Electrolyte, battery and electric device
By using ether solvents and lithium salts with sterically hindered functional groups in the electrolyte solution, the problems of oxidation and decomposition of the electrolyte and negative electrode side reactions under high cutoff voltage are solved, and the high oxidation stability and cycling stability of the battery are achieved.
Patent Information
- Application Number
- CN202410926478.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-19
AI Technical Summary
Under high cutoff voltage, the electrolyte has problems of oxidation and decomposition and side reactions of negative electrode substances, which affects the battery life.
Using a fluoroether-free solvent system, by increasing the ether solvent and lithium salt with sterically hindered functional groups, the solvation capacity is adjusted, the presence of anions and the formation of inorganic lithium fluoride interfaces is promoted, the growth of negative electrode lithium dendrites is inhibited, and the positive electrode is improved. stability.
The positive and negative electrode stability and Coulomb efficiency of the electrolyte are significantly improved, ensuring excellent cycle stability of the battery under high voltage conditions.
Smart Images

Figure BDA0004939991720000081
Abstract
Description
Technical Field
[0001] The present invention relates to the field of batteries, and in particular to an electrolyte, a battery and an electrical device. Background Art
[0002] At present, when the battery is at a high cut-off voltage (>4.3V), the electrolyte not only has the problem of oxidative decomposition, but also has the problem of side reactions with the negative electrode material. For example, in lithium metal batteries that use a nickel-rich layered oxide positive electrode and a metal lithium negative electrode, the high reactivity of the electrode material leads to serious electrode-electrolyte side reactions under high voltage conditions, greatly affecting the battery life. Summary of the invention
[0003] In view of the technical problems in the prior art, the present invention provides an electrolyte, a battery and an electrical device to improve the stability of the electrolyte under high voltage and optimize the cycle stability of the battery.
[0004] An electrolyte comprising:
[0005] Ether solvent; the ether solvent includes at least one of 1.2-di[(1'-ethoxy)ethoxypropane, 2,2-diethoxypropane, 2,2-dimethoxypropane, 1,2-dimethoxypropane, 1,3-dimethoxypropane, and 1,2-diethoxyethane;
[0006] Lithium salts.
[0007] Optionally, the lithium salt includes at least one of lithium perchlorate, lithium tetrafluoroborate, lithium hexafluoroarsenate, lithium trifluoromethylsulfonate, lithium bis(trifluoromethylsulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium trifluoromethylsulfonyl-perfluorobutylsulfonylimide, lithium fluorosulfonyl-perfluorobutylsulfonylimide, lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium difluorophosphate, and lithium nitrate.
[0008] A battery comprises a positive electrode, a negative electrode, a separator, and any one of the above electrolytes.
[0009] Optionally, the positive electrode includes at least one of lithium iron phosphate, lithium iron manganese phosphate, lithium cobalt oxide, lithium manganese oxide, lithium nickel oxide, ternary material, lithium-rich manganese base, lithium nickel manganese oxide and lithium vanadium phosphate.
[0010] Optionally, the negative electrode includes at least one of a graphite negative electrode, a silicon oxygen negative electrode, a silicon carbon negative electrode, a silicon negative electrode, a tin negative electrode, a tin oxide negative electrode, a tin alloy negative electrode, a lithium metal negative electrode, a lithium alloy negative electrode and a lithium-free negative electrode.
[0011] Optionally, the diaphragm includes at least one of polypropylene, polyethylene, PP / PE / PP composite film, polyvinylidene fluoride, polyacrylonitrile, ceramic diaphragm, ceramic polyamide, aramid and non-woven fabric.
[0012] A battery comprises a positive electrode, a negative electrode, a separator, and an electrolyte; the electrolyte comprises any one of the above-mentioned electrolytes; the content of the electrolyte in the electrolyte is 0.5wt.% to 50wt.%.
[0013] Optionally, the electrolyte is a gel electrolyte or a solid electrolyte; the solid electrolyte is an inorganic solid electrolyte, a polymer solid electrolyte or a composite solid electrolyte.
[0014] An electrical device using any of the above batteries as a power source.
[0015] The electrolyte, battery and electrical device provided by the present invention are fluorine-free ether solvent systems. By using ether solvents with more steric hindrance functional groups, the solvation capacity of ether molecules is adjusted by utilizing the steric hindrance effect. The increased steric hindrance can control and weaken the solvation capacity of oxygen atoms, thereby promoting the presence of anions in the internal solvation shell. Anion reduction promotes the formation of an inorganic fluoride-rich lithium (LiF) interface and achieves high oxidation stability. The anion-derived LiF intermediate phase can inhibit the growth of negative electrode lithium dendrites and minimize the cracking of the positive electrode under high pressure conditions, thereby significantly improving the positive and negative electrode stability and Coulomb efficiency of the ether electrolyte. DETAILED DESCRIPTION
[0016] In order to make the technical problems, technical solutions and beneficial effects solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0017] The embodiment of the present invention discloses an electrolyte, comprising:
[0018] Ether solvents, including 1,2-di[(1'-ethoxy)ethoxypropane (DEEP), 2,2-diethoxypropane (2DEP), 2,2-dimethoxypropane (2DMP), 1,2-dimethoxypropane (1DMP),
[0019] At least one of 1,3-dimethoxypropane (3DMP) and 1,2-diethoxyethane (EGDE);
[0020] Lithium salts.
[0021] Understandably, the electrolyte provided in this embodiment can be applied to lithium batteries, sodium ion batteries, etc., and belongs to a non-aqueous electrolyte. Among them, the ether solvent includes at least one of 1.2-di[(1'-ethoxy)ethoxypropane (DEEP), 2,2-diethoxypropane (2DEP), 2,2-dimethoxypropane (2DMP), 1,2-dimethoxypropane (1DMP), 1,3 dimethoxypropane (3DMP), and 1,2-diethoxyethane (EGDE).
[0022] Among them, 1.2-bis[(1'-ethoxy)ethoxypropane (4,6,9-trimethyl-3,5,8,10-tetraoxadodecane, DEEP), CAS number: 67715-79-1, molecular formula: C 11 H 24 O 4 , density 0.93g / cm 3 , boiling point 238.2℃at 760mmHg, molecular weight 220.30600, flash point 40.9℃, refractive index 1.419.
[0023] 2,2-Diethoxypropane (2DEP), CAS No.: 126-84-1, molecular formula: C 7 H 16 O 2 , molecular weight 132.2, boiling point: 116-117℃ (lit.), density: 0.82g / mL at25℃ (lit.), refractive index: n20 / D 1.389 (lit.), flash point: 46°F, storage conditions: 2-8℃.
[0024] 2,2-Dimethoxypropane (2DMP), CAS No. 77-76-9, molecular formula C 5 H 12 O 2 , molecular weight 104.15, melting point -47 ° C. Boiling point 83 ° C (lit.), density 0.847 g / mL, at25 ° C (lit.), vapor density 3.59 (vs air), vapor pressure 60 mmHg (15.8 ° C), refractive index n20 / D1.378 (lit.), flash point 12 ° F, storage conditions below 30 ° C, solubility 180 g / L, form: liquid, specific gravity 0.852 (20 / 4 ° C), color: transparent and colorless, explosive limit: 31%, 58 ° F, water solubility 18 g / 100 mL (25 ° C).
[0025] 1,2-Dimethoxypropane (1DMP), CAS No. 7778-85-0, molecular formula C 5 H 12 O 2 , molecular weight 104.15, boiling point 96°C (lit.), density 0.855 g / mL at 25°C (lit.), vapor pressure 40 mm Hg (20°C), refractive index n20 / D 1.3835 (lit.), flash point 33°F, form transparent liquid color colorless to almost colorless.
[0026] 1,3-Dimethoxypropane (3DMP), CAS No. 17081-21-9, molecular formula C 5 H 12 O 2 , molecular weight 104.15, melting point -82°C, boiling point 106°C, density 0.841±0.06g / cm 3 (predicted value).
[0027] 1,2-Diethoxyethane (Ethylene glycol diethyl ether, EGDE), CAS No. 629-14-1, molecular formula C 6 H 14 O 2 , molecular weight 118.17, melting point -74℃, boiling point 121℃ (lit.), density 0.842g / mLat25℃ (lit.), vapor pressure 9.4mmHg (20℃), refractive index n20 / D1.3923 (lit.), flash point 69°F, storage conditions below 30℃, solubility 34g / l, form: liquid, color: transparent and colorless.
[0028] These ether solvents use ethyl (EGDE), propyl (3DMP) or -CH3 (DEEP, 2DEP, 2DMP, 1DMP) between the two oxygen atoms, which can increase the steric hindrance of the ether structure, adjust the solvation structure of the ether molecule, improve its oxidation resistance, and retain the traditional ether structure -CH2CH2O- that stabilizes the lithium metal negative electrode. The increased steric hindrance of the ether solvent can control and weaken the solvation ability of the oxygen atom, thereby promoting the presence of anions in the internal solvation shell. Anion reduction promotes the formation of the inorganic fluoride-rich lithium (LiF) interface and achieves high oxidation stability. This anion-derived LiF intermediate phase can inhibit the growth of negative electrode lithium dendrites and minimize the cracking of the positive electrode under high pressure conditions, significantly improving the positive and negative electrode stability and Coulomb efficiency of the ether electrolyte, so that the battery system has excellent cycle stability at high cut-off voltage.
[0029] In some examples, the ether solvent includes DEEP+2DEP, and the volume ratio of DEEP to 2DEP is 1:(0.3-3). DEEP and 2DEP both have high boiling points and are not easy to evaporate at high temperatures, which can reduce the evaporation of the solvent and maintain the stability of the electrolyte.
[0030] In some examples, the ether solvent includes DEEP+2DMP, and the volume ratio of DEEP to 2DMP is (3-10): 1. Here, 2DMP has a lower melting point, which can improve the low temperature performance of the battery.
[0031] In some examples, the ether solvent includes DEEP+1DMP, and the volume ratio of DEEP to 1DMP is (1-5):1.
[0032] In some examples, the ether solvent includes DEEP+3DMP, and the volume ratio of DEEP to 3DMP is 1:(0.5-5).
[0033] Lithium salts can be inorganic lithium salts or organic lithium salts suitable for batteries, such as lithium perchlorate (LiClO 4 ) lithium hexafluoroarsenate (LiAsF 6 ), lithium trifluoromethanesulfonate (LiCF 3 SO), lithium bis(trifluoromethylsulfonyl)imide (LiTFSI), etc. Lithium salts can effectively improve the ionic conductivity of the electrolyte, improve the voltage resistance of the electrolyte and the compatibility of lithium metal / graphite. First, after the lithium salt is dissolved in the mixed solvent, it will dissociate into lithium ions and corresponding anions. These lithium ions move in the electrolyte as charge carriers, providing a channel for charge transfer inside the battery. Therefore, adding lithium salts can improve the ionic conductivity of the electrolyte, which helps to improve the charging and discharging efficiency and power performance of the battery. Secondly, the anions of lithium salts have high electrochemical stability. Within the operating voltage range of the battery, these anions are not easy to undergo oxidation or reduction reactions, reducing the occurrence of side reactions. This can prevent the electrolyte from decomposing at high voltage, thereby improving the voltage resistance of the electrolyte and ensuring that the battery works stably over a wide voltage range. Third, in the initial cycle of the battery, the anions of the lithium salt or its reduction products can form a stable solid electrolyte interface film (SEI at the negative electrode and CEI at the positive electrode) on the electrode surface, especially for active electrode materials such as lithium metal and graphite. This interfacial film can prevent other components in the electrolyte from further reacting with the electrode, reduce the growth of lithium dendrites, protect the electrode material from electrolyte erosion, enhance the compatibility of lithium metal and graphite, and improve the safety and cycle stability of the battery.
[0034] The electrolyte provided in this embodiment is a fluorine-free ether solvent system. By using an ether solvent with more steric hindrance functional groups, the solvation capacity of the ether molecules is adjusted by utilizing the steric hindrance effect. The increased steric hindrance can control and weaken the solvation capacity of the oxygen atoms, thereby promoting the presence of anions in the internal solvation shell. Anion reduction promotes the formation of an inorganic fluoride-rich lithium (LiF) interface and achieves high oxidation stability. This anion-derived LiF intermediate phase can inhibit the growth of negative electrode lithium dendrites and minimize the cracking of the positive electrode under high pressure conditions, thereby significantly improving the positive and negative electrode stability and Coulomb efficiency of the ether electrolyte.
[0035] Optionally, the lithium salt includes at least one of lithium hexafluorophosphate, lithium perchlorate, lithium hexafluoroarsenate, lithium trifluoromethylsulfonate, lithium bis(trifluoromethylsulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium trifluoromethylsulfonyl-perfluorobutylsulfonylimide, lithium fluorosulfonyl-perfluorobutylsulfonylimide, lithium bis(oxalatoborate), lithium difluorooxalatoborate, and lithium difluorophosphate.
[0036] It is understandable that the lithium salt can be an inorganic lithium salt or an organic lithium salt suitable for batteries, such as lithium hexafluorophosphate (LiPF 6 ), lithium perchlorate (LiClO 4 ) lithium hexafluoroarsenate (LiAsF 6 ), lithium trifluoromethanesulfonate (LiCF 3 SO), lithium bis(trifluoromethylsulfonyl)imide (LiTFSI), lithium bis(trifluoromethylsulfonyl)imide (LiFSI), lithium trifluoromethylsulfonyl-perfluorobutylsulfonylimide (LiTNFSI), lithium fluorosulfonyl-perfluorobutylsulfonylimide (LiFNFSI), lithium bis(oxalatoborate) (LiBOB), lithium difluorophosphate (LiPO 2 F 2 )wait.
[0037] The lithium salt provided in this embodiment can effectively increase the ionic conductivity of the electrolyte, and improve the voltage resistance and lithium metal / graphite compatibility of the electrolyte.
[0038] Optionally, the concentration of the lithium salt in the electrolyte is 0.5 mol / L to 3 mol / L.
[0039] It is understandable that the concentration of the lithium salt can be determined according to actual needs, such as 0.5 mol / L to 3 mol / L. Preferably, the concentration of the lithium salt in the electrolyte can be 1 mol / L, 1.5 mol / L.
[0040] A battery comprises a positive electrode, a negative electrode, a separator, and any one of the above electrolytes.
[0041] Understandably, the electrolyte provided in the previous embodiment can be used in combination with a positive electrode, a negative electrode and a separator to prepare a battery. Among them, the positive electrode is one of the core components of the battery and greatly affects the energy density of the battery. The positive electrode can be selected from lithium iron phosphate (LFP), lithium iron manganese phosphate (LMFP), lithium cobalt oxide (LCO), lithium manganese oxide (LMO), lithium nickel oxide (LNO), ternary materials (NCM, NCA), lithium-rich manganese-based (LMR), lithium nickel manganese oxide (LNMO), lithium vanadium phosphate (LiNO), lithium vanadium phosphate (LiNO), lithium vanadium phosphate (LiNO), lithium vanadium phosphate (LiNO), lithium vanadium phosphate (LiNO), lithium vanadium phosphate (LiNO), lithium vanadium phosphate (LiNO), lithium vanadium phosphate (LiNO), lithium vanadium phosphate (LiNO), lithium ferromanganese phosphate (LFP), lithium ferromanganese phosphate (LMFP), lithium cobalt oxide (LCO), lithium manganese oxide (LMO), lithium nickel phosphate (LNO), lithium ferromanganese phosphate (LNMO), lithium ferromanganese phosphate (LNO), lithium ferromanganese phosphate (LFP), lithium ferromanganese phosphate (LM ... 3 V 2 (PO 4 ) 3 ,LiVOPO 4 ). The negative electrode is one of the core components of the battery, interacting with the electrolyte to promote the embedding and de-embedding of metal cations. The negative electrode can be selected from at least one of graphite negative electrode, silicon oxygen negative electrode, silicon carbon negative electrode, silicon negative electrode, tin negative electrode, tin oxide negative electrode, tin alloy negative electrode (Sn-Fe, Sn-Co, Sn-Cu, etc.), lithium metal negative electrode, lithium alloy negative electrode (Li-Ag, Li-Al, Li-Sn, Li-Mg, Li-Zn, Li-In, Li-Ga, etc.), and lithium-free negative electrode. The diaphragm is a very thin layer of porous material located between the positive and negative electrodes of the battery, and can be selected from at least one of polypropylene (PP), polyethylene (PE), PP / PE / PP composite film, polyvinylidene fluoride (PVDF), polyacrylonitrile (PAN), ceramic diaphragm, polyimide (PI), aramid (AF), and non-woven fabric.
[0042] The battery provided in this embodiment can be made into a liquid laminate battery, a liquid wound battery or a liquid cylindrical battery. Due to the use of an electrolyte with better performance, the battery system has excellent cycle stability at a high cut-off voltage.
[0043] A battery, comprising a positive electrode, a negative electrode, a separator, and a gel electrolyte; the gel electrolyte comprises any one of the above-mentioned electrolytes; the content of the electrolyte in the electrolyte is 0.5wt.% to 50wt.%. In this embodiment, the battery can be a semi-solid battery, such as a semi-solid laminated battery, a semi-solid wound battery or a semi-solid cylindrical battery, wherein the electrolyte can be a gel electrolyte composed of a solid electrolyte and an electrolyte, and the content of the electrolyte in the electrolyte is 0.5wt.% to 50wt.%. The solid electrolyte can be selected from an inorganic solid electrolyte (oxide solid electrolyte, sulfide solid electrolyte, halide solid electrolyte), a polymer solid electrolyte and a composite solid electrolyte (inorganic filler + polymer matrix), and the solid electrolyte has higher mechanical strength and thermal stability, can better resist deformation and temperature changes, and can provide better safety performance. Compared with liquid electrolytes, gel electrolytes reduce the risk of leakage and improve safety.
[0044] An electrical device using any of the above batteries as a power source.
[0045] Example
[0046] Preparation of electrolyte
[0047] Add the corresponding lithium salt according to the solvent shown in Table 1 to reach the lithium salt concentration shown in Table 1, and stir at room temperature for 12 hours for use.
[0048] Wherein, the solvent used in Comparative Example 1 is 2-dimethoxyethane (DME).
[0049] Preparation of positive electrode
[0050] The positive electrode active material, lithium nickel cobalt manganese oxide (NCM811), the conductive agent CNT (carbon nanotube), and the adhesive PVDF (polyvinylidene fluoride) are mixed at a mass ratio of 97:1.5:1.5. The mixture is fully stirred and mixed in NMP solvent (N-methyl-2-pyrrolidone) to form a uniform positive electrode slurry. The slurry is applied to at least one side of the positive electrode current collector aluminum foil, and after drying, rolling, die-cutting and other processes, a positive electrode sheet that meets the requirements is obtained.
[0051] The negative electrode uses a lithium metal negative electrode.
[0052] The diaphragm uses PE porous polymer film (Polyethylene) as the diaphragm substrate;
[0053] Lithium battery manufacturing
[0054] The positive electrode sheet, the separator and the negative electrode sheet are stacked in order, and the separator is placed between the positive and negative electrodes to play an isolating role. Then the stacked electrode sheets and the separator are placed in the aluminum-plastic film bag formed by punching and forming. The non-aqueous electrolyte prepared above is respectively injected into the baked and dried battery cells. After vacuum packaging, standing, formation and other processes, a lithium battery with a capacity of 1Ah is obtained.
[0055] Performance Testing
[0056] 1. Electrolyte oxidation potential test: The linear scanning potential method was used to test the oxidation potential of the electrolyte membrane using the EC-Lab electrochemical workstation. The test voltage range was 2.5 to 6 V and the scanning rate was 1 mV·s -1 This method uses the device structure of "stainless steel sheet | diaphragm | lithium sheet" for testing, with the stainless steel sheet as the working electrode and the lithium sheet as the reference electrode.
[0057] 2. Battery cycle performance test: In the voltage range of 3.0V ~ 4.3V, temperature 25℃, 0.5C / 0.5D cycle charge and discharge test, record the capacity retention rate of the battery after 100 cycles.
[0058] Table 1 Electrolyte formulation and battery performance
[0059]
[0060] As shown in Table 1, by using the main chain to extend the carbon chain ethyl CH 3 -CH 2 -Replace short chain methyl -CH 3 Or the side chain introduces -CH 3 By increasing the steric hindrance of the ether structure, the oxidation resistance of the traditional short-chain ethers is effectively improved while retaining the stable structure of -CH 2 CH 2 O-, which significantly improves the cycle stability of ether electrolytes in high-voltage positive electrode systems.
[0061] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. An electrolyte, characterized in that: include: Ether solvent; the ether solvent includes at least one of 1.2-di[(1'-ethoxy)ethoxypropane, 2,2-diethoxypropane, 2,2-dimethoxypropane, 1,2-dimethoxypropane, 1,3-dimethoxypropane, and 1,2-diethoxyethane; Lithium salts.
2. The electrolyte according to claim 1, characterized in that The ether solvent includes 1.2-bis[(1'-ethoxy)ethoxypropane and 2,2-diethoxypropane, and the volume ratio of 1.2-bis[(1'-ethoxy)ethoxypropane to 2,2-diethoxypropane is 1:(0.3-3).
3. The electrolyte according to claim 1, characterized in that The lithium salt includes at least one of lithium perchlorate, lithium tetrafluoroborate, lithium hexafluoroarsenate, lithium trifluoromethylsulfonate, lithium bis(trifluoromethylsulfonyl)imide, lithium bis(trifluoromethylsulfonyl)imide, lithium trifluoromethylsulfonyl-perfluorobutylsulfonylimide, lithium fluorosulfonyl-perfluorobutylsulfonylimide, lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium difluorophosphate, and lithium nitrate.
4. A battery, characterized in that: The invention comprises a positive electrode, a negative electrode, a separator, and an electrolyte as claimed in any one of claims 1 to 3.
5. The battery according to claim 4, characterized in that The positive electrode includes at least one of lithium iron phosphate, lithium iron manganese phosphate, lithium cobalt oxide, lithium manganese oxide, lithium nickel oxide, ternary material, lithium-rich manganese base, lithium nickel manganese oxide and lithium vanadium phosphate.
6. The battery according to claim 4, characterized in that The negative electrode includes at least one of a graphite negative electrode, a silicon oxygen negative electrode, a silicon carbon negative electrode, a silicon negative electrode, a tin negative electrode, a tin oxide negative electrode, a tin alloy negative electrode, a lithium metal negative electrode, a lithium alloy negative electrode and a lithium-free negative electrode.
7. The battery according to claim 4, characterized in that The diaphragm includes at least one of polypropylene, polyethylene, PP / PE / PP composite film, polyvinylidene fluoride, polyacrylonitrile, ceramic diaphragm, ceramic polyamide, aramid and non-woven fabric.
8. A battery, characterized in that: It comprises a positive electrode, a negative electrode, a separator, and an electrolyte; the electrolyte comprises the electrolyte according to any one of claims 1 to 3; the content of the electrolyte in the electrolyte is 0.5wt.% to 50wt.%.
9. The battery according to claim 8, characterized in that The electrolyte is a gel electrolyte or a solid electrolyte; the solid electrolyte is an inorganic solid electrolyte, a polymer solid electrolyte or a composite solid electrolyte.
10. An electrical device, characterized in that: A battery as claimed in any one of claims 4 to 9 is used as a power source.
Citation Information
Cited By
Electrolyte, battery, and electric device
WO2026011767A1