Aramid insulation paper with high initial partial discharge voltage as well as preparation method and application of aramid insulation paper
By designing a macro-micro-nano multi-layer structure in aramid insulated paper, combining nano-anometric fibers and micro-scale filling additives, the problem of insufficient initial local discharge voltage of aramid insulated paper in the prior art is solved, and the material is improved The mechanical and electrical properties of the company are suitable for the motor environment of new energy vehicles, and simplifies the preparation process and reduces production costs.
Patent Information
- Application Number
- CN202411065444.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-05
AI Technical Summary
The existing technology is difficult to effectively increase the starting local discharge voltage of aramid insulating paper, and the structure is complex, the preparation process is cumbersome, and the mechanical strength is insufficient, which affects industrial promotion and actual use.
Using a macro-micro-nano multi-layer structure design, the nanofiber and micro-scale fill additives are dispersed between aramid chopped fibers and precipitated fibers to form a multi-layer structure, which increases the starting local discharge voltage of the material and passes through The combination of nanofibers and fill additives enhances the thermal conductivity and stability of the material.
It significantly improves the starting local discharge voltage of aramid insulating paper, reduces cavity density, and enhances mechanical and electrical performance. It is suitable for new energy vehicle motor environments with high working voltage and high temperature changes. It has a simple preparation method and production cost. Low, suitable for large-scale industrial production.
Smart Images

Figure CN118979412A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of special insulating paper, and in particular to aramid insulating paper with high initial partial discharge voltage, and a preparation method and application thereof. Background Art
[0002] The aramid insulation paper used in new energy vehicle motors has a high working voltage and large temperature changes, which puts forward high requirements on the mechanical and electrical properties of the insulation material. The initial partial discharge of the insulation material is an important reason for the final insulation breakdown of high-voltage electrical equipment, and it is also an important sign of insulation degradation. Mild partial discharge has little effect on the insulation of power equipment, and the insulation strength decreases slowly; while strong partial discharge will cause the insulation strength to decrease rapidly. This is an important factor in the insulation damage of high-voltage power equipment. Therefore, how to increase the initial partial discharge voltage of the insulation material and effectively avoid the insulation breakdown caused by partial discharge is a key and difficult problem in this field. There are few technical solutions for improving the initial partial discharge voltage of the insulation paper in the prior art, and the few technical solutions also have certain technical problems. For example, although Chinese Patent 202210542302.6 discloses a high partial discharge insulation material for oil-cooled motors of new energy vehicles and a preparation method thereof, the insulation paper structure of this solution is complex, the preparation process is cumbersome, and the mechanical strength of the material itself is insufficient, which affects its industrial promotion and practical use. Summary of the invention
[0003] The present invention provides an aramid insulating paper with high initial partial discharge voltage and a preparation method and application thereof, so as to solve the technical problems that the prior art is difficult to effectively improve the initial partial discharge voltage of the insulating paper, the paper structure is complex, the production is difficult, and the mechanical strength does not meet the standards.
[0004] In order to solve the above technical problems, the technical solution proposed by the present invention is: A high initial partial discharge voltage aramid insulation paper, comprising the following components in parts by weight: 50 parts of aramid short fibers, 50 parts of aramid fibrids, 3 parts of aramid nanofibers and 1 part of a filling additive; Among them, the aramid chopped fibers are aramid chopped fibers; the aramid nanofibers are aramid nanofibers; and the filling additives are micron-grade filling additives.
[0005] The design idea of the above technical solution is that the present invention selects aramid fibers with different sizes and filling additives as the main components, so that the nano-sized aramid nanofibers and micron-sized filling additives are dispersed and filled in the pores formed by the millimeter-sized aramid short fibers and aramid fibrids, forming a macro-micron-nano multi-level structure, reducing the cavity density inside the aramid insulation paper finally formed, thereby improving the initial partial discharge voltage of the material, and the filling additives dispersed inside the aramid insulation paper enhance the thermal conductivity of the material, alleviating the problem of the initial partial discharge voltage drop caused by the rise in material temperature. At the same time, in addition to the effect of filling the pores, the nano-scale aramid nanofibers will also adhere to / embedded on the surface of the filling additives to form a micron-nano structure, and through the interaction between themselves and the aramid fibrids, the adhesion ability of the filling additives is enhanced, the retention rate of the filling additives and the stability of the overall system are improved, and the initial partial discharge voltage of the material is improved from another aspect.
[0006] As a further preferred embodiment of the above technical solution, the aramid nanofibers and the filling additives are filled in the pores of the aramid insulation paper, and the aramid nanofibers are adsorbed and / or embedded on the surface of the filling additives.
[0007] As a further preferred embodiment of the above technical solution, the filling additive includes at least one of aluminum nitride, boron nitride and silicon carbide. The above additive has the ability to increase the initial partial discharge voltage of the material and has good compatibility with aramid paper.
[0008] As a further preferred embodiment of the above technical solution, the filler additive is ground to have a specific surface area of . The grinding method of the filler additive is wet grinding or dry grinding.
[0009] As a further preferred embodiment of the above technical solution, the size of the aramid short fibers is 1-15 mm, the size of the aramid nanofibers is 50-300 nm, and the particle size of the filler additive is 1-20 μm. The filler additive and the aramid nanofibers are used in combination as a composite additive. Considering the adsorption effect, the size of the aramid nanofibers and the filler additives can be limited to obtain the best adsorption effect.
[0010] As a further preferred embodiment of the above technical solution, the aramid nanofibers and the filling additives are in the shape of spherical or polygonal particles.
[0011] Based on the same technical concept, the present invention also provides a method for preparing the above-mentioned high initial partial discharge voltage aramid insulation paper, comprising the following steps: (1) pre-treating the aramid fibrid; uniformly mixing the filler additive with 0.5 parts by mass of aramid nanofibers to obtain a mixture; and fully mixing the mixture, the pre-treated aramid fibrid, aramid chopped fibers and the remaining aramid nanofibers to obtain a slurry; (2) placing the slurry on a fourdrinier paper machine for wet forming by a dehydration curve, and then post-processing to obtain aramid insulation paper base paper; (3) The aramid insulation paper base paper is rolled up and subjected to high-temperature rolling to obtain the high initial partial discharge voltage aramid insulation paper.
[0012] As a further preferred embodiment of the above technical solution, the pretreatment in step (1) includes treating the aramid fibrid with a pulper and a deflaker in sequence. After the treatment, the aramid fibrid has a large specific surface area (70-120 m 2 / g), moderate beating degree (60~85°SR), and no excessively long fibers (fiber size is not greater than 1.3mm).
[0013] As a further preferred embodiment of the above technical solution, the slurry in step (2) is conveyed to the screen by a hydraulic headbox flow, and the hydraulic headbox flow conveying to the screen means that the aramid long fibers are firstly passed through a turbulence generator in the hydraulic headbox to form turbulence, and then the slurry is evenly and stably distributed along the full width of the paper machine's banner, the turbulence scale generated by the turbulence generator is micro-turbulence, the turbulence intensity generated is 0.2~5%, and the concentration of the slurry is 0.5±0.1%.
[0014] As a further preferred embodiment of the above technical solution, the dehydration curve in step (2) includes three stages: The first stage: using the slurry's own gravity to dehydrate the slurry to form a wet paper base with a high water content; The second stage: providing a lower vacuum suction force to the dehydration element, partially dehydrating under low vacuum conditions, and forming a structure in which aramid short fibers and aramid fibrils encapsulate aramid nanofibers and filling additives in the wet paper web; The third stage: Increase the vacuum suction force of the dehydration element, dehydrate under high vacuum conditions, and remove most of the moisture in the wet paper.
[0015] As a further preferred embodiment of the above technical solution, in the second stage, the vacuum degree of dehydration is -1 to -10 kPa; in the third stage, the vacuum degree of dehydration is -16 to -25 kPa.
[0016] As a further preferred embodiment of the above technical solution, the post-treatment in step (2) includes pressing and drying operations.
[0017] Based on the same technical concept, the present invention also provides an application of the above-mentioned high initial partial discharge voltage aramid insulation paper, and the high initial partial discharge voltage aramid insulation paper is used in the motor of new energy vehicles.
[0018] Compared with the prior art, the present invention has the following beneficial effects: (1) The aramid insulating paper of the present invention forms a macro-micro-nano multi-level structure, which reduces the cavity density in the aramid paper, increases the retention rate of the filling additive, and improves the mechanical and electrical properties of the aramid paper. At the same time, a heat conduction path is formed through the multi-level structure, which can dissipate the heat accumulated on the surface of the aramid paper more quickly, reduce the local discharge phenomenon, and increase the starting local discharge voltage of the aramid paper, which can meet the use requirements of new energy vehicles and other high working voltage and high temperature change working conditions.
[0019] (2) The aramid insulation paper preparation method of the present invention is simple, the raw materials are easily available, the production cost is low, and it is suitable for large-scale industrial production. No chemical additives are used, which reduces pollution to the environment and promotes the green manufacturing of aramid insulation paper. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is a schematic structural diagram of the high initial partial discharge voltage aramid insulation paper of Example 1; Figure 2 Schematic diagram of the positional relationship between the nanofibers and the filling additives in Example 1.
[0021] The present invention will be further described in detail below with reference to the accompanying drawings. DETAILED DESCRIPTION
[0022] The embodiments of the present invention are described in detail below with reference to the accompanying drawings, but the present invention can be implemented in many different ways as defined and covered by the claims.
[0023] Embodiment 1: The high initial partial discharge voltage aramid insulation paper of this embodiment includes the following components in parts by weight: 50 parts of aramid short-cut fibers, 50 parts of aramid fibrids, 3 parts of aramid nanofibers and 1 part of a filling additive; Figure 1 and Figure 2 As shown ( Figure 1 and Figure 2 In the figure, 1 is aramid chopped fibers, 2 is aramid precipitated fibers, 3 is aramid nanofibers, and 4 is a filling additive), the aramid nanofibers and the filling additives are filled in the pores of the aramid insulating paper, and the aramid nanofibers are adsorbed and / or embedded on the surface of the filling additives.
[0024] The size of the aramid short fibers is: 8 mm in length; the aramid nanofibers are spherical particles with a particle size of D90 = 150 nm; the size of the aramid precipitated fibers is: 1.05 mm in length and a specific surface area of 98 m 2 / g, the beating degree is 71°SR, and the slurry concentration is 0.13%; the filling additive is spherical aluminum nitride particles that have been wet-ground, and the particle size D90=10μm.
[0025] The method for preparing the high initial partial discharge voltage aramid insulation paper of this embodiment comprises the following steps: (1) Aramid fiber precipitate (50 parts) was pretreated by using a pulper and a debonder; (2) lightly grinding the filler additive (1 part) and thoroughly mixing it with the aramid nanofiber (0.5 part) to obtain a mixture; (3) adding aramid short fibers (50 parts), the remaining aramid nanofibers (2.5 parts) and the mixture to the treated aramid fibrids, and mixing them thoroughly to obtain a slurry; (4) The slurry is conveyed to the net by a hydraulic headbox; the hydraulic headbox conveying to the net means that the aramid long fibers are firstly passed through the turbulence generator in the hydraulic headbox to form turbulence, and then the slurry is evenly and stably distributed along the full width of the paper machine. The turbulence scale generated by the turbulence generator is micro-turbulence, the turbulence intensity generated is 0.2~5%, and the slurry concentration is 0.5±0.1%; (5) Wet forming using a special dehydration curve on a Fourdrinier paper machine with a forming concentration of 0.12%; the dehydration curve includes three stages: The first stage: using the slurry's own gravity to dehydrate the slurry to form a wet paper base with a high water content; The second stage: provide a lower vacuum suction force to the dehydration element, partially dehydrate under low vacuum conditions (-8kPa), and form a structure in which aramid short fibers and aramid precipitated fibers wrap aramid nanofibers and filling additives in the wet paper base; The third stage: improve the vacuum suction force of the dehydration element, dehydrate under high vacuum conditions (-25kPa), and remove most of the moisture in the wet paper tire; (6) After subsequent pressing and drying, aramid insulation paper base paper is obtained; (7) The base paper is rolled up and subjected to composite hot pressing using an electromagnetic induced high-temperature roller press with a line pressure of 275 N / m and a hot pressing temperature of 310° C., thereby obtaining the high initial partial discharge voltage aramid insulation paper of this embodiment.
[0026] The high initial partial discharge voltage aramid insulation paper of this embodiment is used in motors of new energy vehicles.
[0027] Embodiment 2: The high initial partial discharge voltage aramid insulation paper of this embodiment includes the following components in parts by weight: 50 parts of aramid short fibers, 50 parts of aramid precipitated fibers, 3 parts of aramid nanofibers and 1 part of a filling additive; the aramid nanofibers and the filling additive are filled in the pores of the aramid insulation paper, and the aramid nanofibers are adsorbed and / or embedded on the surface of the filling additive.
[0028] The size of the aramid short fibers is: 9 mm in length; the aramid nanofibers are aramid nanofibers, which are polygonal particles with a particle size of D90 = 100 nm; the size of the aramid precipitated fibers is: 1.05 mm in length and 94 m in specific surface area. 2 / g, the beating degree is 70°SR, and the slurry concentration is 0.12%; the filling additive is polygonal aluminum nitride particles that have been dry-ground, and the particle size D90=15μm.
[0029] The method for preparing the high initial partial discharge voltage aramid insulation paper of this embodiment comprises the following steps: (1) Aramid fiber precipitate (50 parts) was pretreated by using a pulper and a debonder; (2) lightly grinding the filler additive (1 part) and thoroughly mixing it with the aramid nanofiber (0.5 part) to obtain a mixture; (3) adding aramid short fibers (50 parts), the remaining aramid nanofibers (2.5 parts) and the mixture to the treated aramid fibrids, and mixing them thoroughly to obtain a slurry; (4) The slurry is conveyed to the net by a hydraulic headbox; the hydraulic headbox conveying to the net means that the aramid long fibers are firstly passed through the turbulence generator in the hydraulic headbox to form turbulence, and then the slurry is evenly and stably distributed along the full width of the paper machine. The turbulence scale generated by the turbulence generator is micro-turbulence, the turbulence intensity generated is 0.2~5%, and the slurry concentration is 0.5±0.1%; (5) Wet forming using a special dehydration curve on a Fourdrinier paper machine with a forming concentration of 0.12%; the dehydration curve includes three stages: The first stage: using the slurry's own gravity to dehydrate the slurry to form a wet paper base with a high water content; The second stage: provide a lower vacuum suction force to the dehydration element, partially dehydrate under low vacuum conditions (-9kPa), and form a structure in which aramid short fibers and aramid fibrils wrap aramid nanofibers and filling additives in the wet paper base; The third stage: improve the vacuum suction force of the dehydration element, dehydrate under high vacuum conditions (-24kPa), and remove most of the moisture in the wet paper tire; (6) After subsequent pressing and drying, aramid insulation paper base paper is obtained; (7) The base paper is rolled up and subjected to composite hot pressing using an electromagnetically induced high-temperature roller press with a line pressure of 285 N / m and a hot pressing temperature of 305° C., thereby obtaining the high initial partial discharge voltage aramid insulation paper of this embodiment.
[0030] The high initial partial discharge voltage aramid insulation paper of this embodiment is used in motors of new energy vehicles.
[0031] Embodiment 3: The high initial partial discharge voltage aramid insulation paper of this embodiment includes the following components in parts by weight: 50 parts of aramid short fibers, 50 parts of aramid precipitated fibers, 3 parts of aramid nanofibers and 1 part of a filling additive; the aramid nanofibers and the filling additive are filled in the pores of the aramid insulation paper, and the aramid nanofibers are adsorbed and / or embedded on the surface of the filling additive.
[0032] The size of the aramid short fibers is: length 7 mm; the aramid nanofibers are spherical particles with a particle size of D90 = 100 nm; the size of the aramid precipitated fibers is: length 0.40 mm, specific surface area 94 m 2 / g, the beating degree is 70°SR, and the slurry concentration is 0.12%; the filling additive is spherical aluminum nitride particles that have been wet-ground, and the particle size D90=12.5μm.
[0033] The method for preparing the high initial partial discharge voltage aramid insulation paper of this embodiment comprises the following steps: (1) Aramid fiber precipitate (50 parts) was pretreated by using a pulper and a debonder; (2) lightly grinding the filler additive (1 part) and thoroughly mixing it with the aramid nanofiber (0.5 part) to obtain a mixture; (3) adding aramid short fibers (50 parts), the remaining aramid nanofibers (2.5 parts) and the mixture to the treated aramid fibrids, and mixing them thoroughly to obtain a slurry; (4) The slurry is conveyed to the net by a hydraulic headbox; the hydraulic headbox conveying to the net means that the aramid long fibers are firstly passed through the turbulence generator in the hydraulic headbox to form turbulence, and then the slurry is evenly and stably distributed along the full width of the paper machine. The turbulence scale generated by the turbulence generator is micro-turbulence, the turbulence intensity generated is 0.2~5%, and the slurry concentration is 0.5±0.1%; (5) Wet forming using a special dehydration curve on a Fourdrinier paper machine with a forming concentration of 0.12%; the dehydration curve includes three stages: The first stage: using the slurry's own gravity to dehydrate the slurry to form a wet paper base with a high water content; The second stage: provide a lower vacuum suction force to the dehydration element, partially dehydrate under low vacuum conditions (-9kPa), and form a structure in which aramid short fibers and aramid fibrils wrap aramid nanofibers and filling additives in the wet paper base; The third stage: improve the vacuum suction force of the dehydration element, dehydrate under high vacuum conditions (-24kPa), and remove most of the moisture in the wet paper tire; (6) After subsequent pressing and drying, aramid insulation paper base paper is obtained; (7) The base paper is rolled up and subjected to composite hot pressing using an electromagnetically induced high-temperature roller press with a line pressure of 285 N / m and a hot pressing temperature of 305° C., thereby obtaining the high initial partial discharge voltage aramid insulation paper of this embodiment.
[0034] The high initial partial discharge voltage aramid insulation paper of this embodiment is used in motors of new energy vehicles.
[0035] Comparative Example 1: The aramid insulation paper of this comparative example comprises the following components in parts by weight: 50 parts of aramid short fibers and 50 parts of aramid fibrids.
[0036] The size of the aramid short-cut fibers is 6 mm in length, the size of the aramid precipitated fibers is 0.6 mm in length, and the specific surface area is 98 m 2 / g, the beating degree is 71°SR, and the slurry concentration is 0.13%; the filling additive is spherical aluminum nitride particles that have been wet-ground, and the particle size D90=10μm.
[0037] The preparation method of the aramid insulation paper of this comparative example comprises the following steps: (1) Aramid fiber precipitate (50 parts) was pretreated by using a pulper and a debonder; (2) adding aramid short fibers (50 parts) to the treated aramid fibrids and mixing them thoroughly to obtain a slurry; (3) The slurry is conveyed to the net by a hydraulic headbox; the hydraulic headbox conveying to the net means that the aramid long fibers are firstly passed through the turbulence generator in the hydraulic headbox to form turbulence, and then the slurry is evenly and stably distributed along the full width of the paper machine. The turbulence scale generated by the turbulence generator is micro-turbulence, the turbulence intensity generated is 0.2~5%, and the slurry concentration is 0.5±0.1%; (4) Wet forming using a special dehydration curve on a Fourdrinier paper machine with a forming concentration of 0.12%; the dehydration curve includes three stages: The first stage: using the slurry's own gravity to dehydrate the slurry to form a wet paper base with a high water content; The second stage: provide a lower vacuum suction force to the dehydration element, and partially dehydrate under low vacuum conditions (-8kPa); The third stage: improve the vacuum suction force of the dehydration element, dehydrate under high vacuum conditions (-25kPa), and remove most of the moisture in the wet paper tire; (5) After subsequent pressing and drying, aramid insulation paper base paper is obtained; (6) The base paper is rolled up and subjected to composite hot pressing using an electromagnetic induced high-temperature roller press with a line pressure of 275 N / m and a hot pressing temperature of 310° C., thereby obtaining the aramid insulating paper of this comparative example.
[0038] Comparative Example 2: The aramid insulation paper of this comparative example comprises the following components in parts by weight: 50 parts of aramid short fibers, 50 parts of aramid fibrids and 1 part of filler additive.
[0039] The size of the aramid short-cut fibers is: 4 mm in length; the size of the aramid precipitated fibers is: 0.55 mm in length, with a specific surface area of 98 m 2 / g, the beating degree is 71°SR, and the slurry concentration is 0.13%; the filling additive is spherical aluminum nitride particles that have been wet-ground, and the particle size D90=10μm.
[0040] The preparation method of the aramid insulation paper of this comparative example comprises the following steps: (1) Aramid fiber precipitate (50 parts) was pretreated by using a pulper and a debonder; (2) lightly grinding the filler additive (1 part); (3) adding aramid short fibers (50 parts) and a filler additive (1 part) to the treated aramid fibrids, mixing the mixture thoroughly, and obtaining a slurry; (4) The slurry is conveyed to the net by a hydraulic headbox; the hydraulic headbox conveying to the net means that the aramid long fibers are firstly passed through the turbulence generator in the hydraulic headbox to form turbulence, and then the slurry is evenly and stably distributed along the full width of the paper machine. The turbulence scale generated by the turbulence generator is micro-turbulence, the turbulence intensity generated is 0.2~5%, and the slurry concentration is 0.5±0.1%; (5) Wet forming using a special dehydration curve on a Fourdrinier paper machine with a forming concentration of 0.12%; the dehydration curve includes three stages: The first stage: using the slurry's own gravity to dehydrate the slurry to form a wet paper base with a high water content; The second stage: provide a lower vacuum suction force to the dehydration element, and partially dehydrate under low vacuum conditions (-8kPa); The third stage: improve the vacuum suction force of the dehydration element, dehydrate under high vacuum conditions (-25kPa), and remove most of the moisture in the wet paper tire; (6) After subsequent pressing and drying, aramid insulation paper base paper is obtained; (7) The base paper is rolled up and subjected to composite hot pressing using an electromagnetic induced high-temperature roller press with a line pressure of 275 N / m and a hot pressing temperature of 310° C., thereby obtaining the aramid insulating paper of this comparative example.
[0041] Comparative Example 3: The aramid insulation paper of this comparative example comprises the following components in parts by weight: 50 parts of aramid short fibers, 50 parts of aramid fibrids and 3 parts of aramid nanofibers.
[0042] The size of the aramid short fibers is: 5 mm in length; the aramid nanofibers are spherical particles with a particle size of D90 = 150 nm; the size of the aramid precipitated fibers is: 0.70 mm in length and a specific surface area of 98 m 2 / g, the beating degree is 71°SR, and the slurry concentration is 0.13%.
[0043] The preparation method of the aramid insulation paper of this comparative example comprises the following steps: (1) Aramid fiber precipitate (50 parts) was pretreated by using a pulper and a debonder; (2) adding aramid short fibers (50 parts) and aramid nanofibers (3 parts) to the treated aramid fibrids and mixing them thoroughly to obtain a slurry; (3) The slurry is conveyed to the net by a hydraulic headbox; the hydraulic headbox conveying to the net means that the aramid long fibers are firstly passed through the turbulence generator in the hydraulic headbox to form turbulence, and then the slurry is evenly and stably distributed along the full width of the paper machine. The turbulence scale generated by the turbulence generator is micro-turbulence, the turbulence intensity generated is 0.2~5%, and the slurry concentration is 0.5±0.1%; (4) Wet forming using a special dehydration curve on a Fourdrinier paper machine with a forming concentration of 0.12%; the dehydration curve includes three stages: The first stage: using the slurry's own gravity to dehydrate the slurry to form a wet paper base with a high water content; The second stage: provide a lower vacuum suction force to the dehydration element, and partially dehydrate under low vacuum conditions (-8kPa); The third stage: improve the vacuum suction force of the dehydration element, dehydrate under high vacuum conditions (-25kPa), and remove most of the moisture in the wet paper tire; (5) After subsequent pressing and drying, aramid insulation paper base paper is obtained; (6) The base paper is rolled up and subjected to composite hot pressing using an electromagnetic induced high-temperature roller press with a line pressure of 275 N / m and a hot pressing temperature of 310° C., thereby obtaining the aramid insulating paper of this comparative example.
[0044] Comparative Example 4: The aramid insulation paper of this comparative example comprises the following components in parts by weight: 50 parts of aramid short fibers, 50 parts of aramid fibrids, 3 parts of aramid nanofibers and 1 part of filler additive.
[0045] The size of the aramid short fibers is: 6 mm in length; the aramid nanofibers are spherical particles with a particle size of D90 = 150 nm; the size of the aramid precipitated fibers is: 0.80 mm in length and a specific surface area of 98 m 2 / g, the beating degree is 71°SR, and the slurry concentration is 0.13%; the filling additive is unground spherical aluminum nitride particles with a particle size of D90=10μm.
[0046] The preparation method of the aramid insulation paper of this comparative example comprises the following steps: (1) Aramid fiber precipitate (50 parts) was pretreated by using a pulper and a debonder; (2) the filler additive (1 part) is directly mixed with the aramid nanofiber (0.5 part) without grinding to obtain a mixture; (3) adding aramid short fibers (50 parts), the remaining aramid nanofibers (2.5 parts) and the mixture to the treated aramid fibrids, and mixing them thoroughly to obtain a slurry; (4) The slurry is conveyed to the net by a hydraulic headbox; the hydraulic headbox conveying to the net means that the aramid long fibers are firstly passed through the turbulence generator in the hydraulic headbox to form turbulence, and then the slurry is evenly and stably distributed along the full width of the paper machine. The turbulence scale generated by the turbulence generator is micro-turbulence, the turbulence intensity generated is 0.2~5%, and the slurry concentration is 0.5±0.1%; (5) Wet forming using a special dehydration curve on a Fourdrinier paper machine with a forming concentration of 0.12%; the dehydration curve includes three stages: The first stage: using the slurry's own gravity to dehydrate the slurry to form a wet paper base with a high water content; The second stage: provide a lower vacuum suction force to the dehydration element, partially dehydrate under low vacuum conditions (-8kPa), and form a structure in which aramid short fibers and aramid precipitated fibers wrap aramid nanofibers and filling additives in the wet paper base; The third stage: improve the vacuum suction force of the dehydration element, dehydrate under high vacuum conditions (-25kPa), and remove most of the moisture in the wet paper tire; (6) After subsequent pressing and drying, aramid insulation paper base paper is obtained; (7) The base paper is rolled up and subjected to composite hot pressing by an electromagnetically induced high-temperature roller press at a line pressure of 275 N / m and a hot pressing temperature of 310° C., thereby obtaining the voltage aramid insulating paper of this comparative example.
[0047] Comparative Example 5: The aramid insulation paper of this comparative example comprises the following components in parts by weight: 50 parts of aramid short fibers, 50 parts of aramid fibrids, 3 parts of aramid nanofibers and 1 part of filler additive.
[0048] The size of the aramid short fibers is: 8 mm in length; the aramid nanofibers are spherical particles with a particle size of D90 = 150 nm; the size of the aramid precipitated fibers is: 0.9 mm in length and a specific surface area of 98 m 2 / g, the beating degree is 71°SR, and the slurry concentration is 0.13%; the filling additive is spherical aluminum nitride particles that have been wet-ground, and the particle size D90=50μm.
[0049] The preparation method of the aramid insulation paper of this comparative example comprises the following steps: (1) Aramid fiber precipitate (50 parts) was pretreated by using a pulper and a debonder; (2) wet-grinding the filler additive (1 part), and then mixing with aramid nanofiber (0.5 part) to obtain a mixture; (3) adding aramid short fibers (50 parts), the remaining aramid nanofibers (2.5 parts) and the mixture to the treated aramid fibrids, and mixing them thoroughly to obtain a slurry; (4) The slurry is conveyed to the net by a hydraulic headbox; the hydraulic headbox conveying to the net means that the aramid long fibers are firstly passed through the turbulence generator in the hydraulic headbox to form turbulence, and then the slurry is evenly and stably distributed along the full width of the paper machine. The turbulence scale generated by the turbulence generator is micro-turbulence, the turbulence intensity generated is 0.2~5%, and the slurry concentration is 0.5±0.1%; (5) Wet forming using a special dehydration curve on a Fourdrinier paper machine with a forming concentration of 0.12%; the dehydration curve includes three stages: The first stage: using the slurry's own gravity to dehydrate the slurry to form a wet paper base with a high water content; The second stage: provide a lower vacuum suction force to the dehydration element, partially dehydrate under low vacuum conditions (-8kPa), and form a structure in which aramid short fibers and aramid precipitated fibers wrap aramid nanofibers and filling additives in the wet paper base; The third stage: improve the vacuum suction force of the dehydration element, dehydrate under high vacuum conditions (-25kPa), and remove most of the moisture in the wet paper tire; (6) After subsequent pressing and drying, aramid insulation paper base paper is obtained; (7) The base paper is rolled up and subjected to composite hot pressing by an electromagnetically induced high-temperature roller press at a line pressure of 275 N / m and a hot pressing temperature of 310° C., thereby obtaining the voltage aramid insulating paper of this comparative example.
[0050] Comparative Example 6: The difference between this comparative example and Example 3 is that in step (5) of the preparation method, the vacuum degree of partial dehydration under low vacuum conditions in the second stage is adjusted to -15 kPa, and the other components, proportions, processes and parameters are consistent with those in Example 3.
[0051] Comparative Example 7: The difference between this comparative example and Example 3 is that in step (5) of the preparation method, the vacuum degree of partial dehydration under high vacuum conditions in the third stage is adjusted to -30 kPa, and the other components, proportions, processes and parameters are consistent with those in Example 3.
[0052] The performance of the finished products prepared in the above embodiments and comparative examples was tested, and the results are shown in Table 1 below.
[0053] Table 1. Performance test results of aramid insulation paper of various embodiments and comparative examples
[0054] The above test results show that: Comparative Example 1 is compared with Example 1, in which no aramid nanofiber and filler additive are added, and its mechanical properties are slightly decreased, and its electrical strength and initial partial discharge voltage are significantly decreased; Comparative Examples 2, 3, and 4 are not added with aramid nanofibers, filling additives, and filling additives are not ground, respectively, compared with Comparative Example 1. In Comparative Example 2, there are only filling additives, and the performance of the material other than the initial partial discharge voltage is slightly reduced. This is because the filling additives can play a role in heat conduction and alleviate the phenomenon of the initial partial discharge voltage drop caused by the temperature rise. However, the micron-level filling additives have a certain effect on the structure of the aramid insulation paper in the absence of the joint action of nanofibers, which leads to a decline in comprehensive performance; in Comparative Example 3, there are only aramid nanofibers, and the performance of the finished product has an overall increase, but the improvement of the initial partial discharge voltage is not obvious; the surface of the filling additive in Comparative Example 4 is not ground, and there is a lack of stabilizing effect of nanofibers on the filling additives. The aramid nanofibers, aramid precipitated fibers, and short fibers only have a coating and fixing effect on the additives, so the overall performance of the material is slightly reduced.
[0055] In Comparative Example 5, the particle size of the filler additive was increased (the particle size of the aramid nanofiber was fixed), and the performance of the finished paper was significantly reduced. This is because when the particle size is too large, it has a certain destructive effect on the structure of the aramid insulation paper. Comparative Examples 6 and 7 adjust the dehydration curve relative to Examples 2 and 3. Comparative Example 6 increases the vacuum degree of the front-end dehydration curve, and the performance of the finished paper is greatly reduced. This is because when the front-end dehydration vacuum degree is too high, the micron-nano structure in the aramid wet paper tire is easily damaged, resulting in poor paper uniformity and insufficient performance; Comparative Example 7 increases the vacuum degree of the rear-end dehydration curve (since the subsequent paper feeding work cannot be carried out due to incomplete dehydration when the vacuum degree is reduced, the comparative example is not given), and the performance of the finished paper is also greatly reduced, which is also because the microstructure of the aramid paper is damaged. At the same time, too high a vacuum degree in the rear section will accelerate the wear of the forming wire, which is not conducive to production work.
[0056] The above are only preferred embodiments of the present application and are not intended to limit the present application. For those skilled in the art, the present application may have various changes and modifications. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application should be included in the protection scope of the present application. The above are only preferred implementations of the present invention, and the protection scope of the present invention is not limited to the above embodiments. For those skilled in the art, improvements and changes obtained without departing from the technical concept of the present invention should also be regarded as the protection scope of the present invention.
Claims
1. A high initial partial discharge voltage aramid insulation paper, characterized in that: The composition comprises the following components in parts by weight: 40 to 60 parts of aramid chopped fibers, 60 to 40 parts of aramid fibrids, 2 to 5 parts of aramid nanofibers and 1 part of a filling additive; wherein the filling additive is a micron-sized filling additive.
2. The high initial partial discharge voltage aramid insulation paper according to claim 1, characterized in that: The aramid nanofibers and the filling additives are filled in the pores of the aramid insulation paper, and the aramid nanofibers are adsorbed and / or embedded on the surface of the filling additives.
3. The high initial partial discharge voltage aramid insulation paper according to claim 1, characterized in that: The filler additive includes at least one of aluminum nitride, boron nitride, and silicon carbide.
4. The high initial partial discharge voltage aramid insulation paper according to claim 1, characterized in that: The filler additive is ground and has a specific surface area of 50 m 2 / g.
5. The high initial partial discharge voltage aramid insulation paper according to claims 1-4, characterized in that: The size of the aramid chopped fibers is 1 to 15 mm, the size of the aramid nanofibers is 50 to 300 nm, and the particle size of the filling additive is 1 to 20 μm.
6. A method for preparing the high initial partial discharge voltage aramid insulation paper according to any one of claims 1 to 5, characterized in that: The following steps are involved: (1) pretreating the aramid fibrid; uniformly mixing the filler additive with 0.5 parts by mass of aramid nanofibers to obtain a mixture; and fully mixing the mixture, the pretreated aramid fibrid, aramid chopped fibers and the remaining aramid nanofibers to obtain a slurry; (2) placing the slurry on a fourdrinier paper machine for wet forming by a dehydration curve, and then performing post-processing to obtain aramid insulation paper base paper; (3) The aramid insulation paper base paper is rolled up and subjected to high-temperature rolling to obtain the high initial partial discharge voltage aramid insulation paper.
7. The method for preparing aramid insulation paper with high initial partial discharge voltage according to claim 6, characterized in that: In step (2), the slurry is conveyed to the net by a hydraulic headbox flow. The hydraulic headbox flow conveying to the net means that the aramid long fibers are firstly passed through a turbulence generator in the hydraulic headbox to form turbulence, and then the slurry is evenly and stably distributed along the full width of the paper machine. The turbulence scale generated by the turbulence generator is micro-turbulence, and the turbulence intensity generated is 0.2-5%. The concentration of the slurry is 0.5±0.1%.
8. The method for preparing high initial partial discharge voltage aramid insulation paper according to claim 6, characterized in that: The dehydration curve in step (2) includes three stages: The first stage: using the slurry's own gravity to dehydrate the slurry to form a wet paper base with a high water content; The second stage: providing a lower vacuum suction force to the dehydration element, partially dehydrating under low vacuum conditions, and forming a structure in which aramid short fibers and aramid fibrils encapsulate aramid nanofibers and filling additives in the wet paper web; The third stage: Increase the vacuum suction force of the dehydration element, dehydrate under high vacuum conditions, and remove most of the moisture in the wet paper.
9. The method for preparing aramid insulation paper with high initial partial discharge voltage according to claim 8, characterized in that: In the second stage, the vacuum degree of dehydration is -1 to -10 kPa; in the third stage, the vacuum degree of dehydration is -16 to -25 kPa.
10. An application of the high initial partial discharge voltage aramid insulation paper according to any one of claims 1 to 5, characterized in that: The high initial partial discharge voltage aramid insulation paper is used in motors of new energy vehicles.
Citation Information
Patent Citations
Composite papermaking nano reinforced aramid paper and preparation method thereof
CN112609493A
Preparation method of aramid paper added with nanofibers
CN115216991A
Aramid insulation paper-based material for motor slot insulation and preparation method of aramid insulation paper-based material
CN115506176A
Heat-conducting insulation paper and preparation method thereof
CN115595819A
Electrical insulating paper
WO2012093048A1