and the magnitude of the electric field voltage. For example, it can be a solid structure, a porous structure, a hollow structure, a network interwoven structure, a dendritic structure and a coated structure, thereby adjusting its piezoelectric output performance.
[0037] 3. The spinning solution in the present invention is a co-solvent system that can induce the formation of high-voltage electroactive phase nylon 11, and the electrospinning and co-solvent system synergistically enhance the induction and control of the formation of a suitable metastable crystalline phase (high-voltage electroactive crystalline phase), such as the piezoelectric γ phase or the ferroelectric δ′ phase, thereby improving the piezoelectric output capacity of the nylon 11 fiber, so that the obtained nylon 11 fiber has a synergistic effect of high-voltage electrical output and strong flexibility.
[0038] 4. The piezoelectric fiber membrane prepared by the present invention can be used as a separation membrane of the battery, and has the advantages of not being swollen by the electrolyte, being flexible and having high strength. It can be used to prepare flexible self-rechargeable batteries, such as self-rechargeable lithium-ion batteries, which makes it have huge potential application prospects in energy storage devices, emergency energy supply and micro-intelligent wearable energy systems. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 A physical picture of a piezoelectric test of a flexible hollow piezoelectric fiber membrane prepared in an embodiment of the present invention;
[0040] Figure 2 This is a SEM morphology characterization image of the porous nylon 11 piezoelectric fiber membrane prepared in Example 1 of the present invention;
[0041] Figure 3 The piezoelectric voltage and current output performance diagram of the porous nylon 11 piezoelectric fiber membrane prepared in Example 1 of the present invention;
[0042] Figure 4 The battery charge and discharge performance diagram of the porous nylon 11 piezoelectric fiber membrane prepared in Example 1 of the present invention used as a separation membrane for a lithium-ion battery;
[0043] Figure 5This is a battery self-charging performance diagram of the porous nylon 11 piezoelectric fiber membrane prepared in Example 1 of the present invention used as a lithium-ion battery separation membrane;
[0044] Figure 6 The surface and cross-sectional SEM morphology images of the flexible hollow nylon 11 piezoelectric fiber membrane prepared in Example 2 of the present invention;
[0045] Figure 7 This is a graph showing the piezoelectric voltage and current output performance of the flexible hollow nylon 11 piezoelectric fiber membrane prepared in Example 2 of the present invention;
[0046] Figure 8 A real picture of a lithium-ion battery assembled by using the flexible hollow nylon 11 piezoelectric fiber membrane as a lithium-ion battery separation membrane in Example 2 of the present invention;
[0047] Fig. 9 This is a battery charge and discharge performance diagram of a commercial polyolefin PP diaphragm used as a lithium ion battery separation diaphragm in a comparative example of the present invention;
[0048] Fig.10 This is a battery charge and discharge performance diagram of the flexible hollow nylon 11 piezoelectric fiber membrane used as a lithium ion battery separation membrane in Example 2 of the present invention;
[0049] Fig.11 This is a self-charging performance diagram of the lithium-ion battery based on the flexible hollow nylon 11 piezoelectric fiber membrane in Example 2 of the present invention.
[0050] Fig.12 Surface and cross-sectional SEM images of the flexible hollow nylon 11 / BTO composite piezoelectric fiber membrane prepared in Example 3 of the present invention;
[0051] Fig.13 This is a performance diagram of piezoelectric voltage and current output of the flexible hollow nylon 11 / BTO composite piezoelectric fiber membrane prepared in Example 3 of the present invention;
[0052] Fig.14 This is a battery charge and discharge performance diagram of the flexible hollow nylon 11 / BTO composite piezoelectric fiber membrane prepared in Example 3 of the present invention as a lithium-ion battery separation membrane;
[0053] Fig.15 This is a battery self-charging performance diagram of the flexible hollow nylon 11 / BTO composite piezoelectric fiber membrane prepared in Example 3 of the present invention as a lithium-ion battery separation membrane;
[0054] Fig.16 Surface and cross-sectional SEM images of the flexible solid nylon 11 piezoelectric fiber membrane prepared in Example 4 of the present invention;
[0055] Fig.17This is a surface SEM image of the flexible network interwoven nylon 11 piezoelectric fiber membrane prepared in Example 5 of the present invention;
[0056] Fig.18 This is a surface SEM image of the flexible dendritic nylon 11 piezoelectric fiber film prepared in Example 6 of the present invention;
[0057] Fig.19 This is a cross-sectional SEM image of the flexible core-shell nylon 11 piezoelectric fiber membrane prepared in Example 7 of the present invention. DETAILED DESCRIPTION
[0058] The specific implementation modes of the present invention are described below so that those skilled in the art can understand the present invention. However, it should be clear that the present invention is not limited to the scope of the specific implementation modes. For those of ordinary skill in the art, as long as various changes are within the spirit and scope of the present invention as defined and determined by the attached claims, these changes are obvious, and all inventions and creations utilizing the concept of the present invention are protected.
[0059] Example 1
[0060] A method for preparing a flexible porous nylon 11 piezoelectric fiber membrane with high voltage electrical output comprises the following steps:
[0061] (1) 2 g of nylon 11 particles were added to 10 mL of a trifluoroacetic acid solvent and a hexafluoroisopropanol solvent in a volume ratio of 1:9, and the mixture was reacted and dissolved at 60° C. and a stirring speed of 400 rpm for 6 h to obtain a 20 wt % homogeneous nylon 11 solution A;
[0062] (2) adding 1 g of nylon 11 particles to 5 mL of PEG600 solution and 5 mL of trifluoroacetic acid solvent and hexafluoroisopropanol solvent in a volume ratio of 1:9, reacting at 60° C. and stirring at 400 rpm for 6 h to obtain a 10 wt % homogeneous PEG600 / nylon 11 solution B;
[0063] (3) defoaming the homogenized solutions A and B in steps (1) and (2) in a high-speed mixer for 2 min;
[0064] (4) 6 mL of the above-mentioned 20 wt% nylon 11 solution A and 3 mL of the above-mentioned 10 wt% PEG600 / nylon 11 solution B were spun into membranes according to the following spinning procedure: using a coaxial needle model of 18G / 21G, the solution in push injection A was 10 wt% PEG600 / nylon 11 solution B, and the solution in push injection B was 20 wt% nylon 11 solution A, the push injection rate of A was 1.0 mL / h, the push injection rate of B was 2.0 mL / h, the wheelbase from the needle to the roller was 10 cm, the rotation speed of the receiver roller was 100 rpm, the positive voltage was 14.0 kV, and the negative voltage was -1.1 kV.
[0065] (5) The coaxially spun membrane was subjected to vacuum annealing, pure water immersion ultrasonic replacement and drying treatment in sequence, with the vacuum annealing temperature being 60° C., the pure water immersion ultrasonic replacement being 30 min and the freeze drying being 24 h, to obtain a flexible porous nylon 11 piezoelectric fiber membrane.
[0066] Example 2
[0067] A method for preparing a self-charging lithium-ion battery based on a flexible hollow nylon 11 piezoelectric separation membrane comprises the following steps:
[0068] (1) 2 g of nylon 11 particles were added to 10 mL of a trifluoroacetic acid solvent and a hexafluoroisopropanol solvent in a volume ratio of 1:9, and the mixture was reacted and dissolved at 60° C. and a stirring speed of 400 rpm for 6 h to obtain a 20 wt % homogeneous nylon 11 solution A;
[0069] (2) adding 5 mL of the PEG4000 solution to 5 mL of a trifluoroacetic acid solvent and a hexafluoroisopropanol solvent in a volume ratio of 1:9, and reacting at 60° C. and a stirring speed of 400 rpm for 2 h to obtain a 50 wt % homogeneous PEG4000 solution B;
[0070] (3) defoaming the homogenized solutions A and B in steps (1) and (2) in a high-speed mixer for 2 min;
[0071] (4) 6 mL of the above-mentioned 20 wt% nylon 11 solution A and 3 mL of the above-mentioned 50 wt% PEG4000 solution B were spun into membranes according to the following spinning procedure: using a coaxial needle model of 18G / 21G, the solution in push injection A was 50 wt% PEG4000 solution B, and the solution in push injection B was 20 wt% nylon 11 solution A, the push injection rate of A was 1.0 mL / h, the push injection rate of B was 2.0 mL / h, the wheelbase from the needle to the roller was 8 cm, the rotation speed of the receiver roller was 200 rpm, the positive voltage was 14.5 kV, and the negative voltage was -1.2 kV.
[0072] (5) The coaxially spun membrane is subjected to vacuum annealing, pure water immersion ultrasonic replacement and drying treatment in sequence, wherein the vacuum annealing temperature is 60° C., the pure water immersion ultrasonic replacement is 1 h and the freeze drying is 24 h to obtain a flexible hollow nylon 11 piezoelectric fiber membrane;
[0073] (6) The flexible hollow nylon 11 piezoelectric fiber membrane obtained above was used as a lithium-ion battery separator, sandwiched between the positive and negative electrode materials and connected with the positive and negative electrode ears and packaged in an aluminum-plastic film. The flexible lithium-ion battery was prepared according to the steps of packaging, drying, liquid injection, and formation, and was left to stand for 24 hours to test the battery performance.
[0074] Cut the flexible hollow nylon 11 piezoelectric fiber membrane into pieces with a size of 2.5×2.5 cm2 The square samples were packaged with commercial copper tape and polyimide film to prepare Figure 1 The piezoelectric device shown is used for piezoelectric performance testing.
[0075] Example 3
[0076] A method for preparing a flexible hollow nylon 11 / barium titanate composite piezoelectric separation membrane comprises the following steps:
[0077] (1) 2 g of nylon 11 particles and 0.4 g of barium titanate powder (BTO) were added to 10 mL of a trifluoroacetic acid solvent and a hexafluoroisopropanol solvent in a volume ratio of 1:9, and the mixture was reacted and dissolved at 60° C. and a stirring speed of 400 rpm for 6 h to obtain a 20 wt% nylon 11 / BTO blend solution A;
[0078] (2) adding 5 mL of the PEG4000 solution to 5 mL of a trifluoroacetic acid solvent and a hexafluoroisopropanol solvent in a volume ratio of 1:9, and reacting at 60° C. and a stirring speed of 400 rpm for 2 h to obtain a 50 wt % homogeneous PEG4000 solution B;
[0079] (3) defoaming the homogenized solutions A and B in steps (1) and (2) in a high-speed mixer for 2 min;
[0080] (4) 6 mL of the above-mentioned 20 wt% nylon 11 / BTO blend solution A and 3 mL of the above-mentioned 50 wt% PEG4000 solution B were spun into film according to the following spinning procedure: using a coaxial needle model of 18G / 21G, the solution in A was 50 wt% PEG4000 solution B, and the solution in B was 20 wt% nylon 11 solution A. The injection rate of A was 1.0 mL / h, and the injection rate of B was 2.0 mL / h. The wheelbase from the needle to the roller was 8 cm, the rotation speed of the receiver roller was 200 rpm, the positive voltage was 16 kV, and the negative voltage was -1.1 kV.
[0081] (5) The coaxially spun membrane was subjected to vacuum annealing, pure water immersion ultrasonic replacement and drying treatment in sequence, with the vacuum annealing temperature being 60°C, the pure water immersion ultrasonic replacement being 1 hour and the freeze drying being 24 hours, to obtain a flexible hollow nylon 11 / BTO composite piezoelectric fiber membrane.
[0082] Example 4
[0083] A method for preparing a flexible solid nylon 11 piezoelectric separation membrane comprises the following steps:
[0084] (1) 2 g of nylon 11 particles were added to 10 mL of a trifluoroacetic acid solvent and a hexafluoroisopropanol solvent in a volume ratio of 1:9, and the mixture was reacted and dissolved at 60° C. and a stirring speed of 400 rpm for 6 h to obtain a 20 wt% homogeneous nylon 11 solution;
[0085] (2) defoaming the homogenized solution in step (1) in a high-speed mixer for 2 min;
[0086] (3) 6 mL of the above-mentioned 20 wt% nylon 11 homogeneous solution was spun into a film according to the following spinning procedure: using a needle model of 21G, the solution in push A is a 20 wt% homogeneous nylon 11 solution, the push A rate is 1.0 mL / h, the wheelbase from the needle to the roller is 15 cm, the speed of the receiver roller is 200 rpm, the positive voltage is 8 kV, and the negative voltage is -1.1 kV.
[0087] (5) The above-mentioned spun membrane is subjected to vacuum annealing and drying treatment in sequence, with the vacuum annealing temperature being 60° C. and drying for 24 hours to obtain a flexible solid nylon 11 piezoelectric fiber membrane.
[0088] Example 5
[0089] A method for preparing a flexible network interwoven nylon 11 piezoelectric separation membrane comprises the following steps:
[0090] (1) 2 g of nylon 11 particles were added to 10 mL of a trifluoroacetic acid solvent and a hexafluoroisopropanol solvent in a volume ratio of 1:9, and the mixture was reacted and dissolved at 60° C. and a stirring speed of 400 rpm for 6 h to obtain a 20 wt% homogeneous nylon 11 solution;
[0091] (2) defoaming the homogenized solution in step (1) in a high-speed mixer for 2 min;
[0092] (3) 6 mL of the above-mentioned 20 wt% nylon 11 homogeneous solution was spun into a film according to the following spinning procedure: the spinning procedure was as follows: the needle model was 21G, the solution in the push A was a 20 wt% homogeneous nylon 11 solution, the push A rate was 2.0 mL / h, the wheelbase from the needle to the roller was 10 cm, the speed of the receiver roller was 30 rpm, the positive voltage was 8 kV, and the negative voltage was -1.1 kV.
[0093] (5) The above-mentioned spun membrane is subjected to vacuum annealing and drying treatment in sequence, the vacuum annealing temperature is 60° C. and the drying time is 24 hours to obtain a flexible network interwoven nylon 11 piezoelectric fiber membrane.
[0094] Example 6
[0095] A method for preparing a flexible dendritic nylon 11 piezoelectric separation membrane comprises the following steps:
[0096] (1) 1 g of nylon 11 particles was added to 10 mL of a trifluoroacetic acid solvent and a hexafluoroisopropanol solvent in a volume ratio of 1:9, and the mixture was reacted and dissolved at 60° C. and a stirring speed of 400 rpm for 6 h to obtain a 10 wt% homogeneous nylon 11 solution;
[0097] (2) defoaming the homogenized solution in step (1) in a high-speed mixer for 2 min;
[0098] (3) 6 mL of the above-mentioned 10 wt% nylon 11 homogeneous solution was spun into a film according to the following spinning procedure: the spinning procedure was as follows: a needle model of 21G was used, the solution in push injection A was a 10 wt% homogeneous nylon 11 solution, the push injection rate of A was 0.5 mL / h, the wheelbase from the needle to the roller was 8 cm, the speed of the receiver roller was 30 rpm, the positive voltage was 8.5 kV, and the negative voltage was -1.1 kV.
[0099] (5) The above-mentioned spun membrane is subjected to vacuum annealing and drying treatment in sequence, with the vacuum annealing temperature being 60° C. and drying for 24 hours to obtain a flexible dendritic nylon 11 piezoelectric fiber membrane.
[0100] Example 7
[0101] A method for preparing a flexible coated core-shell structure nylon 11 piezoelectric fiber membrane comprises the following steps:
[0102] (1) 2 g of nylon 11 particles were added to 10 mL of a trifluoroacetic acid solvent and a hexafluoroisopropanol solvent in a volume ratio of 1:9, and the mixture was reacted and dissolved at 60° C. and a stirring speed of 400 rpm for 6 h to obtain a 20 wt % homogeneous nylon 11 solution A;
[0103] (2) 1 g of nylon 11 particles was added to 10 mL of a trifluoroacetic acid solvent and a hexafluoroisopropanol solvent in a volume ratio of 1:9, and the mixture was reacted at 60° C. and a stirring speed of 400 rpm for 6 h to obtain a 10 wt % homogeneous nylon 11 solution B;
[0104] (3) defoaming the homogenized solutions A and B in steps (1) and (2) in a high-speed mixer for 2 min;
[0105] (4) 6 mL of the above-mentioned 20 wt% nylon 11 solution A and 3 mL of the above-mentioned 10 wt% nylon 11 solution B were spun into film according to the following spinning procedure: using a coaxial needle model of 18G / 21G, the solution in push injection A was 10 wt% nylon 11 solution B, and the solution in push injection B was 20 wt% nylon 11 solution A, the push injection rate of A was 1.0 mL / h, the push injection rate of B was 2.0 mL / h, the wheelbase from the needle to the roller was 12 cm, the rotation speed of the receiver roller was 100 rpm, the positive voltage was 14.0 kV, and the negative voltage was -1.1 kV.
[0106] (5) The coaxially spun membrane was subjected to vacuum annealing and drying treatments in sequence, with the vacuum annealing temperature being 60° C. and drying for 24 h to obtain a flexible core-shell nylon 11 piezoelectric fiber membrane.
[0107] Comparative Example
[0108] This comparative example provides a method for preparing a lithium-ion battery based on a commercial polyolefin PP separation membrane, comprising the following steps:
[0109] (1) The assembly method of the lithium-ion battery is to align the positive electrode tab, the positive electrode sheet, the commercial polyolefin PP separator, the negative electrode sheet, and the negative electrode tab in order and wrap them in an aluminum-plastic film, heat-seal three sides, and leave one side for injecting electrolyte;
[0110] (2) Drying the preliminarily assembled soft-pack lithium-ion battery in a vacuum oven at 60°C for 12 hours;
[0111] (3) Then the mixture was transferred into a glove box filled with argon atmosphere, 1 mL of lithium hexafluorophosphate electrolyte (1 M LiPF6in EC:DMC=1:1 vol%) was injected, and a vacuum heat sealer was used to completely seal the mixture, thereby finally producing a commercial flexible lithium-ion battery.
[0112] Experimental testing
[0113] 1. Performance test of flexible nylon 11 piezoelectric fiber membrane
[0114] The composition, macro / micro morphology and piezoelectric output performance of the piezoelectric fiber membrane are effectively regulated by combining co-solvent induced crystallization, coaxial electrospinning and in-situ pore formation. The flexible piezoelectric fiber membrane in the embodiment is prepared and assembled as follows: Figure 1 The piezoelectric nanogenerator shown in the figure. The piezoelectric fibers prepared in Examples 1 and 2 were subjected to morphological observation and piezoelectric performance testing. Figure 2 , Figure 3 , Figure 6 and Figure 7 shown.
[0115] Depend on Figure 2 and Figure 6 It can be seen that the nylon 11 piezoelectric fiber prepared by the present invention is porous and hollow, with a filament diameter of about 2.0-2.5 μm, and the porous fiber has uniform gaps and regular morphology, which is conducive to stress concentration to produce a larger piezoelectric output. Further, the piezoelectric output voltage and current are tested.
[0116] like Figure 3 and Figure 7 The test results show that the piezoelectric output voltage and current of the flexible porous nylon 11 piezoelectric fiber membrane prepared by the present invention are 12.5V and 470nA respectively, while the piezoelectric output voltage and current of the flexible hollow nylon 11 piezoelectric fiber membrane are 18.5V and 1.2μA respectively. The piezoelectric performance is greatly improved, indicating that structural optimization can improve the piezoelectric output performance of the material.
[0117] The porous nylon 11 fiber membrane is further used as a separator for lithium-ion batteries to assemble soft-pack batteries. The charge and discharge performance of the soft-pack batteries is shown in the figure below. Figure 4 As shown, it is shown that the piezoelectric diaphragm of the present invention can be used as a substitute for commercial polyolefin PP diaphragm.
[0118] Finally, the self-charging performance of the soft-pack battery was tested. Figure 5 As shown, by continuous tapping (at a frequency of 1.7 Hz, using a force of 9 N for continuous tapping for 90 seconds), the battery can be charged from 0.8 V to 1.029 V, successfully charging 229 mV, and discharging to 0.8 V at a constant current of 0.05 mA for 20 seconds, with a charging capacity of 0.28 μAh. The above results fully demonstrate that the piezoelectric diaphragm in the present invention has good self-charging performance as a separation diaphragm for lithium-ion batteries.
[0119] 2. Battery performance of flexible hollow nylon 11 piezoelectric fiber membrane assembly
[0120] The hollow nylon 11 fiber membrane is used as the separator of the lithium-ion battery to assemble the soft pack battery. The actual picture is as follows Figure 8 As shown. Taking the commercial polyolefin PP diaphragm as the diaphragm of lithium-ion battery as a comparison, the charge and discharge performance of soft-pack battery with flexible hollow nylon 11 piezoelectric fiber membrane as the separation diaphragm of lithium-ion battery is shown in the figure below. Fig. 9 and Fig.10 shown.
[0121] Depend on Fig. 9 and Fig.10 It can be seen that the charge and discharge performance of the flexible hollow nylon 11 piezoelectric fiber membrane as a lithium-ion battery separation membrane is similar to that of the commercial polyolefin PP membrane, and the piezoelectric membrane in the present invention has a lower leakage voltage (0.7V) than the commercial polyolefin PP membrane (1.0V), indicating that the piezoelectric membrane in the present invention can be used as a substitute for the commercial polyolefin PP membrane.
[0122] Finally, the self-charging performance of the soft-pack battery under this structure was tested. Fig.11 It can be seen that at a frequency of 1.7 Hz, using a force of 9 N for continuous tapping for 600 seconds, the battery can be charged from 0.8 V to 1.015 V, successfully charging 215 mV, and discharging to 0.8 V at a constant current of 0.05 mA for 35.5 seconds, with a charging capacity of 0.4931 μAh. The above results fully demonstrate that the piezoelectric diaphragm in the present invention has good self-charging performance as a separation diaphragm for lithium-ion batteries.
[0123] 3. Morphology of flexible hollow nylon 11 / BTO composite piezoelectric fiber membrane and performance of assembled battery
[0124] The piezoelectric fiber prepared in Example 3 was subjected to morphological observation and piezoelectric performance test. Fig.12 and Fig.13 As shown. Fig.12 It can be seen from the figure that the nylon 11 / BTO composite piezoelectric fiber membrane is in a hollow tubular shape and is loaded with BTO nanoparticles, indicating that the hollow nylon 11 / BTO composite piezoelectric fiber membrane can be prepared by the method of the present invention. Fig.13 It can be seen that the piezoelectric output voltage of the hollow nylon 11 / BTO composite piezoelectric fiber membrane is 33 V and 1.25 μA, which is significantly improved, indicating that structural optimization and composite piezoelectric fillers can improve the piezoelectric output performance of the material.
[0125] The hollow nylon 11 / BTO composite piezoelectric fiber membrane was further used as a separator for lithium-ion batteries to assemble soft-pack batteries. The charge and discharge performance of the soft-pack battery is shown in the figure below. Fig.14 As shown. Fig.14 It can be seen that the charge and discharge performance of the flexible hollow nylon 11 piezoelectric fiber membrane as a lithium-ion battery separation membrane is similar to that of the commercial polyolefin PP membrane, and the piezoelectric membrane in the present invention has a lower leakage voltage (0.7V) than the commercial polyolefin PP membrane (1.0V), indicating that the piezoelectric membrane in the present invention can be used as a substitute for the commercial polyolefin PP membrane.
[0126] Finally, the self-charging performance of the soft-pack battery under this structure was tested. At a frequency of 1.7Hz, the battery can be charged from 0.8V to 1.02V with a force of 9N for 600s, successfully charging 220mV, and discharging to 0.8V with a constant current of 5μA for 3216s, with a charging capacity of 4.47μAh ( Fig.15 ), the above results fully demonstrate that the piezoelectric diaphragm of the present invention has very excellent self-charging performance as a separation diaphragm of lithium-ion batteries.
[0127] Finally, it should be noted that the above specific implementation methods are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to examples, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.
Claims
1. A method for preparing a structurally adjustable flexible nylon 11 piezoelectric separation fiber membrane, characterized in that: The following steps are involved: (1) adding nylon 11 particles and inorganic nanofillers into a co-solvent system for reaction to obtain a homogeneous matrix solution A; wherein the amount of the inorganic nanofiller may be 0; (2) adding nylon 11 particles and polyethylene glycol into a co-solvent system for reaction to obtain a homogeneous matrix solution B; wherein the amount of nylon 11 particles used may be 0; (3) The homogeneous matrix solutions A and B were defoamed and then formed into membranes by coaxial electrospinning to obtain structurally adjustable flexible nylon 11 piezoelectric separation fiber membranes.
2. The preparation method according to claim 1, characterized in that: In step (1), the mass ratio of nylon 11 particles to the co-solvent system is 1:1-5; the mass ratio of nylon 11 particles to the inorganic nanofiller is 1-2:0-0.
5.
3. The preparation method according to claim 1, characterized in that: In step (2), the mass ratio of nylon 11 particles, polyethylene glycol and co-solvent system is 0-2.5:5-20:5-15.
4. The preparation method according to claims 1 to 3, characterized in that: The co-solvent system includes an organic protonic acid solvent and a benign solvent in a volume ratio of 1:1 to 10; The organic protonic acid solvent is at least one of formic acid, acetic acid, propionic acid, oxalic acid, benzoic acid, malonic acid, trichloroacetic acid and trifluoroacetic acid; The benign solvent is at least one of hexafluoroisopropanol, acetone and dichloromethane.
5. The preparation method according to claim 1 or 2, characterized in that: The inorganic nano filler is at least one of nano barium titanate, nano zinc oxide, lead zirconate titanate, carbon nanotubes and graphene nano sheets.
6. The preparation method according to claim 1, characterized in that: The reaction temperature in step (1) and step (2) is 25-70° C., and the stirring speed is 200-600 rpm.
7. The preparation method according to claim 1, characterized in that: The coaxial electrospinning process in step (3) is: The solution in A is a homogenous matrix solution B, and the rate is 1.0-2.5 mL / h; The solution in the bolus B is the homogeneous matrix solution A, and the rate is 2.0-7.5 mL / h; The distance between the needle and the roller is 5-15 cm; The receiver drum has a rotation speed of 30-500rpm; The positive voltage is 12-18V and the negative voltage is -1.0~-1.5V.
8. A structurally adjustable flexible nylon 11 piezoelectric separation fiber membrane, characterized in that: The method is prepared by any one of claims 1 to 8.
9. Use of the flexible nylon 11 piezoelectric separation fiber membrane according to claim 8 in the preparation of flexible energy harvesting devices and energy storage devices.
10. A lithium ion battery, characterized in that: The lithium-ion battery uses the flexible nylon 11 piezoelectric separation fiber membrane described in claim 8 as a separator between the positive electrode material and the negative electrode material.
Citation Information
Patent Citations
Fabrication of nanofibers as dry adhesives and applications of the same
CA2880289A1
Antimicrobial polymer compounds and fibres thereof
CN102791751A
Core-shell fiber film material capable of spontaneously generating static electricity as well as preparation method and application of core-shell fiber film material
CN117166137A
Preparation method of barium titanate ceramic film and film
CN117466640A
Analyte sensors and methods of manufacturing analyte sensors
IN201947035022A