Electrochemical device and electronic device
By using a positive electrode active substance containing tungsten and fluorovinyl carbonate electrolyte in lithium-ion batteries, combined with an insulating layer and primer of aluminum, the performance deterioration and safety hazards of lithium-ion batteries under low temperature conditions are solved. , achieving higher low temperature magnification and high temperature and high pressure safety.
Patent Information
- Application Number
- CN202411070203.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-29
- Publication Date
- 2024-11-19
AI Technical Summary
Existing lithium-ion batteries have severe performance declines under low temperature conditions and have safety risks, such as the risk of combustion or explosion caused by overcharge and discharge, and traditional improvements such as the addition of aromatic compounds or inorganic coatings will affect the low temperature performance and energy density. .
Using the positive electrode active substance containing tungsten elements and the electrolyte containing fluorinated vinyl carbonate, the lattice stability and interface stability are improved through the tungsten elements, the ionic and electronic impedance of the surface of the positive electrode active substance is reduced, and the insulating layer of the aluminum element is combined with Primer, optimizes the low temperature magnification and high temperature and high pressure safety of electrochemical devices.
It significantly improves the low-temperature rate performance and high-temperature and high-pressure safety of lithium-ion batteries, reduces particle cracks and crushing, improves the safety of short circuits and thermal abuse, and avoids safety accidents caused by overcharge and discharge.
Smart Images

Figure BDA0004980685120000101 
Figure BDA0004980685120000111 
Figure BDA0004980685120000112
Abstract
Description
[0001] This application is a divisional application of the invention patent with application number 202180012321.1 (international application number: PCT / CN2021 / 142398) filed on December 29, 2021, and the invention name is "Electrochemical device and electronic device". Technical Field
[0002] The present application relates to the field of energy storage, and in particular to an electrochemical device and an electronic device, in particular a lithium-ion battery. Background Art
[0003] With the development of technology and the increasing demand for mobile devices, people's demand for electrochemical devices (e.g., lithium-ion batteries) under different usage conditions has increased significantly, which has put forward higher requirements on the performance of lithium-ion batteries, which is reflected in: higher capacity, suitable cycle life, good high temperature performance, good low temperature performance, good high rate discharge performance, anti-overcharge performance and safety, etc.
[0004] Since the potential difference between the positive and negative active materials used in lithium-ion batteries is generally above 2 V, only organic solvent electrolyte systems with wider electrochemical windows can be used. However, these lithium-ion batteries are not suitable for use under extreme working conditions (e.g., low temperature), which poses potential safety risks.
[0005] In view of the above, there is a real need to provide an electrochemical device and an electronic device with improved low temperature performance and safety. Summary of the invention
[0006] The embodiments of the present application solve the problems existing in the prior art to some extent by providing an electrochemical device and an electronic device with improved low temperature performance and safety.
[0007] In one aspect of the present application, the present application provides an electrochemical device comprising: a positive electrode, a negative electrode and an electrolyte, the positive electrode comprising a positive electrode collector and a positive electrode active material layer formed on the positive electrode collector, the positive electrode active material layer comprising a positive electrode active material, the positive electrode active material containing a tungsten element, and the electrolyte comprising fluoroethylene carbonate.
[0008] According to an embodiment of the present application, based on the mass of the positive electrode active material, the content of the tungsten element is x%; based on the mass of the electrolyte, the content of the fluoroethylene carbonate is a%; x and a satisfy: 1≤a / x≤70.
[0009] According to an embodiment of the present application, based on the mass of the positive electrode active material, the content of the tungsten element is x%, and 0.05≤x≤1.
[0010] According to an embodiment of the present application, based on the mass of the electrolyte, the content of the fluoroethylene carbonate is a%, and 0.1≤a≤7.
[0011] According to an embodiment of the present application, the electrolyte further includes a compound having a sulfur-oxygen double bond, and based on the mass of the electrolyte, the content of the compound having a sulfur-oxygen double bond is b%, and 0.01≤b≤5.
[0012] According to an embodiment of the present application, based on the mass of the positive electrode active material, the content of the tungsten element is x%, and b and x satisfy: 1≤b / x≤50.
[0013] According to an embodiment of the present application, the positive electrode further includes an insulating layer, and the insulating layer is formed on the positive electrode collector and overlaps with the positive electrode active material layer in a partial area, or the insulating layer is formed on the positive electrode collector and does not overlap with the positive electrode active material layer.
[0014] According to an embodiment of the present application, the insulating layer includes a compound containing an aluminum element, and based on the mass of the insulating layer, the content of the aluminum element is y1%; based on the mass of the positive electrode active material, the content of the tungsten element is x%; and y1 and x satisfy: 50≤y1 / x≤650.
[0015] According to an embodiment of the present application, the value range of y1 is 30 to 65.
[0016] According to an embodiment of the present application, the positive electrode further includes a primer layer formed between the positive electrode current collector and the positive electrode active material layer.
[0017] According to an embodiment of the present application, the undercoat layer includes an aluminum element, and the content of the aluminum element is y2% based on the mass of the undercoat layer; the content of the tungsten element is x% based on the mass of the positive electrode active material; and y2 and x satisfy: 20≤y2 / x≤550.
[0018] According to an embodiment of the present application, the value range of y2 is 20 to 50.
[0019] According to an embodiment of the present application, the electrolyte also includes at least one of succinonitrile, adiponitrile, ethylene glycol di(2-cyanoethyl) ether, 1,3,6-hexanetrinitrile, 1,2,3-tri(2-cyanoethoxy)propane, 1,3-propanesultone, vinyl sulfate, vinylene carbonate or 1-propylphosphoric acid cyclic anhydride.
[0020] According to an embodiment of the present application, the positive electrode active material includes lithium nickel cobalt manganese oxide.
[0021] In another aspect of the present application, the present application provides an electronic device, which includes the electrochemical device according to the present application.
[0022] The tungsten-containing positive electrode active material used in the present application has high lattice stability, which can significantly improve the safety of the electrochemical device under high temperature and high pressure. When used in combination with an electrolyte including fluoroethylene carbonate, the low-temperature rate performance of the electrochemical device can be significantly improved.
[0023] Additional aspects and advantages of the embodiments of the present application will be described, shown, or explained in part in the subsequent description through implementation of the embodiments of the present application. DETAILED DESCRIPTION
[0024] The embodiments of the present application will be described in detail below. The embodiments of the present application should not be interpreted as limiting the present application.
[0025] Unless expressly stated otherwise, the following terms used herein have the meanings indicated below.
[0026] In the detailed description and claims, a list of items connected by the term "at least one of" may mean any combination of the listed items. For example, if items A and B are listed, the phrase "at least one of A and B" means only A; only B; or A and B. In another example, if items A, B, and C are listed, the phrase "at least one of A, B, and C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may include a single element or multiple elements. Item B may include a single element or multiple elements. Item C may include a single element or multiple elements. The term "at least one of" has the same meaning as the term "at least one of."
[0027] The organic solvent electrolyte system used in traditional electrochemical devices (e.g., lithium-ion batteries) is easy to burn under extreme conditions (e.g., overcharge, overheating or overcooling), which poses a serious safety hazard. In addition, the negative active materials of lithium-ion batteries are usually graphite materials, silicon-carbon composite materials or silicon oxide materials. These materials have poor kinetic properties under low temperature conditions or high rate conditions, resulting in serious performance degradation of lithium-ion batteries. In addition, the low-temperature discharge performance of traditional lithium-ion batteries is poor, and their performance deteriorates severely below -10°C, and they cannot even discharge. The high-rate performance of traditional lithium-ion batteries is also poor. When they are continuously discharged at a rate of 5C, they will cause a high temperature rise due to untimely heat dissipation, and there is a risk of thermal runaway. At the same time, the abuse of user terminals may also cause lithium-ion batteries to be overcharged, causing safety accidents such as combustion and explosion.
[0028] Adding additives such as aromatic compounds such as fluorobenzene and biphenyl to the electrolyte is one of the means to solve the safety problem of lithium-ion batteries. However, these additives not only increase the impedance of the battery, but also cause a decrease in low-temperature performance. Safety can also be improved by providing an inorganic coating on the surface of the pole piece, but it will still lead to a loss of energy density or a decrease in low-temperature performance. The industry has added tungsten to the positive electrode material, the purpose of which is to change the surface energy of the material's microstructure, so that the material's cycle stability is greatly improved. However, no reports have been found on the improvement of safety by adding tungsten to the positive electrode material. In addition, it is generally believed that the use of fluoroethylene carbonate in the electrolyte is for negative electrode film formation and to reduce side reactions between the negative electrode and the electrolyte. Based on existing knowledge, it is impossible to predict the impact of the simultaneous use of a positive electrode active material containing tungsten and an electrolyte including fluoroethylene carbonate on the low-temperature rate and safety performance of the electrochemical device.
[0029] The present application solves the problems related to low-temperature rate and safety performance of electrochemical devices by using a positive electrode active material containing tungsten and an electrolyte including fluoroethylene carbonate. Doping tungsten in the positive electrode active material can effectively inhibit lattice distortion and improve lattice stability, thereby inhibiting the volume change of particles in the charge and discharge cycle under high or low temperature conditions to reduce particle cracks and breakage, and it can also improve interface stability. The use of an electrolyte including fluoroethylene carbonate can significantly reduce the ionic resistance and electronic resistance of the surface of the positive electrode active material. The specific combination of the positive electrode active material and the electrolyte of the present application can not only effectively improve the low-temperature rate performance of the electrochemical device, but also significantly improve the safety of the electrochemical device (for example, short circuit safety and thermal abuse safety, etc.).
[0030] I. Positive electrode
[0031] The positive electrode includes a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector. The positive electrode active material layer can be one layer or multiple layers. The positive electrode active material layer includes a positive electrode active material, and each layer of the multiple layers of positive electrode active material can contain the same or different positive electrode active materials.
[0032] A main feature of the electrochemical device of the present application is that the positive electrode active material contains tungsten element.
[0033] In some embodiments, based on the mass of the positive electrode active material, the content of the tungsten element is x%, and 0.05≤x≤1. In some embodiments, 0.01≤x≤0.5. In some embodiments, x is 0.05, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1 or in the range consisting of any two of the above values. When the content of tungsten in the positive electrode active material is within the above range, the low temperature rate performance and high temperature and high pressure safety of the electrochemical device can be further improved.
[0034] In some embodiments, the positive electrode further includes an insulating layer, and the insulating layer is formed on the positive electrode collector and overlaps with the positive electrode active material layer in a partial area, or the insulating layer is formed on the positive electrode collector and does not overlap with the positive electrode active material layer.
[0035] In some embodiments, the insulating layer includes a compound containing aluminum. In some embodiments, the compound containing aluminum includes ceramic aluminum oxide. When the insulating layer includes a compound containing aluminum, the low temperature rate performance and high temperature and high pressure safety of the electrochemical device can be further improved.
[0036] In some embodiments, based on the mass of the insulating layer, the content of the aluminum element is y1%, and y1 and x satisfy: 50≤y1 / x≤650. In some embodiments, 60≤y1 / x≤600. In some embodiments, 100≤y1 / x≤500. In some embodiments, 200≤y1 / x≤400. In some embodiments, y1 / x is 50, 60, 70, 80, 90, 100, 150, 200, 250, 300, 350, 400, 450, 500, 550, 600, 650 or is within the range of any two of the above values. When the content of the aluminum element in the insulating layer and the content of the tungsten element in the positive electrode active material satisfy the above relationship, the defects on the surface of the crystal structure of the positive electrode active material can be reduced, the continuous destruction of the passivation layer on the surface of the positive electrode active material during the charge and discharge cycle of the electrochemical device can be effectively suppressed, and the number of repairs can be reduced, thereby fully improving the interface stability of the positive electrode active material layer, thereby further improving the low temperature rate performance and high temperature and high pressure safety of the electrochemical device.
[0037] In some embodiments, the value range of y1 is 30 to 65. In some embodiments, the value range of y1 is 40 to 60. In some embodiments, y1 is 30, 35, 40, 45, 50, 55, 60, 65 or in a range consisting of any two of the above values. When the content of aluminum in the insulating layer is within the above range, the low temperature rate performance and high temperature and high pressure safety of the electrochemical device can be further improved.
[0038] In some embodiments, the positive electrode further includes a primer layer formed between the positive electrode current collector and the positive electrode active material layer.
[0039] In some embodiments, the primer layer includes aluminum. In some embodiments, the primer layer includes ceramic aluminum oxide. When the primer layer includes a compound containing aluminum, the low temperature rate performance and high temperature and high pressure safety of the electrochemical device can be further improved.
[0040] In some embodiments, based on the mass of the undercoat layer, the content of the aluminum element is y2%, and y2 and x satisfy: 20≤y2 / x≤550. In some embodiments, 50≤y2 / x≤500. In some embodiments, 100≤y2 / x≤400. In some embodiments, 200≤y2 / x≤400. In some embodiments, y2 / x is 20, 30, 40, 50, 100, 150, 200, 250, 300, 350, 400, 450, 500, 550 or is within the range consisting of any two of the above values. When the content of the aluminum element in the undercoat layer and the content of the tungsten element in the positive electrode active material satisfy the above relationship, the positive electrode interface stability during the charge and discharge cycle of the electrochemical device can be effectively suppressed, thereby further improving the low temperature rate performance and high temperature and high pressure safety of the electrochemical device.
[0041] In some embodiments, y2 is in the range of 20 to 50. In some embodiments, y2 is in the range of 20 to 35. In some embodiments, y2 is 20, 25, 30, 35, 40, 45, 50 or in the range consisting of any two of the above values. When the content of aluminum in the primer layer is within the above range, the low temperature rate performance and high temperature and high pressure safety of the electrochemical device can be further improved.
[0042] In some embodiments, the positive electrode active material comprises lithium cobalt oxide. In some embodiments, the positive electrode active material comprises lithium nickel cobalt manganese oxide. Compared with lithium cobalt oxide, after tungsten is added to lithium nickel cobalt manganese oxide, the crystal structure is more stable, and the improvement of the low temperature rate performance and high temperature and high pressure safety of the electrochemical device is more significant.
[0043] In some embodiments, a substance with a different composition from that of the positive electrode active material may be attached to the surface of the above-mentioned positive electrode active material. Examples of surface-attached substances may include, but are not limited to: oxides such as aluminum oxide, silicon dioxide, titanium dioxide, zirconium oxide, magnesium oxide, calcium oxide, boron oxide, antimony oxide, bismuth oxide, etc.; sulfates such as lithium sulfate, sodium sulfate, potassium sulfate, magnesium sulfate, calcium sulfate, aluminum sulfate, etc.; carbonates such as lithium carbonate, calcium carbonate, magnesium carbonate, etc.; carbon, etc. By attaching substances to the surface of the positive electrode active material, the oxidation reaction of the electrolyte on the surface of the positive electrode active material can be suppressed, and the life of the electrochemical device can be improved. When the amount of surface-attached substances is too small, the effect cannot be fully manifested; when the amount of surface-attached substances is too much, it will hinder the entry and exit of lithium ions, so that the resistance sometimes increases. In this application, the positive electrode active material having a substance with a different composition attached to the surface of the positive electrode active material is also referred to as a "positive electrode active material."
[0044] In some embodiments, the shape of the positive electrode active material particles includes, but is not limited to, block, polyhedron, sphere, ellipsoid, plate, needle and column, etc. In some embodiments, the positive electrode active material particles include primary particles, secondary particles or a combination thereof. In some embodiments, the primary particles can be agglomerated to form secondary particles.
[0045] There is no limitation on the type of positive electrode conductive material, and any known conductive material can be used. Examples of positive electrode conductive materials may include, but are not limited to, graphite such as natural graphite and artificial graphite; carbon black such as acetylene black; carbon materials such as amorphous carbon such as needle coke; carbon nanotubes; graphene, etc. The above positive electrode conductive materials may be used alone or in any combination.
[0046] There is no particular restriction on the type of positive electrode binder used in the manufacture of the positive electrode active material layer. In the case of a coating method, any material that can be dissolved or dispersed in the liquid medium used in the manufacture of the electrode can be used. Examples of positive electrode binders may include, but are not limited to, one or more of the following: resin polymers such as polyethylene, polypropylene, polyethylene terephthalate, polymethyl methacrylate, polyimide, aromatic polyamide, cellulose, and nitrocellulose; rubber polymers such as styrene-butadiene rubber (SBR), nitrile rubber (NBR), fluororubber, isoprene rubber, polybutadiene rubber, and ethylene-propylene rubber; styrene-butadiene-styrene block copolymers or their hydrogenates, ethylene-propylene-diene terpolymers (EPDM), Thermoplastic elastomer polymers such as styrene·ethylene·butadiene·ethylene copolymers, styrene·isoprene·styrene block copolymers or their hydrogenated products; soft resin polymers such as syndiotactic-1,2-polybutadiene, polyvinyl acetate, ethylene·vinyl acetate copolymers, propylene·α-olefin copolymers; fluorine-based polymers such as polyvinylidene fluoride (PVDF), polytetrafluoroethylene, fluorinated polyvinylidene fluoride, polytetrafluoroethylene·ethylene copolymers; polymer compositions having ion conductivity of alkali metal ions (especially lithium ions), etc. The above positive electrode binders can be used alone or in any combination.
[0047] There is no limitation on the type of solvent used to form the positive electrode slurry, as long as it is a solvent that can dissolve or disperse the positive electrode active material, the conductive material, the positive electrode binder and the thickener used as needed. Examples of solvents used to form the positive electrode slurry may include any of aqueous solvents and organic solvents. Examples of aqueous media may include, but are not limited to, water and mixed media of alcohol and water. Examples of organic media may include, but are not limited to, aliphatic hydrocarbons such as hexane; aromatic hydrocarbons such as benzene, toluene, xylene, methylnaphthalene; heterocyclic compounds such as quinoline and pyridine; ketones such as acetone, methyl ethyl ketone, and cyclohexanone; esters such as methyl acetate and methyl acrylate; amines such as diethylenetriamine and N,N-dimethylaminopropylamine; ethers such as diethyl ether, propylene oxide, and tetrahydrofuran (THF); amides such as N-methylpyrrolidone (NMP), dimethylformamide, and dimethylacetamide; aprotic polar solvents such as hexamethylphosphoramide and dimethyl sulfoxide, etc.
[0048] Thickeners are generally used to adjust the viscosity of the slurry. In the case of using an aqueous medium, a thickener and a styrene-butadiene rubber (SBR) emulsion can be used for slurrying. The type of thickener is not particularly limited, and examples thereof may include, but are not limited to, carboxymethyl cellulose, methyl cellulose, hydroxymethyl cellulose, ethyl cellulose, polyvinyl alcohol, oxidized starch, phosphorylated starch, casein, and salts thereof. The above thickeners may be used alone or in any combination.
[0049] The type of positive electrode current collector is not particularly limited, and it can be any material known to be suitable for use as a positive electrode current collector. Examples of positive electrode current collectors may include, but are not limited to, metal materials such as aluminum, stainless steel, nickel plating, titanium, tantalum, and carbon materials such as carbon cloth and carbon paper. In some embodiments, the positive electrode current collector is a metal material. In some embodiments, the positive electrode current collector is aluminum.
[0050] In order to reduce the electronic contact resistance between the positive electrode current collector and the positive electrode active material layer, the surface of the positive electrode current collector may include a conductive additive. Examples of the conductive additive may include, but are not limited to, carbon and precious metals such as gold, platinum, and silver.
[0051] The positive electrode can be made by forming a positive electrode active material layer containing a positive electrode active material and a binder on a current collector. The manufacture of a positive electrode using a positive electrode active material can be carried out by a conventional method, that is, the positive electrode active material and the binder, as well as the conductive material and the thickener as required, are dry-mixed to form a sheet, and the obtained sheet is pressed onto the positive electrode current collector; or these materials are dissolved or dispersed in a liquid medium to form a slurry, and the slurry is applied to the positive electrode current collector and dried to form a positive electrode active material layer on the current collector, thereby obtaining a positive electrode.
[0052] In some embodiments, the mass fraction of the positive electrode active material in the positive electrode active material layer is 95%, preferably 96%, and more preferably 97%. In some embodiments, the mass fraction of the positive electrode active material in the positive electrode active material layer is 98%. In some embodiments, the mass fraction of the positive electrode active material in the positive electrode active material layer is 99%. When the mass fraction of the positive electrode active material in the positive electrode active material layer is within the above range, the energy density of the electrochemical device can be significantly improved.
[0053] When the positive electrode active material is a primary particle, the average particle size of the positive electrode active material refers to the primary particle size of the positive electrode active material particles. When the primary particles of the positive electrode active material particles aggregate to form secondary particles, the average particle size of the positive electrode active material particles refers to the secondary particle size of the positive electrode active material particles.
[0054] In some embodiments, the average particle size of the positive electrode active material is D μm, and the value of D ranges from 5 to 30. In some embodiments, the value of D ranges from 10 to 25. In some embodiments, the value of D ranges from 12 to 20. In some embodiments, D is 5, 7, 9, 10, 12, 15, 18, 20, 25, 30 or in the range consisting of any two of the above values.
[0055] When the average particle size of the positive electrode active material is within the above range, a positive electrode active material with a high tap density can be obtained, which can suppress the reduction of the performance of the electrochemical device, and can prevent the generation of stripes and other problems during the preparation of the positive electrode of the electrochemical device (i.e., when the positive electrode active material, the conductive material and the adhesive are slurried with a solvent and applied in a thin film). By mixing two or more positive electrode active materials with different average particle sizes, the filling property during the preparation of the positive electrode can be further improved.
[0056] The average particle size of the positive electrode active material can be measured using a laser diffraction / scattering particle size distribution measuring device: when using LA-920 manufactured by HORIBA as a particle size distribution meter, a 0.1% sodium hexametaphosphate aqueous solution is used as the dispersion medium used in the measurement, and the refractive index is set to 1.24 after 5 minutes of ultrasonic dispersion. The average particle size of the positive electrode active material can also be measured by a laser diffraction particle size analyzer (Shimadzu SALD-2300) and a scanning electron microscope (ZEISS EVO18, the number of samples is not less than 100).
[0057] II. Electrolyte
[0058] The electrolyte used in the electrochemical device of the present application includes an electrolyte and a solvent for dissolving the electrolyte. Another main feature of the electrochemical device of the present application is that the electrolyte includes fluoroethylene carbonate.
[0059] In some embodiments, based on the mass of the electrolyte, the content of the fluoroethylene carbonate is a%, and x and a satisfy: 1≤a / x≤70. In some embodiments, 2≤a / x≤60. In some embodiments, 5≤a / x≤50. In some embodiments, 10≤a / x≤30. In some embodiments, a / x is 1, 2, 3, 5, 8, 10, 20, 30, 40, 50, 60, 70 or is within the range consisting of any two of the above values. When the content of fluoroethylene carbonate in the electrolyte and the content of tungsten in the positive electrode active material satisfy the above relationship, the defects on the surface of the crystal structure of the positive electrode active material can be reduced, the continuous destruction of the passivation layer on the surface of the positive electrode active material during the charge and discharge cycle of the electrochemical device can be effectively suppressed, and the number of repairs can be reduced, thereby fully improving the interfacial stability of the positive electrode active material layer, thereby further improving the low temperature rate performance and high temperature and high pressure safety of the electrochemical device.
[0060] In some embodiments, 0.1≤a≤7. In some embodiments, 0.1≤a≤5. In some embodiments, 0.5≤a≤3. In some embodiments, 1≤a≤2. In some embodiments, a is 0.1, 0.2, 0.5, 1, 2, 3, 4, 5, 6, 7 or in a range consisting of any two of the above values. When the content of fluoroethylene carbonate in the electrolyte is within the above range, the low temperature rate performance and high temperature and high pressure safety of the electrochemical device are further improved.
[0061] In some embodiments, the electrolyte further comprises a compound having a sulfur-oxygen double bond.
[0062] In some embodiments, based on the mass of the electrolyte, the content of the compound having a sulfur-oxygen double bond is b%, and 0.01≤b≤5. In some embodiments, 0.01≤b≤2. In some embodiments, 0.05≤b≤1. In some embodiments, 0.1≤b≤0.5. In some embodiments, x is 0.01, 0.02, 0.05, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5 or in a range consisting of any two of the above values. When the content of the compound having a sulfur-oxygen double bond in the electrolyte is within the above range, the low temperature rate performance and high temperature and high pressure safety of the electrochemical device are further improved.
[0063] In some embodiments, b and x satisfy: 1≤b / x≤50. In some embodiments, 2≤b / x≤20. In some embodiments, 5≤b / x≤10. In some embodiments, b / x is 1, 2, 3, 5, 8, 10, 20, 30, 40, 50 or is within the range consisting of any two of the above values. When the content of the sulfur-oxygen double bond compound in the electrolyte and the content of the tungsten element in the positive electrode active material satisfy the above relationship, the defects on the surface of the crystal structure of the positive electrode active material can be reduced, and the continuous destruction of the passivation layer on the surface of the positive electrode active material during the charge and discharge cycle of the electrochemical device can be effectively suppressed, and the number of repairs can be reduced, thereby fully improving the interface stability of the positive electrode active material layer, thereby further improving the low temperature rate performance and high temperature and high pressure safety of the electrochemical device.
[0064] In some embodiments, the compound containing a sulfur-oxygen double bond comprises at least one of the following compounds: cyclic sulfate, chain sulfate, chain sulfonate, cyclic sulfonate, chain sulfite, or cyclic sulfite.
[0065] In some embodiments, the cyclic sulfate includes, but is not limited to, one or more of the following: 1,2-ethylene glycol sulfate, 1,2-propylene glycol sulfate, 1,3-propylene glycol sulfate, 1,2-butylene glycol sulfate, 1,3-butylene glycol sulfate, 1,4-butylene glycol sulfate, 1,2-pentanediol sulfate, 1,3-pentanediol sulfate, 1,4-pentanediol sulfate, 1,5-pentanediol sulfate, and the like.
[0066] In some embodiments, the chain sulfate ester includes, but is not limited to, one or more of the following: dimethyl sulfate, ethyl methyl sulfate, diethyl sulfate, and the like.
[0067] In some embodiments, the linear sulfonate includes, but is not limited to, one or more of the following: fluorosulfonates such as methyl fluorosulfonate and ethyl fluorosulfonate, methyl methanesulfonate, ethyl methanesulfonate, butyl dimethanesulfonate, methyl 2-(methylsulfonyloxy)propionate and ethyl 2-(methylsulfonyloxy)propionate, and the like.
[0068] In some embodiments, the cyclic sulfonate includes, but is not limited to, one or more of the following: 1,3-propane sultone, 1-fluoro-1,3-propane sultone, 2-fluoro-1,3-propane sultone, 3-fluoro-1,3-propane sultone, 1-methyl-1,3-propane sultone, 2-methyl-1,3-propane sultone, 3-methyl-1,3-propane sultone, 1-propylene-1,3-sultone, 2-propylene-1,3-sultone, 1-fluoro-1-propylene-1,3-sultone, 2-fluoro-1-propylene-1,3-sultone, 3-fluoro-1-propylene-1,3-sultone Esters, 1-fluoro-2-propylene-1,3-sultone, 2-fluoro-2-propylene-1,3-sultone, 3-fluoro-2-propylene-1,3-sultone, 1-methyl-1-propylene-1,3-sultone, 2-methyl-1-propylene-1,3-sultone, 3-methyl-1-propylene-1,3-sultone, 1-methyl-2-propylene-1,3-sultone, 2-methyl-2-propylene-1,3-sultone, 3-methyl-2-propylene-1,3-sultone, 1,4-butanesultone, 1,5-pentanesultone, methylene methanedisulfonate and ethylene methanedisulfonate, etc.
[0069] In some embodiments, the linear sulfite includes, but is not limited to, one or more of the following: dimethyl sulfite, ethyl methyl sulfite, diethyl sulfite, and the like.
[0070] In some embodiments, the cyclic sulfite includes, but is not limited to, one or more of the following: 1,2-ethylene glycol sulfite, 1,2-propylene glycol sulfite, 1,3-propylene glycol sulfite, 1,2-butylene glycol sulfite, 1,3-butylene glycol sulfite, 1,4-butylene glycol sulfite, 1,2-pentanediol sulfite, 1,3-pentanediol sulfite, 1,4-pentanediol sulfite, 1,5-pentanediol sulfite, and the like.
[0071] In some embodiments, the compound containing a sulfur-oxygen double bond comprises a compound of formula I:
[0072]
[0073] in:
[0074] W is selected from
[0075] L is each independently selected from a single bond or a methylene group;
[0076] m is 1, 2, 3 or 4;
[0077] n is 0, 1 or 2; and
[0078] p is 0, 1, 2, 3, 4, 5 or 6.
[0079] In some embodiments, the compound of formula I comprises at least one of the following:
[0080]
[0081] In some embodiments, the bicyclic sultone comprises a compound of Formula II:
[0082]
[0083] wherein A1, A2, A3 and A4 are each independently selected from substituted or unsubstituted C1-3 alkylene, and when substituted, the substituent is selected from C1-5 alkyl, halogen or halogenated C1-5 alkyl.
[0084] In some embodiments, the compound of formula II comprises at least one of the following:
[0085]
[0086]
[0087] In some embodiments, the electrolyte further comprises at least one of succinonitrile, adiponitrile, ethylene glycol di(2-cyanoethyl) ether, 1,3,6-hexanetrinitrile, 1,2,3-tri(2-cyanoethoxy)propane, 1,3-propanesultone, vinyl sulfate, vinyl carbonate or 1-propylphosphoric acid cyclic anhydride. In some embodiments, the content of the above compounds is 0.1%-6% based on the mass of the electrolyte. In some embodiments, the content of the above compounds is 0.5%-5% based on the mass of the electrolyte. In some embodiments, the content of the above compounds is 1%-3% based on the mass of the electrolyte. These compounds help stabilize the interface between the positive electrode and the electrolyte, thereby further improving the overcharge resistance and safety of the electrochemical device under high temperature and high pressure.
[0088] In some embodiments, the electrolyte further comprises any non-aqueous solvent known in the prior art that can be used as a solvent for the electrolyte.
[0089] In some embodiments, the non-aqueous solvent includes, but is not limited to, one or more of the following: cyclic carbonates, chain carbonates, cyclic carboxylates, chain carboxylates, cyclic ethers, chain ethers, phosphorus-containing organic solvents, sulfur-containing organic solvents, and aromatic fluorine-containing solvents.
[0090] In some embodiments, examples of the cyclic carbonate may include, but are not limited to, one or more of the following: ethylene carbonate (EC), propylene carbonate (PC) and butylene carbonate. In some embodiments, the cyclic carbonate has 3-6 carbon atoms.
[0091] In some embodiments, examples of the linear carbonates may include, but are not limited to, one or more of the following: dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate (DEC), methyl n-propyl carbonate, ethyl n-propyl carbonate, di-n-propyl carbonate, etc. Examples of fluorine-substituted linear carbonates may include, but are not limited to, one or more of the following: bis(fluoromethyl) carbonate, bis(difluoromethyl) carbonate, bis(trifluoromethyl) carbonate, bis(2-fluoroethyl) carbonate, bis(2,2-difluoroethyl) carbonate, bis(2,2,2-trifluoroethyl) carbonate, 2-fluoroethyl methyl carbonate, 2,2-difluoroethyl methyl carbonate, and 2,2,2-trifluoroethyl methyl carbonate, etc.
[0092] In some embodiments, examples of the cyclic carboxylic acid ester may include, but are not limited to, one or more of the following: one or more of γ-butyrolactone and γ-valerolactone. In some embodiments, part of the hydrogen atoms of the cyclic carboxylic acid ester may be substituted with fluorine.
[0093] In some embodiments, examples of the chain carboxylic acid esters may include, but are not limited to, one or more of the following: methyl acetate, ethyl acetate, propyl acetate, isopropyl acetate, butyl acetate, sec-butyl acetate, isobutyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, isopropyl propionate, methyl butyrate, ethyl butyrate, propyl butyrate, methyl isobutyrate, ethyl isobutyrate, methyl valerate, ethyl valerate, methyl pivalate and ethyl pivalate, etc. In some embodiments, some hydrogen atoms of the chain carboxylic acid ester may be substituted by fluorine. In some embodiments, examples of fluorine-substituted chain carboxylic acid esters may include, but are not limited to, methyl trifluoroacetate, ethyl trifluoroacetate, propyl trifluoroacetate, butyl trifluoroacetate and 2,2,2-trifluoroethyl trifluoroacetate, etc.
[0094] In some embodiments, examples of the cyclic ether may include, but are not limited to, one or more of the following: tetrahydrofuran, 2-methyltetrahydrofuran, 1,3-dioxolane, 2-methyl1,3-dioxolane, 4-methyl1,3-dioxolane, 1,3-dioxane, 1,4-dioxane and dimethoxypropane.
[0095] In some embodiments, examples of the chain ether may include, but are not limited to, one or more of the following: dimethoxymethane, 1,1-dimethoxyethane, 1,2-dimethoxyethane, diethoxymethane, 1,1-diethoxyethane, 1,2-diethoxyethane, ethoxymethoxymethane, 1,1-ethoxymethoxyethane and 1,2-ethoxymethoxyethane, etc.
[0096] In some embodiments, examples of the phosphorus-containing organic solvent may include, but are not limited to, one or more of the following: trimethyl phosphate, triethyl phosphate, dimethyl ethyl phosphate, diethyl methyl phosphate, ethylidene methyl phosphate, ethylidene ethyl phosphate, triphenyl phosphate, trimethyl phosphite, triethyl phosphite, triphenyl phosphite, tris(2,2,2-trifluoroethyl) phosphate, and tris(2,2,3,3,3-pentafluoropropyl) phosphate, etc.
[0097] In some embodiments, examples of the sulfur-containing organic solvent may include, but are not limited to, one or more of the following: sulfolane, 2-methylsulfolane, 3-methylsulfolane, dimethyl sulfone, diethyl sulfone, ethyl methyl sulfone, methyl propyl sulfone, dimethyl sulfoxide, methyl methanesulfonate, ethyl methanesulfonate, methyl ethanesulfonate, ethyl ethanesulfonate, dimethyl sulfate, diethyl sulfate, and dibutyl sulfate. In some embodiments, some hydrogen atoms of the sulfur-containing organic solvent may be substituted by fluorine.
[0098] In some embodiments, the aromatic fluorine-containing solvent includes, but is not limited to, one or more of the following: fluorobenzene, difluorobenzene, trifluorobenzene, tetrafluorobenzene, pentafluorobenzene, hexafluorobenzene, and trifluoromethylbenzene.
[0099] In some embodiments, the solvent used in the electrolyte of the present application includes cyclic carbonates, chain carbonates, cyclic carboxylates, chain carboxylates, and combinations thereof. In some embodiments, the solvent used in the electrolyte of the present application includes an organic solvent selected from the group consisting of the following substances: ethylene carbonate, propylene carbonate, diethyl carbonate, ethyl propionate, propyl propionate, n-propyl acetate, ethyl acetate, and combinations thereof. In some embodiments, the solvent used in the electrolyte of the present application includes: ethylene carbonate, propylene carbonate, diethyl carbonate, ethyl propionate, propyl propionate, γ-butyrolactone, and combinations thereof.
[0100] In some embodiments, the electrolyte is not particularly limited, and any substance known as an electrolyte can be used arbitrarily. In the case of a lithium secondary battery, a lithium salt is generally used. Examples of electrolytes may include, but are not limited to, inorganic lithium salts such as LiPF6, LiBF4, LiClO4, LiAlF4, LiSbF6, LiWF7; lithium tungstates such as LiWOF5; lithium carboxylates such as HCO2Li, CH3CO2Li, CH2FCO2Li, CHF2CO2Li, CF3CO2Li, CF3CH2CO2Li, CF3CF2CO2Li, CF3CF2CF2CO2Li, CF3CF2CF2CF2CO2Li; lithium salts such as FSO3Li, CH3SO3Li 、CH2FSO3Li、CHF2SO3Li、CF3SO3Li、CF3CF2SO3Li、CF3CF2CF2SO3Li、CF3CF2CF2CF2SO3Li and other lithium sulfonate salts; LiN(FCO)2、LiN(FCO)(FSO2)、LiN(FSO2)2、LiN(FSO2)(CF3SO2)、LiN(CF3SO2)2、LiN(C2F5SO2)2、Cyclic 1,2-perfluoroethane bissulfonyl imide lithium、Cyclic 1,3-perfluoropropane bissulfonyl imide Lithium, LiN(CF3SO2)(C4F9SO2) and other imide lithium salts; LiC(FSO2)3, LiC(CF3SO2)3, LiC(C2F5SO2)3 and other methylated lithium salts; (malonate) borate lithium salts such as bis(malonate) borate and difluoro(malonate) borate lithium salts; (malonate) phosphate lithium salts such as tris(malonate) phosphate, difluorobis(malonate) phosphate, tetrafluoro(malonate) phosphate; and LiPF4(CF3)2, LiPF4(C2F5)2, Fluorine-containing organic lithium salts such as LiPF4(CF3SO2)2, LiPF4(C2F5SO2)2, LiBF3CF3, LiBF3C2F5, LiBF3C3F7, LiBF2(CF3)2, LiBF2(C2F5)2, LiBF2(CF3SO2)2, LiBF2(C2F5SO2)2; lithium oxalate borate salts such as lithium difluorooxalatoborate and lithium bis(oxalato)borate; lithium oxalate phosphate salts such as lithium tetrafluorooxalato phosphate, lithium difluorobis(oxalato) phosphate and lithium tris(oxalato) phosphate, etc.
[0101] In some embodiments, the electrolyte is selected from LiPF6, LiSbF6, FSO3Li, CF3SO3Li, LiN(FSO2)2, LiN(FSO2)(CF3SO2), LiN(CF3SO2)2, LiN(C2F5SO2)2, cyclic 1,2-perfluoroethane bissulfonyl imide lithium, cyclic 1,3-perfluoropropane bissulfonyl imide lithium, LiC(FSO2)3, LiC(CF3SO2)3, LiC(C2F5SO2)3, LiBF3CF3, LiBF3C2F5, LiPF3(CF3)3, LiPF3(C2F5)3, lithium difluorooxalatoborate, lithium bis(oxalate)borate or lithium difluorobis(oxalato)phosphate, which helps to improve the output power characteristics, high-rate charge and discharge characteristics, high-temperature storage characteristics and cycle characteristics of the electrochemical device.
[0102] The content of the electrolyte is not particularly limited as long as it does not impair the effect of the present application. In some embodiments, the total molar concentration of lithium in the electrolyte is greater than 0.3 mol / L, greater than 0.4 mol / L or greater than 0.5 mol / L. In some embodiments, the total molar concentration of lithium in the electrolyte is less than 3 mol / L, less than 2.5 mol / L or less than 2.0 mol / L. In some embodiments, the total molar concentration of lithium in the electrolyte is within the range formed by any two of the above values. When the electrolyte concentration is within the above range, there will not be too little lithium as a charged particle, and the viscosity can be kept within an appropriate range, thereby easily ensuring good conductivity.
[0103] When more than two electrolytes are used, the electrolyte includes at least one salt selected from the group consisting of monofluorophosphate, borate, oxalate and fluorosulfonate. In some embodiments, the electrolyte includes a salt selected from the group consisting of monofluorophosphate, oxalate and fluorosulfonate. In some embodiments, the electrolyte includes a lithium salt. In some embodiments, based on the weight of the electrolyte, the content of the salt selected from the group consisting of monofluorophosphate, borate, oxalate and fluorosulfonate is greater than 0.01% or greater than 0.1%. In some embodiments, based on the weight of the electrolyte, the content of the salt selected from the group consisting of monofluorophosphate, borate, oxalate and fluorosulfonate is less than 20% or less than 10%. In some embodiments, the content of the salt selected from the group consisting of monofluorophosphate, borate, oxalate and fluorosulfonate is within the range of any two of the above values.
[0104] In some embodiments, the electrolyte comprises one or more substances selected from the group consisting of monofluorophosphate, borate, oxalate and fluorosulfonate and one or more salts other than this. As salts other than this, the lithium salts exemplified above can be cited, and in some embodiments, they are LiPF6, LiN(FSO2)(CF3SO2), LiN(CF3SO2)2, LiN(C2F5SO2)2, cyclic 1,2-perfluoroethane bissulfonyl imide lithium, cyclic 1,3-perfluoropropane bissulfonyl imide lithium, LiC(FSO2)3, LiC(CF3SO2)3, LiC(C2F5SO2)3, LiBF3CF3, LiBF3C2F5, LiPF3(CF3)3, LiPF3(C2F5)3. In some embodiments, the salt other than this is LiPF6.
[0105] In some embodiments, the content of the other salt is greater than 0.01% or greater than 0.1% based on the weight of the electrolyte. In some embodiments, the content of the other salt is less than 20%, less than 15%, or less than 10% based on the weight of the electrolyte. In some embodiments, the content of the other salt is within the range formed by any two of the above values. The other salt having the above content helps to balance the conductivity and viscosity of the electrolyte.
[0106] III. Negative electrode
[0107] The negative electrode includes a negative electrode current collector and a positive electrode active material layer disposed on one or both surfaces of the negative electrode current collector, and the negative electrode active material layer contains a negative electrode active material. The negative electrode active material layer can be one or more layers, and each layer of the multi-layer negative electrode active material can contain the same or different negative electrode active materials. The negative electrode active material is any substance that can reversibly embed and deintercalate metal ions such as lithium ions. In some embodiments, the chargeable capacity of the negative electrode active material is greater than the discharge capacity of the positive electrode active material to prevent lithium metal from being accidentally precipitated on the negative electrode during charging.
[0108] As a current collector for holding the negative electrode active material, any known current collector can be used. Examples of negative electrode current collectors include, but are not limited to, metal materials such as aluminum, copper, nickel, stainless steel, and nickel-plated steel. In some embodiments, the negative electrode current collector is copper.
[0109] In the case where the negative electrode current collector is a metal material, the negative electrode current collector may include, but is not limited to, metal foil, metal cylinder, metal strip, metal plate, metal film, metal mesh, stamped metal, foamed metal, etc. In some embodiments, the negative electrode current collector is a metal film. In some embodiments, the negative electrode current collector is a copper foil. In some embodiments, the negative electrode current collector is a rolled copper foil based on a rolling method or an electrolytic copper foil based on an electrolytic method.
[0110] In some embodiments, the thickness of the negative electrode current collector is greater than 1 μm or greater than 5 μm. In some embodiments, the thickness of the negative electrode current collector is less than 100 μm or less than 50 μm. In some embodiments, the thickness of the negative electrode current collector is within the range of any two of the above values.
[0111] There is no particular limitation on the negative electrode active material, as long as it can reversibly absorb and release lithium ions. Examples of negative electrode active materials may include, but are not limited to, carbon materials such as natural graphite and artificial graphite; metals such as silicon (Si) and tin (Sn); or oxides of metal elements such as Si and Sn. Negative electrode active materials may be used alone or in combination.
[0112] The negative electrode active material layer may further include a negative electrode binder. The negative electrode binder can improve the bonding between the negative electrode active material particles and the bonding between the negative electrode active material and the current collector. The type of negative electrode binder is not particularly limited, as long as it is a material that is stable to the solvent used in the electrolyte or electrode manufacturing. In some embodiments, the negative electrode binder includes a resin binder. Examples of resin binders include, but are not limited to, fluororesins, polyacrylonitrile (PAN), polyimide resins, acrylic resins, polyolefin resins, and the like. When an aqueous solvent is used to prepare the negative electrode mixture slurry, the negative electrode binder includes, but is not limited to, carboxymethyl cellulose (CMC) or its salt, styrene-butadiene rubber (SBR), polyacrylic acid (PAA) or its salt, polyvinyl alcohol, and the like.
[0113] The negative electrode can be prepared by applying a negative electrode mixture slurry containing a negative electrode active material, a resin binder, etc. on a negative electrode current collector, drying it, and then rolling it to form a negative electrode active material layer on both sides of the negative electrode current collector, thereby obtaining a negative electrode.
[0114] IV. Isolation membrane
[0115] In order to prevent short circuit, a separator is usually provided between the positive electrode and the negative electrode. In this case, the electrolyte of the present application is usually used by infiltrating the separator.
[0116] There is no particular restriction on the material and shape of the isolation membrane, as long as the effect of the present application is not significantly impaired. The isolation membrane may be a resin, glass fiber, inorganic substance, etc. formed of a material that is stable to the electrolyte of the present application. In some embodiments, the isolation membrane includes a porous sheet or a non-woven fabric-like material with excellent liquid retention. Examples of materials for resin or glass fiber isolation membranes may include, but are not limited to, polyolefins, aromatic polyamides, polytetrafluoroethylene, polyether sulfone, etc. In some embodiments, the polyolefin is polyethylene or polypropylene. In some embodiments, the polyolefin is polypropylene. The materials of the above isolation membranes may be used alone or in any combination.
[0117] The isolation film may also be a material formed by laminating the above materials, and examples thereof include, but are not limited to, a three-layer isolation film formed by laminating polypropylene, polyethylene, and polypropylene in this order.
[0118] Examples of inorganic materials may include, but are not limited to, oxides such as aluminum oxide and silicon dioxide, nitrides such as aluminum nitride and silicon nitride, and sulfates (e.g., barium sulfate, calcium sulfate, etc.) The form of the inorganic material may include, but is not limited to, granular or fibrous.
[0119] The separator may be in the form of a thin film, examples of which include, but are not limited to, nonwoven fabrics, woven fabrics, microporous films, etc. In the thin film form, the separator has a pore size of 0.01 μm to 1 μm and a thickness of 5 μm to 50 μm. In addition to the above-mentioned independent thin film separators, the following separators may also be used: a separator formed by forming a composite porous layer containing the above-mentioned inorganic particles on the surface of the positive electrode and / or the negative electrode using a resin-based adhesive, for example, a separator formed by using a fluororesin as an adhesive to form a porous layer on both sides of the positive electrode with aluminum oxide particles having a particle size of 90% less than 1 μm.
[0120] The thickness of the isolation membrane is arbitrary. In some embodiments, the thickness of the isolation membrane is greater than 1 μm, greater than 5 μm, or greater than 8 μm. In some embodiments, the thickness of the isolation membrane is less than 50 μm, less than 40 μm, or less than 30 μm. In some embodiments, the thickness of the isolation membrane is within the range formed by any two of the above values. When the thickness of the isolation membrane is within the above range, the insulation and mechanical strength can be ensured, and the rate characteristics and energy density of the electrochemical device can be ensured.
[0121] When a porous material such as a porous sheet or non-woven fabric is used as an isolation membrane, the porosity of the isolation membrane is arbitrary. In some embodiments, the porosity of the isolation membrane is greater than 10%, greater than 15%, or greater than 20%. In some embodiments, the porosity of the isolation membrane is less than 60%, less than 50%, or less than 45%. In some embodiments, the porosity of the isolation membrane is within the range formed by any two of the above values. When the porosity of the isolation membrane is within the above range, insulation and mechanical strength can be ensured, and membrane resistance can be suppressed, so that the electrochemical device has good safety characteristics.
[0122] The average pore size of the isolation membrane is also arbitrary. In some embodiments, the average pore size of the isolation membrane is less than 0.5 μm or less than 0.2 μm. In some embodiments, the average pore size of the isolation membrane is greater than 0.05 μm. In some embodiments, the average pore size of the isolation membrane is within the range formed by any two of the above values. If the average pore size of the isolation membrane exceeds the above range, short circuit is likely to occur. When the average pore size of the isolation membrane is within the above range, the electrochemical device has good safety characteristics.
[0123] V. Electrochemical Device Components
[0124] The electrochemical device assembly includes an electrode group, a current collecting structure, an outer casing and a protective element.
[0125] The electrode group may be any of a laminated structure formed by laminating the above-mentioned positive electrode and the negative electrode with the above-mentioned separator, and a structure formed by spirally winding the above-mentioned positive electrode and the negative electrode with the above-mentioned separator. In some embodiments, the proportion of the mass of the electrode group in the internal volume of the battery (electrode group occupancy) is greater than 40% or greater than 50%. In some embodiments, the electrode group occupancy is less than 90% or less than 80%. In some embodiments, the electrode group occupancy is within the range formed by any two of the above values. When the electrode group occupancy is within the above range, the capacity of the electrochemical device can be ensured, and at the same time, the reduction of characteristics such as repeated charge and discharge performance and high temperature storage associated with the increase in internal pressure can be suppressed.
[0126] There is no particular limitation on the current collection structure. In some embodiments, the current collection structure is a structure that reduces the resistance of the wiring portion and the joint portion. When the electrode group is the above-mentioned stacked structure, it is suitable to use a structure formed by bundling the metal core portions of each electrode layer and welding them to the terminal. When the electrode area of a sheet increases, the internal resistance increases, so it is also suitable to set more than two terminals in the electrode to reduce the resistance. When the electrode group is the above-mentioned winding structure, the internal resistance can be reduced by setting more than two lead structures at the positive electrode and the negative electrode respectively, and bundling them at the terminal.
[0127] The material of the outer casing is not particularly limited, as long as it is a material that is stable to the electrolyte used. The outer casing can be made of, but not limited to, nickel-plated steel, stainless steel, aluminum or aluminum alloy, magnesium alloy and other metals, or a laminated film of resin and aluminum foil. In some embodiments, the outer casing is a metal or laminated film of aluminum or aluminum alloy.
[0128] The metal outer casing includes, but is not limited to, a packaged closed structure formed by welding metals to each other by laser welding, resistance welding, and ultrasonic welding; or a riveted structure formed by using the above-mentioned metals through a resin gasket. The outer casing using the above-mentioned laminated film includes, but is not limited to, a packaged closed structure formed by thermally bonding resin layers to each other. In order to improve the sealing performance, a resin different from the resin used in the laminated film can also be sandwiched between the above-mentioned resin layers. When the resin layer is thermally bonded to form a closed structure through the collector terminal, due to the bonding between the metal and the resin, a resin with a polar group or a modified resin into which a polar group is introduced can be used as the sandwiched resin. In addition, the shape of the outer casing is also arbitrary, for example, it can be any of cylindrical, square, laminated, button-shaped, large, etc.
[0129] The protection element may be a positive temperature coefficient (PTC) whose resistance increases when abnormal heat is released or excessive current flows, a temperature fuse, a thermistor, or a valve (current cutoff valve) that cuts off the current flowing in the circuit by causing the internal pressure or internal temperature of the battery to rise sharply when abnormal heat is released. The above protection element may be selected to be an element that does not work in normal use of high current, or may be designed in a form that does not cause abnormal heat release or thermal runaway even if the protection element is not present.
[0130] The electrochemical device of the present application includes any device that generates an electrochemical reaction, and specific examples thereof include a lithium metal secondary battery or a lithium ion secondary battery.
[0131] The present application further provides an electronic device, which includes the electrochemical device according to the present application.
[0132] The use of the electrochemical device of the present application is not particularly limited, and it can be used for any electronic device known in the prior art. In some embodiments, the electrochemical device of the present application can be used for, but not limited to, laptop computers, pen-input computers, mobile computers, e-book players, portable phones, portable fax machines, portable copiers, portable printers, head-mounted stereo headphones, video recorders, LCD televisions, portable cleaners, portable CD players, mini-discs, transceivers, electronic notepads, calculators, memory cards, portable recorders, radios, backup power supplies, motors, cars, motorcycles, power-assisted bicycles, bicycles, lighting fixtures, toys, game consoles, clocks, power tools, flashlights, cameras, large household batteries and lithium-ion capacitors, etc.
[0133] The preparation of lithium-ion batteries is described below by taking lithium-ion batteries as an example and combining specific embodiments. Those skilled in the art will understand that the preparation method described in this application is only an example, and any other suitable preparation method is within the scope of this application.
[0134] Example
[0135] 1. Preparation of lithium-ion batteries
[0136] 1. Preparation of negative electrode
[0137] Artificial graphite, styrene-butadiene rubber and sodium carboxymethyl cellulose were mixed with deionized water in a mass ratio of 96%:2%:2%, and stirred evenly to obtain a negative electrode slurry. The negative electrode slurry was coated on a 9 μm copper foil, dried, cold pressed, cut into pieces, and welded to the pole ears to obtain a negative electrode.
[0138] 2. Preparation of positive electrode
[0139] (1) Preparation of nickel cobalt manganese oxide positive electrode active material containing tungsten element: Anhydrous ethanol and deionized water are mixed in a volume ratio of 7:3, and 0.05 mol of nickel nitrate hexahydrate, 0.02 mol of cobalt nitrate hexahydrate and 0.03 mol of manganese acetate tetrahydrate are added thereto, and ultrasonic stirring is performed to completely dissolve them. The above-mentioned mixed solution is transferred to a 500 mL high-pressure reactor, 0.6 mol of ammonium bicarbonate is added thereto, and the mixture is heated to 120°C for 8 hours, cooled, centrifuged, and the precipitate is collected, washed with anhydrous ethanol 3 times, and vacuum dried at 60°C for 8 hours to obtain a nickel cobalt manganese hydroxide precursor. Subsequently, lithium carbonate, tungsten oxide and the prepared cobalt manganese hydroxide precursor are fully mixed and ground, calcined at 900°C in a tube furnace for 20 hours, cooled and ground again to obtain a nickel cobalt manganese oxide positive electrode active material containing tungsten element.
[0140] (2) Preparation of lithium cobalt oxide positive electrode active material containing tungsten element: A certain amount of Co3O4 and LiOH powder were weighed and fully mixed and ground in an agate mortar, and then calcined at 900°C for 10 hours. A specific amount of sodium tungstate was added to the calcined mixture, and ethanol was used as a solvent. After ball milling for 10 hours, the mixture was calcined at 800°C for 10 hours to obtain a lithium cobalt oxide positive electrode active material containing tungsten element.
[0141] Alumina, carbon nanotubes and polypropionate were mixed with deionized water in a mass ratio of 65:25:10 and stirred evenly to obtain an insulating layer or primer slurry. The insulating layer or primer slurry was coated on a 12 μm aluminum foil.
[0142] The positive electrode active material, carbon nanotubes and polyvinylidene fluoride are mixed with N-methylpyrrolidone (NMP) in a mass ratio of 97:1:2, and stirred evenly to obtain a positive electrode active material layer slurry. The positive electrode active material layer slurry is coated on a primer layer or aluminum foil, dried, cold pressed, cut into pieces, and welded to the tabs to obtain a positive electrode.
[0143] 3. Preparation of electrolyte
[0144] In a dry argon environment, EC, PC, PP and DEC (weight ratio of 1:1:1:1) were mixed, and LiPF6 was added and mixed evenly to form a basic electrolyte, wherein the concentration of LiPF6 was 12.5%. Different amounts of additives were added to the basic electrolyte to obtain electrolytes of different embodiments and comparative examples.
[0145] The abbreviations and names of the components in the electrolyte are shown in the following table:
[0146] Material Name abbreviation Material Name abbreviation Ethylene carbonate EC Ethylene carbonate PC Diethyl carbonate DEC Fluoroethylene carbonate FEC Succinonitrile SN Adiponitrile ADN Ethylene glycol di(2-cyanoethyl) ether EDN 1,3,6-Hexanetrinitrile HTCN 1,2,3-Tris(2-cyanoethoxy)propane TCEP 1,3-Propane sultone PS Vinyl Sulfate DTD Compound of formula I-1 Formula 1-1 Compound of formula I-3 Formula I-3 Compound of formula I-4 Formula 1-4 Compound of formula II-1 Formula 2-1 Lithium difluorophosphate LDP 1-Propylphosphonic acid cyclic anhydride T3P Ethylene carbonate VC Propyl Propionate PP
[0147] 4. Preparation of isolation membrane
[0148] A polyethylene porous polymer film is used as the isolation membrane.
[0149] 5. Preparation of lithium-ion batteries
[0150] The obtained positive electrode, separator and negative electrode are wound in order and placed in an outer packaging foil, leaving a liquid injection port. The electrolyte is poured from the liquid injection port, packaged, and then subjected to formation, capacity and other processes to obtain a lithium-ion battery.
[0151] 2. Test Method
[0152] 1. Test method for overcharge deformation rate of lithium-ion batteries
[0153] At 25°C, let the lithium-ion battery stand for 30 minutes, then charge it to 4.45V at a constant current rate of 0.5C, then charge it to 0.05C at a constant voltage rate at 4.45V, let it stand for 60 minutes, and measure the thickness 1. Then charge it to 60 minutes at a constant current rate of 0.1C, let it stand for 30 minutes, repeat the 0.1C charging and standing for 5 times, so that the lithium-ion battery reaches 150% state of charge (SOC), and measure the thickness 2. Calculate the overcharge deformation rate of the lithium-ion battery by the following formula:
[0154] Overcharge deformation rate = [(thickness 2 - thickness 1) / thickness 1] × 100%.
[0155] 2. Test method for high temperature short circuit deformation rate of lithium-ion batteries
[0156] At 25°C, the lithium-ion battery was left to stand for 30 minutes, then charged to 4.7V at a constant current rate of 0.5C, and then charged to 0.05C at a constant voltage rate of 4.7V, and left to stand for 60 minutes, and the thickness T1 of the lithium-ion battery was measured. The lithium-ion battery was then short-circuited for 10 seconds at 100mΩ, and then the thickness T2 of the lithium-ion battery was measured. The high-temperature short-circuit deformation rate of the lithium-ion battery was calculated by the following formula:
[0157] Short circuit deformation rate = [(T2-T1) / T1] x 100%.
[0158] 3. Test method for low temperature rate performance of lithium-ion batteries
[0159] At -20°C, the lithium-ion battery was discharged to 3.0V at 0.2C, left standing for 5 minutes, charged to 4.7V at 0.5C, charged to 0.05C at constant voltage and left standing for 5 minutes, and then discharged at 0.2C and 5.0C to obtain discharge capacity 1 and discharge capacity 2. The low temperature rate of the lithium-ion battery is calculated by the following formula:
[0160] Low temperature rate = [discharge capacity 2 / discharge capacity 1] × 100%.
[0161] 3. Test Results
[0162] Table 1 shows the effects of positive electrode active materials and electrolytes on low temperature rate performance and high temperature and high pressure safety of lithium ion batteries. Examples 1-1 to 1-19 and Comparative Examples 1-1 to 1-3 use lithium nickel cobalt manganese oxide containing / not containing tungsten as the positive electrode active material. Example 1-20 and Comparative Examples 1-4, 1-5, and 1-6 use lithium cobalt oxide containing / not containing tungsten as the positive electrode active material.
[0163] Table 1
[0164]
[0165]
[0166] As shown in Comparative Example 1-1, when the positive electrode active material is undoped lithium nickel cobalt manganese oxide and the electrolyte does not contain FEC, the overcharge deformation rate and short circuit deformation rate of the lithium ion battery are high and the low temperature rate is low. As shown in Comparative Example 1-2, when the positive electrode active material is lithium nickel cobalt manganese oxide containing tungsten but the electrolyte does not contain FEC, the overcharge deformation rate and short circuit deformation rate of the lithium ion battery are high and the low temperature rate is low. As shown in Comparative Example 1-3, when the electrolyte contains FEC but the positive electrode active material is undoped lithium nickel cobalt manganese oxide, the overcharge deformation rate and short circuit deformation rate of the lithium ion battery are high and the low temperature rate is low.
[0167] As shown in Examples 1-1 to 1-19, when the positive electrode active material is lithium nickel cobalt manganese oxide containing tungsten and the electrolyte contains FEC, the overcharge deformation rate and short circuit deformation rate of the lithium-ion battery can be significantly reduced and its low-temperature rate can be significantly improved.
[0168] When the content a% of FEC in the electrolyte and the content x% of tungsten in the positive electrode active material satisfy 1≤a / x≤70, the overcharge deformation rate and short-circuit deformation rate of the lithium-ion battery can be further reduced and its low-temperature rate can be significantly improved.
[0169] When the FEC content in the electrolyte is in the range of 0.1% to 7%, the overcharge deformation rate and short-circuit deformation rate of the lithium-ion battery can be further reduced and its low-temperature rate can be significantly improved.
[0170] When the content of tungsten in the positive electrode active material is 0.05% to 1%, the overcharge deformation rate and short circuit deformation rate of the lithium-ion battery can be further reduced and its low-temperature rate can be significantly improved.
[0171] In addition, as shown in Comparative Examples 1-4 to 1-6 and Example 1-20, when the positive electrode active material is lithium cobalt oxide containing tungsten and the electrolyte contains FEC, the overcharge deformation rate and short circuit deformation rate of the lithium ion battery can be significantly reduced and its low temperature rate can be significantly improved. Compared with lithium cobalt oxide containing tungsten, lithium nickel cobalt manganese oxide containing tungsten has a more obvious effect on improving the performance of lithium ion batteries.
[0172] Table 2 shows the influence of the content of the sulfur-oxygen double bond compound in the electrolyte and its relationship with the tungsten element in the positive electrode active material on the low temperature rate performance and high temperature and high pressure safety of the lithium ion battery. Except for the parameters listed in Table 2, the settings of Examples 2-1 to 2-25 are the same as those of Example 1-1.
[0173] Table 2
[0174]
[0175]
[0176] The results show that further adding 0.01% to 5% of a compound with a sulfur-oxygen double bond to the electrolyte containing FEC can further reduce the overcharge deformation rate and short-circuit deformation rate of the lithium-ion battery and significantly improve its low-temperature rate.
[0177] When the content b% of the sulfur-oxygen double bond compound in the electrolyte and the content x% of the tungsten element in the positive electrode active material satisfy 1≤b / x≤50, the overcharge deformation rate and short-circuit deformation rate of the lithium-ion battery can be further reduced and its low-temperature rate can be significantly improved.
[0178] Table 3 shows the influence of the aluminum content in the insulating layer and the tungsten content in the positive electrode active material on the low temperature rate performance and high temperature and high pressure safety of the lithium ion battery. Except for the parameters listed in Table 3, the configurations of Examples 3-1 to 3-16 are the same as those of Example 1-1.
[0179] Table 3
[0180]
[0181] The results show that when the aluminum content y1% in the positive electrode insulating layer and the tungsten content x% in the positive electrode active material satisfy 50≤y1 / x≤650, the overcharge deformation rate and short-circuit deformation rate of the lithium-ion battery can be further reduced and its low-temperature rate can be significantly improved.
[0182] When the aluminum content in the positive electrode insulating layer is 30% to 65%, the overcharge deformation rate and short circuit deformation rate of the lithium-ion battery can be further reduced and its low-temperature rate can be significantly improved.
[0183] Table 4 shows the influence of the aluminum content in the primer layer and the tungsten content in the positive electrode active material on the low temperature rate performance and high temperature and high pressure safety of the lithium ion battery. Except for the parameters listed in Table 4, the configurations of Examples 4-1 to 4-15 are the same as those of Example 1-1.
[0184] Table 4
[0185]
[0186] The results show that when the aluminum content y2% in the positive electrode bottom coating and the tungsten content x% in the positive electrode active material satisfy 20≤y2 / x≤550, the overcharge deformation rate and short-circuit deformation rate of the lithium-ion battery can be further reduced and its low-temperature rate can be significantly improved.
[0187] When the aluminum content in the positive electrode bottom coating is 20% to 50%, the overcharge deformation rate and short-circuit deformation rate of the lithium-ion battery can be further reduced and its low-temperature rate can be significantly improved.
[0188] Table 5 shows the effect of further adding additional compounds to the electrolyte on the low temperature rate performance and high temperature and high pressure safety of the lithium ion battery. Except for the parameters listed in Table 5, the configuration of Examples 5-1 to 5-15 is the same as that of Example 1-1.
[0189] Table 5
[0190]
[0191] The results show that when at least one of succinonitrile, adiponitrile, ethylene glycol di(2-cyanoethyl) ether, 1,3,6-hexanetrinitrile, 1,2,3-tri(2-cyanoethoxy)propane, 1,3-propanesultone, vinyl sulfate, vinylene carbonate or 1-propylphosphoric acid cyclic anhydride is further added to the electrolyte containing dinitrile compounds, the overcharge deformation rate and short-circuit deformation rate of the lithium-ion battery can be further reduced and its low-temperature rate can be improved.
[0192] References to "embodiments", "partial embodiments", "one embodiment", "another example", "example", "specific example" or "partial example" throughout the specification mean that at least one embodiment or example in the present application includes the specific features, structures, materials or characteristics described in the embodiment or example. Therefore, descriptions appearing in various places throughout the specification, such as: "in some embodiments", "in an embodiment", "in one embodiment", "in another example", "in an example", "in a specific example" or "example", do not necessarily refer to the same embodiment or example in the present application. In addition, the specific features, structures, materials or characteristics herein may be combined in one or more embodiments or examples in any suitable manner.
[0193] Although illustrative embodiments have been demonstrated and described, those skilled in the art should understand that the above embodiments should not be construed as limitations on the present application, and that changes, substitutions and modifications may be made to the embodiments without departing from the spirit, principles and scope of the present application.
Claims
1. An electrochemical device comprising: A positive electrode, a negative electrode and an electrolyte, wherein the positive electrode comprises a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector, the positive electrode active material layer comprises a positive electrode active material, the positive electrode active material contains tungsten, and the electrolyte comprises fluoroethylene carbonate; Wherein, the positive electrode further includes a primer layer, and the primer layer is formed between the positive electrode current collector and the positive electrode active material layer.
2. The electrochemical device according to claim 1, wherein: Based on the mass of the positive electrode active material, the content of the tungsten element is x%; Based on the mass of the electrolyte, the content of the fluoroethylene carbonate is a %; x and a satisfy: 1≤a / x≤70. 3 . The electrochemical device according to claim 1 , wherein the content of the tungsten element is x % based on the mass of the positive electrode active material, and 0.05≤x≤1. 4 . The electrochemical device according to claim 1 , wherein the content of the fluoroethylene carbonate is a % based on the mass of the electrolyte, and 0.1≤a≤7. 5 . The electrochemical device according to claim 1 , wherein the electrolyte further comprises a compound having a sulfur-oxygen double bond, and the content of the compound having a sulfur-oxygen double bond is b % based on the mass of the electrolyte, and 0.01≤b≤5. 6 . The electrochemical device according to claim 5 , wherein the content of the tungsten element is x%, based on the mass of the positive electrode active material, and b and x satisfy: 1≤b / x≤50.
7. The electrochemical device according to claim 1, wherein the positive electrode further comprises an insulating layer, and The insulating layer is formed on the positive electrode current collector and overlaps with the positive electrode active material layer in a partial region, or The insulating layer is formed on the positive electrode current collector and does not overlap with the positive electrode active material layer.
8. The electrochemical device according to claim 7, wherein: The insulating layer includes a compound containing an aluminum element, and the content of the aluminum element is y1% based on the mass of the insulating layer; Based on the mass of the positive electrode active material, the content of the tungsten element is x%; and y1 and x satisfy: 50≤y1 / x≤650. 9 . The electrochemical device according to claim 8 , wherein the value of y1 ranges from 30 to 65.
10. The electrochemical device according to claim 9, wherein: The primer layer includes aluminum, and the content of the aluminum is y2% based on the mass of the primer layer; Based on the mass of the positive electrode active material, the content of the tungsten element is x%; and y2 and x satisfy: 20≤y2 / x≤550. The electrochemical device according to claim 10 , wherein the value of y2 ranges from 20 to 50.
12. The electrochemical device according to claim 1, wherein the electrolyte further comprises at least one of succinonitrile, adiponitrile, ethylene glycol bis(2-cyanoethyl) ether, 1,3,6-hexanetrinitrile, 1,2,3-tris(2-cyanoethoxy)propane, 1,3-propane sultone, vinyl sulfate, vinylene carbonate, or 1-propylphosphoric acid cyclic anhydride.
13. The electrochemical device according to claim 1, wherein the positive electrode active material comprises lithium nickel cobalt manganese oxide.
14. An electronic device comprising the electrochemical device according to any one of claims 1 to 13.