Cotton fabric high-color-depth digital printing method
Through the dual effects of exoglucanase and NMMO, the problem of difficult to take into account the medium and high color depth and pattern clarity of cotton fabric digital printing is achieved, and the printing effect of high color depth, high pattern clarity and soft feel is achieved, which significantly improves the printing effect of high color depth, high pattern clarity and soft feel. It has color fastness and water saving and environmental protection.
Patent Information
- Application Number
- CN202311689547.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-11
- Publication Date
- 2024-11-19
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing cotton fabric digital printing technology is difficult to take into account high color depth, high pattern clarity and soft feel. In traditional methods, reactive dyes have low color fixation rate, hard fabrics, poor feel, and increasing color depth will affect the printing clarity and Number of washes.
Using the dual effects of exoglucanase and NMMO, in the dissolving state of the fibers on the surface of cotton fabric, the reactive dyes are quickly adsorbed to the fibers. By combining pretreatment and inkjet printing, the amount of pretreatment paste and the number of washings are reduced, and the number of water is washed is improved. Color depth and color fastness, and cellulose solubility and dye adsorption effect are ensured by controlling NMMO concentration.
The printing effect with high color depth, high pattern clarity and soft feel is achieved, which significantly improves the printing color fastness and reduces the number of washes, saves water and environmentally friendly, and avoids the rough feel and color migration problems in traditional processes.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of digital printing, and in particular to a high color depth digital printing method for cotton fabric. Background Art
[0002] At present, digital printing of cotton fabrics mainly uses reactive dye printing inks. Most reactive dye digital printing uses monochlorotriazine type reactive dyes. Monochlorotriazine type reactive dyes have low activity and slow reaction speed, and are suitable for high-temperature printing. However, the fixation rate of most monochlorotriazine type reactive dyes is only 60%-70%. Digital printing is continuous surface printing, and the reaction time between dye and fiber is short, so it is difficult to obtain reactive dye digital printing products with high color depth.
[0003] There are currently three main methods for improving the color depth of reactive printing inks. First, increase the proportion of reactive dyes in the printing ink, but high concentrations of reactive dyes will increase the viscosity of the ink itself, reduce the stability of the ink, make the ink easily penetrate the surface of the fabric, and increase the difficulty of subsequent sewage treatment; second, after the cotton fabric is mercerized with sodium hydroxide solution, the adsorption and reaction properties of the fiber are significantly improved. The higher the mass concentration of sodium hydroxide, the better the color depth of the fabric after printing. The fixation rate of reactive dyes can be increased to 75%-85% through mercerization treatment, but the fabric is stiff and has a poor feel after mercerization treatment; third, the color depth of the print can also be improved by adding urea to the ink. Urea has good hygroscopicity. Increasing the amount of urea will increase the permeability of the ink, the width of the printed pattern line will increase accordingly, and the clarity of the print will be significantly reduced; therefore, there is currently no digital printing of cotton fabrics that takes into account the color depth of the print, the clarity of the pattern, and the feel of the fabric.
[0004] Chinese patent document CN110863373A discloses a reactive digital printing paste composition and a preparation method thereof.
[0005] The shortcoming of this document is that by changing the anionic paste into a combination of cationic paste and non-ionic paste, the positive charge on the fiber surface of the cotton fabric after pretreatment can increase the adsorption of active digital printing ink on the fabric surface. However, the cationic paste that does not react with the fiber will also combine with the anionic active dye, causing the active dye to coagulate, affecting the color depth and clarity of the print.
[0006] The present invention uses the dual effects of exoglucanase and NMMO. When the surface fibers of cotton fabric are dissolved, the active dye is quickly adsorbed into the fibers, the fabric has less floating color and excellent color fastness, and can be directly evaporated after inkjet printing, which can reduce the amount of pre-treated printing paste and the number of washing times after printing, saving water and being environmentally friendly. Exoglucanase can gradually hydrolyze the cellulose chain from one end of the cellulose molecular chain into oligosaccharides such as cellobiose, which is conducive to the migration of dyes into the fiber; NMMO (N-methylmorpholine-N-oxide) is a kind of amine oxide, the NO bond in NMMO is extremely polar, and the oxygen atom forms a hydrogen bond with the cellulose hydroxyl group through the lone pair of electrons, thereby weakening the interaction between cellulose macromolecules. Through the control of certain conditions, NMMO can gradually dissolve amorphous cellulose, and the partially dissolved cellulose can enhance the adsorption of dyes and prevent infiltration during the evaporation process, and can promote the migration of dyes into the fiber, thereby improving the depth and color fastness of the printed color. Summary of the invention
[0007] The purpose of the present invention is to solve the problem of high color depth of digital printing of cotton fabric with reactive dyes, and to provide a high color depth digital printing method for cotton fabric with high color depth, high pattern clarity and soft hand feel.
[0008] To achieve the above object, the present invention preferably adopts the following scheme: S1. Fabric pretreatment: S2. Drying once; S3. Padding exoglucanase solution; S4. Stacking; S5. Secondary drying; S6. Inkjet printing: Add NMMO to the conventional ink formula; S7. Evaporation. S8. Washing; The printing method of the present invention has low dye usage, high color depth, high pattern clarity, and can significantly improve the shortcomings of rough hand feel caused by traditional processes. Through the dual effects of exoglucanase and NMMO, the active dye can be quickly adsorbed into the fiber when the surface fiber of the cotton fabric is dissolved, the fabric has less floating color and excellent color fastness, and can be directly evaporated after inkjet printing, which can reduce the amount of pre-treatment printing paste and the number of washing times after printing, saving water and protecting the environment.
[0009] S1. The pretreatment pulp formula is: Thickener 1.5%-2.5% Urea 1-5% Baking soda 2-4% Sodium sulfate 2-4% Water 80-95% The thickener in the pre-treated slurry can be reduced to 60%-80% of the amount used in traditional digital printing processes, and will not cause ink penetration; S2. Primary drying: 100℃-120℃ continuous drying for 2-5min; S3. Dipping and rolling exoglucanase solution: dipping and rolling exoglucanase solution, Preferably, the exoglucanase concentration in S3 is preferably 0.3-0.6 g / L based on the mass fraction of the active dye in the ink. If the exoglucanase concentration is too low, the fiber surface cannot be effectively hydrolyzed. If the exoglucanase concentration is too high, the fiber will be severely hydrolyzed, affecting the strength of the fabric. S4. Stacking: The cotton fabric impregnated with exoglucanase was stacked for 25min-35min; S5. Secondary drying: Cotton fabric is dried at 85℃-95℃ for 2-3min; S6. Inkjet printing: The ink formula is: Softened water 20%-50% NMMO 38-48% Reactive dyes 1-9% Surfactant 1-10% Other additives 1-5% Preferably, the mass concentration of the NMMO solution in S6 is preferably 38-48% based on the mass fraction of the active dye in the ink, which can make the cotton fiber completely swell and slightly dissolve on the surface. If the NMMO concentration is too low, the cotton fiber can only swell. If the NMMO concentration is too high, the cotton fiber will be greatly dissolved, and the fabric strength will be seriously lost. S7. Steaming: steaming the cotton fabric at 100°C-105°C for 10-15min; By utilizing the dual effects of exoglucanase and NMMO, the active material is not prone to color migration when the fiber surface is slightly dissolved. It can be directly evaporated without drying after inkjet printing, which reduces one drying process compared with the traditional process. S8. Washing: One wash with cold water, one wash with 45℃ water, one wash with cold water In the scheme of the present invention, the active dye completely enters into the fiber, the fiber surface has less floating color, and compared with the traditional process, one high-temperature water washing of 90° C. is reduced.
[0010] The beneficial effects of the present invention are: The invention utilizes the dual effects of exoglucanase and NMMO. The exoglucanase can gradually hydrolyze the cellulose chain into oligosaccharides from one end of the cellulose molecular chain, which is beneficial for the dye to enter the inner layer of the fiber. A certain concentration of NMMO can make the cotton fiber completely swell and slightly dissolve on the surface. The active dye can be quickly adsorbed into the fiber when the surface fiber of the cotton fabric is slightly dissolved. On the one hand, the hydrolysis of the active dye can be reduced and the depth of the printed color can be improved. On the other hand, the active dye completely enters the fiber, the floating color on the fiber surface is less, and the color fastness is excellent.
[0011] When the fiber surface is slightly dissolved, the activity is not easy to cause color migration. On the one hand, the pattern is clear and the slightly dissolved fiber surface feels plump and soft. On the other hand, it can be directly evaporated without drying after inkjet printing, which reduces a drying process and can reduce the amount of pre-treatment printing paste and the number of washing times after printing, saving water and being environmentally friendly. DETAILED DESCRIPTION
[0012] In order to further understand the content and effect of the present invention, the following examples and comparative examples are listed for illustration: In a preferred embodiment, The printing effects of the embodiments and comparative examples of the present invention are verified by the following tests: 1. 40S×40S pure cotton poplin weight 170g / m 2 2. Performance Testing 2.1 Printed fabric feel According to the standard FZ / T01166 "Textile Fabric Tactile Testing and Evaluation Method: Multi-index Integration Method", the Fengbao instrument is used to test the softness of printed fabrics. The higher the value, the softer the fabric, and the lower the value, the stiffer the fabric.
[0013] 2.2 Printing color depth Use X-rite colorimeter to test the K / S value of printed fabrics. The larger the K / S value, the higher the color depth; the smaller the K / S value, the lower the color depth.
[0014] 2.3 Color fastness to rubbing The test is carried out according to the standard GB / T 3920 "Textiles - Tests for colour fastness - Colour fastness to rubbing" and the rating is carried out according to GBT6151 "Textiles - Tests for colour fastness - General rules", with grade 5 being the highest colour fastness and grade 1 being the worst.
[0015] Among various color fastnesses, the color fastness to rubbing of digital printed fabrics is generally poor, so the color fastness to rubbing is preferably tested in the present invention.
[0016] 2.4 Printing clarity Visually check whether the edges of the printed pattern are unclear or have bleeding.
[0017] 2.5 Breaking strength The breaking strength of fabrics was tested according to the standard GB / T 3923.1 “Tensile properties of textile fabrics Part 1_Determination of breaking strength and elongation at break (strip method)”. Example
[0018] Process flow: Fabric pretreatment sizing → primary drying → impregnation with exoglucanase solution → stacking → secondary drying → inkjet printing → steaming → washing → drying S1. The pretreatment pulp formula is: Thickener 2% Urea 3% Baking soda 2% Sodium sulfate 2% Water 91% S2. Primary drying: 110℃ for 3min; S3. Padding 0.4 g / L exoglucanase solution; S4. Stack for 25 minutes; S5. Secondary drying: drying at 90°C for 2 min; S6. Inkjet printing: The ink formula is: Softened water 38wt% NMMO 42wt% CI Reactive Yellow 145 3.1wt% CI Reactive Red 111 1.9wt% Sodium alginate 12wt% Dispersant 1wt% Bactericide 1wt% Defoamer 1wt% S7. Steaming: steaming at 102°C for 10 min; S8. Washing: One wash with cold water, one wash with 45℃ water, one wash with cold water Example
[0019] Compared with Example 1, the difference is that the mass fraction of the active dye in the ink is increased, and the concentration of exoglucanase and the mass fraction of NMMO are increased accordingly.
[0020] S3 was dipped in 0.6 g / L exoglucanase solution, and the inkjet printing ink formula in S6 was: Softened water 29.1wt% NMMO 48wt% CI Reactive Yellow 145 5wt% CI Reactive Red 111 4.9wt% Sodium alginate 10wt% Dispersant 1wt% Bactericide 1wt% Defoamer 1wt% S7. Steaming: steaming at 102°C for 10 min; S8. Washing: One wash with cold water, one wash with 45℃ water, one wash with cold water Comparative Example 1 Traditional process: fabric pretreatment sizing → primary drying → inkjet printing → secondary drying → steaming → washing S1. The pretreatment pulp formula is: Thickener 4% Urea 8% Baking soda 3% Sodium sulfate 3% Water 82% S2. Primary drying: 110℃ for 3min; S3. Inkjet printing: The ink formula is: Softened water 72wt% CI Reactive Yellow 145 3.1wt% CI Reactive Red 111 1.9wt% Sodium alginate 20wt% Dispersant 1wt% Bactericide 1wt% Defoamer 1wt% S7. Steaming: steaming at 102°C for 10 min; S8. Washing: One wash with cold water, one wash with 45℃ water, one wash with 90℃ water, one wash with cold water Comparative Example 2 Compared with Example 1, the difference is that no NMMO is added to the printing ink.
[0021] Comparative Example 3 Compared with Example 1, the difference is that the cloth is not impregnated with the exoglucanase solution after being sizing and dried once.
[0022] Comparative Example 4 Compared with Example 1, the difference is that 30wt% NMMO is added to the printing ink.
[0023] Comparative Example 5 Compared with Example 1, the difference is that 55wt% NMMO is added to the printing ink.
[0024] Comparative Example 6 Compared with Example 1, the difference is that the cloth is sized once and then dried and then dipped in 0.15 g / L exoglucanase solution.
[0025] Comparative Example 7 Compared with Example 1, the difference is that the cloth is sized once and then dried and then impregnated with 0.8 g / L exoglucanase solution.
[0026] The digital printing method of the present invention has very good printing performance, and it performs well in five aspects, namely, feel, color depth, color fastness, print clarity and breaking strength. In Example 1, under the premise of ensuring print clarity and reducing the breaking strength by only 6.38%, the softness is improved from 26.31 of the conventional process comparative example 1 to 30.21, and the dyeing K / S value is improved from 12.33 to 18.45. The color depth is improved by 49.6%, and the color fastness to friction is improved from level 3-4 to level 4-5; in comparative examples 2, 3, 4, 5, 6 and 7, the five aspects of feel, color depth, color fastness, print clarity and breaking strength cannot be taken into account, indicating that to achieve the printing effect of the present invention, it is crucial to impregnate the exoglucanase solution of a suitable concentration and add the NMMO of a suitable concentration to the printing ink, and both are indispensable.
[0027] Although the present invention has been disclosed as above by the embodiments, it is not intended to limit the protection scope of the present invention. For those skilled in the art, changes and modifications made without departing from the concept and scope of the present invention should all fall within the protection scope of the present invention.
Claims
1. A method for high color depth digital printing of cotton fabric, characterized in that: The following steps are involved: S1. Fabric pretreatment; S2. One-time drying; S3. Padding 0.3-0.6 g / L exoglucanase; S4. Stacking for 25min-35min; S5. Secondary drying; S6. Inkjet printing: Add 38%-48% by mass of NMMO to the conventional ink formula; S7. Evaporation; S8. Wash with water.
2. A method for high color depth digital printing of cotton fabric according to claim 1, characterized in that: In S1, the pre-treatment pulp formula is: Thickener 1.5%-2.5% Urea 1-5% Baking soda 2-4% Sodium sulfate 2-4% Water 80-95% The thickener in the pre-treated pulp can be reduced to 60%-80% of the amount used in traditional digital printing processes, and will not cause ink penetration.
3. The method for high color depth digital printing of cotton fabric according to claim 1, characterized in that: In S2, drying is carried out continuously at 100°C-120°C for 2-5 minutes.
4. The method for high color depth digital printing of cotton fabric according to claim 1, characterized in that: In the S3, there is a dipping and a rolling step, wherein 0.3-0.6 g / L exoglucanase is added for dipping and rolling. The exoglucanase can gradually hydrolyze the cellulose chain from one end of the cellulose molecular chain into oligosaccharides, which is beneficial for the dye to enter the inner layer of the fiber.
5. The method for high color depth digital printing of cotton fabric according to claim 1, characterized in that: In S4, the cotton fabric impregnated with the exoglucanase is cold-piled for 25 min-35 min to provide time for the exoglucanase to hydrolyze the surface layer of cellulose.
6. The method for high color depth digital printing of cotton fabric according to claim 1, characterized in that: In S5, the cotton fabric is dried at 85° C.-95° C. for 2-3 minutes.
7. The method for high color depth digital printing of cotton fabric according to claim 1, characterized in that: In S6, the ink formula is: Softened water 20%-50% NMMO 38-48% Reactive dyes 1-9% Surfactant 1-10% Other additives 1-5% The 38-48% concentration of NMMO can make the cotton fiber completely swell and slightly dissolve on the surface. If the NMMO concentration is too low, the cotton fiber can only swell. If the NMMO concentration is too high, the cotton fiber will be greatly dissolved and the fabric strength will be seriously lost.
8. The method for high color depth digital printing of cotton fabric according to claim 1, characterized in that: In S7, the cotton fabric is steamed at 100°C-105°C for 10-15 minutes; since the NMMO in S6 dissolves the surface of the cotton fiber, the reactive dye can easily enter the interior of the fiber. Compared with the traditional digital printing process, direct steaming without drying will not cause dye migration.
9. The method for high color depth digital printing of cotton fabric according to claim 1, characterized in that: In S8, one cold water wash, one 45°C water wash, and one cold water wash are performed. Since the reactive dye completely enters the fiber and no floating color is produced, one water wash can be reduced compared with the traditional digital printing process.