Experimental platform and method for electric arc induced battery thermal runaway
By designing an experimental platform for arc-induced thermal runaway, the arc-induced thermal runaway of the battery is simulated, and the electrical and thermal characteristics of the arc are analyzed, the research gap in arc faults in the battery system is solved, and arc detection and protection performance are improved.
Patent Information
- Application Number
- CN202411015435.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-19
AI Technical Summary
The existing technology lacks research on the mechanism of arc-induced battery disasters in battery systems, which has led to the electrical safety problems of arc faults in battery systems that have not been effectively solved. It is urgently necessary to simulate experimental platforms and methods for arc-induced battery thermal runaway.
An experimental platform for arc-induced thermal runaway battery was designed, including arc generation unit, detection unit and analysis unit. The arc fault was collected by simulated by moving electrodes, batteries to be tested, DC voltage-regulated power supply and adjustable resistors. Data, analyze the electrical and thermal characteristics of the arc, and quantitatively analyze the degree of thermal runaway from the battery.
By simulating arc-induced thermal runaway from the battery, we have improved our understanding of the arc evolution process, filled the gap in the field of arc safety of battery systems, and improved the safety performance of arc detection and protection.
Smart Images

Figure CN118980890A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of battery experiments, and in particular to an experimental platform and method for arc-induced thermal runaway of batteries. Background Art
[0002] With the continuous development of renewable energy generation, energy storage systems and electric vehicles have become important components of the power system. As the voltage levels of electric vehicles and energy storage battery systems continue to increase, the maximum voltage of electric vehicles can reach 800V, and the maximum voltage of energy storage power stations can reach 1500V. Therefore, the electrical safety issues within the battery system are becoming more and more serious. In order to ensure the normal operation of the battery system in energy storage power stations and electric vehicles, the safety of the battery should be paid attention to first. The safety issues of batteries in battery systems mainly consider the problem of battery thermal runaway. At present, there are three main methods to induce battery thermal runaway: mechanical abuse, electrical abuse, and thermal abuse.
[0003] Arc fault is one of the common electrical safety problems in battery systems. Loose metal connectors, damaged wires, and loose wiring contacts can cause the circuit to be seemingly connected but not connected, which in turn causes arc problems. At present, research on arcs in battery systems is still in its infancy, mainly focusing on arc detection problems in battery systems, and there is a clear lack of research on the battery disaster mechanism induced by arcs in battery systems. When an arc problem occurs in a battery system, the arc itself is formed by electricity, and the evolution process is accompanied by obvious high temperature phenomena. Therefore, the arc has the characteristics of electrical-thermal coupling, rather than a single electrical or thermal abuse method. The arc is a new way to induce thermal runaway of the battery. Therefore, the battery system of electric vehicles and energy storage power stations urgently needs an experimental platform and method that can simulate arc-induced battery thermal runaway. Summary of the invention
[0004] In view of the above-mentioned defects of the prior art, the present invention provides an experimental platform for arc-induced battery thermal runaway, comprising:
[0005] An arc generating unit, comprising a moving electrode, a battery to be tested, a DC regulated power supply and an adjustable resistor;
[0006] A detection unit, including a current sensor, a voltage sensor, a temperature sensor and an image acquisition device;
[0007] The analysis unit conducts arc experiments through the arc generating unit, receives the current data, voltage data, temperature data and image data collected by the detection unit, records the battery arc evolution process, analyzes the electrical and thermal characteristics of the battery arc and conducts quantitative analysis of battery thermal runaway.
[0008] Furthermore, the battery is provided with n temperature monitoring points, and each of the temperature monitoring points is provided with a temperature sensor.
[0009] Furthermore, the arc occurs between the movable electrode and the battery to be tested, one temperature monitoring point is located at the center of the battery shell, and the remaining temperature monitoring points are arranged in sequence at the same distance starting from the edge of the battery shell at the arc occurrence position.
[0010] Furthermore, the batteries to be tested include batteries with different SOC values, and the SOC values are 0%, 30%, 60% and 100%, respectively.
[0011] The second aspect of the present invention provides an experimental method for arc-induced battery thermal runaway, which is implemented based on the arc-induced battery thermal runaway experimental platform described in the first aspect of the present invention and includes the following steps:
[0012] Conduct arc-battery thermal runaway experiment on the experimental battery, and collect arc voltage, current, temperature and image;
[0013] The battery arc evolution process is recorded by an image acquisition device, and the evolution process is divided into the experimental startup stage, arc evolution stage, arc extinction stage, thermal runaway stage, and battery cooling stage according to the image information;
[0014] Analyze the electrical characteristics of the battery arc, and generate electrical characteristic waveforms and electrical characteristic data of the battery arc experiment with different SOCs based on the arc voltage, battery voltage and loop current at different times;
[0015] Analyze the thermal characteristics of battery arc, and generate thermal characteristic data of battery arc experiments with different SOCs based on the temperature values of each temperature monitoring point at different times;
[0016] Quantitatively analyze the degree of thermal runaway of the battery and determine the number of broken positive pole ears of the battery based on the number of times the battery voltage drops and rebounds.
[0017] Furthermore, the electrical characteristic data include arc voltage variation curves, battery voltage variation curves and loop current variation curves of batteries with different SOCs.
[0018] Furthermore, the thermal characteristic data includes the temperature change curve of the temperature monitoring point of the SOC battery and the time data required for each temperature point to start to rise sharply due to the voltage failure of different SOC batteries. The location where the first failure of the battery occurs is inferred through the time data.
[0019] Compared with the prior art, the present invention has the following technical effects:
[0020] The present invention changes the arc evolution process by adjusting the input voltage and load resistance, realizes arc-induced thermal runaway of the battery, and further simulates the thermal runaway phenomenon when the battery has an arc fault. The acquisition unit collects the voltage, current, temperature data and image information in the experimental process, and quantitatively analyzes the battery arc evolution process, the electrical characteristics and thermal characteristics of the battery arc and the battery thermal runaway, filling the gap in the field of arc safety of the battery system, improving the understanding of the arc evolution of the battery system, simulating the disaster-causing path of the arc to the battery, and playing an important role in developing arc detection of the battery system and improving the safety performance of arc protection.
[0021] The concept, specific structure and technical effects of the present invention will be further described below in conjunction with the accompanying drawings to fully understand the purpose, characteristics and effects of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is a structural principle diagram of an experimental platform for arc-induced battery thermal runaway according to a specific embodiment of the present invention;
[0023] Figure 2 is an electrical characteristic waveform of a battery arc test with different SOCs in a specific embodiment of the present invention, Figure 2 a is the battery electrical characteristic waveform when SOC is 0%; Figure 2 b is the battery electrical characteristic waveform when the SOC is 30%; Figure 2 c is the battery electrical characteristic waveform when the SOC is 60%; Figure 2 d is the battery electrical characteristic waveform when SOC is 100%;
[0024] Figure 3 It is a temperature waveform of a battery arc test with different SOCs in a specific embodiment of the present invention; Figure 3 a is the temperature waveform when SOC is 0%; Figure 3 b is the temperature waveform when SOC is 30%; Figure 3 c is the temperature waveform when SOC is 60%; Figure 3 d is the temperature waveform when SOC is 100%;
[0025] Figure 4 This is the corresponding relationship diagram between the center temperature of the large surface of the battery and the temperature rise rate; Figure 5 is the time distribution from voltage failure to temperature starting to rise sharply in a specific embodiment of the present invention;
[0026] Figure 6 In a specific embodiment of the present invention, the physical process of arc disaster when the battery SOC is 0% is described. Figure 6 a is the arc evolution stage, Figure 6 b is the short-circuit stage inside the winding core; Figure 6 c is the stage of core lug fracture;
[0027] Figure 7 is an electrical characteristic diagram of a faulty winding core in a specific embodiment of the present invention, Figure 7 a is the electrical characteristic curve of Cell1 when the battery SOC is 0%; Figure 7 b is the electrical characteristic curve of Cell 2 when the battery SOC is 0%; Figure 7 c is the electrical characteristic curve of Cell 3 when the battery SOC is 0%; Figure 7 d is the electrical characteristic diagram of the faulty core of the battery with different SOC. DETAILED DESCRIPTION
[0028] The following describes the embodiments of the present invention by specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that the following embodiments and features in the embodiments can be combined with each other without conflict.
[0029] It should be noted that the illustrations provided in the following embodiments are only used to illustrate the basic concept of the present invention in a schematic manner, and thus the illustrations only show components related to the present invention rather than being drawn according to the number, shape and size of components in actual implementation. In actual implementation, the type, quantity and proportion of each component may be changed arbitrarily, and the component layout may also be more complicated.
[0030] While some exemplary embodiments of the present invention have been described for the purpose of illustration, it should be understood that the present invention may be implemented in other ways not specifically shown in the drawings.
[0031] like Figure 1 As shown, in a specific embodiment, an experimental platform for arc-induced battery thermal runaway is provided, comprising:
[0032] The arc generating unit includes a mobile electrode, a battery to be tested, a DC regulated power supply and an adjustable resistor. The DC power supply (China Itech, IT6018D-1500-40) is used to simulate the output voltage U of the battery system. dc , which can simulate the variable DC voltage of the energy storage system up to 1500V, with an accuracy within 0.2%. The adjustable resistor (Itech, China, 63206A-600-56) is used to change the circuit resistance R, and then adjust the loop current of the experimental platform, with an accuracy within 0.2%.
[0033] In this embodiment, a 20Ah prismatic battery produced by Lishen Company is selected as the research object, and its relevant parameters are shown in Table 1.
[0034] Table 1 Battery cell models
[0035]
[0036] The detection unit includes a current sensor, a voltage sensor, a temperature sensor, an image acquisition device and a high-speed data acquisition device. In this embodiment, the current sensor is a Hall current sensor, the temperature sensor is a K-type thermocouple, and the image acquisition device is a camera. The Hall current sensor (CHB25-NP from China Sensor Electronics Company) measures the change of current in the circuit (≤25A) with an accuracy within 0.8%. The K-type thermocouple is used to measure the temperature at different positions of the battery, with a maximum temperature of 1300°C. The battery voltage U during the experiment B , arc voltage U arc , loop current I dc and temperature T B The parameters are recorded by an online high-speed data acquisition device (DPO4010B-L MR6000 of HIOKI Corporation, Japan) with a maximum sampling speed of 10MS / s. The camera is used to monitor the arc evolution and the disaster-causing process of the battery.
[0037] In order to comprehensively collect the temperature change data of the battery, n temperature monitoring points are provided on the upper cover of the battery to be tested, and temperature sensors are installed on the temperature monitoring points. When the arc occurs between the movable electrode and the battery to be tested, one of the temperature monitoring points is located at the center of the battery shell, and the remaining temperature monitoring points are arranged in sequence at the same distance starting from the edge of the battery shell at the arc occurrence position. In this embodiment, when the battery electrode is used as the arc occurrence position, 6 temperature monitoring points are set, namely #1, #2, #3, #4, and #5, among which point #1 is at the edge of the shell and the upper cover just above the arc position, and adjacent monitoring points #1-#5 are arranged in sequence at a distance of 1 cm, and #6 is placed at the center of the large surface of the battery. The 6 thermocouples are arranged at 6 preset temperature points, respectively, to obtain the battery temperature array T B (T1-T6) is used to obtain the temperature change law of the core induced by the arc evolution process. Assume that the critical temperature between the gradual temperature rise and the rapid temperature rise in T6 is defined as T TR , indicating thermal failure of the battery, the TTR threshold is set to 1℃ / s
[0038] The arc experiment is carried out by the arc generating unit, and the parameters are set as follows:
[0039] 1) Circuit parameters: power supply voltage U dc=300V, load resistance R=20Ω;
[0040] 2) AFG parameters: the separation gap of the stepper motor is L = 1 mm, and the stepper motor is controlled by a computer;
[0041] 3) Battery parameters: Select four different SOCs: 0%, 30%, 60%, and 100%.
[0042] The analysis unit is used to receive the current data, voltage data, temperature data and image data collected by the detection unit, record the evolution process of the battery arc, analyze the electrical characteristics and thermal characteristics of the battery arc and quantitatively analyze the thermal runaway of the battery. The analysis unit is a computer.
[0043] To ensure the safety of the experiment, the arc generating unit is placed in an explosion-proof box. After the circuit is connected, power is turned on. According to the set parameters, the contact between the moving electrode and the battery pole is controlled to separate. The air is broken down by the voltage and current to generate an arc. Each detection device collects the voltage, current, temperature, image and other data of the arc in real time. The analysis unit stores and processes the arc data. Before each experiment, a new electrode must be replaced to ensure the stability of the arc generation.
[0044] Based on the arc-induced battery thermal runaway experimental platform described in the above embodiment, an arc-induced battery thermal runaway experimental method is provided in a specific embodiment, comprising the following steps:
[0045] S1. Conduct arc-battery thermal runaway experiment on the experimental battery, and collect the voltage, current, temperature and image of the arc;
[0046] S2. Record the battery arc evolution process through an image acquisition device, and divide the evolution process into experimental startup stage, arc evolution stage, arc extinguishing stage, thermal runaway stage, and battery cooling stage according to the image information.
[0047] In the early stages of the arc evolution, the arc appears blue-white and is dazzlingly bright; as the arc evolves, a large amount of metal sparks sputter, accompanied by a thin outer layer of orange light, and the arc ignites the insulating material of the battery cover to form a flame.
[0048] Under the continuous action of the arc, for batteries with a SOC of 0% and a SOC of 30%, the consumption of copper electrodes and negative electrodes increases the arc length, requiring a larger incident power to maintain combustion, and the arc burning causes a large amount of metal oxides to adhere to the surface of the copper electrode and the negative electrode to hinder combustion. Finally, the arc will be extinguished. 10.1s after the arc of the battery with a SOC of 30% was extinguished, a large amount of white smoke (gas-liquid mixture) began to leak from the negative column of the battery. As the gas production continued to increase, the entire explosion-proof box was filled, indicating that the internal thermal fault of the battery was serious. The main components of the white smoke (gas-liquid mixture) include gases produced by irreversible reactions in the winding core and electrolyte vapor; through image analysis, it can be seen that the insulating sealing material near the negative column was severely burned by the arc due to the continuous high temperature of the arc, resulting in a gap between the negative column and the upper cover, providing a channel for the white smoke generated inside the battery to leak out.
[0049] For batteries with a SOC of 60% and a SOC of 100%, flame jetting occurs near the negative pole of the battery before the arc is extinguished, and the flame jetting rate is related to the speed of smoke leakage. As the internal gas production becomes more and more serious, the battery shell continues to expand. Batteries with a SOC of 100% cannot withstand excessive internal pressure, which will cause the top cover to be opened and the internal coil to be ejected. At the moment the coil is ejected, the flame burns violently. Normally, lithium iron phosphate batteries will produce a large amount of white smoke during thermal runaway, but flame jetting rarely occurs, similar to batteries with a SOC of 30%. The white smoke leaked from batteries with a SOC of 60% and batteries with a SOC of 100% is ignited by the arc, causing flame jetting. At this time, the flame jetting phenomenon occurs earlier than the arc is extinguished, indicating that a serious fault has occurred inside the battery. As the flame eruption rate increases, the arc is eventually blown out.
[0050] S3. Analyze the electrical characteristics of the battery arc, and generate electrical characteristic waveforms and electrical characteristic data of battery arc experiments with different SOCs according to the arc voltage, battery voltage, and loop current at different times.
[0051] Among the arc electrical characteristics, arc voltage and arc current are both important characteristics, and battery voltage is the most intuitive parameter to reflect battery health. Figure 2 As shown, the electrical characteristic waveforms of the battery arc experiment at four different SOCs of 0%, 30%, 60% and 100%, which mainly include the arc voltage change curve, the battery voltage change curve and the loop current change curve.
[0052] At the start-up stage of the experiment, the DC power supply is closed and the power supply voltage U dc =300V, loop current I dc=14.8A, the battery voltage starts to increase, and at the same time the current flowing through the electrodes and the battery is equal to the loop current, and the voltage between them is zero (the same is true for the arc resistance).
[0053] When the moving electrode is separated from the pole, the arc voltage rises sharply to the minimum arc voltage, indicating the start of the arc, and the arc current drops sharply from the load current. In this embodiment, the minimum arc voltage U corresponding to the battery with different SOC arc,min =15.5±0.3V, that is, the minimum arc voltage has nothing to do with the battery SOC. When the arc is generated, due to the introduction of nonlinear arc resistance, the loop current I dc The current drop value ΔI is:
[0054]
[0055] It can be seen from the above formula that the current drop value ΔI is only related to the arc voltage U arc It is related to the load resistance R. As the arc voltage increases, the arc current decreases continuously, and the arc as a whole presents a negative resistance characteristic. At the moment of arc generation, there is a minimum current drop value ΔI min =U arc,min / R, which is also only compatible with U arc,min It is related to R, and in this embodiment, the minimum current drop value ΔI=0.775±0.015A.
[0056] During the arc evolution, the arc voltage is basically stable in the range of 20-30V. When the arc occurs, the battery is still in the charging state. Due to the existence of arc resistance, the loop current is lower than that in the startup stage, and the battery charging rate is lower than that in the startup stage.
[0057] When the arc is extinguished, the arc current suddenly decreases to zero, and the arc voltage rises to the power supply voltage value. When the arc is completely extinguished, the arc voltage is equal to the power supply voltage, the current flowing through the electrode is zero, and the arc resistance theoretically reaches a value close to infinity.
[0058] During the arc extinguishing stage, the battery voltage of batteries with different SOCs dropped and rebounded. When the SOC was 0%, the battery voltage dropped and rebounded three times, and when the SOC was 30%, 60%, and 100%, the battery voltage dropped and rebounded five times, which confirmed that the batteries of each SOC had voltage failure. Figure 2 It can be seen that the arcing times of batteries with SOC of 0%, 30%, 60% and 100% SOC are 202.9s, 185.6s, 178.8s and 171.4s respectively. It can be seen that the larger the battery SOC value, the shorter the time required for the arc to cause a disaster.
[0059] S4. Analyze the thermal characteristics of the battery arc, and generate thermal characteristic data of the battery arc experiment with different SOCs according to the temperature values of each temperature monitoring point at different times.
[0060] Arc temperature is a key parameter of arc thermal characteristics and is mainly used to characterize arc-induced disasters. Figure 3 As shown, the temperature waveforms of arc experiments for different SOC batteries. Among them, the temperature arrays T1-T6 are used to represent the changes in battery surface temperature. During the arc action process, the external sources of battery heat mainly include arc heating and Joule heating. As can be seen from the figure, the battery surface temperature arrays T1-T6 are gradually increasing, and the temperature T1 closer to the arc location increases the fastest, with a strong local heating effect. The other temperature rise rates decrease from T1 to T6, proving that arc heating is the most important factor inducing battery temperature rise, that is, the arc conducts continuous heat conduction to the inside of the battery through the pole and the upper cover, and the surface thermocouple measurement point #1 closest to the arc is easily heated directly by the outer flame of the arc, resulting in significant fluctuations in temperature T1.
[0061] Under the action of the electric arc, the T1-T4 temperature arrays on the battery surface can reach the temperature of the battery's self-generated heat (111.6°C, derived from the battery adiabatic thermal runaway experiment) in a short period of time; among them, the time required for batteries with SOC of 0%, 30%, 60% and 100% are 166.3s, 121.2s, 104.2s and 84.9s respectively. It can be seen that under the same arc conditions, the side reactions generated inside the high SOC battery are more serious, and the time to cause internal disasters is less.
[0062] After the arc was extinguished, batteries with different SOCs all experienced a stage of rapid temperature rise. Combined with the battery voltage drop phenomenon shown in the figure, it is preliminarily speculated that the battery core may have an internal short circuit failure. From the experimental phenomena, it can be seen that except for the 0% SOC battery, the batteries with other SOCs eventually evolved into thermal runaway under the action of internal short circuit. This further shows that in the cooling stage, the surface temperature of the battery with an SOC of 0% drops rapidly, while the surface temperature of the battery with other SOC values drops more slowly. It is worth noting that Figure 3 The accelerated cooling phenomenon of the temperature curves in d after 315s is caused by the battery core with a SOC of 100% being ejected from the shell.
[0063] Figure 4 The corresponding relationship between the battery temperature rise rate and temperature T6 with different SOC is shown. When the temperature rise rate reaches 1°C / s, the battery is considered to have thermal failure. Figure 4 The temperature rise rate of each battery in the test exceeds 1℃ / s. This shows that under the influence of internal short circuit failure, batteries with different SOC levels will eventually fail thermally. The inflection point temperature of T6 represents the thermal failure of T TR Indicates that Figure 3shown.
[0064] Combination Figure 3 and Figure 4 By comparing the time required for each temperature point to start to rise sharply due to voltage failure of batteries with different SOC, the location where the first battery failure occurs can be determined. Figure 5 It can be seen that the temperature increases rapidly from T3 to T4, indicating that failure first occurs near the inside of the battery shown in T3 to T4.
[0065] S5. Quantitatively analyze the degree of thermal runaway of the battery and determine the number of broken positive pole ears of the battery according to the number of drops and rebounds of the battery voltage.
[0066] like Figure 6 a represents the arc evolution stage. In the figure, N represents the number of normal winding cores in the battery. In the arc evolution stage, the winding core remains intact, and N=5. In this embodiment, the battery is composed of five winding cores connected in parallel. The charging current of each winding core during the arc evolution process is 0.2I dc , and the internal resistance of each winding core is R b =5*r=10mΩ. During the evolution of the arc, the arc current continuously charges the battery through the series circuit, and the high temperature accompanied by the arc conducts continuous heat to the inside of the battery through the negative pole and the shell. Taking the prismatic battery experiment with a SOC of 0% as an example, the overall arc burning time is 205.3s. For short-term and low-rate (<0.75C) battery charging, the open circuit voltage E basically does not increase much.
[0067] As the heat conduction continued, the arc caused serious damage and expansion of the core membrane near the negative pole, especially in Cell 1, Cell 2 and Cell 3. The connection between the aluminum foil and copper foil of the three cores formed Figure 6 b shows the internal short circuit stage of the winding core. The internal short circuit equivalent resistance R of Cell 1 Id The sum is the internal short-circuit current I of Cell 1 Id satisfy:
[0068]
[0069] Simplifying the above formula, we can get:
[0070]
[0071] Taking the electrical failure process of a faulty winding core of a battery with a SOC of 0% as an example, the arc successively causes internal short circuit failures and positive electrode ear breakage in Cell 1, Cell 2, and Cell 3. Figure 7 As shown in a, when a short circuit occurs in Cell 1, the equivalent resistance R Id Maintained at around 22mΩ, the internal short-circuit current IId The maximum can reach 124A. Therefore, the outer positive ear of Cell 1 was melted by the continuous short-circuit high current (>6C discharge rate), and then the internal short-circuit equivalent resistance reached about 270mΩ, while the short-circuit current decreased to about 11A, which made the inner positive ear unable to be melted.
[0072] One tab is close to the outside of the winding core, and the other is on the inside of the winding core, which causes the positive tab on the inside of Cell 1 to not fuse. Figure 6 b, the internal short-circuit equivalent resistance R Id The positive and negative electrodes are short-circuited by resistor R Is , the internal short-circuit point and the outer positive ear resistance R Ot_is And the internal short-circuit point and the inner positive ear resistance R It_is Together, the resistor R Ot_is and resistor R It_is First connect in parallel, then connect with R Is In series connection, since the internal short circuit fault occurs near the outer positive ear, the distance from the internal short circuit point to the outer ear is much smaller than the distance to the inner ear. Figure 6 b It can also be seen that R It_is < <R Ot_is Therefore, the internal short-circuit current I of Cell 1 is Id Only flows through R Ot_is The branch where it is located causes the outer positive terminal to fuse, such as Figure 6 c. However, after the positive terminal of Cell 1 is blown, R It_is and R Is However, a large series resistance (about 270mΩ) is formed, which causes the short-circuit current to decrease (about 11A). Therefore, the inner positive ear cannot be fused, which causes one positive ear of Cell 1 to break while the other ear remains intact.
[0073] Since both Cell 2 and Cell 3 have internal short circuits, the corresponding internal short circuit equivalent resistance R is determined. Id And the internal short-circuit current I Id ,like Figure 7b and 7c. It can be obtained from the experimental data that the short-circuit current of the corresponding outer positive ears of Cell 2 and Cell 3 is about 114A and 83A, and then the corresponding outer inner ears are fused. However, the inner positive ears cannot continue to be fused under the action of the large series resistance. In addition, during the disassembly of the core, it was determined that Cell 4 and Cell 5 did not have internal short-circuit faults, so Cell 4 and Cell 5 could only discharge from the short-circuit branches retained by Cell 1, Cell 2 and Cell 3. Due to the large short-circuit resistance and the continuous decrease in the capacity of the core, the short-circuit current is too small to fuse any of the positive ears of Cell 4 and Cell 5, and Cell 4 and Cell 5 maintain short-circuit discharge until the discharge is completed.
[0074] Figure 7 d is the maximum current and duration of the internal short circuit corresponding to each faulty core of different SOC batteries during the internal short circuit process. For batteries with the same SOC, statistics show that the earlier the core fails, the greater the internal short circuit current, and as the faulty cores occur in sequence, the internal short circuit current decreases in sequence (Cell 1>Cell 2>Cell 3>Cell 4>Cell5). This is because the battery continues to discharge and the capacity decreases. In addition, the decrease in the internal short circuit current leads to an increase in the duration of the internal short circuit, and the time required to melt the tabs will also increase. Through waveform analysis, it can be seen that the battery with an SOC of 0% only has an internal short circuit in 3 cores, so the internal short circuit current flowing through Cell 4 and Cell 5 is 0. For the faulty cores with the same serial number of batteries with different SOCs, in the overall trend, the larger the SOC, the greater the maximum internal short circuit current when the fault occurs, the shorter the duration of the internal short circuit, and the shorter the time required to melt the tabs.
[0075] In addition, it can be seen from the collected voltage data that Figure 7 The number of times the battery voltage drops and rises is exactly equal to the number of positive tabs that are broken. Therefore, the number of positive tabs that are broken can be determined simply by the number of times the battery voltage drops and rises.
[0076] An arc experimental platform suitable for batteries was built, and an experimental method for battery arc was designed. Subsequently, after a large number of battery arc experiments, the evolution law of the arc was mastered. It can be seen from the above embodiments that the path of the arc causing thermal runaway of the battery is: first, the diaphragm of the winding core is constantly broken under the high temperature erosion of the arc, causing an internal short circuit fault of the winding core; further, the short-circuit large current melts the positive ear on the outside of the winding core, forming an open circuit fault; further, the internal short circuit of the battery causes abnormal temperature rise and a large amount of heat accumulation, and the diaphragm further disintegrates, causing a large area of internal short circuit, followed by internal short circuit faults and ear fracture faults in multiple winding cores; finally, the internal short circuit problem of the battery evolves into an unstoppable thermal runaway disaster. It can be seen that the internal cause of arc-induced thermal runaway of the battery is attributed to the large-area internal short circuit problem. Moreover, the larger the battery SOC, the shorter the time required for the arc fault to induce battery failure, and the more obvious the degree of battery disaster (flame spread, mass loss and expansion thickness) is. It has improved the understanding of arc evolution and disasters in battery systems and filled the gap in the field of arc safety protection in battery systems. It is crucial for the subsequent improvement of arc detection methods in battery systems and the improvement of the safety performance of arc protection.
[0077] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. Experimental platform for arc-induced battery thermal runaway, It is characterized in that include: An arc generating unit, comprising a moving electrode, a battery to be tested, a DC regulated power supply and an adjustable resistor; A detection unit, including a current sensor, a voltage sensor, a temperature sensor and an image acquisition device; The analysis unit conducts an arc experiment through the arc generating unit, receives the current data, voltage data, temperature data and image data collected by the detection unit, records the battery arc evolution process, analyzes the electrical and thermal characteristics of the battery arc and quantitatively describes the battery thermal runaway.
2. According to the arc-induced battery thermal runaway experimental platform of claim 1, It is characterized in that The battery is provided with n temperature monitoring points, and the temperature monitoring points are provided with temperature sensors.
3. According to the arc-induced battery thermal runaway experimental platform of claim 2, It is characterized in that The arc occurs between the movable electrode and the battery to be tested. One temperature monitoring point is located at the center of the battery shell, and the remaining temperature monitoring points are arranged in sequence at the same distance starting from the edge of the battery shell at the arc occurrence position.
4. According to the arc-induced battery thermal runaway experimental platform of claim 2, It is characterized in that The batteries to be tested include batteries with different SOC values, and the SOC values are 0%, 30%, 60% and 100% respectively.
5. Experimental method for arc-induced battery thermal runaway, It is characterized in that The experimental platform for arc-to-battery thermal runaway according to any one of claims 1 to 4 is implemented, comprising the following steps: Conduct arc-battery thermal runaway experiment on the experimental battery, and collect arc voltage, current, temperature and image; The battery arc evolution process is recorded by an image acquisition device, and the evolution process is divided into the experimental startup stage, arc evolution stage, arc extinction stage, thermal runaway stage, and battery cooling stage according to the image information; Analyze the electrical characteristics of the battery arc, and generate electrical characteristic waveforms and electrical characteristic data of the battery arc experiment with different SOCs based on the arc voltage, battery voltage and loop current at different times; Analyze the thermal characteristics of battery arc, and generate thermal characteristic data of battery arc experiments with different SOCs based on the temperature values of each temperature monitoring point at different times; Quantitatively analyze the degree of thermal runaway of the battery and determine the number of broken positive pole ears of the battery based on the number of times the battery voltage drops and rebounds.
6. According to the experimental method of arc-induced battery thermal runaway according to claim 5, It is characterized in that The electrical characteristic data include arc voltage variation curves, battery voltage variation curves and loop current variation curves of batteries with different SOCs.
7. According to the experimental method of arc-induced battery thermal runaway according to claim 5, It is characterized in that The thermal characteristic data includes the temperature change curve of the temperature monitoring point of the SOC battery and the time data required for each temperature point to start to rise sharply due to the voltage failure of different SOC batteries. The location where the first failure of the battery occurs is inferred through the time data.
Citation Information
Cited By
Device and method for detecting arc fault of battery module
CN119619762A
Battery arc testing device and battery arc testing method
CN119846402A
Method for determining safety boundary of electric arc caused by thermal runaway injection of battery
CN120233264A
Arc discharge device for triggering battery failure and test method
CN121633749A
Electric breaking arc induced failure battery combustion test device
CN122568324A