Lithium ion cylindrical battery and power utilization device

By using negative electrode active material coating and expansion tape design of silicon particles and graphite materials in lithium-ion cylindrical batteries, the structural stability problems caused by changes in silicon particles are solved, and the high mechanical stability and safety of the battery are achieved, ensuring that Excellent performance of the battery after long cycle applications.

CN118983538APending Publication Date: 2024-11-19JIANGSU RELIANCE ENERGY TECHNOLOGY CO LTD

Patent Information

Application Number
CN202411066551.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Excessive changes in the volume of silicon particles in lithium-ion cylindrical batteries lead to a decrease in structural stability, affecting the mechanical strength and safety performance of the battery.

Method used

A lithium-ion cylindrical battery was designed, using a negative electrode active material coating of silicon particles and graphite materials, and an expansion tape was installed on the outside of the battery. By adjusting the average particle size of the silicon particles, the thickness of the expansion tape and the design of the protective layer, the negative electrode was ensured. The pole plate still maintains high mechanical structural stability and safety after long cycle applications.

Benefits of technology

It realizes high mechanical structure stability and safety of lithium-ion batteries after long cycle applications, significantly improves the stability and safety performance of the batteries under complex operating conditions, and ensures the long-term reliability and safety of the batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118983538A_ABST
    Figure CN118983538A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of lithium ion batteries, and discloses a cylindrical lithium ion battery and an electric device, the cylindrical lithium ion battery comprises a shell, a roll core and an electrolyte, the roll core and the electrolyte are arranged in the shell, the roll core is formed by winding a positive plate, a diaphragm and a negative plate together, and an expansion adhesive tape is arranged on the outer side of the roll core. The negative plate comprises a negative current collector and a negative active material coating coated on at least one surface of the negative current collector, the negative active material comprises silicon particles and a graphite material, and the mass content x% of the silicon element, the average particle size D [mu] m of the silicon particles and the thickness T [mu] m of the expansion adhesive tape meet the following relational expression: 0.5 x < = T / (3D) < = 3x; according to the invention, by designing the pores of the negative pole piece in the lithium ion battery and modifying the negative active material particles, the lithium ion battery still has extremely high mechanical structure stability after long-cycle application, and still can maintain the particle integrity after violent roller damage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium ion batteries, and in particular relates to a lithium ion cylindrical battery and an electrical device. Background Art

[0002] Lithium-ion batteries are also called rocking chair batteries. During the charging process, lithium ions are extracted from the positive electrode particles and embedded in the negative electrode particles, while the discharge process is the opposite. In the process of continuous lithium extraction and insertion, the volume of the particles will change repeatedly. In the process of continuous expansion and contraction, the mechanical structural stability of the particles will gradually decrease, and cracks will occur. After the particles are broken, a new interface will be generated, which will trigger local side reactions, generate heat and gas, and even cause safety hazards. The occurrence of side reactions will also increase the thickness of the interface and increase the impedance. The fragmentation of particles will cause the loss of effective lithium insertion sites and reduce capacity, and the structural stability will reduce performance degradation. Therefore, the performance of lithium-ion batteries is closely related to the mechanical strength of their active material particles. Lithium-ion batteries with high-strength active material particles will have better cycle performance and safety performance. In particular, if the active material after the cycle can still retain its high mechanical strength, it can better ensure the long-term application reliability of lithium-ion batteries. It not only has long cycle performance and excellent safety, but also can ensure its high safety performance after long-term circulation.

[0003] The core and shell of the cylindrical battery are welded together through electronic connectors, but there is a certain gap between the core and the shell. Therefore, in some complex working conditions, such as severe vibration, the core will be twisted and displaced, causing the electronic connector to fail. Therefore, for cylindrical batteries with more complex application scenarios, expansion tape will be used to improve their safety performance. After absorbing the electrolyte, the expansion tape will expand and enhance the friction between the core and the shell, thereby improving the mechanical structure stability and safety of its application under complex working conditions. In addition, the expansion glue also provides a buffer for the core and reduces its stress.

[0004] When a cylindrical battery uses a silicon-based negative electrode, the huge volume change effect of silicon particles will cause the stress and strain of the core to change more greatly, thereby causing the volume of the core to change more greatly or even deform, making it more difficult to fix the core structure.

[0005] Therefore, it is necessary to develop a new cylindrical battery with negative electrode particles having high particle mechanical strength to solve the problem that the volume change of silicon particles in existing lithium-ion cylindrical batteries is too large and affects the structural stability. Summary of the invention

[0006] The purpose of the present invention is to provide a lithium ion cylindrical battery and an electrical device.

[0007] The technical solution of the present invention is:

[0008] A lithium-ion cylindrical battery comprises a shell, a winding core loaded into the shell and an electrolyte, wherein the winding core is formed by winding a positive electrode sheet, a separator and a negative electrode sheet together, an expansion tape is arranged on the outside of the winding core, the negative electrode sheet comprises a negative electrode current collector and a negative electrode active material coating coated on at least one surface of the negative electrode current collector, the negative electrode active material comprises silicon particles and a graphite material, wherein the mass content of the silicon element is x%, the average particle size of the silicon particles is D microns and the thickness of the expansion tape is T microns, and the following relationship is satisfied: 0.5x≤T / (3D)≤3x.

[0009] Furthermore, the expansion tape includes a substrate and an adhesive layer on the surface of the substrate, wherein the substrate includes a synthetic resin (one or more materials selected from polyethylene PE, polyvinyl chloride PVC, polypropylene PP, polystyrene PS, polymethyl methacrylate PMMA, phenolic resin, polyurethane, and polyether), and the adhesive layer includes polyacrylate.

[0010] Furthermore, the growth rate of the specific surface area of ​​the negative electrode active material is less than 200% after the battery cell is cycled 600 times and subjected to a drum test.

[0011] Furthermore, the negative electrode active material coating also includes a pore structure, wherein the porosity A% of the negative electrode plate before the battery cell cycle and the porosity B% of the negative electrode plate after the battery cell cycle 600 times satisfy the following relationship: 15≤A≤35; 50%≥|AB| / A≥3%.

[0012] Furthermore, the graphite material includes one or more of artificial graphite or natural graphite; the surface of the negative electrode active material is provided with a protective layer for providing buffering, the initial thickness of the protective layer is T1 microns, the thickness of the battery cell after cycling is T2 microns, and satisfies the following relationship: T1 / D≥0.1%; (T2-T1) / D≤100%.

[0013] Furthermore, the protective layer includes carbon elements and metal elements, wherein the metal elements are at least one or more of Al, Zr, Ti, Sr, Mg, Na, Mo, Ca, Ba, La and Y.

[0014] Furthermore, the content of the metal element is 100-2000ppm.

[0015] Furthermore, the positive electrode sheet includes a positive electrode current collector and a positive electrode active material coating coated on at least one surface of the positive electrode current collector, and the positive electrode active material includes any one or a combination of two of lithium nickel cobalt manganese oxide or lithium nickel cobalt aluminum oxide; wherein the nickel atoms account for no less than 75% of the total number of lithium nickel cobalt manganese oxide or lithium nickel cobalt aluminum oxide atoms.

[0016] Furthermore, the mass proportion of silicon in the negative electrode active material is 2-30%.

[0017] Furthermore, the electrolyte includes a solvent and an additive, the solvent includes any one or more combinations of ethylene carbonate, dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate, and the additive includes any one or more combinations of vinylene carbonate, methyl formate, ethyl acetate, and propyl propionate.

[0018] Another technical solution of the present invention is:

[0019] An electrical device comprises the lithium-ion cylindrical battery as described above.

[0020] The present invention provides a lithium ion cylindrical battery and an electric device, which have the following beneficial effects:

[0021] 1. By designing the pores of the negative electrode sheet in the lithium-ion battery and modifying the negative electrode active material particles, it is achieved that after long-cycle application, it still has extremely high mechanical structural stability, and after severe roller damage, it can still maintain its particle integrity; such a negative electrode and the lithium-ion battery manufactured by it have excellent long-cycle performance, and the hot box performance of the battery cell after the cycle is still very excellent, ensuring its extremely high safety;

[0022] 2. In addition, the volume change caused by the expansion of silicon combined with the expansion glue design can significantly improve the structural stability of the core, thereby enhancing its long-cycle performance and stability under vibration conditions, ensuring its safety. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 Schematic diagrams of positive and negative electrodes of lithium-ion cylindrical batteries involved in some embodiments are shown;

[0024] Figure 2 Schematic diagrams of winding pole pieces and separators of lithium-ion cylindrical batteries according to some embodiments are shown, wherein (a) is a stereoscopic diagram and (b) is a cross-sectional diagram;

[0025] Figure 3 Schematic diagrams of the winding core and expansion tape structure of lithium-ion cylindrical batteries involved in some embodiments are shown, wherein (a) is a front view of the battery cell and (b) is a horizontal cross-sectional view.

[0026] In the figure:

[0027] 1. Shell; 2. Positive terminal; 3. Negative terminal; 4. Winding core; 5. Positive electrode sheet; 6. Negative electrode sheet; 7. Diaphragm; 8. Expansion tape. DETAILED DESCRIPTION

[0028] At least one embodiment provides a lithium-ion cylindrical battery, comprising a shell, a winding core loaded into the shell and an electrolyte, wherein the winding core is formed by winding a positive electrode sheet, a separator and a negative electrode sheet together, an expansion tape is provided on the outside of the winding core, the negative electrode sheet comprises a negative electrode collector and a negative electrode active material coating coated on at least one surface of the negative electrode collector, the negative electrode active material comprises silicon particles and a graphite material, wherein the mass content of the silicon element is x%, the average particle size of the silicon particles is D microns and the thickness of the expansion tape is T microns, satisfying the following relationship: 0.5x≤T / (3D)≤3x.

[0029] Test method:

[0030] Take a battery cell, discharge it to 2.5V at 0.2C at 25℃, then let it stand for half an hour, disassemble it, obtain the expansion glue, soak it in DMC for 1 hour and wash it 3 times; bake it in a 60℃ vacuum oven for 12 hours; then fix and flatten it, and measure the thickness with a thickness gauge; it is required to test at least 20 points in different positions, and the test area must not be less than 1cm 2 , 3 data are tested at each point. Afterwards, these results are calculated to get the average value, which is the thickness T.

[0031] In addition, the negative electrode sheet was cross-sectioned and characterized by SEM and EDS, at least 100 silicon particles were tested to obtain their average particle size D, and the thickness of the protective layer on the surface of the negative electrode particles was measured;

[0032] In addition, at least 10 surface scans of different areas are tested, and a single surface scan area contains at least 10 complete negative electrode particles. The total amount of Si and C elements is corrected to 100%, and the average value of Si element is calculated from the surface scan results to obtain the mass content of Si element x%.

[0033] In this embodiment, specifically, the growth rate of the specific surface area of ​​the negative electrode active material is less than 200% after the negative electrode active material has been cycled through the battery cell for 600 times and has undergone a drum test.

[0034] Test method:

[0035] Take a ternary high nickel-graphite mixed silicon battery with a rated capacity of 4Ah as an example. A fresh lithium-ion battery is obtained. At 25°C, it is first discharged to 2.5V at a rate of 0.1C, and then left to stand for 10 minutes. Then, it is charged to 4.2V at a constant current of 0.1C, and then charged to 0.05C at a constant voltage. After standing for 10 minutes, it is discharged to 2.5V at a constant current of 0.1C, and its capacity is calibrated to C0. After that, it is cycled at a rate of 1C charge and 1C discharge, and the standing time after the charging and discharging steps is 10 minutes. The discharge capacity of the first cycle is recorded as C1, and the cycle is continued until the discharge capacity reaches C1*80%.

[0036] The cycled battery cell is discharged at a rate of 0.1C to 2.5V, and then disassembled after standing for 2 hours to obtain the negative electrode plate; the negative electrode plate is calcined at 300°C in a muffle furnace in nitrogen or inert gas for more than 12 hours, washed with ethanol three times after cooling, filtered, and baked in a vacuum oven at 80°C for 8 hours; thereafter, the specific surface area of ​​the powder is measured by BET and recorded as S1; thereafter, the powder is processed according to the national standard GB / T 2006-2008 "Determination of Mechanical Strength of Coke" (the equipment size is proportionally reduced by 20 times, and the amount of powder used in a single test is ≥6g). After the processing is completed, the powder is tested again and its specific surface area is recorded by BET as S2; (S2-S1) / S1 is the specific surface area growth rate.

[0037] In this embodiment, specifically, the negative electrode active material coating also includes a pore structure, wherein the porosity A% of the battery cell electrode sheet before the battery cell cycle and the porosity B% of the battery cell electrode sheet after the battery cell cycle 600 times satisfy the following relationship: 15≤A≤35; 50%≥|AB| / A≥3%.

[0038] Test method:

[0039] The porosity was tested by mercury intrusion porosimeter. Each battery cell was first discharged to 2.5V at 0.2C at 25°C and then left to stand for 30 minutes. The battery was disassembled to obtain the pole piece, which was soaked in DMC for 1 hour and rinsed 3 times. The pole piece was then baked in a vacuum oven at 60°C for 12 hours. The porosity of the dried pole piece was tested.

[0040] It is required to divide the battery cell into 5 parts with equal spacing in the length direction, and take 5 samples at the center position in the width direction for testing, and calculate the average value.

[0041] In this embodiment, specifically, the protective layer includes carbon elements and metal elements, wherein the metal element is at least one of Al, Zr, Ti, Sr, Mg, Na, Mo, Ca, Ba, La and Y.

[0042] In this embodiment, specifically, the content of the metal element in the protective layer of the negative electrode active material is 100-2000 ppm.

[0043] In this embodiment, specifically, the positive electrode sheet includes a positive electrode current collector and a positive electrode active material coating coated on at least one surface of the positive electrode current collector, and the positive electrode active material includes any one or a combination of two of lithium nickel cobalt manganese oxide and lithium nickel cobalt aluminum oxide; wherein the nickel atoms account for no less than 75% of the total nickel cobalt manganese or nickel cobalt aluminum atoms.

[0044] In this embodiment, specifically, the mass proportion of silicon element in the negative electrode active material is 2-30%.

[0045] In this embodiment, specifically, the electrolyte includes a solvent and an additive, the solvent includes any one or more combinations of ethylene carbonate, dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate, and the additive includes any one or more combinations of vinylene carbonate, methyl formate, ethyl acetate, and propyl propionate.

[0046] At least one embodiment provides an electric device including the lithium-ion cylindrical battery as described above.

[0047] In order to make the above-mentioned objects, features and advantages of the present invention more clearly understood, the technical solutions of the present invention are further described below in conjunction with embodiments. However, the present invention is not limited to the embodiments listed, and should also include any other known changes within the scope of the rights claimed by the present invention.

[0048] The term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.

[0049] Example 1: This example demonstrates a method for preparing a lithium-ion cylindrical battery according to the following steps.

[0050] A lithium-ion cylindrical battery comprises a shell, a winding core placed in the shell and an electrolyte. The winding core is formed by winding a positive electrode sheet, a separator and a negative electrode sheet together, and an expansion tape is arranged on the outside of the winding core.

[0051] A positive electrode sheet comprises a positive electrode current collector aluminum foil and a positive electrode coating coated on both sides of the aluminum foil; wherein, calculated by weight percentage, the positive electrode coating comprises 96.5% of NCA88, 0.4% of a multi-walled carbon nanotube conductive agent, 1.6% of a Super-P (conductive carbon black) conductive agent, and 1.5% of a polyvinylidene fluoride (PVDF) binder; the above substances are added to NMP and stirred to form a positive electrode slurry with a solid content of 60%, which is then coated on the positive electrode collector to form a positive electrode sheet.

[0052] The negative electrode sheet includes a negative electrode current collector copper foil and a negative electrode coating coated on both sides of the copper foil. The negative electrode coating includes 91% artificial graphite, 5% silicon, 1.0% conductive agent acetylene black, 1% thickener CMC and 2% negative electrode binder polyacrylic acid PAA, calculated by weight percentage, wherein the average particle size of the silicon particles is 6.3 microns, and the BET before the cycle is 5.1m 2 / g, BET after recycling is 8.6m 2 / g, the growth rate is 69%, the porosity of the battery cell electrode is 26% before the cycle and 21.3% after the cycle, Al is used for the protective layer, the Al content is 660ppm, the initial thickness is 0.05 microns, and the thickness after the cycle is 2.5 microns; the above substances are added into deionized water and stirred to form a negative electrode slurry with a solid content of 40%, which is coated on the negative electrode collector to form a negative electrode sheet.

[0053] Expandable tape, thickness 122.6 microns.

[0054] Ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1 to obtain an organic solvent, and then fully dried lithium salt LiPF6 is dissolved in the mixed organic solvent to prepare an electrolyte with a concentration of 1 mol / L.

[0055] The diaphragm comprises a high-pore dynamic diaphragm, a base film PE thickness of 9 microns, a ceramic coating thickness of 1 micron on both sides, and a PVDF coating thickness of 1 micron. The air permeability of the diaphragm is ≥80s / 100mL.

[0056] See also Figure 1 , the positive and negative electrode sheets are rolled, slit and die-cut respectively, and then wound together with the separator. The positive, negative and separator are wound by a winding machine to form a roll core, and the positive and negative pole ears are cut, stacked or flattened on the roll core. Then, the positive bus bar and the negative bus bar are welded to the roll core respectively, and then the negative bus bar is welded to the steel shell. An insulating sheet is placed on top of the positive bus bar, and the positive bus bar is welded to the cap to obtain a cylindrical battery roll core, which is loaded into the battery shell. After completing the injection, sealing and formation processes, an experimental battery is obtained.

[0057] Specifically, the parameters and performance results in Example 1 are shown in Table 1 below.

[0058] Table 1

[0059]

[0060]

[0061] Specifically, the thickness T of the expansion tape in Example 1 was adjusted to obtain the parameters and performances of Examples 1-3 and Comparative Examples 1-2, as shown in Table 2 below.

[0062] Table 2

[0063]

[0064] It can be seen from Table 1 that when 0.5x≤T / (3D)≤3x is not satisfied, the cycle retention rate of the test battery, the performance of the hot box test after cycling, and the drum test will be greatly reduced.

[0065] Specifically, the specific surface area and porosity in Example 1 were adjusted to obtain the parameters and properties of Example 1, Examples 4-7 and Comparative Examples 3-5, as shown in Table 3 below.

[0066] Table 3

[0067]

[0068]

[0069] It can be seen from Table 3 that when 50% ≥ |AB| / A ≥ 3% or BET before cycle / BET after cycle < 200% is not satisfied, the cycle retention rate, post-cycle hot box test and drum test performance of the test battery will be greatly reduced.

[0070] Specifically, the thickness layer, protective layer and positive and negative electrode sheets in Example 1 were adjusted to obtain the parameters and performances of Example 1 and Examples 8-16 and Comparative Examples 6-9, as shown in Tables 4 and 5 below, where Table 4 is the parameter values ​​and Table 5 is the test performance.

[0071] Table 4

[0072]

[0073]

[0074] Table 5

[0075] Cycle retention rate Heat box after circulation Roller test Example 1 89.50% 5 / 5 5 / 5 Example 8 82.20% 4 / 5 5 / 5 Example 9 73.40% 3 / 5 4 / 5 Comparative Example 6 50.30% 0 / 5 2 / 5 Comparative Example 7 30.20% 0 / 5 2 / 5 Example 10 87.20% 5 / 5 5 / 5 Embodiment 11 86.80% 5 / 5 5 / 5 Example 12 83.30% 5 / 5 5 / 5 Example 13 80.10% 4 / 5 5 / 5 Comparative Example 8 70.80% 2 / 5 4 / 5 Comparative Example 9 64.50% 2 / 5 2 / 5 Embodiment 14 84.30% 5 / 5 5 / 5 Embodiment 15 77.30% 3 / 5 4 / 5

[0076] It can be seen from Tables 4 and 5 that when T1 / D≥0.1%, (T2-T1) / D≤100% or the metal element content is between 100-2000ppm, the cycle retention rate, post-cycle hot box test and drum test performance of the test battery will be greatly reduced.

[0077] Cyclic performance test

[0078] Take a cylindrical battery, such as 217004Ah, place it in a 25℃ constant temperature box for more than 4 hours, and test it according to the following steps:

[0079] (1) Discharge the battery at a constant current of 0.1C to 2.5V cutoff and leave it for 5 minutes;

[0080] (2) Charge the battery at a constant current of 0.2C to a cutoff of 4.2V, and at a constant voltage of 0.05C to a cutoff, and let it stand for 5 minutes;

[0081] (3) Discharge the battery at a constant current of 0.2C to a cutoff of 2.5V, and let it stand for 5 minutes. Read the capacity value C0 at this time.

[0082] (4) Charge the battery at a constant current of 1.0C to 4.2V, and charge at a constant voltage of 0.05C to a cutoff, and let it stand for 5 minutes;

[0083] (5) Discharge the battery at a constant current of 2.0C to a cutoff of 2.5V and let it stand for 5 minutes;

[0084] Repeat steps (4) and (5) 600 times;

[0085] The cycle performance of a single battery, i.e., the capacity retention rate, is obtained by the ratio of the 600th discharge capacity to the first discharge capacity in step (4) and step (5).

[0086] Hot box test

[0087] Take a battery after 600 cycles, place it in a 25℃ constant temperature box for more than 4 hours, and test it according to the following steps:

[0088] (1) Discharge the battery at a constant current of 0.1C to 2.5V cutoff and leave it for 5 minutes;

[0089] (2) Charge the battery at a constant current of 0.2C to a cutoff of 4.2V, and at a constant voltage of 0.05C to a cutoff, and let it stand for 5 minutes;

[0090] (3) Place the battery in an incubator, set the heating rate to 5K / min, heat to 130°C, and keep it for 1 hour, then stop heating and allow it to cool to below 30°C by self-heating;

[0091] (4) If the battery does not catch fire or emit smoke, it is considered to have passed. Otherwise, it is considered to have failed. At least 5 batteries shall be tested and the pass rate shall be recorded.

[0092] Vibration test / roller test

[0093] Take a cylindrical battery, such as 217004Ah, place it in a 25℃ constant temperature box for more than 4 hours, and test it according to the following steps:

[0094] (1) Discharge the battery at a constant current of 0.1C to 2.5V cutoff and leave it for 5 minutes;

[0095] (2) Charge the battery at a constant current of 0.2C to a cutoff of 4.2V, and at a constant voltage of 0.05C to a cutoff, and let it stand for 5 minutes;

[0096] (3) Test the open circuit voltage V1, initial internal resistance ACR, and R1 of the battery cell;

[0097] (4) The battery was tested in a drum at 66 rpm for 100 minutes;

[0098] (5) Remove the battery and let it sit for 10 minutes;

[0099] (6) Test the open circuit voltage V2 and internal resistance ACR R2 of the battery. V2 ≥ 95% V1 and R2 ≤ 125% R1 are considered to have passed the drum test.

[0100] Test 5 batteries in parallel and calculate the pass rate.

[0101] In summary, the lithium-ion cylindrical battery and the electrical device of the present invention achieve extremely high mechanical structural stability after long-cycle application by designing the pores of the negative electrode plate in the lithium-ion battery and modifying the negative electrode active material particles, and can still maintain its particle integrity after severe roller damage; such a negative electrode and the lithium-ion battery manufactured therefrom have excellent long-cycle performance, and the hot box performance of the battery cell after the cycle is still very excellent, ensuring its extremely high safety; in addition, the volume change caused by the expansion of silicon is combined with the expansion glue design to significantly improve the structural stability of the winding core, so as to enhance its long-cycle performance and stability under vibration conditions, and ensure its safety. The battery of the embodiment of the present application can obtain a 600-cycle cycle retention rate of between 73% and 95%, a hot box test pass rate of more than 60% after the cycle, and a roller test pass rate of more than 80%.

[0102] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the claims of the present invention.

Claims

1. A lithium-ion cylindrical battery, comprising a housing, a winding core contained in the housing, and an electrolyte, It is characterized in that The winding core is formed by winding a positive electrode sheet, a separator and a negative electrode sheet together, an expansion tape is arranged on the outside of the winding core, the negative electrode sheet includes a negative electrode current collector and a negative electrode active material coating coated on at least one surface of the negative electrode current collector, the negative electrode active material includes silicon particles and graphite material, wherein the mass content of the silicon element is x%, the average particle size of the silicon particles is D micrometers and the thickness of the expansion tape is T micrometers, and the following relationship is satisfied: 0.5x≤T / (3D)≤3x.

2. The lithium-ion cylindrical battery according to claim 1, It is characterized in that The growth rate of the specific surface area of ​​the negative electrode active material is less than 200% after the battery cell is cycled 600 times and subjected to a drum test.

3. The lithium-ion cylindrical battery according to claim 1, It is characterized in that The negative electrode active material coating also includes a pore structure, wherein the porosity A% of the negative electrode sheet before the battery cell is cycled and the porosity B% of the negative electrode sheet after the battery cell is cycled 600 times satisfies the following relationship: 15≤A≤35; 50%≥|AB| / A ≥3%.

4. The lithium-ion cylindrical battery according to claim 1, It is characterized in that The graphite material includes one or more of artificial graphite or natural graphite; The surface of the negative electrode active material is provided with a protective layer for providing buffering, and the initial thickness of the protective layer is T 1 micron, the thickness of the battery after cycling is T 2 micrometers, and satisfy the following relationship: T 1 / D≥0.1%; (T 2 -T 1 ) / D≤100%。 5. The lithium ion cylindrical battery according to claim 4, It is characterized in that The protective layer includes carbon elements and metal elements, wherein the metal elements are at least one or more of Al, Zr, Ti, Sr, Mg, Na, Mo, Ca, Ba, La and Y.

6. The lithium ion cylindrical battery according to claim 5, It is characterized in that The content of the metal element is 100-2000ppm.

7. The lithium ion cylindrical battery according to claim 1, It is characterized in that The positive electrode sheet includes a positive electrode current collector and a positive electrode active material coating coated on at least one surface of the positive electrode current collector, wherein the positive electrode active material includes any one of lithium nickel cobalt manganese oxide or lithium nickel cobalt aluminum oxide or a combination of both; wherein the nickel atoms account for no less than 75% of the total number of lithium nickel cobalt manganese oxide or lithium nickel cobalt aluminum oxide atoms.

8. The lithium-ion cylindrical battery according to claim 1, It is characterized in that The mass proportion of silicon in the negative electrode active material is 2-30%.

9. The lithium ion cylindrical battery according to claim 1, It is characterized in that The electrolyte includes a solvent and an additive, wherein the solvent includes any one or more combinations of ethylene carbonate, dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate, and the additive includes any one or more combinations of vinylene carbonate, methyl formate, ethyl acetate, and propyl propionate.

10. An electrical device, It is characterized in that It comprises a lithium ion cylindrical battery as described in any one of claims 1 to 9.

Citation Information

Patent Citations

  • Lithium ion battery electrode, preparation method thereof and lithium ion battery

    CN102931378A

  • Negative electrode and lithium ion secondary battery thereof

    CN111668452A

  • Method for manufacturing secondary battery

    CN114051666A

  • High-safety lithium ion battery positive plate, preparation method thereof and lithium ion battery

    CN114709365A

  • Secondary battery and electronic device

    CN117334906A

Cited By

  • Lithium ion battery and method for predicting, regulating and controlling diaphragm resistance of lithium ion battery

    CN119627034A