Lithium mixed oxide particles encapsulated with alumina and titania and methods of use thereof
By dry mixing with a specific mixture of alumina and titanium dioxide on the cathode material of lithium-ion battery, aggregation particles with high BET surface area is solved, and the problems of coating instability and fragility in the prior art are significantly improved. Electrochemical properties and cycle life.
Patent Information
- Application Number
- CN202411069347.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2017-02-17
- Filing Date
- 2018-02-13
- Publication Date
- 2024-11-19
AI Technical Summary
In the prior art, the reaction of metal oxide coating with electrolyte on the cathode material of lithium-ion battery still has problems of instability and fragility, and it is difficult to effectively improve the electrochemical properties and stability of the coating.
Using a specific mixture of alumina and titanium dioxide as coating material, the mixing time and power range is controlled by dry mixing under shear conditions, using a powerful mixer and high-speed mixing tool, to form aggregated primary particles with high BET surface area, ensuring The weight ratio of alumina to titanium dioxide is in the range of 10:90-70:30, avoiding heat treatment to maintain adhesion.
More stable coating adhesion and electrochemical properties are achieved, reducing internal resistance growth, extending battery cycle life and improving battery capacity retention capabilities.
Smart Images

Figure SMS_13 
Figure HDA0004980378890000011
Abstract
Description
[0001] This application is a divisional application of the invention application with international application number PCT / EP2018 / 053580, Chinese national application number 201880012071.X, and invention title "Lithium Mixed Oxide Particles Encapsulated with Alumina and Titanium Dioxide and Method of Using the Same" filed on February 13, 2018. Technical Field
[0002] The present invention relates to a method for preparing mixed lithium oxide particles coated with alumina and titanium dioxide. The present invention also relates to specific alumina- and titanium dioxide-coated mixed lithium oxide particles. Background Art
[0003] It is known that coating mixed lithium oxide particles with metal oxides can inhibit undesirable reactions between the electrolyte and the electrode material.
[0004] WO2012022624 discloses a method for preparing (Ni x Mn y Co z ) a (Al2O3) b where 0.3 ≤ x ≤ 0.9, 0 ≤ y ≤ 0.45, 0 < z ≤ 0.4, x + y + z = 1 and a + 2b = 1, b ≤ 0.4, and the precursor compound [Ni x Mn y Co z OOH in dry form is contacted with alumina (such as pyrolytic alumina) under shear conditions. This forms a solid coating of alumina. Subsequent heat treatment gives the product.
[0005] WO00 / 70694 discloses mixed lithium oxide particles coated with oxides or mixed oxides of Zr, Al, Zn, Y, Ce, Sn, Ca, Si, Sr, Mg, and Ti. They are obtained by suspending the uncoated particles in an organic solvent, mixing the suspension with a solution of a hydrolyzable metal compound and a hydrolysis solution, and then filtering, drying, and calcining the coated particles.
[0006] There is a similar disclosure in US2004091779. Here, the composition is Li 1+x Ni α Mn β Co γ M' δ O 2-z X zThe cathode material, where M' = Mg, Zn, Al, Ga, B, Zr, Ti; X = F, S, Cl, I; 0 < x < 0.333, 0.2 ≤ α ≤ 0.6, 0.2 ≤ β ≤ 0.667, 0 ≤ γ ≤ 0.333, δ ≤ 0 ≤ 0.2, 0 < z < 0.5, is coated with one or more oxides of Al, Bi, Ga, Ge, In, Mg, Pb, Si, Sn, Ti, TI, Zn, Zr.
[0007] There is a similar disclosure in WO2011 / 031544. Here, the cathode material Li 1+x M 1-x O 2-z F z (where M is a metal other than Li and 0.01 < x < 0.3, 0 < z < 0.2) is coated with one or more metal oxides of Al2O3, Bi2O3, B2O3, ZrO2, MgO, Cr2O3, MgAl2O4, Ga2O3, SiO2, SnO2, CaO2, SrO, BaO, TiO2, Fe2O3, MoO3, MoO2, CeO2, La2O3, ZnO.
[0008] WO2014 / 142803 claims a method for depositing an oxide coating on an inorganic substrate, where an aqueous composition containing a tetraalkylammonium polyoxyanion and lithium hydroxide is deposited on the surface of the inorganic substrate and heat-treated until the lithium polyoxyanion has been converted to an oxide. The tetraalkylammonium polyoxyanion includes those of the general formula A x O y z- where A is a transition metal or a metal or metalloid selected from Al, Si, B, Ga, Ge, As, Sn, Sb, Tl, Pb, and Bi or a combination thereof, where O is an oxygen atom and the values of x, y, and z depend on the valence of A in the polyoxyanion, and y > x.
[0009] US2015340689 discloses an active cathode material having a core of a material capable of intercalating and deintercalating lithium, and providing a coating of nanoscale zirconia and a further coating of oxides of Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr or a mixture of these.
[0010] WO2005011044 discloses a cathode material obtained by dry mixing lithium oxide with an electro-inert nanoscale metal oxide, and the metal oxide is selected from the group consisting of Al2O3, SiO2, MgO, TiO2, SnO2, B2O3, Fe2O3, ZrO2, and mixtures thereof.
[0011] It is known to coat cathode materials for lithium-ion batteries with metal oxides (including mixtures of metal oxides). The coatings can reduce unwanted reactions of the electrolyte with the cathode material. However, improving these coatings remains a challenge. Summary of the invention
[0012] The present invention claims a process in which a specific mixture of aluminium oxide and titanium dioxide is used as coating material.Although the cited prior art includes a mixture of aluminium oxide and titanium dioxide, it does not give any indication of a process using the specific mixture.
[0013] The present invention provides a method for preparing coated mixed lithium oxide particles, wherein mixed lithium oxide particles and a mixture comprising aluminum oxide and titanium dioxide are dry mixed under shear conditions by a mixing unit having a specific power of 0.1-1 kW, preferably 0.2-0.8 kW / kg of the total of mixed lithium oxide particles and the mixture used.
[0014] Dry mixing is understood to mean that no liquid is used. However, there may be moisture adhering to the raw materials or these raw materials may include water of crystallization.
[0015] If the specific power is less than 0.1 kW / kg of the total of the mixed lithium oxide particles and the mixture used, this may result in an uneven coating that is not firmly bonded to the core.
[0016] A specific power of more than 1 kW / kg of the mixed lithium oxide particles and the mixture used in total leads to poor electrochemical properties. In addition, there is a risk that the coating becomes brittle and tends to crack.
[0017] The power of the mixing unit can vary within wide limits. Thus, mixing units with a power of 0.1 to 5 kW can be used on the laboratory scale or mixing units with a power of 10 to 1000 kW can be used on the production scale.
[0018] The volume of the mixing unit can likewise be varied within wide limits. Thus, mixing units with a volume of 1 to 10 liters or mixing units with a volume of 0.1 to 2.5 m 3 A mixing unit is used on a production scale.
[0019] Preferably, in the method according to the invention, a forced mixer is used in the form of an intensive mixer with high-speed mixing means. It has been found that speeds of 10-30 ms -1 , preferably 15-25ms -1 The best results are obtained with mixing tools. Commercially available mixing units are known, for example, Henschel mixers or Eirich mixers.
[0020] The mixing time is preferably from 0.1 to 120 minutes, more preferably from 0.2 to 60 minutes, very preferably from 0.5 to 10 minutes.
[0021] The heat treatment may be followed by mixing. In the prior art, such treatment is envisaged in order to firmly bind the coating to the mixed lithium oxide particles. Generally, such treatment is not necessary in the method according to the invention, since the mixture of aluminum oxide and titanium dioxide has sufficient firmness on the mixed lithium oxide particles. Therefore, a preferred embodiment of the method according to the invention does not envisage any heat treatment after mixing.
[0022] In the context of the present invention, a mixture is understood to mean a physical mixture in which aluminum oxide particles are present together with titanium dioxide particles. The mixture may likewise be a mixed oxide in which the mixed oxide components are present in mixed form at the atomic level and may also have Ti—O—Al bonds. It has been found that physical mixtures show better results with regard to the stability of the coating.
[0023] The weight ratio of aluminum oxide to titanium dioxide is preferably selected to be 10:90-90:10, more preferably 30:70-70:30.
[0024] It has been found that when the BET surface area of the alumina particles is greater than 50 m 2 / g, more preferably at least 100m 2 / g, and most preferably 100-150m 2 / g, the best results regarding adhesion on the mixed lithium oxide particles were obtained.
[0025] The aluminum oxide particles used in the method according to the invention are preferably those selected from the group consisting of gamma-, theta-, delta-alumina and mixtures thereof. These aluminum oxide phases lead to good adhesion on the mixed lithium oxide particles. In contrast, alpha-aluminum oxide particles produce worse results. If the aluminum oxide phases are present in the form of a mixture, they can take the form of phases that are firmly fused to one another within the particles.
[0026] In the process according to the invention, the mixture contains not only aluminum oxide particles but also titanium dioxide particles. The titanium dioxide particles used preferably have a BET surface area of at least 40 m 2 / g, more preferably 40-100m 2 / g.
[0027] Preferably, the BET surface area of the aluminum oxide particles used is greater than the BET surface area of the titanium dioxide particles used.
[0028] In a particular embodiment of the method according to the invention, at least one of the types of particles of the alumina particles or titania particles is in the form of aggregated primary particles. More preferably, alumina particles and titania particles are used which are both in the form of aggregated primary particles.
[0029] These aggregated primary particles can be obtained in particular by pyrolysis. "Pyrolysis" is understood here to mean the hydrolysis of aluminum or titanium compounds in a flame produced by the reaction of a fuel gas, preferably hydrogen and oxygen. This first forms highly dispersed and non-porous primary particles, which melt to form aggregates in the later stages of the reaction, and these clusters further aggregate to produce agglomerates. When the aggregates are firmly fused to each other, the agglomerates can be completely or partially broken into aggregates under shear conditions.
[0030] The diameter of the primary particles can be estimated from the BET surface area and is about 10-25 nm in the case of pyrolyzed particles. The diameter of the aggregates is about 50-1000 nm and the diameter of the agglomerates is 1-2 μm.
[0031] The particles have hydroxyl groups on their surface. The particles thus produced have a purity of at least 99.5% by weight, usually at least 99.8% by weight. Pyrolysis powders in the form of aggregated particles are commercially available, for example Alu 65, Alu C. Alu 130, TiO2P25 and P90, both from Evonik Resource Efficiency GmbH.
[0032] The mixed lithium oxides preferably used in the process according to the invention are selected from lithium-cobalt oxide, lithium-nickel-manganese-cobalt oxide, lithium-nickel-cobalt-aluminum oxide, lithium-manganese oxide, lithium-nickel-manganese oxide, or mixtures of these.
[0033] The proportion of (aluminum oxide + titanium dioxide) is preferably 0.05% by weight to 5% by weight, more preferably 0.1% by weight to 2% by weight, based in each case on the sum of the mixed lithium oxide particles and (aluminum oxide + titanium dioxide). If the proportion is less than 0.05% by weight, complete coating of the mixed lithium oxide particles cannot be ensured. In the case of exceeding 5% by weight, no additional effect is observed.
[0034] The invention also provides coated mixed lithium oxide particles obtainable by the process of the invention.
[0035] The present invention also provides coated mixed lithium oxide particles comprising a mixture of aluminum oxide and titanium dioxide as coating material, wherein the aluminum oxide and titanium dioxide are in the form of aggregated primary particles and the weight ratio of aluminum oxide to titanium dioxide is 10:90-90:10, preferably 30:70-70:30.
[0036] The coated mixed lithium oxide particles preferably have a diameter of 2-20 μm, and the coating has a thickness of 50-500 nm.
[0037] Finally, the present invention also provides a battery cell comprising the coated mixed lithium oxide particles. DETAILED DESCRIPTION
[0038] Example
[0039] raw material
[0040] Alu 130, BET surface area 130 ± 20 m 2 / g; Al2O3 content ≥99.8% by weight.
[0041] TiO2P25, BET surface area 50±15m 2 / g; titanium dioxide content ≥99.5% by weight, all from Evonik Resource Efficiency GmbH.
[0042] Lithium cobalt oxide powder, LCO LC412; average diameter d 50 =11±2μm (by laser diffraction), BET surface area <0.5m 2 / g;Gelon.
[0043] Example:
[0044] The 5g Alu 130 and 5g TiO2P25 was mixed with low energy input. 990 g of LCO LC412 were added to this mixture and the mixture was then mixed in a 0.25 kW powerful laboratory mixer for 1 minute.
[0045] Specific power = 0.25kW / kg; specific energy = 0.042kWh / kg = 15kJ / kg.
[0046] Ratio of (alumina + titanium dioxide) = 1 wt%
[0047] The speed of the hybrid tool is 22ms -1 .
[0048] Coated LCO powders with a layer thickness of 100-200 nm were obtained.
[0049] Figure 1 The effect of the coating on the battery capacity as a function of the number of cycles is shown. This will (A) be obtained by the method according to the invention with a 50:50 Alu 130 and LCO powder coated with a mixture of TiO2P25 and (B) only coated with Alu 130 LCO powder and (C) uncoated LCO powder were compared.
[0050] Axis display: x-axis = number of cycles; y-axis = normalized battery capacity in %;
[0051] Charging switch voltage = 4.4V; temperature = 45°C.
[0052] (A) shows higher battery capacity over the entire cycle range.
[0053] It is known that cycling of a battery produces decomposition products that can increase the internal resistance of the battery and its temperature. Therefore, the DCIR value should be very low and relatively stable over hundreds of cycles. In the case of both uncoated LCO and Al2O3 coated LCO, it seems that a layer that is always less permeable to current grows around the active cathode material, which manifests itself as a higher DCIR.
[0054] The table shows that this effect is less pronounced in the case of the mixed lithium oxide particles which have been coated according to the invention.
[0055] Table: Electrochemical cells with and without coating in Ohm·cm 2 Internal resistance of the meter (DCIR*)
[0056]
[0057] * DC internal resistance; pouch full-cell tests; voltage range: 3.0-4.4V; temperature = 45°C; formed at 0.02C / 0.3C; cycled at 1C / 1C; electrode size: 25cm 2 .
Claims
1. A method for preparing coated mixed lithium oxide particles, characterized in that The mixed lithium oxide particles and a mixture comprising aluminum oxide and titanium dioxide, each in the form of aggregated primary particles, are dry-mixed under shearing conditions by a mixing unit having a specific power of 0.1-1 kW per kg of the mixed lithium oxide particles and the total of the mixture used.
2. The method according to claim 1, characterized in that The power of the mixing unit is 0.1-1000kW.
3. The method according to claim 1 or 2, characterized in that The volume of the mixing unit used is from 1 liter to 2.5m 3 .
4. The method according to claims 1 to 3, characterized in that The speed of the hybrid tool is 10-30ms -1 .
5. The method according to claims 1 to 4, characterized in that The duration of mixing is from 0.1 minutes to 120 minutes.
6. The method according to claims 1 to 5, characterized in that The weight ratio of alumina to titanium dioxide is 10:90-90:
10.
7. The method according to claims 1 to 6, characterized in that Use a BET surface area of at least 115m 2 / g of alumina particles.
8. The method according to claims 1 to 7, characterized in that The alumina particles are selected from the group consisting of γ-alumina, θ-alumina, δ-alumina and mixtures thereof.
9. The method according to claims 1 to 8, characterized in that Use a BET surface area of at least 40m 2 / g of titanium dioxide particles.
10. The method according to claims 1 to 9, characterized in that The BET surface area of the alumina particles used is greater than the BET surface area of the titania particles used.
11. The method according to claims 1 to 10, characterized in that The mixed lithium oxide particles are selected from the group consisting of lithium-cobalt oxide, lithium-nickel-manganese-cobalt oxide, lithium-nickel-cobalt-aluminum oxide, lithium-manganese oxide, lithium-nickel-manganese oxide or mixtures thereof.
12. The method according to claims 1 to 11, characterized in that The proportion of (aluminum oxide + titanium dioxide) is 0.05% to 5% by weight, based on the sum of the mixed lithium oxide particles and (aluminum oxide + titanium dioxide).
13. Coated mixed lithium oxide particles comprising a mixture of aluminum oxide and titanium dioxide as coating material, characterized in that The alumina and the titania are in the form of aggregated primary particles, and the weight ratio of the alumina to the titania is 10:90 to 90:
10.
14. A battery cell comprising the coated mixed lithium oxide particles according to claim 13.