CHA-type zeolites and methods of synthesizing said zeolites
By preparing hydrogen-form CHA zeolites with SAR values of 8 to 35, the problem of poor processability in existing technologies has been solved, the physical strength of the catalyst and the efficiency of waste gas treatment have been improved, and the stringent environmental emission standards have been met.
Patent Information
- Application Number
- CN202380033199.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-11-23
- Filing Date
- 2023-05-17
- Publication Date
- 2024-11-19
AI Technical Summary
Existing hydrogen-form chalcogenide (CHA) zeolites have poor processability in catalyst preparation, which affects the physical strength of the catalyst and the uniformity of the coating, and makes it difficult to meet strict environmental emission standards.
Hydrogen-form CHA zeolite with an SAR of 8 to 35 is prepared by forming a reactive gel containing precursor zeolite, organic structure directing agent (OSDA), sodium hydroxide and/or potassium hydroxide and silica source, and heating it at an appropriate temperature, thus avoiding the use of organic structure directing agent, reducing environmental impact and improving processability.
The prepared CHA zeolite has high crystallinity and low lattice defects, which improves the physical strength of the catalyst and the uniformity of the coating, enhances the efficiency of waste gas treatment, and meets stringent environmental emission standards.
Smart Images

Figure BDA0005076345340000051 
Figure BDA0005076345340000131 
Figure BDA0005076345340000141
Abstract
Description
Technical Field
[0001] The present invention relates to chabazite-type (CHA) zeolites. More specifically, the present invention relates to hydrogen-type chabazite-type zeolites having a silica-alumina ratio (SAR) of 8 to 35. The present invention also relates to methods for making chabazite-type zeolites, especially zeolites having a SAR of 8 to 35. The present invention also relates to catalyst articles comprising chabazite-type zeolites and methods for treating exhaust gases, the methods comprising contacting the exhaust gases with a catalyst article comprising chabazite-type zeolites. Background Art
[0002] Since the discovery of silica-rich CHA-type zeolite SSZ-13 in 1985 (US 4,544,538), this zeolite has been extensively studied and produced on an industrial scale, particularly as a NO x Eliminate the key component of the NH3-SCR catalyst in the application. Meanwhile, various improvements related to SSZ-13 have been reported, such as reducing the crystal size to improve the accessibility of the internal porous space of the zeolite for the catalytic reaction (see US 6,709,644 and US 10,407,314), preparing larger crystals (US 10,029,247) or crystals with reduced silanol defects (US 10,407,314 and US 10,953,390) to improve the durability of the zeolite under severe working conditions, and producing zeolites with alternative OSDA for cost-saving manufacturing (US 8,007,764 and US 10,953,390).
[0003] Environmental regulations worldwide have become increasingly stringent. Emission standards in developing countries are catching up to the higher standards required by developed countries. For these reasons, there is still a pressing need to further improve CHA products or make them have better performance, especially for NH3-SCR applications.
[0004] When used as a component material in catalyst preparation, the processability of zeolite also has a significant impact on the physical or mechanical properties of the final catalyst product. For example, it is usually one of the key factors affecting the uniformity and physical strength of the washcoat layer and the impact on back pressure. Therefore, there is a need to further improve processability.
[0005] To address these challenges, the applicant has discovered a novel SSZ-13 type CHA zeolite and a method for synthesizing the same, which has significant advantages over the prior art including improved processability. In addition, the inventors have discovered that the CHA zeolite of the present invention having an XRD peak intensity ratio as defined herein has low lattice defects and high crystallinity. Summary of the invention
[0006] One aspect of the present disclosure relates to a hydrogen-type chabazite-type (CHA) zeolite having a SAR of 8 to 35, and a ratio of XRD peak intensities corresponding to [2 1 1] and [-1 1 1] reflections being equal to or greater than 0.80.
[0007] Another aspect of the present disclosure relates to a method for making a chabazite-type (CHA) zeolite having a SAR of 8 to 35, the method comprising:
[0008] (i) forming a reaction gel comprising a precursor zeolite, an organic structure directing agent (OSDA), sodium hydroxide and / or potassium hydroxide and optionally a silica source, and
[0009] (ii) heating the reaction gel to a temperature and for a duration suitable for the growth of the CHA zeolite.
[0010] Another aspect of the present disclosure relates to a catalyst article for treating exhaust gas, the catalyst article comprising the CHA zeolite in hydrogen form as described herein.
[0011] Another aspect of the present disclosure relates to a method of treating an exhaust gas, the method comprising contacting the exhaust gas with a catalyst article described herein. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 The powder X-ray diffraction (XRD) pattern and SEM image of the H-type CHA structure prepared in Example 1 are shown.
[0013] Figure 2 The powder X-ray diffraction (XRD) pattern and SEM image of the H-type CHA structure prepared in Example 2 are shown.
[0014] Figure 3 The powder X-ray diffraction (XRD) pattern and SEM image of the H-type CHA structure prepared in Example 3 are shown.
[0015] Figure 4 The powder X-ray diffraction (XRD) pattern and SEM image of the H-type CHA structure prepared in Example 4 are shown.
[0016] Figure 5 The powder X-ray diffraction (XRD) pattern and SEM image of the H-type CHA structure prepared in Example 5 are shown.
[0017] Figure 6 The powder X-ray diffraction (XRD) pattern and SEM image of the H-type CHA structure prepared in Example 6 are shown.
[0018] Figure 7The powder X-ray diffraction (XRD) pattern and SEM image of the H-type CHA structure prepared in Example 7 are shown.
[0019] Figure 8 The powder X-ray diffraction (XRD) pattern and SEM image of the H-type CHA structure prepared in Example 8 are shown.
[0020] Fig. 9 The powder X-ray diffraction (XRD) pattern and SEM image of the H-type CHA structure prepared in Example 9 are shown.
[0021] Fig.10 The powder X-ray diffraction (XRD) pattern and SEM image of the H-type CHA structure prepared in Example 10 are shown.
[0022] Fig.11 The powder X-ray diffraction (XRD) pattern and SEM image of the H-type CHA structure prepared in Example 11 are shown.
[0023] Fig.12 The powder X-ray diffraction (XRD) pattern and SEM image of the H-type CHA structure prepared in Example 12 are shown.
[0024] Fig.13 The powder X-ray diffraction (XRD) pattern and SEM image of the H-type CHA structure prepared in Example 13 are shown.
[0025] Fig.14 The powder X-ray diffraction (XRD) pattern and SEM image of the H-type CHA structure prepared in Example 14 are shown.
[0026] Fig.15 The powder X-ray diffraction (XRD) pattern and SEM image of the H-type CHA structure prepared in Example 15 are shown.
[0027] Fig.16 The powder X-ray diffraction (XRD) pattern and SEM image of the H-type CHA structure prepared in Example 16 are shown.
[0028] Fig.17 The powder X-ray diffraction (XRD) pattern and SEM image of the H-type CHA structure prepared in Example 17 are shown.
[0029] Fig.18 The powder X-ray diffraction (XRD) pattern and SEM image of the H-type CHA structure prepared in Example 18 are shown.
[0030] Fig.19 The powder X-ray diffraction (XRD) pattern and SEM image of the H-type CHA structure prepared in Example 19 are shown.
[0031] Fig.19b The powder X-ray diffraction (XRD) pattern and SEM image of the H-type CHA structure prepared in Example 20 are shown.
[0032] Fig. 20 The powder X-ray diffraction (XRD) pattern and SEM image of the H-type CHA structure prepared in Comparative Example A are shown.
[0033] Fig.21 The powder X-ray diffraction (XRD) pattern and SEM image of the H-type CHA structure prepared in Comparative Example B are shown.
[0034] Fig. 22 The powder X-ray diffraction (XRD) pattern and SEM image of the H-type CHA structure prepared in Comparative Example C are shown.
[0035] Fig.23 The NOx conversion rate of Example 1 is shown
[0036] Fig.24 The N2O prepared in Example 1 is shown
[0037] Fig.25 The NOx conversion rates of reference CHA and CHA1 are shown
[0038] Fig.26 The N2O prepared by reference CHA and CHA1 is shown.
[0039] Fig. 27 The NOx conversion rate of Example 2 is shown
[0040] Fig.28 The N2O prepared in Example 2 is shown
[0041] Fig.29 The NOx conversion rates of reference CHA and CHA2 are shown.
[0042] Fig.30 The N2O prepared by reference CHA and CHA2 is shown. DETAILED DESCRIPTION
[0043] A first aspect of the present invention relates to a hydrogen-type chabazite-type (CHA) zeolite having a SAR of 8 to 35, and a ratio of XRD peak intensities corresponding to [2 1 1] and [-1 1 1] reflections being equal to or greater than 0.80.
[0044] The present disclosure will now be further described. In the following paragraphs, different aspects / embodiments of the present disclosure are defined in more detail. Unless there is a clear contrary description, each aspect / embodiment so defined may be combined with any other aspect / embodiment or multiple aspects / embodiments. In particular, any feature indicated as being preferred or advantageous may be combined with any other one or more features indicated as being preferred or advantageous.
[0045] Zeolites are structures formed from alumina and silica, and the SAR determines the reactive sites within the zeolite structure. Small pore zeolites, including CHA zeolites, have a structure composed of eight tetrahedral atoms (Si 4+ and Al 3+ ) pores, each connected by a shared oxygen. These eight-membered ring pores allow small molecules to enter the void space within the crystal, such as in automobile exhaust purification (NO x Removal) during the NO x or into methanol on its way to light olefins, while limiting the entry and exit of larger molecules critical to overall catalyst performance. CHA zeolites may also be referred to as zeolites having a CHA framework structure, as known in the art.
[0046] The CHA zeolite according to the present invention is a hydrogen-type (H-type) CHA zeolite. The term "H-type" CHA zeolite refers to a CHA zeolite in which the framework charge is substantially balanced by protons. In this form, the CHA zeolite generally contains H in the exchange sites. + and a mixture of alkali metal and / or alkaline earth metal cations. The H-form of the CHA zeolite may be ≥90%, ≥95%, ≥96%, ≥97%, ≥98%, or ≥99% (by weight) in the H-form. The amount of the CHA zeolite in the H-form may vary depending on the specific CHA zeolite batch and the process used to form the CHA zeolite.
[0047] In a preferred embodiment, the CHA zeolite according to the present invention does not contain or is substantially free of one or more of the following: fluorine, fluorine-containing compounds, fluoride ions, phosphorus, phosphorus-containing compounds and phosphorus ions. Preferably, the CHA zeolite according to the present invention does not contain or is substantially free of all of the following: fluorine, fluorine-containing compounds, fluoride ions, phosphorus, phosphorus-containing compounds and phosphorus ions. "Substantially free" means that the zeolite contains less than 0.1%, for example less than 0.08%, less than 0.05%, less than 0.03%, less than 0.02%, less than 0.01%, less than 0.005%, less than 0.001% (based on the total weight of the zeolite by weight) of undesirable components.
[0048] The H-type CHA zeolite of the present invention has a ratio of XRD peak intensities corresponding to the [2 1 1] and [-1 1 1] reflections equal to or greater than 0.80. In a preferred embodiment, the ratio is equal to or greater than 0.85, 0.9, 0.95, 1.0, 1.5. In another embodiment, the ratio is in the range of 0.8 to 2.5, 0.85 to 2, 0.9 to 1.9, 1 to 1.8 or 1.1 to 1.7.
[0049] Those skilled in the art will use their common knowledge to calculate the ratio of the XRD peak intensities of the [2 1 1] and [-1 1 1] reflections. As will be fully understood, the X-ray diffraction data contains a (2θ) peak in the range of 24.5 to 25.5 (±0.2 s-θ degrees) corresponding to the [2 1 1] reflection, and a (2θ) peak in the range of 15 to 17 corresponding to the [-1 1 1] reflection. The ratio of the XRD peak intensities corresponding to the [2 1 1] and [-1 1 1] reflections is calculated by calculating the total peak height from the baseline to the peak top of the [2 1 1] and [-1 1 1] reflections, and then calculating the ratio of the peak heights of the [2 1 1]:[-1 1 1] reflections, i.e., by using the following equation:
[0050]
[0051] Copper is used as the X-ray source to calculate the XRD peak intensity according to the present invention. The peak intensity can be calculated using a CHA zeolite in equilibrium with ambient conditions. For example, the ambient conditions can be a temperature of 18° C. to 25° C. and a humidity of at most 60%, such as at most 50%, at most 40%, or at most 30%.
[0052] In one embodiment, the CHA zeolite of the present invention has a SAR of 8 to 17 and a ratio of the XRD peak intensities corresponding to the [2 1 1] and [-1 1 1] reflections of equal to or greater than 0.95. In another embodiment, the SAR may be 8 to 17, 9 to 16, 10 to 15, 11 to 14 or 12 to 13 (for example, when the ratio of the XRD peak intensities corresponding to the [2 1 1] and [-1 1 1] reflections is equal to or greater than 0.95). In another embodiment, (for example, when the SAR is 8 to 17), the ratio of the XRD peak intensities corresponding to the [2 1 1] and [-1 1 1] reflections is equal to or greater than 0.95, for example, equal to or greater than 1, 1.05, 1.1, 1.15, 1.2, 1.25, 1.3, 1.35, 1.4, 1.45 or 1.5. In another embodiment, (e.g., when the SAR is 8 to 17), the ratio of the XRD peak intensities corresponding to the [21 1] and [-1 1 1] reflections is in the range of 0.95 to 2.5, 1 to 2.25, 1.1 to 2, 1.2 to 1.9, 1.3 to 1.8, 1.4 to 1.7 or 1.5 to 1.6.
[0053] In one embodiment, the CHA zeolite of the present invention has a SAR of 17 to 24 and a ratio of the XRD peak intensities corresponding to the [2 1 1] and [-1 1 1] reflections of equal to or greater than 0.85. In another embodiment, the SAR may be 17 to 24, 18 to 23, 19 to 22, or 20 to 21 (e.g., when the ratio of the XRD peak intensities corresponding to the [2 1 1] and [-1 1 1] reflections is equal to or greater than 0.85). In another embodiment, (e.g., when the SAR is 17 to 24), the ratio of the XRD peak intensities corresponding to the [2 1 1] and [-1 1 1] reflections is equal to or greater than 0.85, for example, equal to or greater than 0.9, 0.95, 1, 1.05, 1.1, 1.15, 1.2, 1.25, 1.3, 1.35, 1.4, 1.45, or 1.5. In another embodiment, (e.g., when the SAR is 17 to 24), the ratio of the XRD peak intensities corresponding to the [2:1:1] and [-1:1:1] reflections is in the range of 0.85 to 2.5, 0.9 to 2.25, 0.95 to 2, 1 to 1.9, 1.1 to 1.8, 1.25 to 1.75, 1.4 to 1.7 or 1.5 to 1.6.
[0054] In one embodiment, the CHA zeolite of the present invention has a SAR of 24 to 34 and a ratio of the XRD peak intensities corresponding to the [2 1 1] and [-1 1 1] reflections of equal to or greater than 0.80. In another embodiment, the SAR may be 25 to 33, 26 to 32, 27 to 31 or 28 to 30 (e.g., when the ratio of the XRD peak intensities corresponding to the [2 1 1] and [-1 1 1] reflections is equal to or greater than 0.80). In another embodiment, (e.g., when the SAR is 24 to 34), the ratio of the XRD peak intensities corresponding to the [2 1 1] and [-1 1 1] reflections is equal to or greater than 0.80, for example, equal to or greater than 0.85, 0.9, 0.95, 1, 1.05, 1.1, 1.15, 1.2, 1.25, 1.3, 1.35, 1.4, 1.45 or 1.5. In another embodiment, (e.g., when the SAR is 24 to 34), the ratio of the XRD peak intensities corresponding to the [2:1:1] and [-1:1:1] reflections is in the range of 0.80 to 2.5, 0.85 to 2.25, 0.9 to 2, 0.95 to 1.9, 1 to 1.8, 1.25 to 1.75, 1.4 to 1.7 or 1.5 to 1.6.
[0055] Preferably, the CHA zeolite of the present invention has a SAR of at most 35, preferably at most 33, preferably at most 30, more preferably at most 28 and even more preferably at most 25. In some embodiments, it is also preferred that the CHA zeolite has a SAR of at least 8 or at least 9. In some embodiments, it is preferred that the CHA zeolite has a SAR of 8 to 35, 9 to 33, 10 to 30, 11 to 28, 12 to 25, 13 to 22, 14 to 21, 15 to 20, 16 to 19 or 17 to 18. In other embodiments, the SAR is preferably 8 to 33, 8 to 30, 9 to 30, 9 to 28, 9 to 25, 10 to 22 or 10 to 20.
[0056] In another embodiment, the CHA zeolite of the present invention has a SAR between 16 and 35, preferably between 17 and 30, for example between 17 and 25 or between 17 and 23. In some embodiments, it is preferred that the CHA zeolite has a SAR of 17 to 25, between 17.5 and 24, between 18 and 23 or between 19 and 22.
[0057] The present invention can provide a device having a diameter of less than 35 m, either alone or in combination with any of the above desirable features. 2 / g, preferably not more than 30m 2 / g, more preferably not more than 25m 2 / g of mesoporous surface area. In some embodiments, the CHA zeolite may have a mesoporous surface area of no greater than 24 m 2 / g, not more than 22m 2 / g, not more than 21m 2 / g, not more than 20m 2 / g, not more than 19m 2 / g, not more than 18m 2 / g, not more than 17m 2 / g, not more than 16m 2 / g, not more than 15m 2 / g, not more than 14m 2 / g, not more than 12m 2 / g or not more than 10m 2 / g of mesoporous surface area. In certain embodiments, CHA zeolites may have 0 m 2 / g to 35m 2 / g, 1m 2 / g to 30m 2 / g, 2m 2 / g to 25m 2 / g, or 3m 2 / g to 24m 2 / g, 4m 2 / g to 22m 2 / g, 5m 2 / g to 20m 2 / g, 6m 2 / g to 18m 2 / g, 7m 2 / g to 17m 2 / g, 8m 2 / g to 15m 2 / g or 9m 2 / g to 12m 2 / g of mesoporous surface area. This unique combination of features has been achieved as a result of the unique synthetic methods described herein. Specifically, the inventors have identified specific gel formulations that may be able to produce gels having the desired SAR as described herein and a mesoporous surface area of less than 35 m / s. 2 / g of mesoporous surface area of CHA zeolite.
[0058] Mesoporous surface area can be measured using any conventional technique in the art. For example, according to the Brunauer-Emmett-Teller (BET) method, Ar or N2 adsorption isotherms on activated samples are measured at 87K or 77K, respectively. Prior to measurement, the sample is heated under vacuum to remove physically adsorbed water. The pore size distribution is measured by non-local density functional theory (NLDFT). The mesoporous surface area is calculated by the difference between the apparent BET and micropore surface areas.
[0059] The present invention can provide a BET surface area of 500 m2 / g to 800m 2 / g; preferably 600m 2 / g to 800m 2 / g; or more preferably 650m 2 / g to 800m 2 / g of CHA zeolite.
[0060] The present invention can provide a micropore volume of 0.2 cm 2 / g to 0.3cm 2 / g; preferably 0.22cm 2 / g to 0.28cm 2 / g; or more preferably 0.23cm 2 / g to 0.26cm 2 / g of CHA zeolite.
[0061] Preferably, the CHA zeolite has a crystallinity greater than 90%, such as greater than 95% or greater than 98%. The CHA zeolite may be substantially free of other crystalline phases, and generally it is not an intergrowth of two or more framework types. As used herein, the term "substantially free" means that the zeolite contains less than about 10%, 8%, 6%, 4%, 2%, or 1% by weight of a specified framework impurity or all impurities.
[0062] Preferably, the CHA zeolite has granular particles. That is, preferably the zeolite has a particle morphology whereby the zeolite crystals have a three-dimensional shape, as compared to rod-shaped particles having a substantially one-dimensional shape or disc-shaped or plate-shaped particles having a two-dimensional shape. Preferably, the zeolite has granular particles comprising or consisting of cubic crystals.
[0063] Preferably, the CHA zeolite comprises uniform and non-aggregated cubic crystals and / or uniform and non-aggregated aggregates. Aggregates are individual crystals that are tightly bound to each other to form relatively uniform particles, i.e., not single or individual crystals. Aggregates may include twins.
[0064] Preferably, CHA zeolite has an average crystal size (e.g., average longest side crystal size) of not more than 15 microns, preferably not more than 12 microns or 10 microns. In some embodiments, CHA zeolite may have an average crystal size (e.g., average longest side crystal size) of 0.25 micron to 15 microns, preferably 0.5 micron to 13 microns, 1 micron to 12 microns, 1.5 microns to 11 microns, 2 microns to 10 microns, 3 microns to 9.5 microns, 4 microns to 9 microns, or 5 microns to 8 microns. In some embodiments, the average crystal size may be 0.25 micron to 5 microns, 0.3 micron to 4 microns, 0.5 micron to 3 microns, 0.6 micron to 2 microns, 0.7 micron to 1.5 microns, or 0.75 micron to 1 micron. Such average crystal size can be measured using standard microscopic techniques such as scanning electron microscopes (SEM). The statistically significant portion of the zeolite produced is measured.
[0065] In another aspect of the present invention, there is provided a method for producing a chabazite-type (CHA) zeolite having a SAR of 8 to 35, the method comprising:
[0066] (i) forming a reaction gel comprising a precursor zeolite, an organic structure directing agent (OSDA), sodium hydroxide and / or potassium hydroxide and optionally a silica source, and
[0067] (ii) heating the reaction gel to a temperature and for a duration suitable for the growth of the CHA zeolite.
[0068] It is particularly preferred that the process described herein is used to prepare the H-type CHA zeolite described herein.
[0069] The process of the present invention for preparing the CHA zeolites described herein is an interzeolite conversion (IZC) route.
[0070] The precursor zeolite can be selected from ferrierite (FER), faujasite (FAU), MFI, BEA and LTL. These zeolite frameworks are all known in the prior art (e.g., see WO2019242618 disclosing FER, BEA and MFI frameworks and WO2021101947 disclosing LTL frameworks). Preferably, the precursor zeolite is FER. The precursor zeolite may have a SAR value of 2 to 30, such as 10 to 20. In one embodiment, the precursor zeolite has a SAR value of 16 to 20 or 17 to 19. In another embodiment, the precursor zeolite has a SAR value of 12 to 16. In a specific embodiment, the precursor zeolite is FER and has a SAR value of 2 to 30, 10 to 20, 12 to 20, 16 to 19 or 17 to 20, such as 16, 17, 18 or 19.
[0071] The precursor zeolite may have any counter ions. For example, the counter ions may be sodium, lithium, cesium, protons (H + ), ammonium or an organic cation. In a preferred embodiment, the counter ion is a sodium counter ion.
[0072] In one embodiment, the precursor zeolite is prepared from a reaction gel that does not contain an organic structure directing agent (OSDA).In an alternative embodiment, the ferrierite is prepared from a reaction gel that contains a structure directing agent, preferably an organic structure directing agent (OSDA).
[0073] Applicants have surprisingly discovered that the precursor zeolite does not need to be prepared using an organic structure directing agent (OSDA). This makes the process more efficient and reduces its environmental impact. OSDA is usually removed by calcination to prevent impurities in the final product; this energy intensive step is no longer required. This enables the precursor zeolite to be prepared at a much lower cost than precursors that require the use of OSDA. Furthermore, it has been found that the precursor zeolite formed without the use of OSDA has comparable or even better properties than precursors formed with OSDA.
[0074] The precursor zeolite can be prepared by a method comprising the following steps:
[0075] (a) forming a reaction gel comprising an aluminum source, sodium hydroxide and / or potassium hydroxide and a silicon dioxide source,
[0076] (b) heating the reaction gel to a temperature and for a duration suitable for the growth of the FER zeolite, and optionally
[0077] (c) The obtained FER zeolite is filtered and washed.
[0078] The method for preparing a precursor zeolite may include forming a reaction gel, which may also be referred to as a reaction mixture. Such reaction gels are well known in the field of zeolite synthesis. The reaction gel of the method for preparing a precursor zeolite may include an aluminum source, sodium hydroxide / potassium hydroxide and a silica source. Examples of aluminum sources include sodium aluminate, aluminum salts such as aluminum sulfate, aluminum nitrate, aluminum chloride, aluminum hydroxide, aluminum alkoxide and aluminum oxide, preferably one or more of aluminum hydroxide and aluminum sulfate. Examples of silica sources include sodium silicate, potassium silicate, silica gel, silica sol, pyrogenic silica, silicon alkoxide and precipitated silica, preferably silica sol. Silica sol is a colloidal suspension of silica in water. In other preferred embodiments, the silica source and the aluminum source may include the same material, such as silica-alumina or a zeolite such as FER framework zeolite. In a preferred embodiment, the reaction gel includes aluminum hydroxide, sodium hydroxide and a silica sol solution.
[0079] In another embodiment, the reaction gel used to prepare the precursor zeolite may also contain OSDA. Examples of suitable OSDA include N,N,N-trialkylcyclohexyl ammonium derivatives, such as N,N,N-dimethylethylcyclohexyl ammonium; N,N,N-trialkylbenzyl ammonium derivatives, such as benzyltrimethylammonium; trialkyl (cyclohexylmethyl) ammonium derivatives, such as trimethyl (cyclohexylmethyl) ammonium; [NR1R2R3R4]+, and wherein R1, R2; R3 and R4 are independently alkyl groups having one to four carbon atoms, wherein the alkyl group may be optionally substituted with one or more hydroxyl groups, such as tetraethylammonium. In another embodiment, OSDA is selected from a list comprising (e.g., consisting of) N,N,N-trimethyl-1-adamantyl ammonium, N,N,N-dimethylethylcyclohexyl ammonium, trimethyl (cyclohexylmethyl) ammonium and tetraethylammonium. In one embodiment, the reaction gel used to prepare the precursor zeolite may also include an OSDA selected from the list comprising (e.g., consisting of) N,N,N-trimethyl-1-adamantylammonium, N,N,N-dimethylethylcyclohexylammonium, trimethyl(cyclohexylmethyl)ammonium and tetraethylammonium, benzyltrimethylammonium, N,N,N-triethylcyclohexylammonium, N,N,N-trimethylcyclohexylammonium, N,N,N-diethylmethylcyclohexylammonium and triethylmethylammonium. In another embodiment, the OSDA may be N,N,N-dimethylethylcyclohexylammonium, used alone or in combination with another OSDA (e.g., N,N,N-trimethyl-1-adamantylammonium and / or benzyltrimethylammonium). In another embodiment, the OSDA may be benzyltrimethylammonium, used alone or in combination with another OSDA (e.g., N,N,N-trimethyl-1-adamantylammonium and / or N,N,N-dimethylethylcyclohexylammonium).
[0080] In a preferred embodiment, the reaction gel used to prepare the precursor zeolite is a gel that does not contain an organic structure directing agent, that is, the reaction gel does not contain ODSA. "Does not contain an organic structure directing agent" means that the reaction gel used to prepare the precursor zeolite contains less than 1 wt% of an organic structure directing agent based on the total weight of the reaction gel, such as less than 0.9 wt%, less than 0.5 wt%, less than 0.3 wt%, less than 0.2 wt%, less than 0.1 wt% or less than 0.01 wt% of an organic structure directing agent. In a preferred embodiment, the reaction gel used to prepare the precursor zeolite contains 0 wt% of an organic structure directing agent.
[0081] The reaction gel used to prepare the precursor zeolite is heated at a temperature suitable for the growth of the FER zeolite and for a duration suitable for the growth of the FER zeolite. Preferably, the temperature to which the reaction gel is heated for such a suitable duration is 100°C to 220°C; more preferably 110°C to 210°C, 120°C to 200°C, 130°C to 190°C, or even 140°C to 180°C. The duration for which the reaction gel is heated to a suitable temperature is preferably at least 10 hours, more preferably 20 hours to 5 days, 1 day to 4 days, for example 3 days. It is particularly preferred to heat the reaction gel to these temperatures and maintain these durations at these temperatures, for example maintaining at least 10 hours at a temperature of 100°C to 220°C.
[0082] Preferably, the FER zeolite product produced by heating the reaction gel to such temperature and duration is recovered by typical vacuum filtration. Preferably, the filtered product is washed with demineralized (also called deionized) water to remove residual mother liquor. Preferably, the zeolite product is washed until the filtrate conductivity is less than 0.1 mS. Preferably, the filtered and washed product is then dried at a temperature greater than 100° C., preferably about 120° C. The FER zeolite product can be filtered by vacuum filtration and washed with demineralized water.
[0083] In another embodiment, the method for preparing the precursor zeolite may further include the step of loading one or more enhancing metals onto the FER zeolite formed in step (b) or step (c). These enhancing metals may be loaded onto the FER zeolite by initial wetness, ion exchange, or during the preparation of the washcoat slurry.
[0084] The enhancing metal is a non-framework metal. As used herein, a "non-framework metal" is a metal located within the pores of the molecular sieve and / or on at least a portion of the surface of the molecular sieve, preferably as an ionic species, excluding aluminum, and excluding atoms that constitute the framework of the molecular sieve. Preferably, the presence of the enhancing metal promotes the treatment of exhaust gases such as exhaust gases from diesel engines, including such as NO x Reduction, NH3 oxidation and NO x Storage method.
[0085] The reinforcing metal includes certain transition metals such as copper (Cu), iron (Fe), manganese (Mn), nickel (Ni), molybdenum (Mo) and zinc (Zn), preferably copper and / or iron, and most preferably copper. Certain reinforcing metals are noble metals such as gold (Au) and silver (Ag), and platinum group metals such as platinum (Pt), palladium (Pd), ruthenium (Ru) and rhodium (Rh). In addition, the reinforcing metal may be one or more rare earth metals such as cerium (Ce), praseodymium (Pr), neodymium (Nd), europium (Eu), erbium (Er), gadolinium (Gd), ytterbium (Yb) and yttrium (Y). (Although yttrium can be described as a transition metal, it is referred to herein as a rare earth metal due to its lanthanide-like properties.) Preferred rare earth metals include yttrium and erbium.
[0086] In an alternative embodiment, the FER mixture (which contains the FER zeolite product and the related mother liquor) obtained by heating the reaction gel at such a temperature and duration in step (b) is directly used, that is, the FER mixture formed by heating the reaction gel at such a temperature and duration is directly used without separating the FER zeolite from the mother liquor. In other words, the FER zeolite product and the related mother liquor formed in step (b) can be directly used as a precursor zeolite in the process for manufacturing chabazite-type (CHA) zeolite, making the process more efficient.
[0087] In an alternative embodiment, the FER is produced by methods described in the art, such as those described in US 4,650,654 and WO2020 / 021054.
[0088] The method of the present invention involves a first step of forming a reaction gel. The first step reaction gel comprises a precursor zeolite, an organic structure directing agent (OSDA), sodium hydroxide and / or potassium hydroxide and optionally a silica source.
[0089] The synthesis of zeolite crystals usually involves an organic template (also called a structure directing agent or SDA; similarly, an SDA cation may be referred to as an SDA + ) is used. During crystallization, alumina and silica combine together to form a crystalline structure around the OSDA. The reactants, reaction conditions, and OSDA species all affect the type or types of frameworks synthesized. When sufficient crystallization occurs, the crystals are removed from the mother liquor and dried. After the crystals are separated from the mother liquor, the organic SDA is thermally degraded and removed from the crystalline structure, leaving a porous molecular sieve.
[0090] The organic structure directing agent (OSDA) may be selected from N,N,N-trialkylcyclohexylammonium derivatives, such as N,N,N-dimethylethylcyclohexylammonium; N,N,N-trialkylbenzylammonium derivatives, such as benzyltrimethylammonium; trialkyl(cyclohexylmethyl)ammonium derivatives, such as trimethyl(cyclohexylmethyl)ammonium; [NR1R2R3R4]+, and wherein R1, R2; R3 and R4 are independently alkyl groups having one to four carbon atoms, wherein the alkyl groups may be optionally substituted with one or more hydroxyl groups, such as tetraethylammonium. In another embodiment, the OSDA is selected from a list comprising (e.g., consisting of) N,N,N-trimethyl-1-adamantylammonium, N,N,N-dimethylethylcyclohexylammonium, trimethyl(cyclohexylmethyl)ammonium and tetraethylammonium. In another embodiment, the OSDA may be N,N,N-dimethylethylcyclohexylammonium, used alone or in combination with another OSDA (e.g., N,N,N-trimethyl-1-adamantyl ammonium). Another preferred example of an OSDA cation for use in this method is N,N,N-trimethyladamantyl ammonium (TMAd + An alternative preferred example of the OSDA cation is N,N,N-dimethylethylcyclohexylammonium (DMECHA + ). The OSDA cation is usually associated with an anion, which can be any anion that is not detrimental to the formation of the zeolite. Representative anions include elements of Group 17 of the periodic table (e.g., fluorine, chlorine, bromine and iodine), hydroxide, acetate, sulfate, tetrafluoroborate, carboxylate, etc. In some embodiments, the OSDA anion is selected from hydroxide, halide, sulfate and / or carbonate. In a preferred embodiment, the anion is a hydroxide anion, i.e., OSDA is in the hydroxide form. In another preferred embodiment, OSDA is selected from TMAd+ and / or DMECHA+, more preferably selected from TMAdOH and / or DMECHAOH.
[0091] In a preferred embodiment, OSDA is selected from one or more of the following: N,N,N-trimethyl-1-adamantylammonium, N,N,N-dimethylethylcyclohexylammonium, trimethyl(cyclohexylmethyl)ammonium, tetraethylammonium, benzyltrimethylammonium, N,N,N-triethylcyclohexylammonium, N,N,N-trimethylcyclohexylammonium, N,N,N-diethylmethylcyclohexylammonium and triethylmethylammonium. In an even more preferred embodiment, OSDA is selected from one or more of the following: N,N,N-trimethyl-1-adamantylammonium, N,N,N-dimethylethylcyclohexylammonium and benzyltrimethylammonium. For example, OSDA may be N,N,N-trimethyl-1-adamantylammonium. OSDA may be N,N,N-dimethylethylcyclohexylammonium. The OSDA may be benzyltrimethylammonium, preferably in combination with another OSDA such as one selected from N,N,N-trimethyl-1-adamantylammonium, N,N,N-dimethylethylcyclohexylammonium, trimethyl(cyclohexylmethyl)ammonium, tetraethylammonium, benzyltrimethylammonium, N,N,N-triethylcyclohexylammonium, N,N,N-trimethylcyclohexylammonium and N,N,N-diethylmethylcyclohexylammonium.
[0092] In another embodiment, the OSDA may be N,N,N-dimethylethylcyclohexylammonium, used alone or in combination with another OSDA (e.g., N,N,N-trimethyl-1-adamantylammonium and / or benzyltrimethylammonium). In another embodiment, the OSDA may be benzyltrimethylammonium, used alone or in combination with another OSDA (e.g., N,N,N-trimethyl-1-adamantylammonium and / or N,N,N-dimethylethylcyclohexylammonium).
[0093] The OSDA may include trimethyl(cyclohexylmethyl)ammonium, such as trimethyl(cyclohexylmethyl)ammonium hydroxide, trimethyl(cyclohexylmethyl)ammonium halide, trimethyl(cyclohexylmethyl)ammonium sulfate, and / or trimethyl(cyclohexylmethyl)ammonium carbonate.
[0094]
[0095] The OSDA may include N,N,N-trimethyl-1-adamantyl ammonium, such as N,N,N-trimethyl-1-adamantyl ammonium hydroxide, N,N,N-trimethyl-1-adamantyl ammonium halide, N,N,N-trimethyl-1-adamantyl ammonium sulfate, and / or N,N,N-trimethyl-1-adamantyl ammonium carbonate.
[0096]
[0097] The OSDA may include trimethylphenylammonium, such as trimethylphenylammonium hydroxide, trimethylphenylammonium halide, trimethylphenylammonium sulfate, and / or trimethylphenylammonium carbonate.
[0098]
[0099] The OSDA may include N-ethyl-N,N-dimethylcyclohexylammonium, such as N-ethyl-N,N-dimethylcyclohexylammonium hydroxide, N-ethyl-N,N-dimethylcyclohexylammonium halide, N-ethyl-N,N-dimethylcyclohexylammonium sulfate and / or N-ethyl-N,N-dimethylcyclohexylammonium carbonate.
[0100]
[0101] The OSDA may include trimethylcyclohexylammonium, such as trimethylcyclohexylammonium hydroxide, trimethylcyclohexylammonium halide, trimethylcyclohexylammonium sulfate, and / or trimethylcyclohexylammonium carbonate.
[0102]
[0103] The OSDA may include benzyltrimethylammonium, such as benzyltrimethylammonium hydroxide, benzyltrimethylammonium halide, benzyltrimethylammonium sulfate, and / or benzyltrimethylammonium carbonate.
[0104]
[0105] The OSDA may include tetraethylammonium, such as tetraethylammonium hydroxide, tetraethylammonium halide, tetraethylammonium sulfate, or tetraethylammonium carbonate.
[0106]
[0107] The reaction gel of the first step of the method of the present invention is formed by adding one or both of sodium hydroxide and potassium hydroxide. When only one of sodium hydroxide and potassium hydroxide is used to form the reaction gel, sodium hydroxide is preferred.
[0108] The reaction gel of the first step of the method of the present invention may also contain a silicon dioxide source. Preferably, the silicon dioxide source is one or more of sodium silicate, potassium silicate, silica gel, silica sol, pyrogenic silica, silicon alkoxide and precipitated silica, preferably silica sol. Silica sol is a colloidal suspension of silicon dioxide in water.
[0109] In some embodiments, the reaction gel of the first step of the method does not contain an additional source of alumina.
[0110] As is known in the art, the reaction composition can be described by the equivalents of SiO2, Al2O3, M2O (where M is Na and / or K), OSDA, and H2O present in the reaction gel. In other words, the reaction gel composition can be described by the ratio Al2O3:aSiO2:bOSDA:cM2O:dH2O, where the reaction composition is normalized to the molar amount of Al2O3 equivalents (1 mole). It should be understood that the scale and absolute molar numbers of the reaction can vary.
[0111] In some embodiments, it is preferred that the gel contains 0.1 to 4 moles of OSDA relative to the molar amount of Al2O3 equivalents (i.e., 1 mole of Al2O3, which is provided by the alumina source, such as 2 moles of Al(OH)3). Preferably, the gel contains 0.2 to 2.5 moles of OSDA, more preferably 0.3 to 2 moles of OSDA relative to the molar amount of Al2O3 equivalents (i.e., "b" in the gel composition is 0.1 to 4, preferably 0.2 to 2.5, more preferably 0.3 to 2).
[0112] In some embodiments, the total amount of M2O equivalents, i.e., Na2O and K2O equivalents (one or both may be present), relative to the molar amount of Al2O3 equivalents is at least 1 mole, preferably 1 mole to 25 moles, more preferably 5 moles to 22 moles, more preferably 6 moles to 20 moles. Likewise, it can be said that "c" in the gel composition can be any of these ranges or values.
[0113] In some embodiments, it is preferred that the gel contains at least 20 moles, preferably 20 to 60 moles, 20 to 55 moles, or 20 to 50 moles of SiO2 equivalents relative to the molar amount of Al2O3 equivalents. Likewise, it can be said that "a" in the gel composition can be any of these ranges or values. In some preferred embodiments, about 30 moles of SiO2 equivalents are preferred.
[0114] In some embodiments, it is preferred that the gel contains water and that the water is present in an amount of at least 700 moles, preferably 750 moles to 3000 moles, relative to the molar amount of the Al2O3 equivalent. Likewise, it can be said that the "d" in the gel composition can be any of these ranges or values. For example, in some embodiments, higher amounts of water are preferred, such as 800 moles to 2600 moles, preferably 900 moles to 2500 moles.
[0115] In some embodiments, it is preferred that the molar ratio of water to silicon dioxide in the gel, i.e., the H2O / SiO2 molar ratio in the gel is 25 to 50, preferably 26 to 49, 27 to 48.5, 30 to 48, 32 to 47 or 33 to 46. In a preferred embodiment, the H2O / SiO2 molar ratio in the gel is 26 to 49, 30 to 48 or 32 to 47.
[0116] In some embodiments, it is preferred that the molar ratio of water to silicon dioxide in the gel, i.e., the H2O / SiO2 molar ratio in the gel is 2 to 50, preferably 3 to 40, 4 to 30, 5 to 20, 6 to 15 or 7 to 12. In a preferred embodiment, the H2O / SiO2 molar ratio in the gel is 5 to 15, 7 to 14 or 8 to 10.
[0117] A particular advantage of the inventive method is that the inventors have found that the method does not require the use of seeds to form the desired CHA zeolite. Therefore, preferably, the reaction gel of the second step does not include seeds (i.e., CHA seeds). "Does not include seeds" means that the reaction gel includes seeds less than 1 wt %, such as less than 0.9 wt %, less than 0.5 wt %, less than 0.3 wt %, less than 0.2 wt %, less than 0.1 wt % or less than 0.01 wt % based on the total weight of the reaction gel. In a preferred embodiment, the reaction gel includes 0 wt % seeds.
[0118] In one embodiment, the reaction gel of the second step does not contain seeds (i.e., the reaction gel contains less than 1 wt % of seeds, such as less than 0.9 wt %, less than 0.5 wt %, less than 0.3 wt %, less than 0.2 wt %, less than 0.1 wt % or less than 0.01 wt % of seeds, based on the total weight of the reaction gel), and OSDA is selected from the list comprising (e.g., consisting of) N,N,N-trimethyl-1-adamantylammonium, N,N,N-dimethylethylcyclohexylammonium, trimethyl(cyclohexylmethyl)ammonium, benzyltrimethylammonium and tetraethylammonium.
[0119] In a particularly preferred embodiment of the present invention, the reaction gel of the first step of the process of the present invention consists of a precursor zeolite, an organic structure directing agent (OSDA), sodium hydroxide and / or potassium hydroxide, a silica source and water and optionally further sodium and / or potassium salts.
[0120] The method of the present invention also includes the step of heating the reaction gel of the first step to a temperature suitable for the growth of CHA zeolite and for a duration suitable for the growth of CHA zeolite. Preferably, the temperature to which the reaction gel is heated for such a suitable duration is 100°C to 200°C; more preferably 110°C to 190°C, 120°C to 180°C, 120°C to 170°C, or even 125°C to 165°C. The duration for heating the reaction gel to a suitable temperature is preferably at least 10 hours, more preferably 20 hours to 60 hours. It is particularly preferred to heat the reaction gel to these temperatures and maintain these durations at these temperatures, for example, maintaining at least 10 hours at a temperature of 100°C to 200°C.
[0121] Preferably, the zeolite product produced by heating the reaction gel to such temperature and duration is recovered by typical vacuum filtration. Preferably, the filtered product is washed with demineralized (also called deionized) water to remove residual mother liquor. Preferably, the zeolite product is washed until the filtrate conductivity is less than 0.1 mS. Preferably, the filtered and washed product is then dried at a temperature greater than 100°C, preferably about 120°C.
[0122] The CHA zeolite product synthesized by the method of the present invention may include one or more non-framework alkali metals and / or alkaline earth metals. These metals are usually introduced into the reaction mixture in combination with a hydroxide ion source. Examples of such metals include sodium and / or potassium, as well as magnesium, calcium, strontium, barium, lithium, cesium and rubidium.
[0123] It is generally desirable to remove the alkali metal cations by ion exchange and replace them with hydrogen, ammonium or any desired metal ions. Thus, the zeolite formed by the process of the present invention may be a Na-type zeolite, a K-type zeolite or a combination of N, K-type, etc., or may be an H-type zeolite, an ammonium-type zeolite or a metal-exchanged zeolite. In a preferred embodiment, the CHA zeolite formed by the process of the present invention is an H-type zeolite.
[0124] Typical ion exchange techniques involve contacting the synthetic zeolite with a solution containing a salt of one or more cations desired to be replaced.While a variety of salts may be used, chlorides and other halides, nitrates, sulfates and carbonates are particularly preferred.
[0125] Representative ion exchange techniques are widely known in the art. Ion exchange occurs after synthesis and can occur before or after calcination of the zeolite. After contact with a salt solution of the desired replacement cation, the zeolite is typically washed with water and dried at a temperature ranging from 65°C to about 315°C, typically between 80°C and 150°C. After washing, the zeolite can be calcined in an inert gas and / or air at a temperature ranging from about 315°C to 850°C for a period of time ranging from 1 hour to 48 hours or more to produce a catalytically active and stable product.
[0126] In another embodiment, the method for making a chabazite-type (CHA) zeolite having a SAR of 8 to 35 may further include the step of loading one or more enhancing metals onto the CHA zeolite formed in step (ii). These enhancing metals (i.e., enhancing metals as described herein) may be loaded onto the CHA zeolite by incipient wetness, ion exchange, or during preparation of the washcoat slurry.
[0127] In another aspect of the present invention, there is provided a catalyst article for treating exhaust gas, the catalyst article comprising a CHA zeolite as described herein.
[0128] In yet another aspect, a method of treating an exhaust gas is provided, the method comprising contacting the exhaust gas with a catalyst article described herein.
[0129] In another aspect of the present invention, there is provided a hydrogen-type chabazite-type zeolite having a SAR of from 8 to 35 formed by the process as described herein.
[0130] Example
[0131] General steps :
[0132] The synthesis gel mixture is prepared by blending the selected raw materials at room temperature according to the synthesis gel composition. The resulting fluid mixture is then transferred to a stirred reactor and sealed. In the crystallization step, the synthesis gel is crystallized by hydrothermal treatment. The crystallization temperature is 120°C to 165°C, depending on the gel composition. The synthesis gel is continuously mixed by stirring and crystallization is performed. The duration of crystallization is 10 hours to less than 100 hours.
[0133] After crystallization, the resulting zeolite product is recovered by typical vacuum filtration. In the washing step, the residual mother liquor is removed from the solid product using demineralized water until the filtrate conductivity is below 0.1 mS. In the drying step, the filtered solid product is dehydrated by drying in an oven at 120°C overnight.
[0134] Synthesis of FER - Example 1: Preparation of FER from Synthesis Gel without OSDA
[0135] First, 14.07 g of aluminum hydroxide (55.8 wt% Al2O3) was dissolved in 32.84 g of sodium hydroxide solution (50.0 wt%) and 1221.8 g of the softened mixture under stirring at room temperature. Then, 231.3 g of silica sol solution (40.0 wt% SiO2) was added to the resulting clear solution and stirred continuously for 30 minutes. The molar composition of the resulting gel was 20.0SiO2-1.00Al2O3-2.67Na2O-1000.0H2O. The prepared initial gel was transferred to an autoclave and crystallized at 180°C under stirring for 3 days. The crystallized solid product was filtered and washed with demineralized water and dried at 120°C overnight. XRD and XRF measurement results showed that a zeolite with a FER framework structure and a SAR of 17.1 was obtained.
[0136] Synthesis of FER - Example 2: Preparation of FER from Synthesis Gel without OSDA
[0137] First, 11.27 g of aluminum hydroxide (55.8 wt% Al2O3) was dissolved in a mixture of 32.88 g of sodium hydroxide solution (50.0 wt%) and 1224.4 g of demineralized water under stirring at room temperature. Next, 231.5 g of silica sol solution (40.0 wt% SiO2) was added to the resulting clear solution and stirred continuously for 30 minutes. The molar composition of the resulting gel was 25.0SiO2-1.00Al2O3-3.33Na2O-1000.0H2O. The prepared initial gel was transferred to an autoclave and crystallized at 180°C under stirring for 3 days. The crystallized solid product was filtered and washed with demineralized water and dried at 120°C overnight. XRD and XRF measurement results showed that a zeolite with a FER framework structure and a SAR of 19.7 was obtained.
[0138] Synthesis of FER - Example 3: Preparation of FER from Synthesis Gel without OSDA
[0139] First, 47.5 g of sodium silicate solution (9.00 wt % Na2O, 28.8 wt % SiO2) was diluted with 723.5 g of demineralized water under stirring at room temperature. Separately, 11.34 g of sodium aluminate powder (52.7 wt % Al2O3) was dissolved in 351.0 g of demineralized water to form a clear solution under stirring at room temperature. Then, the latter solution was added to the former solution under vigorous stirring at room temperature, and 166.67 g of silica sol solution (40.0 wt % SiO2) was subsequently added to the mixture. The resulting mixture was continuously stirred for 15 minutes, and the molar composition was 22.8SiO2-1.00Al2O3-2.50Na2O-1140.0H2O. The prepared initial synthesis gel was transferred to an autoclave and crystallized at 180°C for 4 days under stirring. The crystallized solid product was filtered and washed with demineralized water and dried overnight at 120°C. XRD and XRF measurement results indicated that a zeolite having a FER framework structure and a SAR of 19.0 was obtained.
[0140] Synthesis of CHA - Example 1: Using FER without OSDA as aluminum source and N,N,N-trimethyl-1-adamantane TMAdOH as OSDA to synthesize CHA
[0141] 1,700 g of the initial synthesis gel was prepared by mixing the following ingredients: 109.0 g of the OSDA-free FER powder prepared according to Synthesis of FER - Example 1, 1,217.7 g of demineralized water, 13.91 g of sodium hydroxide solution (50.0 wt%), 136.04 g of TMAdOH solution (25.5 wt%), and 223.33 g of sodium silicate solution (28.8 wt% SiO2, 9.00 Na2O). The resulting mixture was stirred for 30 minutes, and its molar composition was 30.0SiO2-1.00Al2O3-6.00Na2O-2.00TMAdOH-1000.0H2O. The gel was then transferred to an autoclave and crystallized at 150°C under stirring for 26 hours. The crystallized solid product was recovered by vacuum filtration, washed with demineralized water, and dried overnight at 120°C.
[0142] The activated H-type of the synthesized zeolite product is obtained by the following procedure. First, the synthesized zeolite dry powder is calcined to burn off the OSDA substance. Using a muffle furnace, the heating rate is 1°C / min to 550°C and maintained at 550°C for six hours. The calcined product is then subjected to two ammonium exchanges to remove sodium ions from the zeolite product. Ammonium sulfate is used, and the ion exchange is performed at 80°C for two hours. The solid product is recovered by filtration and washing. The filter cake is dried at 120°C. The obtained NH4-type zeolite product is calcined again to convert it into an activated H-type zeolite product. The calcination is performed using a muffle furnace, the heating rate is 1°C / min to 550°C, and maintained at 550°C for two hours.
[0143] XRD, SEM and XRF measurements showed that pure phase CHA with SAR of 19.3 was obtained. Table 1 lists the synthesis batch and the obtained zeolite data.
[0144] Synthesis of CHA - Example 2 - Example 8: Synthesis of CHA by using FER without OSDA as aluminum source and N,N,N-trimethylol 1-Adamantyl ammonium hydroxide (TMAdOH) as OSDA for the synthesis of CHA
[0145] These synthesis examples require the same type of starting chemical reagents and are carried out in a similar manner to Example 1. Specific gel compositions, crystallization conditions, and the resulting activated product data are shown or referenced in Tables 1 and 2. In Examples 2 to 7, the desired OSDA-free FER was prepared according to Synthesis of FER - Example 1. In Example 8, the desired OSDA-free FER was prepared according to Synthesis of FER - Example 2.
[0146] Synthesis of CHA - Example 9: Synthesis of CHA by using pre-crystallized OSDA-free FER batch as aluminum source and N,N,N- Trimethyl-1-adamantyl ammonium hydroxide (TMAdOH) as OSDA for the synthesis of CHA
[0147] First, 357.3 g of synthesis gel for OSDA-free FER was prepared and crystallized according to Synthesis of FER - Example 2. Next, to this slurry, which was essentially a mixture of OSDA-free FER and mother liquor from zeolite, the following additional ingredients were added under stirring: 6.16 g of sodium hydroxide solution (50.0 wt%), 24.34 g of TMAdOH solution (25.5 wt%) and 15.32 g of sodium silicate solution (28.8 wt% SiO2, 9.00 Na2O). The molar composition of the resulting mixture was 30.0 SiO2-1.00 Al2O3-7.50 Na2O-2.00 TMAdOH-1369.0 H2O. The gel was crystallized in an autoclave at 150°C under stirring for 44 hours. The crystallized zeolite product was recovered and processed to an activated form in the same manner as in Example 1.
[0148] XRD, SEM and XRF measurements showed that pure phase CHA with SAR of 17.6 was obtained. Tables 1 and 2 also list the synthesis batch and the obtained zeolite data.
[0149] Synthesis of CHA - Example 10 - Example 14: By using pre-crystallized OSDA-free FER batch as aluminum source and N,N,N-trimethyl-1-adamantyl ammonium hydroxide (TMAdOH) as OSDA to synthesize CHA
[0150] These synthesis examples require a crystallized OSDA-free FER batch prepared according to FER Synthesis-Example 1. The types of other required starting chemical reagents are the same as those of Example 9. The preparation of CHA synthesis gel, crystallization, conversion of the prepared zeolite to the activated form product and characterization are carried out in the same manner as Example 9, see Tables 1 and 2.
[0151] Synthesis of CHA - Example 15: Synthesis of CHA by using FER without OSDA as aluminum source and N,N,N-trimethyl-1-gold A mixture of methyl ammonium hydroxide (TMAdOH) and N-ethyl, N,N-dimethylcyclohexyl ammonium hydroxide (R2OH) was used as OSDA To synthesize CHA
[0152] These synthesis examples were carried out in the same manner as in Example 1, except that N-ethyl, N,N-dimethylcyclohexyl ammonium hydroxide (R2OH) and TMAadOH were also used as OSDA. The preparation of CHA synthesis gel, crystallization, conversion of the prepared zeolite to the activated form product and characterization were carried out in the same manner as in Example 1, see Tables 1 and 2.
[0153] Synthesis of CHA - Example 16: By using pre-crystallized OSDA-free FER batch as aluminum source and N,N, N-Trimethyl-1-adamantyl ammonium hydroxide (TMAdOH) and N-ethyl, N,N-dimethylcyclohexyl ammonium hydroxide (R2OH) The mixture was used as OSDA to synthesize CHA
[0154] These synthesis examples were carried out in the same manner as in Example 9, except that N-ethyl, N,N-dimethylcyclohexyl ammonium hydroxide (R2OH) and TMAadOH were also used as OSDA. The preparation of CHA synthesis gel, crystallization, conversion of the prepared zeolite to the activated form product and characterization were carried out in the same manner as in Example 9, see Tables 1 and 2.
[0155] Synthesis of CHA - Example 17: By using USY as the aluminum source and N,N,N-trimethyl-1-adamantyl hydroxide ammonium hydroxide (TMAdOH) as OSDA to synthesize CHA
[0156] 403.2 g of the initial synthesis gel was prepared by mixing the following ingredients: 12.4 g of USY (SAR 11.26, Na2O 0.15%), 304.8 g of demineralized water, 4.16 g of sodium hydroxide solution (50.0 wt %), 24.4 g of TMAdOH solution (25.5 wt %) and 57.4 g of sodium silicate solution (28.8 wt % SiO2, 9.00 Na2O). The resulting mixture was stirred for 30 minutes and had a molar composition of 30.0 SiO2-1.00 Al2O3-7.47 Na2O-2.00 TMAdOH-1369.0 H2O. The crystallization of the gel, the conversion of the prepared zeolite to the activated form product and the characterization were carried out in the same manner as in Example 1, see Tables 1 and 2.
[0157] Synthesis of CHA - Example 18: By using USY as the aluminum source and N,N,N-trimethyl-1-adamantyl hydroxide A mixture of ammonium hydroxide (TMAdOH) and N-ethyl, N,N-dimethylcyclohexyl ammonium hydroxide (R2OH) was used as OSDA to synthesize CHA.
[0158] 1500.0 g of initial synthesis gel was prepared by mixing the following ingredients: 26.1 g of USY (SAR 11.26, Na2O 0.15%), 1130.2 g of demineralized water, 13.9 g of sodium hydroxide solution (50.0 wt %), 45.0 g of TMAdOH solution (25.5 wt %), 17.5 g of R2OH solution (53.6%) and 267.3 g of sodium silicate solution (28.8 wt % SiO2, 9.00 Na2O). The resulting mixture was stirred for 30 minutes and had a molar composition of 52.8SiO2-1.00Al2O3-15.43Na2O-1.76TMAdOH-1.76R2OH-2428.2H2O. The crystallization of the gel, the conversion of the prepared zeolite to the activated form product and the characterization were carried out in the same manner as in Example 1, see Tables 1 and 2.
[0159] Synthesis of CHA - Example 19: By using USY as the aluminum source and N,N,N-trimethyl-1-adamantyl hydroxide A mixture of ammonium hydroxide (TMAdOH) and N-ethyl, N,N-dimethylcyclohexyl ammonium hydroxide (R2OH) was used as OSDA to synthesize CHA.
[0160] 420.0 g of the initial synthesis gel was prepared by mixing the following ingredients: 21.6 g of USY (SAR 34.0, Na2O 0.00%), 333.5 g of demineralized water, 13.44 g of sodium hydroxide solution (50.0 wt %), 12.60 g of TMAdOH solution (25.5 wt %), 4.91 g of R2OH solution (53.6%) and 33.88 g of sodium silicate solution (28.8 wt % SiO2, 9.00 Na2O). The resulting mixture was stirred for 30 minutes and had a molar composition of 52.8SiO2-1.00Al2O3-15.43Na2O-1.76TMAdOH-1.76R2OH-2428.2H2O. The crystallization of the gel, the conversion of the prepared zeolite to the activated form product and the characterization were carried out in the same manner as in Example 1, see Tables 1 and 2.
[0161] Synthesis of CHA - Example 20: By using Na-type OSDA-free FER batch as aluminum source and N-ethyl, N, N-Dimethylcyclohexylammonium hydroxide (R2OH) as OSDA to synthesize CHA
[0162] 180.0 g of initial synthesis gel was prepared by mixing the following ingredients: 36.07 g of OSDA-free FER powder prepared according to Synthesis of FER - Example 3, 67.2 g of demineralized water, 1.02 g of sodium hydroxide solution (50.0 wt%), 17.30 g of N-ethyl, N, N-dimethylcyclohexyl ammonium hydroxide solution (53.6 wt%) and 58.4 g of sodium silicate solution (28.8 wt% SiO2, 9.00 Na2O). The resulting mixture was stirred for 30 minutes and had a molar composition of 30.0 SiO2-1.00 Al2O3-4.70 Na2O-2.10 R2OH-250.0 H2O. The gel was then transferred to an autoclave and crystallized at 150°C under stirring for 92 hours. The crystallized zeolite product was recovered and processed into an activated form in the same manner as in Example 1. XRD, SEM and XRF measurements showed that pure phase CHA with SAR of 20.4 was obtained. Tables 1 and 2 also list the synthesis batch and the obtained zeolite data.
[0163] Synthesis of CHA - Comparative Example A: Synthesis of CHA by using a precipitated amorphous aluminosilicate filter cake as an aluminum source and N,N,N- Trimethyl-1-adamantyl ammonium hydroxide (TMAdOH) as OSDA for the synthesis of CHA
[0164] First, an amorphous aluminosilicate wet cake was prepared by blending a sodium silicate solution (28.8 wt% SiO2, 9.00 Na2O) solution with a solution prepared by mixing a 25% sulfuric acid solution and an aluminum sulfate solution at 80°C. The resulting mixture was stirred for 30 min, then filtered and thoroughly washed with demineralized water. Next, 127.4 g of the amorphous aluminosilicate cake thus prepared (SAR 30.6) was used to prepare 440.0 g of a synthesis gel for CHA by mixing with other ingredients including 259.0 g of demineralized water, 18.6 g of a sodium hydroxide solution (50.0 wt%) and 35.0 g of a TMAdOH solution (25.5 wt%). The resulting gel was stirred for 30 minutes and had a molar composition of 30.6 SiO2-1.00 Al2O3-7.50 Na2O-2.00 TMAdOH-1000.0 H2O. The crystallization of the gel, the conversion of the prepared zeolite into the activated form product and the characterization were carried out in the same way as in Example 1, see Tables 1 and 2.
[0165] Synthesis of CHA - Comparative Example B: Synthesis of CHA by using precipitated amorphous aluminosilicate dry powder as aluminum source and N,N,N- Trimethyl-1-adamantyl ammonium hydroxide (TMAdOH) as OSDA for the synthesis of CHA
[0166] This synthesis example is the same as Comparative Example A, except that the amorphous aluminosilicate filter cake is dried overnight at 120°C and then used to prepare the CHA synthesis gel, see Tables 1 and 2.
[0167] Synthesis of CHA - Comparative Example C: By using aluminum nitrate as an aluminum source and N,N,N-trimethyl-1-adamantyl hydrogen Ammonium oxide (TMAdOH) as OSDA to synthesize CHA
[0168] 403.2 g of the initial synthesis gel was prepared by mixing the following ingredients: a solution of 6.23 g of aluminum nitrate nonahydrate (98%) dissolved in 283.2 g of demineralized water, 20.6 g of sodium hydroxide solution (50.0 wt %), 23.90 g of TMAdOH solution (25.5 wt %), 15.32 g of sodium silicate solution (28.8 wt % SiO2, 9.00 Na2O) and 53.9 g of silica sol solution (40.0 wt % SiO2). The resulting mixture was stirred for 30 minutes and had a molar composition of 52.8SiO2-1.00Al2O3-15.43Na2O-3.52TMAdOH-6.00NaNO3-2428.2H2O. The crystallization of the gel, the conversion of the prepared zeolite to the activated form product and the characterization were carried out in the same manner as in Example 1, see Tables 1 and 2.
[0169] Evaluation Example: Preparation of Catalysts and Application for NO x Performance measurement of selective catalytic reduction (SCR)
[0170] The activated products of Examples #1 and #2 from the synthesis of CHA were loaded with 3.5 wt% Cu on an anhydrous basis in H-type CHA by incipient wetness impregnation using the required amount of copper (II) acetate dissolved in a predetermined amount of demineralized water. The metal-impregnated zeolite was dried overnight at 80°C and then calcined in air at 550°C for 4 hours. Each calcined Cu-CHA was granulated, crushed and sieved to collect particles with a size between 40 mesh and 60 mesh. The Cu-CHA in granular form thus prepared was referred to as a fresh Cu-CHA sample. The following aging treatments were applied to each fresh Cu-CHA: 650°C for 100 hours in a gas stream containing 10 vol% H2O; 750°C for 80 hours in a gas stream containing 10 vol% H2O; 800°C for 16 hours in a gas stream containing 10 vol% H2O, and 900°C for 5 hours in a gas stream containing 5 vol% H2O.
[0171] The fresh and aged samples of each Cu-CHA catalyst were subjected to NO xNH3-SCR evaluation. For comparison, two commercial CHAs, CHA1 (SAR of 18.5) and CHA2 (SAR of 12.8), were evaluated under exactly the same conditions. The amount of each catalyst used in the test was 0.3 g. A gas stream containing 500 ppm NO, 550 ppm NH3, 350 ppm 10% H2O and 10% O2 was used. The flow rate of the gas stream used was 2.6 L / min, equivalent to 520 liters / hour per gram of catalyst. The sample was heated from room temperature to 150°C under the above gas mixture (except NH3). At 150°C, NH3 was added to the gas mixture and the sample was kept under these conditions for 30 minutes. The temperature was then raised from 150°C to 500°C at a rate of 5°C / min. The downstream gas treated by the catalyst was monitored to determine NO x Conversion and N2O selectivity, see Figures 23 to 30 .
[0172] Figures 23 to 30 It is shown that Example 1 is highly active in NO conversion under all conditions tested, and its overall performance is comparable to that of CHA1. Example 1 performs better than CHA1 when fresh and after mild (650°C, 100h) and moderate aging (750°C, 80h), while CHA1 performs slightly better after moderate and highly severe aging. Under all conditions tested, Example 2 matches or performs slightly better than CHA2 in NO conversion.
[0173] Table 1. List of gel composition and crystallization condition data of CHA synthesis examples and comparative synthesis examples
[0174]
[0175]
[0176] Table 2. List of characterization data of activated CHA products
[0177]
[0178]
Claims
1. A hydrogen-type chabazite-type (CHA) zeolite having a SAR of 8 to 35, and a ratio of XRD peak intensities corresponding to [21 1] and [-1 1 1] reflections being equal to or greater than 0.
80.
2. The hydrogen-type CHA zeolite according to claim 1, which has a SAR of 8 to 17, and a ratio of XRD peak intensities corresponding to [2 1 1] and [-1 1 1] reflections is equal to or greater than 0.
95.
3. The hydrogen-type CHA zeolite according to claim 1, which has a SAR of 17 to 24, and a ratio of XRD peak intensities corresponding to [2 1 1] and [-1 11] reflections is equal to or greater than 0.
85.
4. The hydrogen-type CHA zeolite according to claim 1, which has a SAR of 24 to 34, and a ratio of XRD peak intensities corresponding to [2 1 1] and [-1 11] reflections is equal to or greater than 0.
80.
5. The hydrogen-form CHA zeolite according to any preceding claim, wherein the CHA zeolite comprises uniform and non-aggregated cubic crystals having an average size of 1 μm to 10 μm.
6. The hydrogen-form CHA zeolite according to any preceding claim, wherein the CHA zeolite comprises uniform and non-aggregated aggregated crystals.
7. The hydrogen-type CHA zeolite according to any one of claims 1 to 4, wherein the CHA zeolite comprises a mixture of (a) uniform and non-aggregated cubic crystals having an average size of 1 μm to 10 μm and (b) uniform and non-aggregated aggregated crystals.
8. A CHA zeolite in the hydrogen form according to any preceding claim, wherein the zeolite has a crystallinity greater than 90%.
9. A method for producing a chabazite-type (CHA) zeolite having a SAR of 8 to 35, the method comprising: (i) forming a reaction gel comprising a precursor zeolite, an organic structure directing agent (OSDA), sodium hydroxide and / or potassium hydroxide and optionally a silica source, and (ii) heating the reaction gel to a temperature and for a duration suitable for the growth of the CHA zeolite.
10. The method of claim 9, wherein the precursor zeolite is selected from the group consisting of FER, FAU, MFI, BEA and LTL.
11. The method according to claim 9 or claim 10, wherein the precursor zeolite is prepared from a synthesis gel without an organic structure directing agent or from a synthesis gel with an organic structure directing agent.
12. The method according to any one of claims 9 to 11, wherein the precursor zeolite is prepared by a method comprising the steps of: (a) forming a reaction gel comprising an aluminum source, sodium hydroxide and / or potassium hydroxide and a silicon dioxide source, (b) heating the reaction gel to a temperature and for a duration suitable for the growth of the FER zeolite, and optionally (c) The obtained FER zeolite is filtered and washed.
13. The method of claim 12, wherein the reaction gel does not contain OSDA.
14. A process according to claim 12 or claim 13, wherein the FER zeolite product and associated mother liquor formed in step (b) is used directly without separating the FER zeolite from the mother liquor.
15. The process according to any one of claims 9 to 14, wherein the OSDA used in step (i) is selected from one or more of the following: N,N,N-trimethyl-1-adamantylammonium, N,N,N-dimethylethylcyclohexylammonium, trimethyl(cyclohexylmethyl)ammonium, tetraethylammonium, N-ethyl-N,N-dimethylcyclohexylammonium, benzyltrimethylammonium, N,N,N-triethylcyclohexylammonium, N,N,N-trimethylcyclohexylammonium, N,N,N-diethylmethylcyclohexylammonium, trimethylcyclohexylammonium, trimethylphenylammonium and triethylmethylammonium.
16. The method according to any one of claims 9 to 15, wherein the reaction gel of step (i) does not contain CHA seeds.
17. The method according to any one of claims 9 to 16, wherein the temperature of step (ii) is from 100°C to 200°C, preferably from 110°C to 190°C.
18. The method according to any one of claims 9 to 17, wherein the duration of step (ii) is at least 10 hours, preferably 20 hours to 60 hours.
19. The method according to any one of claims 9 to 18, which is used for preparing the hydrogen-type CHA zeolite according to any one of claims 1 to 8.
20. A catalyst product for treating exhaust gas, the catalyst product comprising the hydrogen-type CHA zeolite according to any one of claims 1 to 8 or the hydrogen-type CHA zeolite obtainable by the method according to any one of claims 9 to 18.
21. A method for treating an exhaust gas, the method comprising contacting the exhaust gas with the catalyst article according to claim 20.
22. A hydrogen-type chabazite-type (CHA) zeolite having a SAR of 8 to 35 and formed by the method of any one of claims 9 to 18.
Citation Information
Patent Citations
Chabazite-type zeolite and process for producing the same
US10029247B2
Chabazite-type zeolite and method of manufacturing chabazite-type zeolite
US10407314B2
CHA-type zeolite and method for producing the same
US10953390B2
Zeolite SSZ-13 and its method of preparation
US4544538A
Process for preparation of ferrierite type zeolites
US4650654A