Method for producing steel and sponge iron manufacturing method

By utilizing the thermal energy of iron ore oxide materials to heat the reducing agent in a direct reduction facility, combined with a carburizing zone or carburizing reactor, efficient and low-emission steel production has been achieved, solving the problems of renewable energy fluctuations and dependence on fossil fuels, and realizing sustainable steel production.

CN118984880APending Publication Date: 2024-11-19LOUSSAVAARA KIIRUNAVAORA AB
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380030426.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-01
Filing Date
2023-03-31
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Existing steel production methods are unable to effectively cope with fluctuations in renewable energy production, resulting in low energy efficiency. Furthermore, the use of fossil fuels leads to high CO2 and NOx emissions, making it difficult for current technologies to achieve sustainable, low-emission steel production on an industrial scale.

Method used

By using the thermal energy of iron ore oxide materials to heat the reducing agent in a direct reduction facility, a chemical reaction is achieved between the iron ore oxide materials and the reducing agent, reducing the dependence on high-temperature heating. Renewable energy sources such as hydropower, wind power, and photovoltaic power are used to produce hydrogen and oxygen. Carbon is incorporated into the process in a carburizing zone or carburizing reactor, forming a highly efficient and low-emission steel production process.

Benefits of technology

It has enabled high-efficiency steel production on an industrial scale, primarily using renewable energy, reducing dependence on fossil fuels, lowering CO2 and NOx emissions, improving energy efficiency, and enabling it to cope with fluctuations in renewable energy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118984880A_ABST
    Figure CN118984880A_ABST
Patent Text Reader

Abstract

The invention relates to a method and an arrangement for producing steel whereby iron ore oxide material (5) is reduced with a reducing agent (H) in a direct reduction plant (7). The reducing agent (H) is generated by electrolyzing water by means of an electrolysis unit (17). The electrical energy required for electrolysis comprises renewable energy originating from hydraulic and / or wind and / or photovoltaic or other renewable energy form (2). If sufficient reducing agent can be obtained, the intermediate product (RM) is produced independently of the current demand. The iron ore oxide material (5), which maintains thermal energy, is charged into a direct reduction plant (7). A thermal energy source is provided from an iron ore oxide material supply plant, such as an iron ore oxide material production unit (3) or a preheating plant (4). The iron ore oxide material (5) is reduced to an intermediate product (RM) by reacting a reducing agent (H) with the iron ore oxide material (5) using the thermal energy of the iron ore oxide material (5).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates primarily to a process for producing steel whereby an iron ore oxide material is reduced with a reducing agent and the intermediate product (direct reduced iron ore material) and eventual accompanying materials so obtained are metallurgically processed.

[0002] The invention also relates to a steel production arrangement and to a data program programmed to cause the steel production arrangement to perform the method.

[0003] The present disclosure may relate to methods for producing carbon-free intermediate products.

[0004] The present invention mainly relates to the mining industry producing direct reduced iron ore materials and / or the steelmaking industry producing steel. In addition, the present invention may also relate to manufacturers and suppliers of iron ore oxide material providing equipment, direct reduction facilities, steel production equipment, etc. Background Art

[0005] Different methods of coping with fluctuations in the production of renewable energy used in a process for producing steel are known today.

[0006] One way to cope with fluctuations could be to store renewable energy with the intermediate product itself and use it as a storage means for storing renewable energy until the intermediate product is processed by the steel industry.

[0007] Current steel production can be carried out by producing pig iron in the so-called hot furnace process. In such production, very large amounts of CO are usually released. 2 Furthermore, the so-called "direct reduction process" is known (processes under the brands MIDREX, FINMET, ENERGIRON / HYL etc.), in which the sponge iron (intermediate product) produced can be in the form of HDRI (hot direct reduced iron), CDRI (cold direct reduced iron) or so-called HBI (hot briquetted iron).

[0008] Today's steelmaking industry often uses sponge iron in the form of HDRI, CDRI and HBI to produce steel, and the sponge iron is usually processed in electric furnaces (which are very energy intensive) or in LD-converters (basic oxygen furnace steelmaking where carbon-rich pig iron is made into steel).

[0009] Today, in order to produce the intermediate products, direct reduction is provided using direct reduction facilities by introducing heated hydrogen into the direct reduction facility to heat the iron ore oxide material charged into the direct reduction facility to provide a chemical reaction between the hydrogen and the iron ore oxide material. If desired, some existing processes utilize hydrogen and carbon monoxide from methane and synthesis gas. For example, in the so-called MIDREX process, methane is converted into carbon-containing molecules (CH 4 +CO 2 =2CO+2H 2 ), provided that the iron ore oxide reacts with the obtained reducing gas; Fe 2 O 3 +6CO(H 2 )=2Fe+3CO 2 (H 2 O)+3CO(H 2 ).

[0010] At least one aspect described herein may relate to a method of processing a carbon-free intermediate product for producing steel while addressing fluctuations in renewable energy production.

[0011] At least one aspect described herein may relate to a method of processing a carbon-containing intermediate product for producing steel while addressing fluctuations in renewable energy production.

[0012] At least one aspect described herein may relate to a method for producing steel by processing a carbon-containing intermediate product by incorporating carbon during reduction of an iron ore oxide material while addressing fluctuations in renewable energy production.

[0013] At least one aspect described herein may relate to a method for producing steel by processing carbon containing intermediate products by incorporating carbon into direct reduced iron ore material in a separate carburizing zone of a direct reduction facility and / or in a carburizing reactor while addressing fluctuations in renewable energy production.

[0014] Therefore, current methods use the intermediate product itself as a storage means for storing renewable energy in order to cope with fluctuations in the production of regeneratively generated electrical energy.

[0015] In most of the steelmaking industry and the methods used to produce steel, a sustainable, comprehensive production concept for producing steel on an industrial scale and in an optimal manner based on renewable resources is lacking.

[0016] Known technology introduces heat energy into the hydrogen injected into the direct reduction facility for generating the heat energy required for the chemical reaction between the hydrogen and the iron ore oxide material. The hydrogen to be injected has a very high temperature (eg 700°C to 1050°C) for providing the chemical reaction.

[0017] However, this preliminary and intense heating of the hydrogen destroys the reduction potential of the hydrogen.

[0018] In some cases and to compensate for the loss of the reduction potential of the heated hydrogen, the hydrogen is reused and reheated, which further destroys the reduction potential of the hydrogen.

[0019] In some cases and in order to compensate for the loss of said reducing potential of the heated hydrogen, additional hydrogen is introduced into the direct reduction facility. However, the additional addition of hydrogen and heating for the production of intermediate products is not an efficient way to provide a steel production process in a fossil-free manner or at least in a substantially fossil-free manner.

[0020] According to the known method, the chemical reaction means that oxygen is reduced from the iron ore oxide material by means of heated hydrogen, whereby the temperature of the iron ore oxide material will increase under the reduction.

[0021] Accordingly, the direct reduced iron ore material is discharged from the direct reduction facility and will have a high temperature due to the transfer of thermal energy of the hydrogen heated during reduction from the hydrogen to the iron ore material.

[0022] Therefore, the direct reduced iron ore material discharged from the direct reduction facility must be cooled, which undermines the energy efficiency of the steel production process and is therefore not optimal.

[0023] Direct reduction of iron ore oxide material may be referred to as a solid state process of reducing iron ore oxide material to direct reduced iron ore material at a temperature below the melting point of the iron ore.

[0024] The prior art described in US2015 / 0259760 aims to solve the problem of how to use renewable resources for steel production on an industrial scale, from the perspective of the production value chain required to produce steel from iron ore, using a direct reduction method to reduce iron ore oxides into intermediate products.

[0025] There have long been several approaches that have proposed effective solutions to the existing technical problem of how to store and cope with fluctuations in the production of renewable energy in an efficient manner.

[0026] The technology described in US2015 / 0259760 uses the intermediate product itself as a storage means for storing renewable energy until an electric furnace or an LD converter is used to process the intermediate product in the steelmaking industry. This storage provided by the prior art is a way to cope with fluctuations in the production of renewable energy. According to US2015 / 0259760, another way to store renewable energy includes that if excess renewable energy is available, the renewable energy can be stored in the form of hydrogen, thereby compensating for temporary fluctuations in the production of renewable energy.

[0027] According to US2015 / 0259760, a direct reduction facility configured for reducing iron ore can utilize hydrogen generated on site at the direct reduction facility, and an electric furnace of the steelmaking industry can use the renewable energy (e.g., wind, hydroelectric or solar). According to US2015 / 0259760, the temperature of the hydrogen can be adjusted by a heater or partial oxidation. The temperature of the hydrogen can be 450°C up to 1200°C, preferably 600°C to 1200°C, and in particular 700°C to 900°C.

[0028] Another prior art document WO 2021 / 225500 A1 discloses heating the reducing gas to 1050° C. for direct reduction.

[0029] Another prior art document US2021 / 0246521 discloses heating the reducing gas to above 700°C for the direct reduction. Summary of the invention

[0030] The aim is to provide a method for producing steel using renewable energy as efficiently as possible while coping with fluctuations in renewable energy production, and / or a method for producing intermediate products such as sponge iron (DRI, HBI, etc.) as efficiently as possible.

[0031] The aim is to provide an energy-saving and time-saving process for producing steel using renewable energy on an industrial scale, both from the perspective of the renewable energy required and to cope with fluctuations in the production of renewable energy.

[0032] The aim is to develop methods for producing steel in a sustainable manner with an integrated production concept based on renewable energy.

[0033] The aim was to provide a method by which it is possible to produce a product in an optimal manner and with CO on an industrial scale. 2 Neutral emissions and / or CO 2 Low emissions and / or no CO 2 production of intermediate products and / or steel.

[0034] The aim is to provide 2A method for producing steel in an energy-efficient manner while reducing NOx emissions.

[0035] The objective is to minimise the use of hydrogen as a reducing agent for the reduction of iron ore oxide materials in a direct reduction facility.

[0036] The aim is to minimise the use of renewable energy required to run the electrolysis unit that produces hydrogen and oxygen.

[0037] The purpose is to maintain the reducing potential of the hydrogen during the reduction of the iron ore oxide material to the intermediate products.

[0038] The objective is to maintain high chemical reactivity and / or driving force of the hydrogen which is essential to provide an efficient chemical reaction between the hydrogen and the iron ore oxide material.

[0039] The aim is to provide carbon-containing intermediate products which are produced in a fossil-free manner or at least in a substantially fossil-free manner.

[0040] The aim is to provide carbon-free intermediate products which are produced in a fossil-free manner or at least in a substantially fossil-free manner.

[0041] The object is to provide a method for producing steel and a steel production arrangement which makes it possible to produce carbon-free and / or carbon-containing intermediate products in an energy-efficient manner.

[0042] The objective is to provide efficient reduction of the iron ore oxide material whilst achieving effective control of the thermal treatment process by selectively maintaining the reduction potential of the reducing agent to achieve efficient production of reduced iron ore material that resists reoxidation.

[0043] The aim is to provide a cost effective delivery supply chain for reduced iron ore material to other industries such as the steel industry.

[0044] The aim is to produce reduced iron ore material that can be used in cost-effective steel production using, for example, an electric arc furnace.

[0045] These objects or at least one of the objects has been achieved by a method for producing steel, whereby an iron ore oxide material is reduced with a reducing agent in a direct reduction facility and intermediate products and final accompanying substances of the directly reduced iron ore material thus obtained are metallurgically treated; the reducing agent is produced by electrolysis of water with the aid of an electrolysis unit; the electrical energy required for the electrolysis can be renewable energy in the form of hydropower and / or wind power and / or photovoltaic or other renewable energy sources, and the intermediate products are produced independently of current demand if sufficient reducing agent is available, wherein the iron ore oxide material is supplied from the iron ore oxide material to the facility; The device is transported to a direct reduction facility and maintains the thermal energy from the iron ore oxide material providing device, the direct reduction facility is configured to introduce a reducing agent, the reducing agent is suitable for reacting with the iron ore oxide material maintaining the thermal energy, thereby heating or further heating the introduced reducing agent by utilizing the thermal energy of the iron ore oxide material to achieve a chemical reaction between the iron ore oxide material and the reducing agent, reducing the iron ore oxide material to an intermediate product, for providing an energy-saving and time-saving process for producing steel using renewable energy on an industrial scale, and for conserving renewable energy to cope with fluctuations in the production of regeneratively generated electrical energy.

[0046] In this way an effective solution is achieved how to store renewable energy in an efficient manner and cope with fluctuations in steel production.

[0047] In this way, an energy-efficient method for producing steel is achieved.

[0048] By directly conveying the iron ore oxide material from the iron ore oxide material supply device to the direct reduction facility, the iron ore oxide material retains the thermal energy derived from the iron ore oxide material supply device, and a very efficient reduction and chemical reaction between the iron ore oxide material and the reducing agent is achieved. For example, it is not necessary to heat the reducing agent to a high temperature (e.g., above 700° C.), instead, the present disclosure utilizes the thermal energy of the iron ore oxide material that retains the thermal energy derived from the iron ore oxide material supply device, thereby preserving the reduction potential of the reducing agent.

[0049] By utilizing the thermal energy of the iron ore oxide material to heat or further heat the introduced reducing agent to achieve a chemical reaction between the iron ore oxide material and the reducing agent, the reduction potential of the reducing agent is maintained, thereby achieving rapid reduction using less reducing agent (reducing the use and production of renewable energy, which means high flexibility in responding to fluctuations in the production of renewable energy used to produce reducing agents by electrolysis).

[0050] Alternatively, if sufficient regeneratively generated electrical energy is available, the reducing agent is produced independently of current demand and the produced reducing agent is temporarily stored to cope with fluctuations in renewable energy production.

[0051] Alternatively, the iron ore oxide material is reduced in a direct reduction facility with a reducing agent, which is produced by the electrolysis of water.

[0052] Alternatively, the electrical energy required for electrolysis comprises renewable energy from hydropower and / or wind power and / or photovoltaic or other forms of renewable energy.

[0053] Alternatively, if sufficient reducing agent is available, the intermediate product is produced independently of current demand.

[0054] Alternatively, if sufficient regeneratively generated electrical energy is available, the reducing agent and / or intermediate product (e.g., direct reduced iron ore material) is always produced independently of current demand; and the unneeded intermediate product is stored until needed / used, so that the renewable energy stored therein is also stored; during the reduction of the iron ore oxide material to the intermediate product, a carbon- or hydrogen-containing gas is added to the reducing agent to incorporate carbon into the intermediate product, the amount of carbon- or hydrogen-containing gas added to the reducing agent used for reduction being at least such that the carbon content in the intermediate product is 0.0005 mass % to 6.3 mass %, and the carbon- or hydrogen-containing gas is methane or other carbon-containing gas from biogas production or from pyrolysis of renewable raw materials, or is synthesis gas from biomass.

[0055] Alternatively, the reducing agent used for reduction has added thereto a carbon-containing or hydrogen-containing gas in an amount at least sufficient to make the carbon content in the intermediate product 1 mass % to 3 mass %.

[0056] Alternatively, the reducing agent used for the reduction comprises hydrogen gas which is used to reduce the iron ore oxide material, thereby providing a chemical conversion to a carbon-free intermediate product.

[0057] Alternatively, the reducing agent (eg consisting of hydrogen and possibly a carbon-containing gas) is introduced into the reduction process at a temperature below the temperature of the iron ore oxide material charged to the direct reduction facility.

[0058] Alternatively, the reducing agent may be preheated to a certain degree before being introduced into the direct reduction facility, wherein the temperature of the introduced reducing agent may be about 300° C. to about 700° C., preferably about 400° C. to about 650° C. In this case, the temperature of the iron ore oxide material to be charged into the direct reduction facility is always higher than the temperature of the reducing agent. For example, if the temperature of the reducing agent is lower than 700° C., the temperature of the iron ore oxide material charged into the direct reduction facility is controlled to be higher, thus higher than 700° C. For example, if the temperature of the reducing agent is lower than 600° C., the temperature of the iron ore oxide material charged into the direct reduction facility is higher, for example, higher than about 650° C.

[0059] By utilizing the thermal energy of the iron ore oxide material to heat or further heat the introduced reducing agent, a chemical reaction between the iron ore oxide material and the reducing agent is achieved in an energy efficient manner. During reduction, the thermal energy of the iron ore oxide material has a value that enables the reducing agent to be heated or further heated to achieve the chemical reaction.

[0060] Alternatively, in the case of carburizing the discharged direct reduced iron ore material, the introduced reducing agent may be preheated to a degree to increase the desired temperature of the direct reduced iron ore material, but the iron ore oxide material still retains thermal energy hotter than the reducing agent during the chemical reaction.

[0061] Alternatively, the overpressure in the reduction is from 0 bar to 15 bar.

[0062] Alternatively, the temperature of the discharged direct reduced iron ore material from the direct reduction facility may be from about 20°C to 500°C or from about 400°C to 700°C, preferably from about 500°C to 650°C.

[0063] For example:

[0064] - The temperature of the iron ore oxide material when charged into the direct reduction facility is about 1100°C.

[0065] - The temperature of the reducing agent (e.g., a hydrogen content of 100 volume %) when introduced into the direct reduction facility is about 500°C, wherein the reducing agent reacts with the iron ore oxide material by utilizing the thermal energy of the iron ore oxide material to heat or further heat the introduced reducing agent to achieve a chemical reaction between the iron ore oxide material and the reducing agent, thereby reducing the iron ore oxide material to an intermediate product.

[0066] - The temperature of the direct reduced iron ore material ready to be discharged from the direct reduction facility and / or ready to be carburized is about 600°C (1100°C - 500°C).

[0067] In this manner, for example, the direct reduced iron ore material has a desired temperature of about 600° C. at which carburization of the direct reduced iron ore material is most effective.

[0068] Alternatively, the control circuit is suitable for controlling the temperature of the iron ore oxide material delivered to the direct reduction facility and / or controlling the internal gas pressure in the direct reduction facility and / or the reducing agent temperature and / or the reducing agent gas pressure of the introduced reducing agent to achieve (with the aim of) a desired temperature (e.g., 600°C).

[0069] Alternatively, the control circuit is adapted to control the iron ore oxide material production unit so that the iron ore oxide material has a specific temperature (eg, about 1100° C.) so that the direct reduced iron ore material reaches the desired temperature (eg, about 600° C.).

[0070] For example, the amount of hydrogen and / or oxygen generated by the electrolysis unit and used by the iron ore oxide material production unit can be adjusted to provide heat for the hardening process (oxidation and / or sintering) performed by the hardening device of the iron ore oxide material production unit, thereby producing iron ore oxide material that retains thermal energy.

[0071] Alternatively, the control circuit is adapted to control the preheating device to provide the iron ore oxide material with a specific temperature (eg, about 1100° C.) so that the direct reduced iron ore material reaches the desired temperature (eg, about 600° C.).

[0072] Alternatively, the discharged direct reduced iron ore material may be carburized in a separate carburizing reactor, wherein the method for reducing the iron ore oxide material is configured to provide a direct reduced iron ore material having a temperature of, for example, about 400°C to 700°C, preferably about 500°C to 650°C to be discharged from the direct reduction facility and directly conveyed to the separate carburizing reactor.

[0073] Alternatively, the direct reduction facility is configured to be charged with iron ore oxide material having a temperature in the range of about 800°C to 1300°C.

[0074] Alternatively, the direct reduction facility is configured to be charged with iron ore oxide material having a temperature in the range of about 700°C to 1400°C.

[0075] Alternatively, the direct reduction facility is configured to be charged with iron ore oxide material having a temperature in the range of about 600°C to 1500°C.

[0076] Alternatively, the direct reduction facility is configured to be charged with iron ore oxide material having a temperature in the range of about 500°C to 1600°C, preferably in the range of about 800°C to 1300°C.

[0077] Alternatively, the direct reduction facility is configured to be charged with iron ore oxide material to retain heat energy, the heat energy being generated by the iron ore oxide material supply facility.

[0078] Alternatively, the iron ore oxide material delivered to the direct reduction facility from the iron ore oxide material supply facility exhibits thermal energy (thermal energy) originating from a manufacturing heat process or preheating device, corresponding to a temperature above 500°C.

[0079] Alternatively, when the thermal energy (heat energy) originating from the manufacturing heat process or the preheating device corresponds to a temperature higher than 900°C, the iron ore oxide material is transported from the iron ore oxide material supply device to the direct reduction facility.

[0080] Alternatively, the substantially or completely endothermic chemical reaction may consume heat energy equivalent to about 300°C to 700°C, preferably about 450°C to 550°C, extracted from the iron ore oxide material retaining heat energy during the reduction and chemical reactions carried out in the direct reduction facility.

[0081] Alternatively, the iron ore oxide material providing device provides the iron ore oxide material (agglomerate or pellet) maintained at a temperature of about 900°C to 1300°C, preferably about 1000°C to 1100°C.

[0082] In this manner less heating of the hydrogen is required to effect the chemical reaction and reduction of the iron ore oxide material.

[0083] In this way it is achieved that the reduction potential of the hydrogen will not be destroyed during the chemical reaction and reduction process.

[0084] Alternatively, the direct reduction facility may be formed as a shaft furnace, a rotary kiln, or a cross-flow or counter-flow heat exchanger or other direct reduction facility configured for reducing iron ore oxide material.

[0085] Alternatively, the direct reduction facility may be configured to operate under pressure.

[0086] By increasing the internal gas pressure in the reduction facility, it is achieved that the gas volume can be reduced, which is cost-effective and space-saving.

[0087] In this way, this promotes the use of smaller or less voluminous reduction facilities and is energy efficient.

[0088] Alternatively, the entire system of the direct reduction facility is subjected to overpressure.

[0089] Alternatively, the interior (eg, chamber) of the direct reduction facility in which the chemical reactions occur is subjected to overpressure (at a pressure greater than atmospheric pressure).

[0090] Alternatively, overpressure is achieved by injecting pressurized hydrogen into the reduction facility.

[0091] Alternatively, the hydrogen is pressurized by means of a compressor device.

[0092] Alternatively, the iron ore oxide material providing device includes an iron ore oxide material production unit configured to produce the iron ore oxide material retaining the thermal energy, and to transport the iron ore oxide material retaining the thermal energy to the direct reduction facility.

[0093] Alternatively, the iron ore oxide material retains thermal energy derived from a manufacturing heat process of the iron ore oxide material production unit.

[0094] Alternatively, the iron ore oxide material providing apparatus comprises a pelletizing apparatus configured to produce the iron ore oxide material retaining thermal energy.

[0095] Alternatively, the iron ore oxide material providing apparatus comprises a preheating device configured to preheat the iron ore oxide material before conveying the iron ore oxide material to the direct reduction facility.

[0096] Alternatively, combining the technical feature of preheating the iron ore oxide material before conveying it to a direct reduction facility with the technical feature of introducing oxygen (which also produces hydrogen) produced by an electrolysis unit into an iron ore oxide material production unit where the iron ore oxide material is manufactured, thereby increasing the oxidation rate, provides a sustainable, comprehensive production concept for producing steel in which renewable energy can be used on an industrial scale.

[0097] Alternatively, the technical feature of preheating the iron ore oxide material before conveying it to the direct reduction facility is combined with the technical feature of introducing oxygen-enriched process gas into the hardening device to increase the oxidation rate in the manufacture of the iron ore oxide material and providing additional operational control through a control circuit connected to the iron ore oxide material production unit, when the iron ore oxide material is charged into the direct reduction facility, the amount of thermal energy of the iron ore oxide material is controlled towards a temperature set according to the desired temperature value of the discharged direct reduced iron ore material, which promotes optimal carburization of the direct reduced iron ore material.

[0098] The introduction of oxygen into the iron ore oxide material production unit provides an efficient manufacturing heat process by which oxygen from the electrolysis of water can be effectively used.Oxygen may be introduced into the granulation unit of the iron ore oxide material production unit to provide oxidation / sintering of the iron ore mixture.

[0099] Alternatively, the preheating device is configured to preheat previously cooled iron ore oxide material to be fed to the direct reduction facility, in part by means of recovered heat from the direct reduction facility and / or the iron ore oxide material production unit.

[0100] Alternatively, the electrolysis unit configured to provide the electrolyzed water also produces oxygen, which is used by the iron ore oxide material production unit to produce iron ore oxide material through the manufacturing heat process, wherein the iron ore oxide material can be effectively directly reduced in the direct reduction facility through the chemical reaction using heat energy recovered from the manufacturing heat process.

[0101] Alternatively, the electrolysis unit also produces oxygen which is used by the iron ore oxide material production unit to produce the iron ore oxide material.

[0102] The electrolysis unit is configured to produce hydrogen and oxygen.

[0103] The hardening of the iron ore mixture provided by the hardening device of the iron ore oxide material production unit is achieved by a hydrogen burner device utilizing hydrogen and oxygen to generate heat.

[0104] Alternatively, carbonaceous material extracted from a carbon source is added to the direct reduced iron ore material in a separate carburizing zone of a direct reduction facility configured for introducing carbon into the iron ore oxide material and / or in a separate carburizing reactor configured for introducing carbon into the iron ore oxide material to provide an intermediate product discharged from the direct reduction facility or the separate carburizing reactor.

[0105] Alternatively, the carbonaceous material comprises pure elemental carbon or is a molecule such as methane, propane or other hydrocarbon or a component of other molecules.

[0106] Alternatively, the carbon source comprises: a carbon capture and utilization unit and / or; a carbon production unit configured to produce carbon or non-fossil produced carbon and / or a biogas production unit configured to produce carbon-containing gas and / or a synthesis gas production unit configured to produce carbon-containing synthesis gas from biomass.

[0107] Alternatively, the carbon production unit includes means for providing a Bosch reaction using iron as a catalyst to produce carbon, for example defined by the formula: CO2(g)+2H2(g)→C(s)+2H2O(g)+heat.

[0108] Alternatively, the carbon production unit may be referred to as a carburizing zone.

[0109] Alternatively, the carbon C may be generated in a separate carburizing zone and / or carburizing reactor.

[0110] Alternatively, the carbon C can be fed directly into a separate carburizing zone and / or a carburizing reactor.

[0111] Alternatively, the carbon production unit comprises a Sabatier reactor for producing methane CH4 by reaction between hydrogen H2 and carbon dioxide CO2, the methane CH4 being a carbon or hydrogen containing gas delivered to the independent carburizing zone and / or independent carburizing reactor.

[0112] Alternatively, the carbon production unit and / or the carbon capture and utilisation unit and / or the biogas production unit and / or the synthesis gas production unit is incorporated as an integrated unit of the preheating plant and / or the iron ore production unit and / or the direct reduction facility and / or the electrolysis unit.

[0113] Alternatively, the carbon production unit comprises a Fischer-Tropsch plant configured to produce a carbonaceous product by reducing methane CH4 produced by the Sabatier reactor, the carbonaceous product being conveyed to a separate carburizing zone and / or a separate carburizing reactor.

[0114] Alternatively, the carbon capture and utilization unit (CCU) comprises a CO2 capture device CCD configured to capture CO2 from the atmosphere, and the captured CO2 may be conveyed to the Sabatier reactor configured to produce carbon corresponding methane CH4.

[0115] Alternatively, a carbon production unit configured to produce non-fossil produced carbon is used by a cement industry facility that manufactures cement from mined calcium minerals.

[0116] Alternatively, the carbon production unit of a cement industry plant comprises a cement kiln configured to capture carbon dioxide CO2 emitted from the cement kiln during cement production, which carbon dioxide CO2 is conveyed to said Sabatier reactor configured to produce carbon corresponding methane CH4.

[0117] Alternatively, the intermediate product comprises an intermediate product that does not contain carbon.

[0118] Alternatively, intermediate products are transported to the steel industry in flammable product storage and conveying facilities.

[0119] Alternatively, the flammable product storage and transfer equipment includes a hot cabinet containing, for example, an inert atmosphere, and the carbon-free intermediate products are transferred from the direct reduction facility to the hot cabinet.

[0120] Alternatively, the control circuit is adapted to control the iron ore oxide material temperature of the iron ore oxide material delivered to the direct reduction facility and / or to control the internal gas pressure in the direct reduction facility and / or the reducing agent temperature and / or reducing agent pressure of the introduced reducing agent.

[0121] Alternatively, in a direct reduction facility, hydrogen from regenerative production (reductant) can be used together with a carbon- or hydrogen-containing gas such as CH4, COG, synthesis gas, etc. The ratio of hydrogen from regenerative production to the carbon- or hydrogen-containing gas stream can be continuously varied as a function of availability. That is, if the regenerative yield of hydrogen-containing gas is low, it is possible to use stored regeneratively produced hydrogen-containing gas or to use natural gas, biogas, gas from pyrolysis or renewable resources.

[0122] Alternatively, the first control circuit is suitable for controlling the temperature of the iron ore oxide material delivered to the direct reduction facility by controlling the iron ore oxide material production unit to discharge the iron ore oxide material at a specific temperature, wherein the specific temperature corresponds to a first temperature value determined according to the desired parameter value of the direct reduced iron ore material and / or the intermediate product.

[0123] Alternatively, the first control circuit is suitable for controlling the temperature of the iron ore oxide material delivered to the direct reduction facility by controlling the iron ore oxide material supply device to discharge the iron ore oxide material from the iron ore oxide material production unit at a specific temperature, wherein the specific temperature has a first temperature value determined according to a desired carburizing parameter value of the direct reduced iron ore oxide material to be carburized.

[0124] Alternatively, the iron ore oxide material providing facility includes an iron ore oxide material production unit and / or a preheating device.

[0125] Alternatively, the iron ore oxide material providing apparatus comprises an iron ore oxide conveying apparatus configured to discharge the iron ore oxide material into the direct reduction facility.

[0126] Alternatively, the first detector member of the carburizing reactor and / or the carburizing zone is electrically coupled to the first control circuit.

[0127] Alternatively, the first sensor device is arranged at the iron ore oxide material discharge outlet of the iron ore oxide material production unit and / or the loading inlet of the direct reduction facility, the first sensor device being coupled to the first control circuit.

[0128] Alternatively, the first sensor device is configured to detect said first temperature value.

[0129] Alternatively, the first control circuit is configured to control the iron ore oxide material production unit to discharge the iron ore oxide material at a first temperature value, wherein the first temperature value is determined according to a desired carburizing parameter value of the direct reduced iron ore material to be carburized, wherein the first control circuit takes into account the desired carburizing parameter value when determining the first temperature value of the iron ore oxide material to be charged into the direct reduction facility.

[0130] Alternatively, the desired carburizing parameter values ​​are parameter values ​​of the direct reduced iron ore material (and / or the iron ore oxide material undergoing reduction) that provide optimal carburizing of the direct reduced iron ore material and / or optimal carburizing of the iron ore oxide material undergoing reduction.

[0131] Alternatively, the second control circuit is suitable for controlling the temperature of the iron ore oxide material delivered to the direct reduction facility by controlling the preheating device to discharge the iron ore oxide material from the preheating device at a specific temperature, wherein the specific temperature has a second value determined according to the desired parameter value of the direct reduced iron ore material and / or the intermediate product.

[0132] Alternatively, the second control circuit is adapted to control the temperature of the iron ore oxide material delivered to the direct reduction facility by controlling the preheating device to discharge the iron ore oxide material from the preheating device at a specific temperature having a second temperature value determined according to a desired carburizing parameter value of the direct reduced iron ore material to be carburized.

[0133] Alternatively, a second sensor device is arranged at the iron ore oxide material discharge outlet of the preheating device and / or the loading inlet of the direct reduction facility, the second sensor device being coupled to the second control circuit.

[0134] Alternatively, the preheating device is provided with a heating element for preheating the iron ore oxidized material to have said specific temperature value before charging the iron ore oxidized material into the direct reduction facility.

[0135] Alternatively, the heating element may be fed with thermal energy extracted from a manufacturing heat process of the iron ore oxide material production unit, which thermal energy is used to preheat the iron ore oxide material.

[0136] Alternatively, the second sensor device is configured to detect said second temperature value.

[0137] A second detector member of the carburizing reactor and / or the carburizing zone is electrically coupled to a second control circuit.

[0138] Alternatively, the second control circuit is configured to control the iron ore oxide material production unit to discharge the iron ore oxide material at a first temperature value, wherein the first temperature value is determined according to a desired carburizing parameter value of the direct reduced iron ore material to be carburized, wherein the second control circuit takes into account the desired carburizing parameter value when determining the first temperature value of the iron ore oxide material to be charged into the direct reduction facility.

[0139] Alternatively, the desired carburizing parameter value is a temperature value of the direct reduced iron ore material (and / or the iron ore oxide material undergoing reduction) that provides optimal carburizing of the direct reduced iron ore material and / or optimal carburizing of the iron ore oxide material undergoing reduction.

[0140] Alternatively, the third control circuit is suitable for controlling the reducing agent pressure of the reducing agent delivered to the direct reduction facility by controlling the first pressurizing device, wherein the first pressurizing device is suitable for pressurizing the reducing agent entering the direct reduction facility at a specific reducing agent pressure, and the specific reducing agent pressure has a first reducing agent pressure value determined according to the desired parameter value of the direct reduced iron ore material and / or intermediate product.

[0141] Alternatively, the third control circuit is adapted to control the reducing agent pressure by controlling the first pressurizing device to inject the reducing agent into the direct reduction facility at the first reducing agent pressure value.

[0142] Alternatively, a third sensor device is arranged at the reducing agent inlet of the direct reduction facility, the third sensor device being connected to the third control circuit.

[0143] Alternatively, the third sensor device is configured to detect the first reductant pressure value.

[0144] Alternatively, a third detector member of the carburizing reactor and / or the carburizing zone is electrically coupled to a third control circuit.

[0145] Alternatively, the third control circuit is configured to control the first pressurizing device to pressurize the reductant in the direct reduction facility at the first reductant pressure value, wherein the first reductant pressure value is determined based on a desired carburizing parameter value of the direct reduced iron ore material to be carburized, wherein the third control circuit takes into account the desired carburizing parameter value when determining the first reductant pressure value.

[0146] Alternatively, the desired carburizing parameter value is a temperature value of the direct reduced iron ore material (and / or the iron ore oxide material undergoing reduction) which provides optimal carburizing of the direct reduced iron ore material and / or optimal carburizing of the iron ore oxide material undergoing reduction.

[0147] Alternatively, the fourth control circuit is suitable for controlling the reduction pressure in the direct reduction facility by controlling a second pressurizing device, wherein the second pressurizing device is suitable for pressurizing the reducing agent entering the direct reduction facility at a specific reduction pressure, wherein the specific reduction pressure has a first reduction pressure value determined according to the desired parameter value of the direct reduced iron ore material and / or intermediate product.

[0148] Alternatively, the fourth control circuit is adapted to regulate the pressure of the reducing agent introduced into the direct reduction facility and / or the pressure of the discharged excess reducing agent by means of a gas pressure regulating device provided in an output gas pipeline of the direct reduction facility.

[0149] Alternatively, the fourth control circuit is adapted to control the reduction pressure by controlling the second pressurizing device to inject the reducing agent into the direct reduction facility, thereby providing the first reduction pressure value in the direct reduction facility.

[0150] Alternatively, a fourth sensor device is arranged at the direct reduction facility, the fourth sensor device being coupled to the fourth control circuit.

[0151] Alternatively, a fourth sensor device is configured to detect the first reduction pressure value.

[0152] A fourth detector member of the carburizing reactor and / or the carburizing zone is electrically coupled to a fourth control circuit.

[0153] Alternatively, the fourth control circuit is configured to control the second pressurizing device to pressurize the reducing agent in the direct reduction facility at the first reduction pressure value, wherein the first reduction pressure value is determined based on the desired carburizing parameter value of the direct reduced iron ore material to be carburized, wherein the fourth control circuit takes into account the desired carburizing parameter value when determining the first reduction pressure value.

[0154] Alternatively, the desired carburizing parameter value is a desired parameter value of the direct reduced iron ore material (and / or the iron ore oxide material undergoing reduction) that provides optimal carburizing of the direct reduced iron ore material and / or optimal carburizing of the iron ore oxide material undergoing reduction.

[0155] For example, the desired parameter value of the direct reduced iron ore material may correspond to a desired carburizing temperature value of the direct reduced iron ore material, a desired iron ore porosity value of the direct reduced iron ore material, a desired iron ore size value of the direct reduced iron ore material, and the like.

[0156] Alternatively, the fifth control circuit is suitable for controlling the reductant temperature of the reductant injected into the direct reduction facility by controlling a heating device, wherein the heating device is configured to heat the reductant at a specific reductant temperature, wherein the specific reductant temperature has a first reductant temperature value determined according to a desired parameter value of the direct reduced iron ore material and / or intermediate product.

[0157] Alternatively, the fifth control circuit is adapted to control the reducing agent temperature by controlling a heating device so as to provide the first reducing agent temperature value.

[0158] Alternatively, a fifth sensor device is arranged at the direct reduction facility, the fifth sensor device being coupled to the fifth control circuit and configured to detect a first reductant temperature value, the first reductant temperature value.

[0159] Alternatively, the fifth control circuit is configured to control the second pressurizing device to pressurize the reducing agent in the direct reduction facility at the first reduction pressure value, wherein the first reduction pressure value is determined based on the desired carburizing parameter value of the direct reduced iron ore material to be carburized, wherein the fifth control circuit takes into account the desired carburizing parameter value when determining the first reduction pressure value.

[0160] Alternatively, a fifth detector member of the carburizing reactor and / or the carburizing zone is electrically coupled to a fifth control circuit.

[0161] Alternatively, the desired carburizing parameter value is a parameter value of the direct reduced iron ore material (and / or the iron ore oxide material undergoing reduction) that provides optimal carburization of the direct reduced iron ore material and / or optimal carburization of the iron ore oxide material undergoing reduction.

[0162] Alternatively, the at least one desired carburizing parameter value corresponds to a desired carburizing temperature value of the direct reduced iron ore material, a desired iron ore porosity value of the direct reduced iron ore material, a desired iron ore size value of the direct reduced iron ore material, or the like.

[0163] Alternatively, the method comprises the steps of: directly reducing the iron ore oxide material by means of a reducing agent having a hydrogen content of at least 80% by volume; wherein the carbon content in the directly reduced iron ore material is then increased by means of a carburizing gas, and thereafter at least partially removing the used carburizing gas while largely avoiding mixing of the carburizing gas with the reducing agent.

[0164] Alternatively, an oxygen-enriched process gas is introduced into the hardening device to increase the oxidation rate, and operation of the iron ore oxide material production unit can be controlled by control circuitry coupled to the iron ore oxide material production unit.

[0165] Thus, the amount of thermal energy of the iron ore oxide material to be charged to the direct reduction facility can be controlled towards a specific temperature set according to a desired temperature value of the discharged direct reduced iron ore material, which promotes optimal carburization of the direct reduced iron ore material.

[0166] Alternatively, the control circuit adjusts the iron ore oxide material temperature and / or the reduction pressure and / or the reducing agent temperature and / or the reducing agent pressure according to the characteristics of the intermediate product required by the customer.

[0167] This or at least one of the objects is achieved by a process product, wherein the intermediate product is a carburized product produced by reduction involving carburization.

[0168] Alternatively, during the reduction of the iron ore oxide material to the intermediate product, a carbon- or hydrogen-containing gas is added to the reducing agent, or as a solid carbonaceous material, so as to incorporate carbon into the intermediate product.

[0169] Alternatively, to compensate for temporary fluctuations in renewable energy production, if excess renewable energy is available, this energy is stored in the form of a reducing agent, while the method for producing steel according to the invention requires less renewable energy for reduction and saves time.

[0170] This storage can take place, for example, in a reducing agent tank. Such a reserve can then be used in the event of fluctuations. Temporary fluctuations can be predictable, such as at night in a solar power plant, or unpredictable, such as fluctuations in wind strength in a wind power plant.

[0171] Longer-term fluctuations may occur, in particular, due to different seasons and can be taken into account in the energy storage in the form of HBI, while the method according to the invention for producing steel requires less renewable energy for reduction and saves time.

[0172] If necessary, carbon- or hydrogen-containing gases, such as natural gas, can also be utilized, and the use of reducing agents can moreover optimally only be carried out with sufficient renewable electrical energy.

[0173] This advantageously results in an optimal potential use of renewable energy, since this energy can be used continuously as a function of the availability of the corresponding form of energy and the missing surplus energy can be supplemented as required with the aid of other energy carriers, while the method for producing steel according to the invention requires less renewable energy for reduction and saves time.

[0174] Therefore, by using renewable energy via the method for producing steel according to the invention, the emissions of carbon dioxide CO2 can be reduced to the currently possible minimum at any time, the method for producing steel according to the invention requiring less renewable energy for reduction and saving time.

[0175] The exemplary processes may be combined, and the first control circuit, the second control circuit, the third control circuit, the fourth control circuit, and the fifth control circuit may be circuits of control circuits that adjust the iron ore temperature and / or the reduction pressure and / or the reducing agent temperature and / or the reducing agent pressure according to the characteristics of the intermediate product required by the consumer.

[0176] Alternatively, the temperature of the direct reduced iron ore material discharged from the direct reduction facility is lower than the temperature at which the iron ore oxide material is charged to the direct reduction facility.

[0177] Alternatively, the temperature of the reducing agent introduced into the direct reduction facility is lower than the temperature of the spent reducing fluid discharged from the direct reduction facility.

[0178] Alternatively, the direct reduction facility includes a spent reducing fluid gas line connected for discharging the spent reducing fluid from the direct reduction facility.

[0179] Alternatively, the spent reducing fluid gas line comprises a regulator device for regulating the pressurized reducing agent injected into the direct reduction facility and / or for regulating the discharged top gas.

[0180] Alternatively, the ratio between the reductant from regenerative production and the carbon- or hydrogen-containing gas stream varies continuously as a function of availability; when sufficient regenerative energy is present, the reductant is produced using the regenerative energy, while in the absence of regenerative energy, the process and configuration switch to a pure carbon- or hydrogen-containing gas stream.

[0181] Alternatively, either of the control circuits provides for regulation of the temperature of the iron ore oxide material to be charged to the direct reduction facility and regulation of the content of reducing agent and / or carbon- or hydrogen-containing gas as part of the total gas flow is performed by at least one control circuit.

[0182] Alternatively, at least one control circuit may also be used to determine and control the predicted production / production of reductant and / or renewable energy and / or carbon- or hydrogen-containing gases flowing out of the biogas production unit or from pyrolysis of renewable resources, and / or to predict an estimated value of required renewable energy based on predicted demand from external consumers.

[0183] In this way it is achieved that the renewable energy can be distributed in the best and most economical way.

[0184] Alternatively, the gas stream discharged as offgas from the direct reduction can be fed to the process as a carbon- or hydrogen-containing gas stream.

[0185] The iron ore oxide material production unit may comprise a grate plant including a drying and preheating unit to prepare the iron ore mix (eg green pellets) for a hardening process.

[0186] Alternatively, the grate apparatus is configured to transfer heat energy to the iron ore mixture under oxidation and produce iron ore oxide material having high thermal energy. The grate apparatus sinter the iron ore mixture to give the pellets additional mechanical strength.

[0187] The chain grate plant can be divided into four zones. In the first two zones, the iron ore mixture is dried, for example by hot air blown in from below the pellet bed. After leaving the first two zones, the iron ore mixture can be conveyed through a tempered pre-heat zone and through a pre-heat zone. The latter two zones are used to increase the temperature of the iron ore mixture before entering, for example, a rotary kiln unit.

[0188] Alternatively, the iron ore oxide material production unit comprises a process gas feed line configured to feed oxygen-depleted process gas to the grate apparatus to dry and / or preheat and / or heat the iron ore mixture.

[0189] Alternatively, after leaving the grate apparatus, the iron ore mixture is subjected to an oxygen-enriched process gas, such as fed into a rotary kiln unit for oxidizing the iron ore mixture into iron ore oxide material retaining said thermal energy.

[0190] In this way, an efficient energy saving approach is achieved by delaying oxidation during drying and / or preheating and / or heating of the iron ore oxide material and subsequent enrichment of oxygen during oxidation provided by the iron ore oxide material production unit.

[0191] In this way, a time-saving manufacturing heat process is achieved, while the waste gases (eg nitrogen) generated by the manufacturing heat process will be reduced.

[0192] Alternatively, in order to provide effective oxidation and / or sintering of iron ore processed in a hardening device (e.g., a belt roaster hardening furnace (the entire hardening process is carried out together), a chain grate rotary kiln (preheater / rotary kiln / cooler) device, a steel belt equipment, etc.) to produce iron ore oxide material, an oxygen-enriched process gas is fed into the hardening device.

[0193] In this way, the oxidation rate of the iron ore oxidation in the hardening device is increased.

[0194] Alternatively, the iron ore oxide material production unit comprises a pelletizing apparatus configured to produce the iron ore oxide material retaining thermal energy.

[0195] Alternatively, the method for producing steel and the steel production arrangement comprise an electrolysis unit which also produces oxygen which is used by the iron ore oxide material production unit to make the iron ore oxide material.

[0196] Alternatively, the carburizing zone corresponds to an independent (isolated) carburizing zone configured to prevent the carbonaceous substance from mixing with the reducing agent.

[0197] Alternatively, the carburizing zone constitutes a carburizing space inside the direct reduction facility, the carburizing space being configured for reducing the iron ore oxide material, and configured for carburizing the iron ore oxide material undergoing reduction and mixing the carbonaceous substance with the reducing agent.

[0198] Alternatively, the carburizing zone is configured to provide an independent (isolated) carburizing chemical reaction between hydrogen H2 and carbon dioxide CO2 to achieve carburization of the direct reduced iron ore material, wherein the direct reduced iron ore material acts as a catalyst to produce carbonaceous material added to the direct reduced iron ore material.

[0199] Alternatively, the carburizing zone is configured to provide an unisolated carburizing chemical reaction between hydrogen H2 and carbon dioxide CO2 to achieve carburization of the iron ore oxide material undergoing reduction, wherein the iron ore oxide material undergoing reduction acts as a catalyst for producing carbonaceous material that is added to the iron ore oxide material undergoing reduction.

[0200] C02+2H2>C+2H20

[0201] C02+H2>CO+H20

[0202] CO+H>C+H20

[0203] Alternatively, the carburizing zone is provided with a carburizing zone-hydrogen inlet device and / or a carburizing zone-carbon-containing substance inlet device.

[0204] Alternatively, the carburizing zone-hydrogen inlet device is configured for feeding hydrogen H 2 into the carburizing zone.

[0205] Alternatively, the carburizing zone-carbonaceous material inlet device is configured for feeding CO2, CH4 or other carbonaceous compounds into the carburizing zone.

[0206] Alternatively, the carburizing zone is configured as an independent carburizing reactor, which is configured with a first reactor fluid inlet device for feeding a first reactor fluid into the independent carburizing reactor and a second reactor fluid inlet device for feeding a second reactor fluid into the independent carburizing reactor, for providing a chemical reaction between the first reactor fluid and the second reactor fluid.

[0207] Alternatively, the first reactor fluid inlet device and / or the second reactor fluid inlet device comprises a regulating device for regulating a property of the first reactor fluid and / or the second reactor fluid.

[0208] Alternatively, the regulating device is electrically coupled to a control circuit adapted to regulate a property, such as concentration, temperature, flow rate, pressure, etc., of the first reactor fluid and / or the second reactor fluid.

[0209] Alternatively, the direct reduced iron ore material and / or the iron ore oxide material undergoing reduction acts as a catalyst for producing carbonaceous materials, such as methane CH4 and / or carbon monoxide CO and / or solid carbon C and / or other carbon compounds, which carburize the direct reduced iron ore material and / or the iron ore oxide material undergoing reduction.

[0210] Alternatively, the carburizing zone is configured for introducing carbon into the direct reduced iron ore material and / or the iron ore oxide material undergoing reduction for providing an intermediate product to be discharged from the direct reduction facility.

[0211] Alternatively, the carburizing zone is configured as the independent carburizing reactor, and the independent carburizing reactor is configured to avoid mixing of the carbonaceous material with the reducing agent.

[0212] Alternatively, the independent carburizing reactor is configured for a chemical reaction between a first reactor fluid comprising a hydrogen content of 50 vol% to 100 vol% and a second reactor fluid comprising carbon dioxide CO2, wherein the direct reduced iron ore material acts as a catalyst for producing CH4 and / or carbon monoxide CO and / or solid carbon C and / or other carbon compounds which carburize the direct reduced iron ore material.

[0213] Alternatively, the first reactor fluid comprises pure hydrogen.

[0214] Alternatively, the second reactor fluid comprises pure carbon dioxide CO2.

[0215] Alternatively, 80% to 100% by volume of the hydrogen content is renewable hydrogen.

[0216] Alternatively, the hydrogen includes fossil hydrogen content produced by carbon capture and / or low carbon hydrogen.

[0217] Alternatively, hydrogen is produced by electrolysis of water using electricity from renewable resources, and / or by reforming of biogas and / or by biochemical conversion of biomass.

[0218] Alternatively, hydrogen is produced from synthetic fuels derived from hydrogen, which are various gaseous and liquid fuels based on hydrogen and carbon.

[0219] Alternatively, the chemical reaction between the first reactor fluid and the second reactor fluid is controlled by a control circuit to provide a carburizing chemical reaction between hydrogen H2 and carbon dioxide CO2 to provide carburizing of the direct reduced iron ore material in an independent carburizing reactor, wherein the direct reduced iron ore material acts as a catalyst for producing CH4 and / or carbon monoxide and / or solid carbon and / or other carbon compounds for carburizing the direct reduced iron ore material.

[0220] C02(g)+2H2(g)→C(s)+2H20(g)

[0221] C0 2 +H2→CO+H2O

[0222] CO+H2>C+H20

[0223] Alternatively, the stand-alone carburizing reactor is configured for introducing carbon into the direct reduced iron ore material to provide an intermediate product to be discharged from the stand-alone carburizing reactor.

[0224] Alternatively, a carbonaceous material comprising carbon dioxide CO2 and / or carbon monoxide CO and / or solid carbon C is fed into the carburizing zone for providing carburization of the direct reduced iron ore material.

[0225] Alternatively, the carburizing zone is configured to provide a Sabatier and / or Fischer-Tropsch reaction or other possible reactions wherein the iron ore oxide material acts as a catalyst to produce CH4 and / or other carbon compounds and / or carbon monoxide and / or carbon which acts as a carburizing agent for providing direct reduction of the iron ore material.

[0226] This object or at least one of the objects has been achieved by providing a steel production configuration for steel production and a method for producing steel, the steel production configuration comprising: an iron ore oxide material providing device configured to provide an iron ore oxide material that retains thermal energy; a direct reduction facility configured to reduce the iron ore oxide material and to utilize the thermal energy of the iron ore oxide material to heat or further heat an introduced reducing agent; the direct reduction facility is configured to introduce a reducing agent, the reducing agent being suitable for reacting with the iron ore oxide material that retains thermal energy to achieve the reduction of the iron ore oxide material. a chemical reaction between a raw material and a reducing agent, for providing an energy-saving and time-saving process for producing steel using renewable energy on an industrial scale, and for conserving renewable energy to cope with fluctuations in the production of regeneratively generated electrical energy; a control circuit configured to control an iron ore oxide material supply device, and to control the reduction of the iron ore oxide material; an iron ore oxide conveying device suitable for loading the iron ore oxide material from the iron ore oxide material supply device into a direct reduction facility; and / or an electrolysis unit configured for electrolyzing water to produce hydrogen and oxygen; and / or a steelmaking industry configured for the production of steel.

[0227] Alternatively, the control circuit is configured to operate to charge iron ore oxide material into a direct reduction facility; wherein the control circuit is configured to control the temperature of the iron ore oxide material delivered to the direct reduction facility and / or control the internal gas pressure in the direct reduction facility and / or the reducing agent temperature and / or the reducing agent gas pressure of the introduced reducing agent.

[0228] This object or at least one of the objects has been achieved by a data program suitable for executing the method disclosed herein, wherein the data program comprises a program code which can be read on a computer for providing a control circuit of the method.

[0229] Alternatively, the carbonaceous material is fed into the carburizing zone together with the reducing agent.

[0230] This object or at least one of the objects has been achieved by providing a method for the process, which includes the following steps: producing iron ore oxide material; loading the iron ore oxide material that retains thermal energy provided by the iron ore oxide material supply equipment into a direct reduction facility from the iron ore oxide material supply equipment; introducing a reducing agent into the direct reduction facility; reducing the iron ore oxide material into an intermediate product by utilizing the thermal energy of the iron ore oxide material to heat or further heat the introduced reducing agent to achieve a chemical reaction; and discharging the intermediate product from the direct reduction facility; and / or transporting the intermediate product to the steelmaking industry.

[0231] Alternatively, the method comprises the further steps of: sending parameter value signals from the detector means of the direct reduction facility to the control circuit; and commanding the conveying device of the iron ore oxide material supply device to stop charging the iron ore oxide material retaining thermal energy into the direct reduction facility.

[0232] Alternatively, the method includes the steps of: if the parameter value signal is an interrupt value, commanding the direct reduction facility to stop the chemical reaction between the iron ore oxide material and the reducing agent;

[0233] Alternatively, the method comprises the further step of sending a stop signal to an operator if the parameter value signal corresponds to an interrupt value.

[0234] Alternatively, the electrical energy required for electrolysis can be partially or entirely renewable energy, which comes from hydropower and / or wind power and / or photovoltaic or other forms of renewable energy.

[0235] Alternatively, the reducing agent (hydrogen) is produced by electrolysis of water. Suitably, the electric energy required for electrolysis is a renewable energy source, which comes from hydropower and / or wind power and / or photovoltaic or other renewable energy forms.

[0236] Alternatively, the present disclosure relates to a method for producing a carburized intermediate product, comprising the steps of reducing an iron ore oxide material by a reducing agent such as hydrogen in a direct reduction facility to provide a reduced iron material, transporting the reduced iron material to a carburizing zone, and carburizing the reduced iron material in the carburizing zone using a carbon-containing substance such as a carburizing gas and / or solid carbon to provide a carburized intermediate product.

[0237] Alternatively, the present invention relates to a method for producing a carburized intermediate product (iron ore oxide material), comprising the steps of: directly reducing the iron ore oxide material by a reducing agent (e.g. hydrogen) having a hydrogen content of at least 80% by volume; wherein the carbon content in the intermediate product is then increased by a carburizing gas, and thereafter the used carburizing gas is at least partially removed, while largely avoiding mixing of the carburizing gas with the reducing agent.

[0238] Alternatively, the technical feature of preheating the iron ore oxide material before conveying it to a direct reduction facility is combined with the further technical feature of introducing oxygen produced by an electrolysis unit into an iron ore oxide material production unit to manufacture the iron ore oxide material, providing a sustainable, comprehensive production concept for the efficient production of steel, in which renewable energy can be used on an industrial scale and fluctuations in renewable energy production can be coped with.

[0239] Alternatively, the carbon production unit and / or Sabatier reactor and / or Fischer-Tropsch plant and / or carbon production unit and / or carbon capture and utilisation unit and / or biogas production unit and / or synthesis gas production unit is incorporated as an integrated unit of the preheating unit and / or iron ore oxide material production unit and / or direct reduction facility and / or electrolysis unit and / or steelmaking industry and is an integrated part of an integrated steel production configuration for producing steel.

[0240] Alternatively, part or all of the electricity required for electrolysis may be derived from nuclear energy.

[0241] The wording reducing agent may be replaced by the wording reducing reagent.

[0242] The reducing agent may be a gas having a hydrogen content of 50% to 100% by volume.

[0243] The word "process" may be changed to "method" or vice versa.

[0244] Alternatively, the upper interior portion of the reduction facility is configured to receive heat-retaining iron ore oxide material to be charged into the reduction facility.

[0245] Alternatively, the iron ore oxide inlet of the reduction facility is configured to convey the iron ore oxide material retaining thermal energy from the iron ore oxide material supply facility via the iron ore oxide conveying device, which is configured to charge the iron ore oxide material retaining thermal energy into the direct reduction facility.

[0246] The first sensor device may be arranged at an iron ore oxide material discharge outlet and / or an iron ore oxide material loading inlet of the iron ore oxide material production unit.

[0247] The wording "heat treatment" may be replaced by the wording "heat hardening".

[0248] The expression "iron ore" may mean a metal ore or an iron ore containing other elements and / or minerals in addition to iron, such as naturally occurring alloying elements or smaller amounts of minerals that do not constitute an alloy.

[0249] The expression "iron ore" may mean iron ore including introduced additives such as quartz, silicon and the like.

[0250] The wording "iron ore" may be replaced by the wording "metal ore".

[0251] The wording "reduction facility" could be changed to "direct reduction facility".

[0252] The control circuit may include a first control circuit and / or a second control circuit and / or a third control circuit and / or a fourth control circuit and / or a fifth control circuit and / or a sixth control circuit.

[0253] Alternatively, the heat treatment includes thermal hardening.

[0254] Alternatively, the heat treatment includes a thermal hardening process including sintering of the reduced iron ore material and / or shrinking of the reduced iron ore material and / or densification of the reduced iron ore material.

[0255] Alternatively, the reduction facility is configured to provide and / or be coupled to a heat treatment apparatus for providing a heat treatment process (preferably below about 700°C, or below about 650°C to 750°C, or below about 600°C to 750°C) of the iron ore oxide material prior to reduction of the iron ore oxide material.

[0256] These objects or at least one of the objects has been achieved by a method for reducing an iron ore oxide material retaining heat energy into a reduced iron ore material; wherein the iron ore oxide material retaining heat energy is provided by an iron ore oxide material providing device and is loaded into an upper inner portion of a reduction facility of a metal material production configuration via an iron ore oxide material loading device; a sixth control circuit is electrically connected to a reducing agent temperature regulating device, the reducing agent temperature regulating device being configured to regulate the temperature of a hydrogen-containing reducing agent to be introduced into the middle portion and / or the lower inner portion of the reduction facility via a reducing agent inlet device; the method The invention is characterized by the following steps: reducing the iron ore oxide material in the upper inner part by utilizing the thermal energy of the iron ore oxide material to heat or further heat the introduced hydrogen-containing reducing agent to provide a chemical reaction between the hydrogen-containing reducing agent and the iron ore oxide material; providing a thermal treatment process to thermally treat the iron ore oxide material undergoing reduction and / or to thermally treat the reduced iron ore material before it is discharged from the lower inner part; and controlling the temperature of the introduced hydrogen-containing reducing agent to adjust the chemical reaction and / or the thermal treatment process to achieve at least one desired passivation parameter value of the reduced iron ore material.

[0257] In this way it is achieved that the chemical reactivity and / or high driving force of hydrogen is largely maintained. Chemical reactivity and / or high driving force are essential to provide efficient reduction of the iron ore oxide material.

[0258] Alternatively, the sixth control circuit is adapted for a coarse setting of the thermal energy and for a fine setting of the temperature of the introduced (preheated or cooled) hydrogen-containing reducing agent in order to achieve at least one desired passivation parameter value.

[0259] In this way, effective regulation of the temperature of the reduction of the iron ore oxide material is achieved, and at the same time, effective regulation of the heat treatment temperature of the reduced iron ore material is achieved.

[0260] Alternatively, the intermediate interior portion and the lower interior portion are configured for introducing a preheated hydrogen-containing reducing agent suitable for reacting with the iron ore oxide material retaining thermal energy.

[0261] Alternatively, a reducing agent comprising hydrogen is introduced into the middle inner portion and the lower inner portion.

[0262] Alternatively, the bottom zone of the upper interior portion is configured for introducing a preheated hydrogen-containing reducing agent suitable for reacting with the iron ore oxide material retaining thermal energy.

[0263] Alternatively, a reducing agent comprising hydrogen is introduced into the bottom zone of the upper interior portion.

[0264] Alternatively, the direct reduction facility is configured to allow the reduced iron ore material to descend into the lower interior portion and / or the intermediate interior portion to provide a thermal treatment process for thermal treatment of the reduced iron ore material using additional thermal energy provided by the preheated hydrogen-containing reducing agent.

[0265] Alternatively, the additional thermal energy is defined as thermal energy added to the thermal energy of the iron ore oxide material retaining thermal energy and / or as thermal energy added to the thermal energy of the reduced iron ore material descending through the intermediate inner portion and / or the lower inner portion.

[0266] Alternatively, the control circuit electrically coupled to the reductant temperature regulating device configured to regulate the temperature of the hydrogen-containing reductant is adapted to control the temperature of the introduced hydrogen-containing reductant to achieve at least one desired passivation parameter value for the reduced iron ore material.

[0267] In this way it is achieved that the intermediate products (eg sponge iron, such as pellets, briquettes etc.) are prevented from having a tendency to revert to an oxidized state when exposed to the elements and the risk of autoignition processes is reduced.

[0268] Alternatively, the sixth control circuit is adapted to control the internal gas pressure in the direct reduction plant and / or the hydrogen temperature and / or the hydrogen pressure of the introduced hydrogen used as reducing agent.

[0269] Alternatively, the reductant inlet device is configured to introduce the reductant into the direct reduction facility.

[0270] Alternatively, the sixth control circuit is electrically coupled to a reducing agent temperature regulating device configured to regulate the temperature of the reducing agent to be introduced into the middle portion and / or lower inner portion of the reduction facility via the reducing agent inlet device of the direct reduction facility.

[0271] Alternatively, the iron ore oxide material loading and conveying unit of the metal material production arrangement is configured to load the iron ore oxide material into an upper interior portion of the direct reduction facility.

[0272] Alternatively, the iron ore oxide loading apparatus is configured to load the iron ore oxide into an upper interior portion of the reduction facility.

[0273] Alternatively, the discharge conveying unit is coupled to an opening of a lower interior portion of the direct reduction facility, the opening being configured for discharging the direct reduced iron ore material from the direct reduction facility.

[0274] Alternatively, the direct reduction facility further comprises a spent reducing fluid outlet device configured to discharge the spent reducing fluid (eg, water vapor and hydrogen) from the direct reduction facility.

[0275] Alternatively, the reducing agent may be preheated prior to introduction into the direct reduction facility, wherein the introduced reducing agent may be preheated to a temperature of about 200°C to about 500°C, or about 300°C to about 600°C, or about 400°C to about 700°C, or about 500°C to about 800°C, or about 600°C to about 900°C, or about 700°C to about 1000°C, or about 800°C to about 1100°C, or about 900°C to about 1200°C, or more (e.g., referred to as high temperature in some cases).

[0276] Alternatively, the temperature of the iron ore oxide material to be charged into the direct reduction facility (e.g., referred to as high temperature in some cases) may have a temperature of about 50°C to about 350°C, or about 100°C to about 400°C, or about 200°C to about 500°C, or about 300°C to about 600°C, or about 400°C to about 700°C, or about 500°C to about 800°C, or about 600°C to about 900°C, or about 700°C to about 1000°C, or about 800°C to about 1100°C, or about 900°C to about 1200°C, or more.

[0277] For example, a reducing agent having a certain temperature (e.g., referred to as a high temperature in some cases) (e.g., any temperature in the range of about 600°C to 1000°C, or about 500°C to 900°C, or about 700°C to 1100°C) to be introduced and / or being introduced into a direct reduction facility meets the direct reduced iron material and / or the iron ore oxide material undergoing direct reduction descending through the direct reduction facility, for the purpose of reducing the cooling rate of the direct reduced iron material and / or the iron ore oxide material undergoing direct reduction descending through the direct reduction facility.

[0278] Alternatively, iron ore oxide material to be charged and / or being charged into the direct reduction facility at a certain temperature (e.g., referred to as high temperature in some cases) (e.g., any temperature in the range of about 600°C to about 900°C or about 700°C to about 1000°C or about 800°C to about 1100°C or about 900°C to about 1200°C or higher) meets its reducing agent, most of which has been used for chemical reaction, in the upper internal part of the reduction facility for partially further providing the chemical reaction, while the iron ore oxide material and / or direct reduced iron material subjected to direct reduction further down in the direct reduction facility is preferably subjected to the heat treatment process, whereby the top gas to be discharged from the reduction facility and formed by the chemical reaction in the upper internal part will be very hot and contain high-temperature water vapor to be fed to the high-temperature electrolysis unit.

[0279] Alternatively, the reduction potential of the hydrogen gas of the reducing agent is lower than the reduction potential of the hydrogen gas of the reducing agent introduced further down in the reduction facility.

[0280] Alternatively, the iron ore oxide material to be charged and / or being charged into the direct reduction facility at a certain temperature (for example, any temperature in the range of about 50°C to about 350°C or about 100°C to about 400°C) meets the reducing agent, most of which has been used for chemical reaction, in the upper internal part of the reduction facility, and the chemical reaction is further provided at least to a certain extent in part by further heating the introduced reducing agent to achieve the chemical reaction between the iron ore oxide material and the reducing agent.

[0281] This makes possible an energy-saving method for the direct reduction of iron ore oxide materials by means of hydrogen and / or a hydrogen-containing reducing agent, wherein the hydrogen can preferably be temporarily stored in a gas tank and / or a storage facility in a geological storage reservoir and / or other buffer facilities, so that the hydrogen of the reducing agent is available and can be used when renewable energy cannot be fully produced, i.e., for coping with fluctuations in the production of regeneratively generated electrical energy.

[0282] Alternatively, the temperature of the iron ore oxide material to be charged to the direct reduction facility may be lower than the temperature of the reducing agent to be and / or being introduced into the direct reduction facility.

[0283] The present invention may relate to a method for producing steel, whereby an iron ore oxide material is reduced with a reducing agent, such as a hydrogen-containing reducing agent, in a direct reduction facility, and the intermediate products and final accompanying materials of the directly reduced metal material thus obtained are subjected to metallurgical treatment; the reducing agent is produced by electrolysis of water with the aid of an electrolysis unit, such as a high-temperature electrolysis unit, and the electrical energy required for the electrolysis may be renewable energy derived from hydropower and / or wind power and / or photovoltaics and / or other forms of renewable energy and / or nuclear power plants (e.g. plants including small modular reactors SMRs), wherein if sufficient reducing agent is available, the reduced iron material produced, such as sponge iron (the so-called intermediate product), is produced independently of current demand.

[0284] The iron ore oxide material is transported from the iron ore oxide material supply facility (eg, a pelletizing facility and / or a preheating device) to the direct reduction facility and retains thermal energy originating from the iron ore oxide material supply facility.

[0285] The direct reduction facility is configured to introduce a reducing agent, which is suitable for reacting with the iron ore oxide material retaining thermal energy, thereby reducing the iron ore oxide material into an intermediate product by utilizing the thermal energy of the iron ore oxide material to further heat the introduced reducing agent to achieve a chemical reaction between the iron ore oxide material and the reducing agent, for providing an energy-saving and time-saving process for producing steel using renewable energy on an industrial scale, and for conserving renewable energy to cope with fluctuations in the production of regeneratively generated electrical energy.

[0286] Alternatively, if sufficient regeneratively generated electrical energy is available, the reducing agent is produced independently of the current demand, the produced reducing agent being temporarily stored to cope with the fluctuations.

[0287] The hydrogen gas of the hydrogen-containing reducing agent and / or the hydrogen-containing reducing agent may be stored in gas tanks and / or storage facilities in geological repositories and / or other buffer facilities.

[0288] Storage facilities in gas tanks or geological repositories may be located between the electrolysis unit and / or high-temperature electrolysis unit and the direct reduction facility.

[0289] Hydrogen and / or a reducing agent comprising hydrogen is configured to be fed and / or transported to a direct reduction facility for use as a reducing agent under fluctuating conditions, such as during summer.

[0290] During spring and autumn, renewable electricity can be generated by a wind energy device connected to and used by an electrolysis unit and / or a high-temperature electrolysis unit. During spring and autumn, the hydrogen and / or the hydrogen-containing reducing agent produced in this way from renewable energy sources is preferably temporarily stored in a storage facility in a gas tank and / or a geological reservoir.

[0291] In this way, efficient storage of renewable energy (in the form of hydrogen and / or hydrogen-containing reducing agents) is achieved, which renewable energy can subsequently be used as reducing agent by the direct reduction facility during the summer when the production of renewable electricity is low, i.e. when sufficient regeneratively generated electrical energy is not available.

[0292] Alternatively, the reducing agent may be preheated to some extent prior to introduction into the direct reduction facility.

[0293] Alternatively, the temperature of the iron ore oxide material to be charged to the direct reduction facility may be higher than the temperature of the reducing agent to be introduced and / or being introduced into the direct reduction facility.

[0294] Alternatively, the temperature of the iron ore oxide material to be charged to the direct reduction facility may be lower than the temperature of the reducing agent to be and / or being introduced into the direct reduction facility.

[0295] The temperature of the iron ore oxide material to be charged into the direct reduction facility may have a temperature of about 50°C to about 350°C, or about 100°C to about 400°C, or about 200°C to about 500°C, or about 300°C to about 600°C, or about 400°C to about 700°C, or about 500°C to about 800°C, or about 600°C to about 900°C, or about 700°C to about 1000°C, or about 800°C to about 1100°C, or about 900°C to about 1200°C, or more.

[0296] The reducing agent may be preheated prior to introduction into the direct reduction facility, wherein the introduced reducing agent may be preheated to a temperature of about 200°C to about 500°C, or about 300°C to about 600°C, or about 400°C to about 700°C, or about 500°C to about 800°C, or about 600°C to about 900°C, or about 700°C to about 1000°C, or about 800°C to about 1100°C, or about 900°C to about 1200°C, or more.

[0297] Alternatively, by introducing relatively warm reducing agent (e.g., about 600°C to 900°C) into the direct reduction facility, it is achieved that the iron ore oxide material that retains heat energy, reaches the middle portion and / or lower interior portion of the direct reduction facility and undergoes direct reduction and / or heat treatment does not cool rapidly in the direct reduction facility.

[0298] Thus, the heat treatment can be carried out efficiently. The passivated and reduced iron material will have a compact and dense structure for achieving an intermediate product that is resistant to reoxidation.

[0299] The intermediate product may be defined as a small, round, pear-shaped, drop-shaped, pellet-shaped, bead-shaped, sphere-shaped or ellipsoidal object of the passivated reduced iron ore material having a compact and dense structure for producing a reoxidation resistant intermediate product.

[0300] Alternatively, the direct reduction facility is configured to allow the reduced iron ore material to descend into the lower inner portion and / or the middle inner portion to provide a thermal treatment process for heat treating the reduced iron ore material using a relatively warm reducing agent providing thermal energy to avoid rapid cooling of the iron ore material undergoing direct reduction and / or thermal treatment.

[0301] Alternatively, the control circuit is connected to the iron ore oxide preheating device and / or the heating device and is configured to control the temperature of the iron ore oxide material to be loaded so that the iron ore oxide material undergoing reduction and / or heat treatment will strive towards a predetermined temperature of about 200°C to 600°C, preferably about 300°C to 500°C during a predetermined period of time long enough to enable the heat treatment process to provide the desired passivation parameter value of the reduced iron ore material and thereby provide an intermediate product that is resistant to reoxidation.

[0302] Alternatively, the predetermined temperature is about 400°C to 800°C, preferably about 500°C to 700°C.

[0303] Alternatively, the predetermined temperature is about 600°C to 1000°C, preferably about 700°C to 900°C.

[0304] Alternatively, the control circuit is further connected to a reductant preheating device configured to preheat the reductant prior to introduction into the direct reduction facility, and is configured to control the temperature of the reductant so that the iron ore oxide material undergoing reduction and / or heat treatment will strive towards a predetermined temperature of about 200°C to 600°C, preferably about 300°C to 500°C, during a predetermined period of time long enough to enable the thermal treatment process to provide the desired passivation parameter value of the reduced iron ore material and thereby provide an intermediate product that is resistant to reoxidation.

[0305] Alternatively, the control circuitry may be adapted to provide a heat treatment process in a direct reduction facility for heat treating the iron ore oxide material undergoing reduction during a predetermined time period by controlling the temperature of the iron ore oxide material retaining thermal energy towards a predetermined temperature so as to achieve desired passivation parameter values ​​with respect to porosity and / or sponge iron size and / or weight per volume of sponge iron produced and / or iron ore particle structure and / or sample cut uniformity and / or shrinkage and / or sintering and / or cold crushing strength etc.

[0306] Alternatively, the desired passivation parameter value may be defined as a value for the rate and / or extent and / or grade and / or portion and / or proportion of reoxidation of the intermediate product (sponge iron and / or reduced iron ore material).

[0307] Alternatively, the desired passivation parameter value for porosity, its definition can be expressed as the ratio of the pore volume of the sponge iron produced to its total volume. The sponge iron size can be expressed as the average diameter of the sponge iron agglomerates typically produced. The weight per volume can be defined as a measure of the iron concentration of the sponge iron agglomerates typically produced. The iron ore particle structure can be defined as the final microstructure of the sponge iron agglomerates produced and the distribution of dense and porous areas. The sample cutting uniformity can define the density of the sponge iron agglomerates produced.

[0308] Alternatively, a heat treatment process provided by a control circuit during a predetermined time period so as to achieve a desired passivation parameter value for the sponge iron produced produces a sponge iron or intermediate product having a highly uniform chemical composition for cost-effective and energy-efficient production in subsequent steel production in a steel plant and / or a final porosity and / or a dense structure with high uniformity in a specific area (e.g. a central area of ​​a sponge iron agglomerate), is resistant to reoxidation, and is produced with low carbon dioxide emissions.

[0309] The present disclosure may not be limited to the examples described above, but many possibilities of modifications or combinations of the examples described herewith will be apparent to a person skilled in the art without departing from the basic idea as defined in the appended claims. BRIEF DESCRIPTION OF THE DRAWINGS

[0310] Hereinafter, exemplary embodiments of the present invention will be described with reference to the accompanying drawings, in which some unimportant details may be deleted from the drawings for the sake of clarity and understanding of the present invention.

[0311] Figure 1 A steel production configuration and process using renewable energy according to a first example is shown;

[0312] Figure 2 shows a steel production configuration and process using renewable energy according to a second example;

[0313] Figures 3a to 3d A steel production configuration and process using, for example, renewable energy and using carbon-containing materials to produce intermediate products with reduced carbon dioxide emissions is shown according to an exemplary embodiment;

[0314] Figures 4a to 4d A steel production arrangement and process including a control circuit adapted to provide desired carburizing parameter values ​​for optimizing carburization and current demand for direct reduced iron ore material / iron ore oxide material subjected to reduction according to an exemplary embodiment is shown;

[0315] Figure 4e A preheating device for a steel production arrangement according to one aspect is shown;

[0316] Figure 5 shows a steel production configuration and process according to an exemplary embodiment;

[0317] Figure 6 An iron ore oxide material production unit of a steel production arrangement according to a fifth example is shown;

[0318] Figure 7 A steel production configuration and process using renewable energy according to a sixth example is shown;

[0319] Figure 8 shows a steel production configuration and process using renewable energy according to a seventh example;

[0320] Fig. 9 shows a direct reduction facility and process according to a steel production configuration of an eighth example;

[0321] Fig.10 A flow chart illustrating an exemplary method and process for the reduction of iron ore oxide materials for a steel production configuration is shown;

[0322] Fig.11 A flow chart illustrating an exemplary method and process for the reduction of iron ore oxide materials for a steel production configuration is shown;

[0323] Fig.12 shows a control circuit for a steel production arrangement and process according to another example;

[0324] Fig.13 An integrated steel production configuration according to one aspect is shown;

[0325] Figures 14a to 14d An exemplary iron ore oxide material production unit is shown; and

[0326] Figures 15a to 15c An exemplary steel production configuration is shown. DETAILED DESCRIPTION

[0327] Figure 1The steel production configuration and process using renewable energy according to the first example are shown. The method for producing steel includes such process steps: wherein the iron ore oxide material 5 (e.g., iron ore pellets) is reduced with hydrogen H in a direct reduction facility 7, and the intermediate product RM (e.g., sponge iron) of the directly reduced iron ore material thus obtained and possible accompanying materials are metallurgically processed by a steel producer 17. The hydrogen H is produced by electrolysis of water with the aid of an electrolysis unit 19. The electric energy required for electrolysis is a renewable energy source derived from a hydropower and / or wind power and / or photovoltaic or other renewable energy supply source 2. If sufficient renewable generated electric energy is available, hydrogen H and / or the intermediate product RM are produced independently of current demand. The iron ore oxide material 5 is transported from a preheating device 4 to the direct reduction facility 7 and retains the thermal energy derived from the preheating device 4. The preheating device 4 is configured to preheat the iron ore oxide material 5 before transporting the iron ore oxide material 5 from the preheating device 4 to the direct reduction facility 7 by a conveying device 95.

[0328] Alternatively, the preheating device 4 is configured to preheat the iron ore oxide material to be fed to the direct reduction facility to a certain extent by recovering heat from the direct reduction facility and / or from the iron ore oxide material production unit 3 configured to produce the iron ore oxide material 5 .

[0329] Alternatively, the technical feature of preheating the iron ore oxide material 5 before conveying it to the direct reduction facility 7 in combination with the further technical feature of introducing oxygen 10 (which also produces hydrogen H) produced by an electrolysis unit 19 into the iron ore oxide material production unit 3 for manufacturing the iron ore oxide material 5 provides a sustainable, comprehensive production concept for the efficient production of steel, in which renewable energy can be used on an industrial scale and fluctuations in the production of renewable energy can be coped with.

[0330] The direct reduction facility 7 is configured to introduce hydrogen H suitable for reacting with the iron ore oxide material 5 maintaining the thermal energy provided by the preheating device 4, thereby reducing the iron ore oxide material 5 into an intermediate product RM by utilizing the thermal energy of the iron ore oxide material 5 to heat or further heat the introduced hydrogen H to achieve a chemical reaction between the iron ore oxide material 5 and the hydrogen H.

[0331] If sufficient regeneratively produced electrical energy is available, hydrogen H and / or intermediate products RM are always produced independently of the current demand. The intermediate products RM not required are stored until required / used, so that the renewable energy stored therein is also stored.

[0332] Alternatively, during the reduction of the iron ore oxide material 5 into the intermediate product RM, a gas containing carbon or hydrogen may be added to the hydrogen H so as to incorporate carbon into the intermediate product RM. The amount of the gas containing carbon or hydrogen added to the hydrogen H for reduction is at least such that the carbon content in the intermediate product is 0.0005 mass % to 6.3 mass %.

[0333] Alternatively, the carbon- or hydrogen-containing gas is methane or other carbon-containing gas from biogas production or from pyrolysis of renewable feedstocks or is synthesis gas from biomass.

[0334] Alternatively, the hydrogen gas H used for reduction has added thereto a carbon-containing or hydrogen-containing gas at least sufficient to make the carbon content in the intermediate product 1 mass % to 3 mass %.

[0335] Alternatively, the hydrogen H consists of pure hydrogen and possibly carbon-containing gases and is introduced at a temperature of 450° C. to 1200° C. into a reduction process utilizing thermal energy from the charged iron ore oxide material retaining the thermal energy from the preheating device 4 .

[0336] Alternatively, the reduction facility 7 is configured to produce a carbon-free intermediate product RM.

[0337] Alternatively, the overpressure in the reduction is from 0 bar to 15 bar.

[0338] Alternatively, the steel production arrangement comprises an iron ore oxide material production unit 3, such as a pelletizing plant, configured for producing iron ore oxide material 5.

[0339] Alternatively, the electrical energy required for the electrolysis includes electricity derived in part from nuclear energy.

[0340] The electrolysis unit 19 is electrically coupled to the hydro and / or wind and / or photovoltaic or other renewable energy supply source 2 and is configured to provide electrolysis of said water which also produces oxygen 10 which is used by the iron ore oxide material production unit 3 to manufacture the iron ore oxide material 5 .

[0341] The preheating device 4 heats the iron ore oxide material 5 before the iron ore oxide material 5 is charged into the direct reduction facility 7 .

[0342] In this way it is provided that the iron ore oxide material 5 to be reduced in the direct reduction facility 7 retains the thermal energy originating from the preheating device 4 .

[0343] In this way, a method is provided for using renewable energy sources for steel production on an industrial scale and for achieving a sustainable and comprehensive production concept for steel production based on renewable energy sources.

[0344] In this way, a method for producing steel that copes with fluctuations in the production of renewable energy used in the method for producing steel is provided, the method for producing steel requiring less renewable energy for reduction and being time-saving.

[0345] This is due to the fact that the reduction potential of hydrogen is maintained during the reduction of the iron ore oxide material to the intermediate product.Maintaining the chemical reactivity and / or driving force of hydrogen is essential to provide an efficient chemical reaction with the iron ore oxide material 5.

[0346] This is due to the fact that the use of hydrogen gas as a reducing agent for reducing the iron ore oxide material 5 is minimized to save renewable energy.

[0347] Alternatively, the transport of the carbon-free intermediate products is carried out via a flammable storage transport train car FL comprising a hot cabinet, into which the carbon-free intermediate products RM are conveyed from the direct reduction facility 7 .

[0348] Figure 2 A steel production configuration and process using renewable energy according to a second example is shown. The method for producing steel comprises process steps in which an iron ore oxide material 5 (e.g. iron ore pellets) is reduced with hydrogen H in a direct reduction facility 7 and the intermediate product RM of the direct reduced iron ore material thus obtained and possible accompanying substances are metallurgically processed by a steel producer 17. Scrap iron SI may be added to the process for producing steel.

[0349] Hydrogen H is produced by electrolysis of water in the electrolysis unit 19. The electric energy required for electrolysis is renewable energy from hydropower and / or wind power and / or photovoltaic or other renewable energy supply sources 2.

[0350] The direct reduction facility 7 is configured to introduce hydrogen H suitable for reacting with the iron ore oxide material 5 retaining thermal energy, thereby reducing the iron ore oxide material 5 to an intermediate product RM by utilizing the thermal energy of the iron ore oxide material 5 to heat or further heat the introduced hydrogen H to achieve a chemical reaction between the iron ore oxide material 5 and the hydrogen H. If sufficient regeneratively generated electrical energy is available, hydrogen H and / or the intermediate product RM are always produced independently of the current demand. The intermediate product RM that is not required is stored until it is required / used, so that the regenerative energy stored therein is also stored.

[0351] The iron ore oxide material production unit 3 is configured to produce heat-retaining iron ore oxide material 5. The heat-retaining iron ore oxide material 5 is transported to the direct reduction facility 7 through the transport device 95. The heat energy comes from the manufacturing heat process of the iron ore oxide material production unit 3.

[0352] Therefore, during the reduction of the iron ore oxide material in the direct reduction facility 7 by utilizing the thermal energy of the iron ore oxide material 5, the reduction potential of the hydrogen H is maintained and not destroyed. In this way, the chemical reactivity of the hydrogen H and / or the high driving force of the hydrogen H, which are essential for providing an effective chemical reaction with the iron ore oxide material 5, are maintained.

[0353] The amount of hydrogen gas H used as a reducing agent for reducing the iron ore oxide material 5 is minimized to save renewable energy.

[0354] In order to compensate for temporary fluctuations in the production of renewable energy, if excess energy is available, this energy is stored in the form of hydrogen, while the method according to the invention for producing steel requires less renewable energy for the reduction and saves time.

[0355] Alternatively, a hydrogen storage tank HT is provided between the electrolysis unit 19 and the direct reduction facility 7. Such a hydrogen storage tank arrangement HT can then be used in the event of fluctuations in the production of renewable energy. Temporary fluctuations can be predictable (e.g. at night in a solar energy plant) or unpredictable (e.g. fluctuations in wind strength in a wind energy plant).

[0356] Longer term fluctuations may occur in particular due to different seasons and can be taken into account in energy storage in the form of HBI (hotbriquetted iron), while the method according to the invention for producing steel requires less renewable energy for reduction and saves time.

[0357] Figures 3a to 3d A steel production configuration and process using renewable energy and using carbon-containing materials to produce intermediate products with reduced carbon dioxide emissions is shown according to an exemplary embodiment.

[0358] Figure 3a A steel production configuration and process using renewable energy according to a third example is shown. Carbonaceous matter 100 is extracted from a carbon source CS and added to the iron ore oxide material during reduction and / or to the direct reduced iron ore material in an independent carburizing zone 101 of a direct reduction facility 7 and / or in an independent carburizing reactor 102 (which is configured to provide carbon to the direct reduced iron ore material), thereby managing the production of a carbonaceous intermediate product RM discharged from the direct reduction facility 7 and / or from the independent carburizing reactor 102.

[0359] Alternatively, the carbonaceous material 100 includes pure carbon elements or is a component of molecules such as methane, propane or other hydrocarbons or other molecules.

[0360] Alternatively, the carbon source CS may comprise a carbon capture and utilization unit (CCU).

[0361] Alternatively, the carbon capture and utilization unit (CCU) includes a CO 2 capture device CCD configured to capture CO 2 from the atmosphere, and the captured CO 2 is transported to the independent carburizing zone 101 and / or the independent carburizing reactor 102 .

[0362] Figure 3b An exemplary steel production configuration and process is shown.

[0363] The direct reduction facility 7 may be loaded with high temperature iron ore oxide material 5, for example, 800° C. to 1300° C., wherein heat energy of the iron ore oxide material 5 to be loaded into the direct reduction facility 7 is generated by an iron ore oxide material supply device (not shown).

[0364] Alternatively, the carburizing zone constitutes an independent (isolated) carburizing zone 101 configured to prevent the carbonaceous substance 100 injected into the carburizing zone 101 from being mixed with the reducing agent RA.

[0365] Alternatively, the carburizing zone constitutes a carburizing volume (not shown) inside the direct reduction facility 7, which is configured for reducing the iron ore oxide material 5 and for carburizing the iron ore oxide material 5 subjected to reduction and mixing the carbonaceous substance 100 with the reducing agent RA.

[0366] Alternatively, the carburizing volume is configured to provide a carburizing chemical reaction between hydrogen H2 and carbon dioxide CO2 to achieve carburization of the reduced iron ore oxide material 5, wherein the reduced iron ore oxide material 5 acts as a catalyst to produce a carbonaceous material added to the reduced iron ore oxide material 5.

[0367] Alternatively, the independent carburizing zone 101 is configured to provide an independent (isolated) carburizing chemical reaction between hydrogen H2 and carbon dioxide CO2 to achieve carburization of the direct reduced iron ore material 5, wherein the direct reduced iron ore material acts as a catalyst to produce carbonaceous material added to the direct reduced iron ore material.

[0368] C02+2H2>C+2H20

[0369] C02+H2>CO+H20

[0370] CO+H2>C+H20

[0371] Alternatively, the independent carburizing zone 101 is provided with a carburizing zone carbonaceous material inlet device (not shown) and / or a carburizing zone hydrogen inlet (not shown).

[0372] Alternatively, the carburizing zone carbonaceous material inlet is configured to feed the carbonaceous material 100 (eg, CO 2 , CH 4 ) or other carbonaceous compounds into the independent carburizing zone 101 .

[0373] Alternatively, the carburizing zone hydrogen inlet is configured to feed hydrogen-containing gas H (H 2 ) into the independent carburizing zone 101 .

[0374] Alternatively, the carburizing zone is configured as an independent carburizing reactor 102, which is configured with a first reactor fluid inlet (not shown) for feeding a first reactor fluid (carbon-containing substance 100) into the independent carburizing reactor 102 and a second reactor fluid inlet (not shown) for feeding a second reactor fluid (hydrogen-containing gas H) into the independent carburizing reactor 102 to provide a chemical reaction between the first reactor fluid and the second reactor fluid.

[0375] Alternatively, the first reactor fluid inlet and / or the second reactor fluid inlet comprises a regulating device (not shown) for regulating a property of the first reactor fluid and / or the second reactor fluid.

[0376] Alternatively, the regulating device is electrically coupled to a control circuit (not shown) adapted to regulate a property of the first reactor fluid and / or the second reactor fluid, such as concentration, temperature, flow rate, pressure, etc.

[0377] Alternatively, the direct reduced iron ore material and / or the iron ore oxide material undergoing reduction acts as a catalyst to produce carbonaceous material, such as methane CH4 and / or carbon monoxide CO and / or solid carbon C and / or other carbon compounds, which carburizes the direct reduced iron ore material and / or the iron ore oxide material undergoing reduction.

[0378] Alternatively, the independent carburizing reactor 102 is configured for carrying out a chemical reaction between a first reactor fluid comprising carbon dioxide CO2 and a second reactor fluid comprising a hydrogen content of 80 volume % to 100 volume %, wherein the direct reduced iron ore material DRI fed into the independent carburizing reactor 102 acts as a catalyst to produce CH4 and / or carbon monoxide CO and / or solid carbon C and / or other carbon compounds that carburize the direct reduced iron ore material DRI.

[0379] Alternatively, a carburizing chemical reaction between hydrogen H2 and carbon dioxide CO2 is provided by controlling the chemical reaction between the first reactor fluid and the second reactor fluid through a control circuit (not shown) to provide carburizing of the direct reduced iron ore material within the independent carburizing reactor 102, wherein the direct reduced iron ore material DRI acts as a catalyst to produce CH4 and / or carbon monoxide and / or solid carbon and / or other carbon compounds for carburizing the direct reduced iron ore material.

[0380] C02(g)+2H2(g)>C(s)+2H20(g)

[0381] C02+H2>CO+H20

[0382] CO+H2>C+H2O

[0383] Figure 3c An exemplary steel production configuration and process using renewable energy is shown. The carbon production unit includes a Sabatier reactor SR that produces methane CH4 from the reaction between hydrogen H2 and carbon dioxide CO2, and the methane CH4 is a carbon- or hydrogen-containing gas that is transported to an independent carburizing zone 101 and / or an independent carburizing reactor 102. The carbon production unit includes a Fischer-Tropsch FT device configured to produce a carbon-containing product by reducing the methane CH4 produced by the Sabatier reactor, and the carbon-containing product is transported to an independent carburizing zone 101 and / or an independent carburizing reactor 102. The intermediate product RM produced is transported to the steelmaking industry 17.

[0384] Figure 3d An exemplary steel production configuration and process using renewable energy is shown.The biogas production unit CS2 is configured for producing carbon-containing gas.

[0385] Alternatively, the steel production arrangement and process using renewable energy may include means for providing a so-called Bosch reaction within a portion of a direct reduction facility and / or separately by adding hydrogen and carbon dioxide to the iron ore oxide material under reduction to carburize the iron ore oxide material.

[0386] Alternatively, the Bosch reaction utilizes iron as a catalyst to produce carbon via CO2(g)+2H2(g)→C(s)+2H2O(g)+thermal energy, which can be produced in a separate carburizing zone of a direct reduction facility and / or in a separate carburizing reactor 102.

[0387] Alternatively, a cement industry plant manufacturing cement from mined calcium minerals uses a carbon production unit CS1 configured for producing non-fossil produced carbon.

[0388] Alternatively, the carbon production unit CS1 of a cement industry plant comprises a cement kiln (not shown) configured to capture carbon dioxide CO2 emitted from the cement kiln during cement production, said carbon dioxide CO2 being used for carburizing the iron ore oxide material under reduction.

[0389] Alternatively, the carbon production unit and / or Sabatier reactor and / or Fischer-Tropsch unit and / or carbon production unit and / or carbon capture and utilization unit and / or biogas production unit and / or synthesis gas production unit are incorporated as an integrated unit of the preheating unit and / or iron ore oxide material production unit and / or direct reduction facility and / or electrolysis unit and / or steelmaking industry17.

[0390] Figures 4a to 4d A steel production configuration and process is shown according to an exemplary embodiment, which includes a control circuit connected to an iron ore material production unit 3 and is suitable for providing desired carburizing parameter values ​​of direct reduced iron ore material and / or iron ore oxide material undergoing reduction to optimize the carburizing of the direct reduced iron ore material and current demands from the steel production industry 17.

[0391] Figure 4a A process is shown using a first control circuit 51, which is suitable for controlling the iron ore oxide material temperature of the iron ore oxide material 5 fed from the iron ore oxide material production unit 3 to the direct reduction facility 7 and / or controlling the internal gas pressure (not shown) in the direct reduction facility 7 and / or the hydrogen temperature and / or hydrogen pressure of introduced hydrogen (not shown) used as a reducing agent.

[0392] The first control circuit 51 may be adapted to control the iron ore oxide material temperature of the iron ore oxide material 5 delivered to the direct reduction facility 7 by controlling the iron ore oxide material production unit 3 to discharge the iron ore oxide material 5 from the iron ore oxide material production unit 3 at a specific temperature having a first temperature value determined by a desired carburizing parameter value of the direct reduced iron ore material to be carburized. The first detector member DCT1 of the carburizing reactor 102 and / or the carburizing zone 101 is electrically coupled to the first control circuit 51.

[0393] Alternatively, the first sensor device S1 is arranged at the iron ore oxide material discharge outlet (not shown) of the iron ore oxide material production unit 3 and / or at the iron ore oxide material loading inlet (not shown) of the direct reduction facility 7 , and the first sensor device S1 is connected to the first control circuit 51 .

[0394] Alternatively, the process for producing steel and / or sponge iron of carburized sponge iron includes the steps of reducing an iron ore oxide material by introducing a reducing agent such as hydrogen into a direct reduction facility 7 to provide a directly reduced iron ore material, transporting the directly reduced iron ore material to a carburizing zone 101, and carburizing the reduced iron ore material in the carburizing zone 101 using a carbon-containing substance such as a carburizing gas and / or solid carbon and / or the introduced hydrogen itself to provide a carburized sponge iron or an intermediate product.

[0395] Alternatively, the first sensor device S1 is configured to detect the first temperature value.

[0396] Alternatively, the first control circuit 51 is configured to control the iron ore oxide material production unit 3 to discharge the iron ore oxide material 5 at said first temperature value determined by a desired carburizing parameter value of the direct reduced iron ore material to be carburized, wherein the first control circuit 51 takes into account the desired carburizing parameter value when determining said first temperature value of the iron ore oxide material 5 to be charged into the direct reduction facility 7.

[0397] Alternatively, the desired carburizing parameter value is a parameter value of the direct reduced iron ore material (and / or the iron ore oxide material undergoing reduction) that provides optimal carburization of the direct reduced iron ore material and / or optimal carburization of the iron ore oxide material undergoing reduction.

[0398] Figure 4b An application of a second control circuit 52 is shown, which is suitable for controlling the temperature of the iron ore oxide material 5 delivered to the direct reduction facility 7 by controlling the preheating device 4 to discharge the iron ore oxide material 5 into the direct reduction facility 7 at a specific temperature, wherein the specific temperature has a second temperature value determined by the desired carburizing parameter value of the direct reduced iron ore material to be carburized.

[0399] Alternatively, a second sensor device S2 is arranged at an iron ore oxide material discharge outlet (not shown) of the preheating device 4 and / or a loading inlet (not shown) of the direct reduction facility 7 , said second sensor device S2 being coupled to the second control circuit 52 .

[0400] Alternatively, the second sensor device S2 is configured to detect the second temperature value.

[0401] The second detector member DCT2 of the carburizing reactor 102 and / or the carburizing zone 101 is electrically coupled to the second control circuit 52 .

[0402] Alternatively, the second control circuit 52 is configured to control the preheating device 4 to discharge the iron ore oxide material 5 at a second temperature value determined by a desired carburizing parameter value of the direct reduced iron ore material to be carburized.

[0403] When determining said second temperature value of the iron ore oxide material 5 to be charged into the direct reduction plant 7, the second control circuit 52 takes into account the desired carburizing parameter value.

[0404] Alternatively, the desired carburizing parameter value is a temperature value of the direct reduced iron ore material (and / or the iron ore oxide material undergoing reduction) that provides optimal carburization of the direct reduced iron ore material and / or optimal carburization of the iron ore oxide material undergoing reduction.

[0405] For example:

[0406] - The specific temperature of the ore oxide material 5 when charged into the direct reduction facility has a temperature of about 1100°C.

[0407] - The reducing agent (e.g., hydrogen content of 100 volume %) has a temperature of about 500° C. when introduced into the direct reduction facility, wherein the reducing agent reacts with the iron ore oxide material by utilizing the thermal energy of the iron ore oxide material to heat or further heat the introduced reducing agent to achieve a chemical reaction between the iron ore oxide material and the reducing agent, thereby reducing the iron ore oxide material to an intermediate product.

[0408] - The temperature of the produced reduced iron ore material ready for discharge from the direct reduction facility and / or ready for carburization is about 600°C (1100°C - 500°C = 600°C).

[0409] In this manner, for example, the reduced iron ore material has a desired temperature of about 600° C. at which carburization of the reduced iron ore material is most effective.

[0410] Alternatively, the desired carburizing parameter value corresponds to a desired iron ore porosity value of the direct reduced iron ore material, a desired iron ore size value of the direct reduced iron ore material, a carbon content value, etc.

[0411] Figure 4c The application of a third control circuit 53 is shown, which is suitable for controlling the hydrogen pressure of hydrogen H delivered to the direct reduction facility 7 by controlling a first pressurizing device 63 suitable for pressurizing the hydrogen entering the direct reduction facility 7 at a specific hydrogen pressure, wherein the specific hydrogen pressure has a first hydrogen pressure value determined by the desired carburizing parameter value of the direct reduced iron ore material to be carburized.

[0412] The iron ore oxide material production unit 3 is configured to discharge the iron ore oxide material 5 retaining thermal energy (thermal energy derived from the manufacturing heat process provided by the iron ore oxide material production) into the direct reduction facility 7 .

[0413] Alternatively, the third control circuit 53 is adapted to control the hydrogen pressure by controlling the first pressurizing device 63 (eg, a pressure pump) to inject hydrogen H into the direct reduction facility 7 at the first hydrogen pressure value.

[0414] Alternatively, a third sensor device S3 is arranged at the hydrogen inlet 69 of the direct reduction facility 7 , said third sensor device S3 being connected to the third control circuit 53 .

[0415] Alternatively, the third sensor device S3 is configured to detect the first hydrogen pressure value.

[0416] A third detector member (not shown) of the carburizing reactor 102 and / or the carburizing zone 101 is electrically coupled to the third control circuit 53 and is configured to detect the desired carburizing parameter value.

[0417] Alternatively, the third control circuit 53 is configured to control the first pressurizing device 63 to pressurize the hydrogen H in the direct reduction facility 7 at the first hydrogen pressure value, wherein the first hydrogen pressure value is determined by the desired carburizing parameter value of the direct reduced iron ore material to be carburized, wherein when determining the first hydrogen pressure value, the third control circuit 53 takes into account the desired carburizing parameter value.

[0418] Alternatively, the desired carburizing parameter value is a temperature value of the direct reduced iron ore material (and / or the iron ore oxide material undergoing reduction) that provides optimal carburization of the direct reduced iron ore material and / or optimal carburization of the iron ore oxide material undergoing reduction.

[0419] Alternatively, the desired carburizing parameter value corresponds to a desired iron ore porosity value of the direct reduced iron ore material, a desired iron ore size value of the direct reduced iron ore material, a carbon content value, etc.

[0420] Figure 4d The application of the process using a fourth control circuit 54 is shown, which is adapted to control the internal reduction pressure in the direct reduction plant 7 by controlling the second pressurizing device 64 .

[0421] The second pressurizing device 64 may include a valve package assembly (not shown) configured to regulate the internal reduction pressure, wherein the interior of the direct reduction facility 7 can be pressurized by controlling the flow of hydrogen, carburizing gas, etc. and by controlling the furnace top gas outlet flow by a regulator device RD connected to the fourth control circuit 54.

[0422] Alternatively, the regulator device RD may be configured to regulate the internal reduction pressure and / or the flow rate of hydrogen, carburizing gas, etc. and may be used to regulate the exhausted top gas.

[0423] The internal reduction pressure is set at a specific internal reduction pressure having a first internal reduction pressure value determined by a desired carburizing parameter value of the direct reduced iron ore material to be carburized.

[0424] Alternatively, the fourth control circuit 54 is adapted to control the internal reduction pressure by controlling the second pressurizing device 64 and / or by controlling the regulator device. The fourth sensor device S4 is arranged in the direct reduction facility 7 and is coupled to the fourth control circuit 54. The fourth sensor device S4 is configured to detect the first internal reduction pressure value.

[0425] The fourth control circuit 54 is configured to control the second pressurizing device 64 (and / or the regulator device RD) to pressurize the interior of the direct reduction facility 7 at said first internal reduction pressure value, which is determined by the desired carburizing parameter value of the direct reduced iron ore material to be carburized.

[0426] A fourth detector member (not shown) of the carburizing zone 101 and / or the carburizing reactor 102 is electrically coupled to the fourth control circuit 54 , the fourth detector member detecting the first internal reduction pressure value.

[0427] When determining the first internal reduction pressure value, the fourth control circuit 54 takes into account the desired carburizing parameter value.

[0428] Alternatively, the desired carburizing parameter value is a parameter value of the direct reduced iron ore material (and / or the iron ore oxide material undergoing reduction) that provides optimal carburization of the direct reduced iron ore material and / or optimal carburization of the iron ore oxide material undergoing reduction.

[0429] Alternatively, the desired carburizing parameter value or parameter values ​​correspond to a desired iron ore porosity value of the direct reduced iron ore material, a desired iron ore size value of the direct reduced iron ore material, a carbon content value, etc.

[0430] Figure 4e A preheating device 4 of an iron ore oxide material supply facility of a steel production arrangement according to one aspect is shown. The iron ore oxide material production unit 3 is configured to discharge the iron ore oxide material 5 retaining thermal energy.

[0431] The iron ore oxide material 5 is cooled by passing through a cooler device 81 which is configured to cool the discharged iron ore oxide material 5 .

[0432] Alternatively, the thermal energy TE′ extracted from the iron ore oxide material 5 discharged through the cooler device 81 is fed back to the iron ore oxide material production unit 3 and used in the manufacturing heat process for manufacturing the iron ore oxide material 5 .

[0433] Alternatively, the cooled iron ore oxide material 5 is stored and / or transported to the direct reduction facility 7. Before the iron ore oxide material 5 is charged into the direct reduction facility 7, the iron ore oxide material 5 is preheated by the preheating device 4.

[0434] Alternatively, the control circuit 50 is adapted to control the preheating device 4 to make the iron ore oxide material 5 have a certain temperature value (eg about 1100° C.) to reach a desired temperature value (eg about 600° C.) of the reduced iron ore material (intermediate product RM).

[0435] Alternatively, the preheating device 4 is configured to preheat the iron ore oxide material 5 to a temperature in the range of about 800°C to 1300°C.

[0436] Alternatively, the preheating device 4 is provided with a heating element 82 which preheats the iron ore oxide material 5 to have the specific temperature value before the iron ore oxide material 5 is charged into the direct reduction facility 7 .

[0437] For example, the heating element 82 may be fed with thermal energy TE″ extracted from a manufacturing heat process of the iron ore oxide material production unit 3 , said thermal energy TE″ being used to preheat the iron ore oxide material 5 .

[0438] For example, the heating element 82 may be configured with a hydrogen burner (not shown) that generates heat to the iron ore mixture using hydrogen and oxygen generated by an electrolysis unit (not shown) and / or another type of combustion device (not shown) and / or an electric heater (etc.).

[0439] Alternatively, the control circuit 50 is configured to control the preheating device 4 to discharge the iron ore oxide material 5 at a specific temperature value determined by a desired parameter value of the direct reduced iron ore material (intermediate product RM).

[0440] For example, the desired parameter value of the direct reduced iron ore material may correspond to a desired carburizing temperature value of the direct reduced iron ore material, a desired iron ore porosity value of the direct reduced iron ore material, a desired iron ore size value of the direct reduced iron ore material, and the like.

[0441] Figure 5 An application of a process using a fifth control circuit 55 is shown, which is suitable for controlling the hydrogen temperature of the hydrogen injected into the direct reduction facility 7 by controlling a heating device 74, which is configured to heat the hydrogen H at a specific hydrogen temperature, wherein the specific hydrogen temperature has a first hydrogen temperature value determined by a desired carburizing parameter value of the direct reduced iron ore material to be carburized.

[0442] Alternatively, the fifth control circuit 55 is adapted to control the hydrogen temperature by controlling the heating device 74 to provide the first hydrogen temperature value. A fifth sensor device S5 is arranged at the direct reduction facility 7, the fifth sensor device S5 is coupled to the fifth control circuit 55 and is configured to detect the first hydrogen temperature value.

[0443] The fifth control circuit 55 may be configured to control the hydrogen temperature according to a desired carburizing parameter value of the direct reduced iron ore material to be carburized. A fifth detector member (not shown) of the carburizing reactor 102 and / or the carburizing zone 101 is electrically coupled to the fifth control circuit 55 .

[0444] Alternatively, the desired carburizing parameter value is a parameter value of the direct reduced iron ore material (and / or the iron ore oxide material undergoing reduction) that provides optimal carburization of the direct reduced iron ore material and / or optimal carburization of the iron ore oxide material undergoing reduction.

[0445] Alternatively, at least one of the desired carburizing parameter values ​​corresponds to a desired carburizing temperature value of the direct reduced iron ore material, a desired iron ore porosity value of the direct reduced iron ore material, a desired iron ore size value of the direct reduced iron ore material, or the like.

[0446] The exemplary processes may be combined, and the first control circuit 51, the second control circuit 52, the third control circuit 53, the fourth control circuit 54 and the fifth control circuit 55 may be circuits of the control circuit 50, which adjust the iron ore oxide material temperature and / or reduction pressure and / or hydrogen temperature and / or hydrogen pressure according to the desired characteristics of the intermediate product RM.

[0447] Figure 6 A steel production configuration and process using an iron ore oxide material providing equipment including an iron ore oxide material production unit 3 is shown, wherein the iron ore oxide material production unit 3 is configured to produce iron ore oxide material 5 that retains the thermal energy, and the iron ore oxide material 5 that retains the thermal energy is transported to a direct reduction facility 7 to produce an intermediate product RM to be processed in a steelmaking industry 17.

[0448] The mined iron ore is transported from the iron ore mine 10M to the sorting and concentrating plant SCP of the iron ore oxide material production unit 3. The iron ore may be subjected to screening, crushing, separation, grinding, flotation processes and further separation may be provided by the sorting and concentrating plant SCP.

[0449] Alternatively, various additives may be mixed into the iron ore mixture 24 or slurry after the grinding, separation and flotation processes.

[0450] The iron ore mixture 24 may be filtered to a certain moisture content, and impurities may be separated from the iron ore mixture 24 to increase the iron content.

[0451] When the enrichment of the iron content in the iron ore mixture 24 is completed, the iron ore mixture 24 is conveyed to the granulation device 78 of the iron ore oxide material production unit 3. At the granulation device 78, clay minerals may be added to the iron ore mixture 24 as a binder, and then agglomerated iron ore mixture (e.g., so-called "green" pellets) may be formed in a rotating drum (not shown). The iron ore mixture 24 may be dried 72 and preheated 74 to increase the structural strength of the iron ore mixture 24.

[0452] The granulation plant 78 may be a grate-rotary kiln granulation plant or a rotary kiln plant, or any other type of pellet production plant. The iron ore oxide material production unit 3 is configured to process the agglomerated iron ore mixture 24 by making a thermal process.

[0453] Alternatively, the iron ore oxide material production unit 3 may produce agglomerated iron ore oxide material 5, such as pellets, to be fed directly into the direct reduction facility 7, so as to utilize the direct entry into the direct reduction facility 7 or via a preheating device (see Figure 1 ; Reference numeral 4) heat of the iron ore oxide material 5 entering the direct reduction facility 7.

[0454] Alternatively, the production of the iron ore oxide material 5 may include the steps of: grinding an iron ore body; separating iron ore particles; producing an iron ore mixture 24 of iron ore particles, and hardening the iron ore mixture 24 by oxidation of the iron ore mixture 24 and / or sintering of the iron ore mixture 24 .

[0455] Alternatively, the step of hardening the iron ore mixture 24 may be preceded by the step of drying the iron ore mixture 24 and / or preheating and / or heating the iron ore mixture 24 .

[0456] In order to achieve that the iron ore oxide material 5 will have satisfactory and suitable final properties before charging the iron ore oxide material 5 into the direct reduction facility 7, the iron ore mixture 24 is preferably preheated in the tempering preheating zone 74 and oxidized in the oxidation zone 77 and / or sintered in the sintering zone 76.

[0457] The iron ore mixture 24 is thus conveyed to a hardening device 22 comprising an oxidation zone 77 and / or a sintering zone 76 .

[0458] Alternatively, the step of preheating and / or heating the iron ore mixture comprises oxidizing the magnetite to hematite.

[0459] In this way, as the magnetite is oxidized to hematite, additional heat energy is generated, thereby further reducing the energy requirements, which is known to achieve efficient handling of fluctuations in the production of renewable energy used in the process for producing steel.

[0460] Alternatively, in order to provide an efficient sintering process and / or oxidation process of the iron ore mixture 24 (agglomerated iron ore mixture, such as so-called “green” pellets), an oxygen-rich process gas OE is fed to the hardening device 22 .

[0461] Alternatively, a hydrogen burner (not shown) is arranged in the hardening device 22 to provide a long flame of ignited gas mixture (hydrogen and oxygen or other and / or ambient air) to harden the iron ore mixture 24 to produce said iron ore oxide material 5 retaining thermal energy.

[0462] Control circuitry (not shown) may be adapted to control the intensity and temperature of the long flame.

[0463] The hydrogen burner may include a housing (not shown) and a hydrogen inlet (not shown) directed toward a combustion chamber (not shown) positioned within the housing.

[0464] The oxygen-enriched process gas OE is provided to increase the oxidation rate and to provide operation control of the iron ore oxide material production unit 3 .

[0465] When the iron ore oxide material 5 is charged into the direct reduction facility 7, the amount of thermal energy of the iron ore oxide material 5 may be controlled by a control circuit.

[0466] The control circuitry may take into account a desired temperature value of the reduced iron ore oxide material to be carburized to optimally carburize the direct reduced iron ore material.

[0467] Alternatively, the oxygen used to enrich the process gas may be oxygen 10 produced by an electrolysis unit 19 also used to produce hydrogen H. In this way a better utilization of the regenerative energy required for driving the electrolysis unit is achieved, while the iron ore oxide material 5 retains the thermal energy that promotes the reduction process and the chemical reactions in the direct reduction facility 7 due to the maintained reduction potential of the hydrogen H.

[0468] The sintering process can be distinguished into heating and oxidation. During the thermal process, ie during the oxidation and / or sintering process (hardening process) of the thermal process, the oxidation can be carried out with an oxygen-rich process gas OE which maintains a high oxygen pressure.

[0469] Alternatively, the oxygen-enriched process gas comprises heated process gas injected at the mixing unit 70' together with oxygen 10. The heated process gas PG is produced by a heat exchanger 79 configured to transfer heat from the spent reducing fluid 8 exhausted by the direct reduction facility 7 to the atmospheric gas AG.

[0470] Pure oxygen 10 may also be delivered from the electrolysis device 19 to the hardening device 22 to enable efficient oxidation and / or sintering of the iron ore mixture 24 .

[0471] Alternatively, oxygen 10 is fed from the electrolysis unit 19, for example via a pipeline assembly (not shown).

[0472] The electrolysis unit 19 is configured to decompose water w into hydrogen H and oxygen 10, and may use renewable energy and / or non-fossil produced energy.

[0473] Hydrogen gas H is introduced into the direct reduction facility 7 to provide direct reduction of the iron ore oxide material 5 through a chemical reaction between the hydrogen gas H and the iron ore oxide material 5 retaining the thermal energy, wherein the chemical reaction utilizes thermal energy.

[0474] The temperature of the direct reduced iron ore material discharged from the direct reduction facility 7 is lower than the temperature of the iron ore oxide material charged into the direct reduction facility 7 .

[0475] The temperature of the hydrogen H introduced into the direct reduction facility 7 is lower than the temperature at which the spent reducing fluid 8 is discharged from the direct reduction facility 7 .

[0476] The spent reducing fluid 8 comprising hydrogen H and water vapour is therefore discharged from the top part of the direct reduction plant 7 into a heat exchanger 79 and the condensing device CD is configured to condense the water vapour of the spent reducing fluid 8 into water.

[0477] The hydrogen H is transported back to the direct reduction facility 7 via a heat exchanger 79 and can be reused for the chemical reaction. A purification unit 71 can be connected to the direct reduction facility 7 to purify the hydrogen H of the spent reducing fluid 8.

[0478] Figure 7 A steel production configuration and process for producing steel using renewable energy and / or non-fossil produced energy according to a sixth example is shown. Iron ore fragments are transported from an iron ore mine 104 to an iron ore oxide material production unit 3. The iron ore oxide material production unit 3 is configured to produce iron ore oxide material 5. The iron ore oxide material 5 retains thermal energy provided by a manufacturing thermal process (including, for example, oxidation and sintering processes) performed by the iron ore oxide material production unit 3.

[0479] Alternatively, the iron ore oxide material 5 retaining thermal energy from the manufacturing heat process is directly transported to the direct reduction facility 7 in such a manner that when the iron ore oxide material 5 is charged into the direct reduction facility 7 to provide a chemical reaction between hydrogen H (reducing agent) and the iron ore oxide material 5, the iron ore oxide material 5 retains the thermal energy (e.g., fully retains the thermal energy or substantially retains the thermal energy or retains the thermal energy to a degree of 50% to 90%).

[0480] Alternatively, when the iron ore oxide material 5 is charged (transported) from the iron ore oxide material production unit 3 to the direct reduction facility 7, the iron ore oxide material 5 maintains thermal energy corresponding to a temperature in the range of about 850°C to about 1300°C, preferably about 1000°C to about 1250°C.

[0481] The iron ore oxide material 5 holding thermal energy from the manufacturing heat process provided by the iron ore oxide material production unit 3 is charged into the direct reduction facility 7. The direct reduction facility 7 is configured for introducing hydrogen H generated by the electrolysis unit 19. The hydrogen H is suitable for reacting with the iron ore oxide material 5 holding the thermal energy.

[0482] Alternatively, the iron ore oxide material 5 is reduced to a direct reduced iron ore material (intermediate product RM) by utilizing the thermal energy of the iron ore oxide material 5 to heat the hydrogen H to achieve a substantially or completely endothermic chemical reaction and / or a substantially or completely endothermic chemical reaction between the hydrogen H and the iron ore oxide material 5.

[0483] The direct reduction facility 7 comprises an iron ore oxide material loading inlet device 9 (eg a first opening) configured for conveying (passing) the iron ore oxide material 5 from the iron ore oxide material production unit 3 into the direct reduction facility 7 .

[0484] The direct reduction facility 7 further comprises a hydrogen inlet device 11 configured for introducing hydrogen H into the direct reduction facility 7 .

[0485] Alternatively, the hydrogen gas H is adapted to react with the iron ore oxide material 5 retaining said thermal energy in a substantially or completely endothermic chemical reaction.

[0486] Alternatively, the hydrogen gas H is adapted to react with the iron ore oxide material 5 retaining said thermal energy in a partially exothermic chemical reaction.

[0487] Alternatively, the hydrogen gas H is adapted to react with the iron ore oxide material 5 retaining said thermal energy by substantially or completely endothermic and by a small amount of exothermic chemical reaction preceding or following the substantially or completely endothermic chemical reaction during reduction of the iron ore oxide material 5.

[0488] Alternatively, the hydrogen H is suitable for reacting with the iron ore oxide material 5 retaining said thermal energy provided by said manufacturing heat process in a substantially or completely endothermic and / or exothermic chemical reaction, wherein the substantially or completely endothermic chemical reaction absorbs a first energy content from the iron ore oxide material 5, and the exothermic chemical reaction releases a second energy content, wherein the first energy content is greater than the second energy content.

[0489] Alternatively, the hydrogen gas H is suitable for absorbing the first energy content to initiate and sustain the chemical reaction.

[0490] Alternatively, the first energy content is 95% to 99% of the total energy content, and the second energy content is 1% to 5% of the total energy content of the chemical reaction.

[0491] The direct reduction facility 7 further comprises a spent reducing fluid outlet device 13 configured to discharge spent reducing fluids such as water vapor and hydrogen from the direct reduction facility 7. The direct reduction facility 7 further comprises a direct reduced iron ore material outlet device 15 configured to discharge direct reduced iron ore material from the direct reduction facility 7. The direct reduced iron ore material is transported to a steelmaking industry 17 to meet the production of steel.

[0492] Alternatively, the direct reduction facility 7 is configured to provide direct reduction of the iron ore oxide material 5 to a direct reduced iron ore material (intermediate product RM) by utilizing the thermal energy of the iron ore oxide material 5 provided by the manufacturing heat process (i.e. the thermal energy derived from the manufacturing heat process) to heat the hydrogen H to achieve a chemical reaction.

[0493] Alternatively, the direct reduction facility 7 and / or the electrolysis unit 19 and / or the steelmaking industry 17 are fully or partially integrated with the iron ore oxide material production unit 3 constituting an integrated direct reduction iron ore material and steelmaking industry 17 .

[0494] Alternatively, according to one aspect, the iron ore oxide material 5 may be cooled by a cooler device (not shown) configured to cool the iron ore oxide material 5 discharged from the iron ore oxide material production unit 3. The heat energy extracted from the discharged iron ore oxide material is fed back to the iron ore oxide material production unit 3 and used to make a thermal process. The cooled iron ore oxide material 5 may be stored and / or transported to the direct reduction facility 7. Before the cooled iron ore oxide material 5 is charged into the direct reduction facility 7, the iron ore oxide material 5 is preheated by a preheating device (not shown), so that the iron ore oxide material 5 again retains heat energy for chemical reactions in the direct reduction facility 7.

[0495] Figure 8 A steel production configuration with an integrated production unit and a process for producing steel according to a seventh example are shown. Iron ore fragments are transported from an iron ore mine 104 to an iron ore oxide material production unit 3. The iron ore oxide material production unit 3 produces an iron ore oxide material 5 which retains thermal energy provided by a manufacturing heat process provided by the iron ore oxide material production unit 3.

[0496] The manufacturing heat process may include, for example, drying and preheating the iron ore mixture, oxidizing the iron ore mixture, and sintering the iron ore mixture in a hardening process managed by the hardening device 22.

[0497] Alternatively, the iron ore oxide material 5 retaining the thermal energy is directly transported to the direct reduction facility 7 to provide a chemical reaction with hydrogen H for directly reducing the iron ore oxide material 5 .

[0498] The electrolysis unit 19 is configured to produce hydrogen H and also produce oxygen 10 which can be used by the hardening device 22 to provide the iron ore oxide material 5 .

[0499] For example, the amount of hydrogen H and / or oxygen 10 produced by the electrolysis unit 19 may be regulated by the control circuit 50 to provide heat used in the hardening process (oxidation and / or sintering) performed by the iron ore oxide material production unit 3 for producing the iron ore oxide material 5 retaining heat energy.

[0500] Alternatively, the iron ore oxide material 5 retaining the heat energy may be cooled, and the heat energy may be reused for the manufacturing heat process through the iron ore oxide material production unit 3. The cooled iron ore oxide material 5 may be transported to a sponge iron generator (not shown), which heats the iron ore oxide material 5 in a preheating device (not shown) to provide the heat energy of the iron ore oxide material to be reduced in a direct reduction facility, so as to provide a chemical reaction with hydrogen for direct reduction of the iron ore oxide material in the direct reduction facility.

[0501] Alternatively, the preheating apparatus is configured to utilize recovered heat from a direct reduction facility, wherein thermal energy is introduced into the cooled iron ore oxide material 5 to provide a thermally retained iron ore oxide material 5.

[0502] The direct reduction facility 7 is configured to receive hydrogen H produced by an electrolysis unit 19 of an integrated production unit which may be configured for steel production.

[0503] Alternatively, the electrolysis unit 19 may be located remotely from the direct reduction facility 7 .

[0504] The chemical reaction produces a spent reducing fluid 8 which is discharged from the direct reduction facility 7 as top gas and which can be reused in the manufacturing heat process via the iron ore oxide material production unit 3 .

[0505] For example, the amount of spent reducing fluid 8 may be regulated by the control circuit 50 to provide heat for a hardening process (oxidation and / or sintering) performed by the iron ore oxide material production unit 3 for producing the iron ore oxide material 5 retaining thermal energy.

[0506] The control circuit 50 may be adapted to control the production heat process and control the conveyance of the spent reducing fluid 8 from the reduction facility 7 back to the iron ore oxide material production unit 3 .

[0507] A control circuit 50 may also be electrically coupled to the electrolysis unit 19 to control the production of hydrogen H and oxygen 10 .

[0508] The control circuit 50 may also be electrically coupled to the direct reduction facility 7 to control and monitor the reduction of the iron ore oxide material 5 to direct reduced iron ore material (intermediate product RM).

[0509] The control circuit 50 may be electrically coupled to the hydrogen conditioning and / or pressurizing equipment (not shown) of the iron ore oxide material production unit 3 to control the manufacturing thermal process for producing the iron ore oxide material 5 .

[0510] The control circuit 50 may be electrically coupled to a preheating device (not shown) to control preheating of the iron ore oxide material 5 before charging the iron ore oxide material 5 into the direct reduction facility 7 .

[0511] The direct reduction facility 7 comprises a direct reduced iron ore material outlet device (not shown) configured to discharge the direct reduced iron ore material (intermediate product RM) to a train 20 for transporting the direct reduced iron ore material to the steelmaking industry 17. The direct reduction facility 7 is thus configured to provide reduction of the iron ore oxide material 5 to the direct reduced iron ore material by utilizing the thermal energy of the iron ore oxide material (the thermal energy source is from the manufacturing heat process) to heat the hydrogen H to achieve the chemical reaction between the iron ore oxide material and the hydrogen H, thereby providing the reduction.

[0512] Alternatively, oxygen 10 is delivered from the electrolysis unit 19 to the iron ore oxide material production unit 3 to support the manufacturing heat process provided by the iron ore oxide material production unit 3 .

[0513] Alternatively, the control circuit 50 may be electrically coupled to the iron ore oxide material production unit 3 to adjust the amount of oxygen 10 introduced into the oxidation and / or sintering process (hardening process) to achieve the manufacturing heat process provided by the iron ore oxide material production unit 3 .

[0514] Alternatively, the control circuit 50 is suitable for controlling the amount of oxygen 10 introduced into any processing unit / production unit of the iron ore oxide material production unit 3 during the oxidation and / or sintering process (hardening process) or which contributes to the production of thermal processes, and regulating / guiding the temperature of the iron ore oxide material to be charged into the direct reduction facility 7 towards a specific temperature value corresponding to a desired temperature value of the direct reduced iron ore material discharged from the direct reduction facility 7 or entering a carburizing zone (not shown).

[0515] Fig. 9A direct reduction facility 7 of a steel production configuration according to another example is shown. The iron ore oxide material production unit 3 produces iron ore oxide material 5, which is maintained at a temperature of, for example, about 900° C. to 1300° C., preferably about 950° C. to 1250° C., when being transported from the iron ore oxide material production unit 3 and entering the direct reduction facility 7.

[0516] The iron ore oxide material 5 may be in the form of iron ore pellets or other suitable agglomerates. After the production of the iron ore oxide material 5, the iron ore oxide material 5 is directly charged into the direct reduction facility 7, while the iron ore oxide material 5 still retains the thermal energy from the production process realized by the iron ore oxide material production unit 3 for producing the iron ore oxide material 5. The reducing agent supply source 30 is connected to the direct reduction facility 7 and is configured to supply hydrogen H to the direct reduction facility 7.

[0517] The downward flow 56 of the high temperature (the heat energy) iron ore oxide material contacts the upward flow 57 of the hydrogen H. The hydrogen H exhibits a lower temperature than the temperature of the iron ore oxide material 5. The direct reduction facility 7 may be defined as a countercurrent heat exchanger and is configured to cool the high temperature input iron ore oxide material 5 under direct reduction, wherein a substantially or completely endothermic chemical reaction is provided by the unheated hydrogen H.

[0518] Alternatively, when discharged from the direct reduction facility 7, the temperature of the intermediate product RM discharged from the direct reduction facility 7 may be about 50°C to 300°C, preferably about 100°C to 200°C.

[0519] Alternatively, when discharged from the direct reduction facility 7, the temperature of the discharged intermediate product RM may be about 20°C to 500°C.

[0520] Alternatively, the discharged direct reduced iron ore material may be subjected to carburization, wherein the method of reducing the iron ore oxide material 5 is determined to produce a higher temperature (eg, about 400°C to 700°C, preferably about 500°C to 650°C) direct reduced iron ore material.

[0521] The temperature of the direct reduced iron ore material is controlled to a desired temperature value that is optimal for effective carburizing or other preparation processes. In the case of producing a carbon-free intermediate product, the discharged direct reduced iron ore material having a high temperature is preferably cooled by a cooler (not shown), and the heat can be recovered and transferred back, for example, to the iron ore oxide material production unit 3.

[0522] Fig.10A flow chart is shown illustrating an exemplary process for producing steel, whereby iron ore is reduced with hydrogen in a direct reduction facility and intermediate products and possible accompanying substances of the direct reduced iron ore material thus obtained are metallurgically processed; the hydrogen is produced by the electrolysis of water; the electrical energy required for the electrolysis is derived from renewable energy in the form of hydropower and / or wind power and / or photovoltaics or other renewable energy sources.

[0523] If sufficient regeneratively generated electrical energy is available, hydrogen and / or intermediate products can be produced independently of current demand.

[0524] The process comprises a first step 101 of starting the process. A second step 102 shows the process. A third step 103 comprises stopping the process.

[0525] The second step 102 may include: transporting iron ore from the iron ore supply equipment to a direct reduction facility that maintains thermal energy originating from the iron ore supply equipment; the direct reduction facility is configured to introduce hydrogen suitable for reacting with the iron ore oxide that maintains thermal energy, thereby reducing the iron ore oxide to an intermediate product by utilizing the thermal energy of the iron ore oxide to heat or further heat the introduced hydrogen to achieve a chemical reaction between the iron ore oxide and the hydrogen.

[0526] The second step 102 may include implementing a method comprising the following steps: producing iron ore oxide material; loading the iron ore oxide material retaining thermal energy into a direct reduction facility; introducing a reducing agent into the direct reduction facility; reducing the iron ore oxide material into an intermediate product by utilizing the thermal energy of the iron ore oxide material to heat or further heat the introduced reducing agent to achieve a chemical reaction; and discharging the intermediate product from the direct reduction facility; and / or transporting the intermediate product to the steelmaking industry.

[0527] Fig.11A flow chart showing an exemplary process for producing steel is shown. The process includes a first step 111 of starting the process. A second step 112 includes producing hydrogen. If sufficient regeneratively generated electrical energy is available, the intermediate product and / or hydrogen can always be produced independently of current demand. A third step 113 includes storing the intermediate product until it is needed / used, so that the renewable energy stored therein is also stored. A fourth step 114 includes adding a carbon- or hydrogen-containing gas to the hydrogen during the reduction of the iron ore oxide to the intermediate product so as to incorporate carbon into the intermediate product. A fifth step 115 includes adding at least a carbon- or hydrogen-containing gas in an amount such that the carbon content in the intermediate product is 0.0005 mass % to 6.3 mass % to the hydrogen used for reduction. A sixth step 116 includes providing the carbon- or hydrogen-containing gas as methane or other carbon-containing gases from biogas production or from pyrolysis of renewable raw materials or syngas from biomass. The seventh step 117 includes producing iron ore oxide material by an iron ore oxide material production unit, wherein the iron ore oxide material maintaining the thermal energy is transported to the direct reduction facility. Alternatively, the eighth step 118 includes introducing an oxygen-enriched process gas into the hardening device to increase the oxidation rate in the manufacture of the iron ore oxide material, and providing additional operational control by connecting to the control circuit of the iron ore oxide material production unit. Alternatively, the ninth step 119 includes controlling the amount of thermal energy of the iron ore oxide material toward a temperature set according to the desired temperature value of the discharged direct reduced iron ore material when the iron ore oxide material is loaded into the direct reduction facility, which promotes optimal carburization of the direct reduced iron ore material. The tenth step 120 may include electrolyzing water to produce hydrogen and oxygen, which can be used by the iron ore oxide material production unit to produce iron ore oxide material maintaining the thermal energy from the iron ore oxide material production unit. The eleventh step 121 comprises extracting carbonaceous material from a carbon source, adding said material to the direct reduced iron ore material in a separate carburizing zone of the direct reduction facility and / or in a separate carburizing reactor configured to introduce carbon into an intermediate product discharged from the direct reduction facility. The twelfth step 122 comprises stopping the method.

[0528] Alternatively, the method includes the following steps: sending a parameter value signal from a detector component of the direct reduction facility to a control circuit; if the parameter value signal is an interrupt value, commanding the direct reduction facility to stop the chemical reaction between the iron ore oxide material and the reducing agent; and commanding a conveying device of an iron ore oxide material supply device to stop loading the iron ore oxide material that retains thermal energy into the direct reduction facility.

[0529] Fig.12A control circuit 50 of an iron ore oxide material production unit of a steel production configuration and process for producing steel according to another example is shown. The control circuit 50 is configured to control a process for producing steel, whereby the iron ore oxide material is reduced with hydrogen in a direct reduction facility, and the intermediate product and possible accompanying materials of the direct reduced iron ore material thus obtained are metallurgically treated. Hydrogen can be produced by electrolysis of water. The electric energy required for electrolysis is a renewable energy source derived from hydropower and / or wind power and / or photovoltaic or other renewable energy forms. If sufficient renewable electric energy is available, hydrogen and / or intermediate products can be produced independently of current demand. The iron ore oxide material is transported to the direct reduction facility from the iron ore oxide material providing device, and the heat energy derived from the iron ore oxide material providing device is maintained. The direct reduction facility is configured to introduce hydrogen suitable for reacting with the iron ore oxide material that maintains heat energy, thereby heating or further heating the introduced hydrogen by utilizing the heat energy of the iron ore oxide material to achieve a chemical reaction between the iron ore oxide material and the hydrogen, thereby reducing the iron ore oxide material to an intermediate product.

[0530] The control circuit 50 may include a computer and non-volatile memory NVM 1320, which is computer memory that can retain stored information even when the computer is not powered.

[0531] The control circuit 50 further comprises a processing unit 1310 and a read / write memory 1350. The NVM 1320 comprises a first memory unit 1330. A computer program (which may be of any type suitable for any operating data) is stored in the first memory unit 1330 to control the functions of the control circuit 50. In addition, the control circuit 50 comprises a bus controller (not shown), a serial communication unit (not shown) providing a physical interface through which information is transmitted in both directions. The control circuit 50 may comprise an I / O module (not shown) of any suitable type providing input / output signal transmission, an A / D converter (not shown) for converting a continuously varying signal from a sensor arrangement (not shown) of the control circuit 50, the sensor arrangement being configured to determine the actual operating status of the iron ore oxide material production unit.

[0532] The control circuit 50 is also configured to provide appropriate regulation of, for example, the flow of process gases, hydrogen, oxygen, the loading rate of iron ore oxide material into the direct reduction facility, the discharge rate of direct reduced iron ore material, etc., in accordance with the received control signals and in accordance with the detected operating conditions and other operating data. The control circuit 50 also includes an input / output unit (not shown) for coordinating time and date. The control circuit 50 includes an event counter (not shown) for counting the number of event multiples generated by independent events in the operation of the iron ore oxide material production unit and the direct reduction facility.

[0533] Furthermore, the control circuit 50 includes an interrupt unit (not shown) associated with the computer for providing multi-tasking and real-time calculations for semi-automatic and / or automatic operation of the iron ore oxide material production unit and the direct reduction facility. The NVM 1320 also includes a second memory unit 1340 for external sensor checks of sensor devices and detector components.

[0534] The data medium for storing the program P may include a program routine for automatically adjusting the operation of the iron ore oxide material production unit and the direct reduction facility according to the operating data. The data medium for storing the program P includes a program code stored on the medium, which can be read on a computer and used to cause the control circuit 50 to perform the process and / or method steps described herein. The program P can also be stored in an independent memory 1360 and / or a read / write memory 1350. In this embodiment, the program P is stored in an executable or compressed data format.

[0535] It should be understood that when the processing unit 1310 is described as performing a specific function, it is referred to that the processing unit 1310 can execute a portion of a program stored in the independent memory 1360 or a portion of a program stored in the read / write memory 1350. The processing unit 1310 is associated with a data port 999 for communicating via a first data bus 1315 connected to a process control unit group of a direct reduction facility, an iron ore oxide material production unit, an electrolysis unit and / or a steelmaking industry for performing the method. The non-volatile memory NVM 1320 is adapted to communicate with the processing unit 1310 via a second data bus 1312. The independent memory 1360 is adapted to communicate with the processing unit 610 via a third data bus 1311. The read / write memory 1350 is adapted to communicate with the processing unit 1310 via a fourth data bus 1314. According to the above process, after temporarily storing the received data, the processing unit 1310 will be ready to execute the program code.

[0536] Preferably, the signal (received by the data port 999) includes information about the operating status of the iron ore oxide material production unit and the direct reduction facility. The signal received at the data port 999 can be used by the control circuit 50 to control and monitor the automatic calibration of the sensor device and the detector member. The operator can manually feed the information and data to the control circuit 50 via a suitable communication device (such as a computer display or touch screen). The method can also be partially performed by the control circuit 50 through the processing unit 1310, which runs the program P stored in the independent memory 1360 or the read / write memory 1350. When the control circuit 50 runs the program P, the method disclosed herein will be performed.

[0537] Fig.13 An integrated steel production configuration according to one aspect is shown. Iron ore is transported from an iron ore mine 10M to an iron ore preparation facility 91 of an iron ore oxide material production unit 3 to provide an iron ore mixture 24. An electrolysis unit 19 is configured to perform electrolysis of water to produce hydrogen H and oxygen 10, and to use renewable energy. Oxygen 10 and hydrogen H are used by an iron ore hardening device 22 to oxidize and / or sinter the iron ore mixture 24 to produce an iron ore oxide material 5 that retains heat energy.

[0538] Optionally, the iron ore oxide material 5 can be loaded into the first direct reduction facility 7' via a conveying device 95 (for example, comprising a fireproof steel transport feeder) to directly reduce the iron ore oxide material 5 using the thermal energy of the iron ore oxide material and the introduced hydrogen H, and the temperature of the hydrogen is lower than the temperature of the loaded iron ore oxide material 5.

[0539] Optionally, the iron ore oxide material 5 may be cooled by a cooler device 81. The iron ore oxide material 5 may be stored and transported / delivered to the preheating device 4 to preheat the iron ore oxide material 5 before charging the iron ore oxide material 5 into the second direct reduction facility 7". The direct reduction of the iron ore oxide material 5 utilizes thermal energy provided to the iron ore oxide material 5 by the preheating device 4. The cooler device 81 is configured to recover thermal energy TE fed back to the iron ore oxide material production unit 3. The preheating device 4 may reuse thermal energy TE from the iron ore hardening facility 92. The preheating device 4 may also utilize thermal energy TE from the second direct reduction facility 7".

[0540] The first direct reduction facility 7' and the second direct reduction facility 7" are configured to produce direct reduced iron ore material (intermediate product RM).

[0541] Optionally, the direct reduced iron ore material is carburized by a carburizing process C, thereby providing a carburized intermediate product RM.

[0542] Carbonaceous matter 100 is extracted from the carbon source CS and added to the iron ore oxide material during reduction and / or to the directly reduced iron ore material in a separate carburizing zone (not shown) of the direct reduction facility 7 and / or in a separate carburizing reactor (not shown) configured to provide a carburized intermediate product RM. The carbonaceous intermediate product RM is ready for transfer to the steelmaking industry 17.

[0543] Optionally, the first direct reduction facility 7 ′ and the second direct reduction facility 7 ″ are configured to produce a carbon-free intermediate product RM ready for delivery to the steelmaking industry 17 .

[0544] Fig.14a An iron ore oxide material production unit 3 of a metal material production arrangement 200 is shown, the iron ore oxide material production unit 3 comprising an iron ore oxide material preheating device 203 and a conveying device (not shown) suitable for conveying an iron ore oxide material 5 retaining thermal energy originating from a manufacturing heat process. The iron ore oxide material preheating device 203 of the iron ore oxide material production unit 3 can produce an iron ore oxide material retaining thermal energy by, for example, a burner device, a heating element, etc. (not shown), wherein the previously cooled iron ore oxide material is preheated by the iron ore oxide material preheating device 203.

[0545] The iron ore oxide material pelletizing device 201 of the iron ore oxide material production unit 3 can produce iron ore oxide material retaining heat energy through a hardening device (not shown) of the iron ore oxide material pelletizing device 201. The iron ore oxide material pelletizing device 201 is configured to process the iron ore mixture 24 into the iron ore oxide material 5 retaining heat energy.

[0546] Optionally, the iron ore oxide material 5 retaining heat energy is transported from the iron ore oxide material pelletizing device 201 to the reduction facility 7, which is configured to reduce the iron ore oxide material into a reduced iron ore material (intermediate product RM) by introducing a reducing agent H into the reduction facility 7. The iron ore oxide material 5 produced by the iron ore oxide material pelletizing device 201 can be directly charged into the reduction facility 7.

[0547] Optionally, the iron ore oxide material 5 retaining heat energy is transported from the iron ore oxide material preheating device 203 to the reduction facility 7, which is configured to reduce the iron ore oxide material into an intermediate product RM by introducing a reducing agent H into the reduction facility 7. Before the iron ore metal oxide material is transported to the iron ore oxide material preheating device 203, the previously cooled iron ore oxide material may be stored at the stockpile 205.

[0548] The thermal energy of the iron ore oxide material is used to heat or further heat the introduced reducing agent H to achieve a chemical reaction to provide an intermediate product RM, and the iron oxide material 5 with retained thermal energy provided by the iron ore oxide material granulation equipment 201 or by the iron ore oxide material preheating device 203 is reduced by the reducing agent H in the reduction facility 7.

[0549] Fig.14b An iron ore oxide material cooler / preheater 207 is shown which is configured to operate as an iron ore oxide material preheater or as an iron ore oxide material cooler apparatus.

[0550] The iron ore oxide material pelletizing device 201 of the iron ore oxide material production unit (not shown) is connected to the iron ore oxide material cooler / preheating device 207, and the iron ore oxide material 5 retaining heat energy is produced by the hardening device (not shown) of the iron ore oxide material pelletizing device 201. The iron ore oxide material pelletizing device 201 is configured to process the iron ore mixture 24 into the iron ore oxide material 5 retaining heat energy.

[0551] The manufacturing thermal process may be adapted to produce iron ore oxide material and comprises the step of hardening the iron ore mixture to produce the iron ore oxide material.The step of hardening the iron ore mixture may comprise the step of oxidizing the iron ore mixture and / or the step of sintering the iron ore mixture.

[0552] The iron ore oxide material 5 retaining thermal energy is transported from the iron ore oxide material pelletizing device 201 to the iron ore oxide material cooler / preheater 207, which cools the iron ore oxide material 5 into cooled iron ore oxide material transported to the stockpile 205. The thermal energy of the iron ore oxide material 5 is recovered by the iron ore oxide material cooler / preheater 207 from the atmospheric process gas 204 fed through the iron ore oxide material cooler / preheater 207.

[0553] The iron ore oxide material cooler / preheater 207 is set in a cooling mode of operation to heat the atmospheric process gas 204 and provide a hot process gas 208 that is transported back to the iron ore oxide material pelletizing plant 201. The hot process gas 208 is used by the iron ore oxide material production unit to produce heat-retaining iron ore oxide material 5. The transport vehicle 206 is configured to transport the cooled iron ore oxide material to a reduction facility (not shown).

[0554] Fig.14c An iron ore oxide material cooler / preheater 207 is shown associated with the iron ore oxide material pelletizing plant 201 of the iron ore material production arrangement 200 .

[0555] Optionally, the iron ore oxide material cooler / preheating device 207 is disconnected from the iron ore oxide material pelletizing device 201, wherein the iron ore oxide material is transported from the iron ore oxide material pelletizing device 201 (preferably directly) to the reduction facility 7 to load the iron ore oxide material 5 that retains the thermal energy of the manufacturing heat process originating from the iron ore oxide material pelletizing device 201.

[0556] The heat energy of the iron ore oxide material 5 is utilized to realize a chemical reaction for providing a reduced iron ore material (intermediate product RM), and the iron ore oxide material 5 which retains the heat energy provided by the iron ore oxide material pelletizing device 201 is reduced by a reducing agent H in the reduction facility 7. The spent reducing fluid outlet (not shown) at the top portion of the reduction facility 7 is configured to pass through a heat exchanger (not shown) to discharge the spent reducing fluid 8 which retains heat, which provides a process gas containing heat which is transported back to the iron ore oxide material pelletizing device 201.

[0557] The iron ore oxide material pelletizing device 201 of the iron ore oxide material production unit 3 includes an iron ore oxide material discharge outlet 214 configured to discharge the iron ore oxide material 5 retaining heat energy from the iron ore oxide material production unit 3 .

[0558] Optionally, the iron ore oxide material 5 retaining thermal energy is transported to the reduction facility 7 via the iron ore oxide material cooler / preheater 207 (set to an operating mode in which the iron ore oxide material retaining thermal energy is not cooled, but additional heat is provided to the iron ore oxide material retaining thermal energy instead) via the transport path 212. The iron ore oxide material is transported from the iron ore oxide material cooler / preheater 207 to the reduction facility 7 via the iron ore oxide material discharge outlet 214 of the iron ore oxide material cooler / preheater 207.

[0559] Fig.14d An iron ore oxide material cooler / preheater 207 of an iron ore material production arrangement 1 is shown.

[0560] The iron ore oxide material cooler / preheater 207 is set in a preheating operation mode to preheat previously cooled iron ore oxide material transported from a stockpile 205 storing previously cooled iron ore oxide material to the iron ore oxide material cooler / preheater 207 before the iron ore oxide material 5 retaining heat energy is charged into the reduction facility 7.

[0561] The thermal energy source is free from the manufacturing heat process provided by the iron ore oxide material cooler / preheater 207 adapted to produce the thermally energy-retaining iron ore oxide material 5 in the preheating mode of operation.

[0562] In the preheating mode of operation, the previously cooled iron ore oxide material may first be heated by a heating source such as an electric heating element 210 or a process gas burner device or other. In addition, heat may be added to the preheating process using a waste reduction fluid 8 that retains heat energy recovered from the reduction facility 7 and / or heat energy from the operating iron ore oxide material pelletizing plant 201 or from other heat sources.

[0563] Alternatively, the spent reducing fluid 8 is conveyed to the iron ore oxide material cooler / preheater 207 and used as fuel for a burner component (not shown) of the iron ore oxide material cooler / preheater 207, which is configured to preheat the iron ore oxide material 5 to be charged into the reduction facility 7.

[0564] Alternatively, the manufacturing thermal process is adapted to provide the iron ore oxide material and includes the step of preheating the iron ore oxide material to provide the iron ore oxide material.

[0565] After the step of preheating the previously cooled iron ore oxide material to produce the iron ore oxide material that retains heat, the following steps are required to produce the reduced iron ore material (intermediate product RM): produce the iron ore oxide material 5; load the iron ore oxide material 5 that retains heat energy into the reduction facility 7; introduce the reducing agent H into the reduction facility 7; reduce the iron ore oxide material 5 to reduced iron ore material by utilizing the heat energy of the iron ore oxide material 5 to heat or further heat the introduced reducing agent H to achieve a chemical reaction; and discharge the intermediate product RM from the reduction facility 7.

[0566] Fig.15a An iron ore material production configuration 200 is shown as an exemplary steel production configuration suitable for reducing heat-retaining iron ore oxide material 5 into reduced iron ore material 16 .

[0567] The metal material production configuration 1 includes an iron ore oxide material production unit 3, such as an iron ore oxide granulation device or an iron ore oxide preheating device, configured to provide an iron ore oxide material 5 that retains thermal energy. The metal material production configuration 1 includes a direct reduction facility 7 configured to reduce the iron ore oxide material 5 that retains thermal energy. The iron ore oxide material loading and conveying unit (not shown) of the metal material production configuration 1 is configured to load the iron ore oxide material 5 into the upper inner part UP of the direct reduction facility 7.

[0568] Alternatively, an iron ore oxide material loading device (not shown) is configured to load the iron ore oxide material into the upper interior portion of the reduction facility.

[0569] The direct reduction facility 7 includes a reducing agent inlet (not shown), which is configured to introduce a hydrogen-containing reducing agent H into the lower internal portion of the direct reduction facility 7, whereby the hydrogen-containing reducing agent H is suitable for heating or further heating the introduced hydrogen-containing reducing agent H by utilizing the thermal energy of the iron ore oxide material 5 to provide a chemical reaction between the hydrogen-containing reducing agent H and the iron ore oxide material 5, and reacting with the iron ore oxide material 5 that retains thermal energy to reduce the iron ore oxide material 5.

[0570] The hydrogen gas of the reducing agent H containing hydrogen gas may be generated by an electrolysis unit (not shown) including a reducing agent temperature regulator 18 configured to regulate (preheat or cool) the temperature of the reducing agent H containing hydrogen gas.

[0571] The direct reduction facility 7 is configured to provide a heat treatment process for heat treating the iron ore oxide material 5 and / or the reduced iron ore material 16 subjected to reduction in the direct reduction facility 7. The metal material production arrangement 1 comprises a sixth control circuit 50 electrically connected to the reducing agent temperature regulator 18 to preheat the reducing agent H containing hydrogen.

[0572] The sixth control circuit 56 is adapted to control the temperature of the introduced preheated hydrogen-containing reducing agent H to provide at least one desired passivation parameter value of the reduced iron ore material 16 forming the intermediate product RM.

[0573] The sixth control circuit 56 is electrically coupled to the iron ore oxide material production unit 3 and is adapted to control the temperature of the heat-retaining iron ore oxide material 5 to be charged into the upper inner portion UP. The reduced iron ore material 16 exhibiting at least one desired passivation parameter value is discharged from the direct reduction facility 7 and transported to a steel producer (not shown), while the reduced iron ore material (intermediate product RM) resists reoxidation due to the passivation of the reduced iron ore material 16.

[0574] The direct reduction facility 7 is also configured to allow the reduced iron ore material 16 to descend into the lower inner portion LP to provide a heat treatment process for heat treating the reduced iron ore material using additional heat energy provided by the hydrogen-containing reducing agent.

[0575] It has been shown that utilizing the present disclosure is beneficial by the fact that the chemical reactivity of the hydrogen-containing reducing agent H and / or the high driving force of hydrogen are maintained when introduced into a direct reduction plant.

[0576] Chemical reactivity and / or high driving force are essential to provide efficient reduction of the iron ore oxide material. The introduced hydrogen-containing reducing agent H contains 80% to 100% hydrogen, preferably 100% hydrogen. The sixth control circuit 50 is adapted to control the temperature of the introduced preheated hydrogen-containing reducing agent H towards a predetermined temperature to provide sintering and / or heat treatment of the iron ore oxide material 5 subjected to reduction during a predetermined period of time.

[0577] Alternatively, the heat treatment includes thermal hardening.

[0578] Alternatively, the heat treatment comprises a thermal hardening process involving sintering of the reduced iron ore material and / or shrinking of the reduced iron ore material and / or densification of the reduced iron ore material.

[0579] Alternatively, the temperature of the iron ore oxide material retaining heat energy to be charged into the upper inner portion UP is controlled by the sixth control circuit 50 to be within the range of 900°C to 1500°C, preferably 1000°C to 1300°C.

[0580] Alternatively, the temperature of the reducing agent containing hydrogen is controlled by the sixth control circuit 56 to be in the range of 100°C to 400°C, preferably 200°C to 300°C, or 0°C to 300°C, preferably 100°C to 200°C.

[0581] Fig.15b A flow chart of an iron ore material production configuration 200 is shown providing an exemplary steel production configuration suitable for reducing heat-retaining iron ore oxide material 5 into reduced iron ore material 16 .

[0582] The heat-retaining iron ore oxide material 5 is charged into the direct reduction facility 7. The direct reduction facility 7 may be defined as having an upper inner portion UP, an intermediate inner portion IP, and a lower inner portion LP. The preheated hydrogen-containing reducing agent H is introduced into the intermediate inner portion IP, and flows upward to meet the heat-retaining iron ore oxide material 5 conveyed downward, whereby the upper inner portion UP serves as a countercurrent heat exchange zone to provide a chemical reaction between the heat-retaining iron ore oxide material 5 and the preheated hydrogen-containing reducing agent 6.

[0583] Alternatively, the iron ore oxide material retaining heat energy and under reduction is transported by gravity from the upper inner portion UP to the middle and / or lower portion.

[0584] Alternatively, the temperature of the preheated hydrogen-containing reducing agent H introduced to meet the iron ore oxide material 5 retaining heat energy in the upper inner portion UP is controlled by a sixth control circuit (not shown) to provide the spent reducing fluid 8 produced by the reduction to contain 100% water vapor or substantially 100% water vapor. Due to the high temperature of the loaded iron ore oxide material 5, despite the fact that the preheated hydrogen-containing reducing agent H contains a large amount of water vapor, effective reduction of the iron ore oxide material 5 is achieved.

[0585] An additional introduction of a preheated hydrogen-containing reducing agent H' may be provided into the intermediate inner portion IP and / or the lower inner portion LP. The temperature of the additionally introduced preheated hydrogen-containing reducing agent H' is controlled by a sixth control circuit to adjust the temperature towards a predetermined temperature, thereby achieving sintering and / or heat treatment of the reduced iron ore material 16 during a predetermined period of time to provide at least one desired passivation parameter value of the reduced iron ore material 16.

[0586] Fig.15c An iron ore material production arrangement 200 of an exemplary steel production arrangement suitable for reducing the iron ore oxide material 5 retaining heat energy into the reduced iron ore material 16 is shown. The metal material production arrangement 1 comprises an iron ore oxide material production unit 3, such as an iron ore oxide pelletizing plant or an iron ore oxide preheating plant, configured to provide the iron ore oxide material 5 retaining heat energy. The metal material production arrangement 1 comprises a direct reduction facility 7 configured to reduce the iron ore oxide material 5 retaining heat energy.

[0587] The iron ore oxide material loading and conveying unit 12 of the iron ore material production configuration 1 is configured to load the iron ore oxide material 5 into the upper internal part UP of the direct reduction facility 7 via an iron ore oxide material loading device a including, for example, a transport fireproof steel belt (not shown), and the transport fireproof steel belt is configured to load the iron ore oxide material 5 retaining thermal energy into the top part of the upper internal part UP.

[0588] The direct reduction facility 7 includes a reducing agent inlet device b configured to introduce a preheated hydrogen-containing reducing agent H into the middle inner part IP of the direct reduction facility 7, whereby the preheated hydrogen-containing reducing agent H is suitable for reacting with the iron ore oxide material 5 retaining thermal energy to reduce the iron ore oxide material 5 by utilizing the thermal energy of the iron ore oxide material 5 to heat or further heat the introduced preheated hydrogen-containing reducing agent H to provide a chemical reaction between the preheated hydrogen-containing reducing agent H and the iron ore oxide material 5. The hydrogen of the preheated hydrogen-containing reducing agent H may be generated by an electrolysis unit (not shown).

[0589] The iron ore oxide material 5 retaining heat energy descends through the upper inner portion UP, and is continuously reduced in the upper inner portion UP to become the reduced iron ore material 16. The temperature of the introduced preheated hydrogen-containing reducing agent H further increases as the introduced preheated hydrogen-containing reducing agent H rises in the upper inner portion UP, where the iron ore oxide material 5 retaining heat energy meets the introduced preheated hydrogen-containing reducing agent H, and the iron ore oxide material 5 retaining heat energy is cooled.

[0590] The upper inner portion UP serves as a countercurrent heat exchange zone and promotes the chemical reaction between the iron ore oxide material and the preheated reducing agent H containing hydrogen.

[0591] Furthermore, the intermediate inner portion IP is configured for providing a heat treatment process for heat treating the reduced iron ore material 16 in the intermediate inner portion IP. The reduced iron ore material 16 descends from the upper inner portion UP into the intermediate inner portion IP.

[0592] The sixth control circuit 56 is electrically coupled to the reductant preheater 18 configured to preheat the hydrogen-containing reductant H to be introduced into the intermediate inner portion IP via the reductant inlet b.

[0593] The sixth control circuit 56 controls the temperature of the reduced iron ore material 16 towards a predetermined temperature (e.g. set in the range of 200°C to 600°C, preferably 300°C to 500°C) during a predetermined time period that is long enough to enable the heat treatment process to be used to provide at least one desired passivation parameter value of the reduced iron ore material 16.

[0594] In this manner, the heat treatment process is achieved by controlling the temperature of the introduced preheated hydrogen-containing reducing agent H through the sixth control circuit 56 to maintain the temperature of the reduced iron ore material 16 in the intermediate inner portion IP at an elevated predetermined temperature for an extended period of time.

[0595] In this way, it is achieved that a heat treatment process for heat treating the reduced iron ore material utilizes the additional thermal energy provided by the preheated hydrogen-containing reducing agent H, wherein the heat treatment process is controlled by the sixth control circuit 56 .

[0596] Alternatively, the direct reduction facility 7 is configured to allow the reduced iron ore material 16 to descend into the lower inner portion LP and / or the intermediate inner portion IP to provide a heat treatment process for heat treating the reduced iron ore material 16 using additional heat energy provided by the preheated hydrogen-containing reducing agent H.

[0597] Alternatively, the additional thermal energy is defined as thermal energy added to the thermal energy of the iron ore oxide material 5 retaining thermal energy and / or as thermal energy added to the still unutilized thermal energy of the reduced iron ore material descending through the intermediate inner portion IP and / or the lower inner portion LP.

[0598] Alternatively, the sixth control circuit 56 is configured to control the additional thermal energy by adjusting the temperature of the introduced preheated hydrogen-containing reducing agent to provide at least one desired passivation parameter value for the reduced iron ore material.

[0599] The sixth control circuit 56 may be electrically coupled to a further reducing agent preheater 18 ′ configured to preheat the hydrogen-containing reducing agent H introduced into the lower inner portion LP and / or the middle inner portion of the reduction facility.

[0600] The introduced preheated hydrogen-containing reducing agent H fed into the lower inner portion LP may contain 80% to 100% hydrogen, preferably 100% hydrogen. The sixth control circuit 56 is adapted to control the temperature of the introduced preheated hydrogen-containing reducing agent H fed into the lower inner portion LP towards a predetermined temperature to provide sintering and / or heat treatment of the reduced iron ore material 16 during a predetermined period of time.

[0601] Alternatively, the additional thermal energy is defined as thermal energy added to the thermal energy of the iron ore oxide material 5 retaining thermal energy and / or as thermal energy added to the still unutilized thermal energy of the reduced iron ore material descending through the intermediate inner portion IP and / or the lower inner portion LP.

[0602] The sixth control circuit 56 is configured to control the additional thermal energy by adjusting the introduced preheated temperature to provide at least one desired passivation parameter value of the reduced iron ore material.

[0603] Fig.15d A closed loop diagram of a closed loop algorithm used by an iron ore material production configuration of an exemplary steel production configuration is shown. The sixth control circuit 56 is electrically coupled to the iron ore oxide material provider unit 3, such as an iron ore oxide pelletizing plant or an iron ore oxide preheating plant, and is adapted to regulate the temperature of the heat-retaining iron ore oxide material to be charged into the direct reduction facility.

[0604] The sixth control circuit 56 may be adapted to control the temperature of the iron ore oxide material retaining thermal energy towards a predetermined temperature value PDTV to provide a heat treatment process in a direct reduction facility for heat treating the iron ore oxide material undergoing reduction and / or the reduced iron ore material during a predetermined time period, thereby achieving at least one desired passivation parameter value DPPV of the reduced iron ore material.

[0605] The at least one desired passivation parameter value DPPV may relate to a porosity parameter and / or a size parameter and / or a weight parameter and / or an iron ore particle structure parameter and / or a sample cutting uniformity parameter and / or a shrinkage parameter and / or a sintering parameter and / or a cold crushing strength parameter and the like.

[0606] The passivation parameter detector PPD is associated with the reduction facility for detecting the actual passivation parameter value APPV. The sixth control circuit 56 may perform calculation and comparison procedures for regulating the temperature of the iron ore oxide material retaining the heat energy through the iron ore oxide material provider unit 3 .

[0607] Alternatively, the sixth control circuit 56 may be adapted to control the temperature of the charged iron ore oxide material in such a way that the predetermined temperature value PDTV for providing the heat treatment produces a temperature value for the heat treatment to reach at least one desired passivation parameter value DPPV.

[0608] The sixth control circuit 56 repeats the closed-loop algorithm until at least one desired passivation parameter value DPPV is reached.

[0609] The sixth control circuit 56 is electrically coupled to the reducing agent temperature regulating device 18 configured for regulating the temperature of the hydrogen-containing reducing agent to be introduced into the reduction facility of the metallic material production arrangement to achieve at least one desired passivation parameter value DPPV for reducing the iron ore material.

[0610] The closed loop diagram may use a starting process in which an input temperature value IN of a preheated hydrogen-containing reducing agent is used.

[0611] The sixth control circuit 56 is adapted to control the reducing agent temperature regulating device 18 in such a way that the temperature of the introduced preheated hydrogen-containing reducing agent is adjusted towards a predetermined temperature value PDTV to provide a heat treatment process in the reduction facility for heat treating the iron ore oxide material and / or the reduced iron ore material subjected to reduction during a predetermined time period so as to reach at least one desired passivation parameter value DPPV of the reduced iron ore material. When determining the predetermined temperature value PDTV, the sixth control circuit 56 takes into account the at least one desired passivation parameter value DPPV. The at least one desired passivation parameter value DPPV of the reduced iron ore material is determined taking into account reaching an effective passivation of the reduced iron ore material.

[0612] The at least one desired passivation parameter value DPPV may relate to a porosity parameter and / or a size parameter and / or a weight parameter and / or an iron ore particle structure parameter and / or a sample cutting uniformity parameter and / or a shrinkage parameter and / or a sintering parameter and the like.

[0613] A passivation parameter detector PPD is associated with the reduction facility for detecting an actual passivation parameter value APPV.

[0614] The actual passivation parameter value APPV of the reduced metallic material is detected by a passivation parameter detector PPD electrically coupled to the sixth control circuit 56. The sixth control circuit 56 performs a calculation and comparison routine to adjust the reductant temperature regulating device 18 in such a way that the temperature of the introduced preheated hydrogen-containing reductant is adjusted towards a predetermined temperature value PDTV to reach at least one desired passivation parameter value DPPV.

[0615] The sixth control circuit 56 repeats the closed-loop algorithm until at least one desired passivation parameter value DPPV is reached.

[0616] The sixth control circuit 56 is configured to compare the actual passivation parameter value APPV with at least one desired passivation parameter value DPPV and control the reductant temperature regulating device 18 to regulate the temperature of the reductant containing hydrogen until the at least one desired passivation parameter value DPPV is reached.

[0617] The iron ore oxide material retaining heat energy may be iron ore oxide pellets which are preheated to contain heat energy. The iron ore oxide pellets may be produced by a pelletizing plant processing an iron ore mixture and transported to the reduction facility via a conveyor belt.

[0618] The upper interior portion of the reduction facility is configured for reducing the iron ore oxide pellets, and the reduction facility is configured to provide a chemical reaction between a reducing agent comprising hydrogen and the iron ore oxide pellets.

[0619] The lower section and / or the middle section are configured for use in a heat treatment process for heat treating the iron ore oxide material.

[0620] The reduced and heat-hardened iron ore material is discharged from the lower inner portion through a discharge transport unit coupled to the opening of the lower inner portion.

[0621] Alternatively, the computer of the sixth control circuit 56 is electrically coupled to the iron ore oxide material loading equipment to control the loading rate into the reduction facility.

[0622] The computer may be electrically connected to the iron ore oxide material supplier unit for controlling the temperature of the iron ore oxide pellets to be loaded, and / or to the reducing agent temperature regulating device for controlling the temperature of the introduced hydrogen-containing reducing agent, and / or to the discharge transport unit.

[0623] Alternatively, the reducing agent H comprising hydrogen may be preheated prior to introduction into the direct reduction facility 7, wherein the introduced reducing agent H may be preheated to a temperature of about 200°C to about 500°C, or about 300°C to about 600°C, or about 400°C to about 700°C, or about 500°C to about 800°C, or about 600°C to about 900°C, or about 700°C to about 1000°C, or about 800°C to about 1100°C, or about 900°C to about 1200°C, or higher (e.g., referred to as high temperature in some cases).

[0624] Alternatively, the temperature of the iron ore oxide material to be charged to the direct reduction facility (e.g., referred to as high temperature in some cases) may have a temperature of about 50°C to about 350°C, or about 100°C to about 400°C, or about 200°C to about 500°C, or about 300°C to about 600°C, or about 400°C to about 700°C, or about 500°C to about 800°C, or about 600°C to about 900°C, or about 700°C to about 1000°C, or about 800°C to about 1100°C, or about 900°C to about 1200°C, or more.

[0625] For example, the reducing agent having the temperature (e.g., referred to as high temperature in some cases) (e.g., any temperature in the range of about 600°C to 1000°C, or about 500°C to 900°C, or about 700°C to 1100°C) to be introduced and / or being introduced into the direct reduction facility 7 encounters the direct reduced iron material and / or the iron ore oxide material undergoing direct reduction descending through the direct reduction facility 7, for reducing the cooling rate of the direct reduced iron material and / or the iron ore oxide material undergoing direct reduction descending through the direct reduction facility 7.

[0626] Alternatively, the iron ore oxide material to be charged and / or being charged into the direct reduction facility 7 at said temperature (e.g., referred to as high temperature in some cases) (e.g., any temperature in the range of about 600°C to about 900°C or about 700°C to about 1000°C or about 800°C to about 1100°C or about 900°C to about 1200°C or higher) meets in the upper inner part of the reduction facility 7 the reducing agent H, most of which has been used for the chemical reaction, for partially further providing the chemical reaction, while the iron ore oxide material 5 undergoing direct reduction and / or the direct reduced iron material further down in the direct reduction facility 7 undergoes the thermal treatment process, whereby the top gas to be discharged from the reduction facility and formed by the chemical reaction in the upper inner part will be very hot and contain high-temperature water vapor to be fed to the high-temperature electrolysis unit.

[0627] Alternatively, the reduction potential of the hydrogen gas of the reducing agent is lower than the reduction potential of the hydrogen gas of the reducing agent introduced further down in the reduction facility.

[0628] Alternatively, the iron ore oxide material to be charged and / or being charged into the direct reduction facility at a certain temperature (for example, any temperature in the range of about 50°C to about 350°C or about 100°C to about 400°C) meets the reducing agent, most of which has been used for chemical reaction, in the upper internal part of the reduction facility, for achieving the chemical reaction between the iron ore oxide material and the reducing agent by further heating the introduced reducing agent, thereby further providing the chemical reaction in part to at least a certain extent.

[0629] This achieves an energy-saving method for the direct reduction of iron ore oxide materials by means of hydrogen and / or a hydrogen-containing reducing agent, wherein the hydrogen can preferably be temporarily stored in a gas tank and / or a storage facility in a geological storage reservoir and / or other buffer facilities, so that the hydrogen of the reducing agent is available and can be used when renewable energy cannot be fully generated, i.e. for coping with fluctuations in the production of regeneratively generated electrical energy.

[0630] Alternatively, the temperature of the iron ore oxide material to be charged to the direct reduction facility may be lower than the temperature of the reducing agent to be and / or being introduced into the direct reduction facility.

[0631] The present invention may relate to a method for producing steel, wherein an iron ore oxide material is reduced in a direct reduction facility with a reducing agent, such as a hydrogen-containing reducing agent, and the intermediate products of the directly reduced metal material thus obtained and the final accompanying materials are subjected to metallurgical treatment; the reducing agent is produced by electrolysis of water with the aid of an electrolysis unit, such as a high-temperature electrolysis unit, and the electrical energy required for the electrolysis may be renewable energy derived from hydropower and / or wind power and / or photovoltaics and / or other forms of renewable energy and / or nuclear power plants (e.g. plants including small modular reactors SMRs), wherein if sufficient reducing agent is available, the reduced iron material produced, such as sponge iron (the so-called intermediate product), is produced independently of current demand.

[0632] The iron ore oxide material is transported from an iron ore oxide material supply facility (eg a pelletizing facility and / or a preheating device) to a direct reduction facility, and heat energy originating from the iron ore oxide material supply facility is retained.

[0633] The direct reduction facility is configured to introduce a reducing agent, which is suitable for reacting with the iron ore oxide material retaining thermal energy, thereby reducing the iron ore oxide material into an intermediate product by utilizing the thermal energy of the iron ore oxide material to further heat the introduced reducing agent, thereby providing an energy-saving and time-saving process for producing steel using renewable energy on an industrial scale, and for conserving renewable energy to cope with fluctuations in the production of renewable produced electrical energy.

[0634] Alternatively, if sufficient regeneratively produced electrical energy is available, reducing agent is produced independently of the current demand, said produced reducing agent being temporarily stored to cope with said fluctuations.

[0635] The hydrogen gas of the hydrogen-containing reducing agent and / or the hydrogen-containing reducing agent may be stored in gas tanks and / or in storage facilities of geological repositories and / or other buffer facilities.

[0636] Storage facilities in gas tanks or geological repositories may be located between the electrolysis unit and / or the high-temperature electrolysis unit and the direct reduction facility.

[0637] Hydrogen and / or a reducing agent comprising hydrogen is configured to be fed and / or transported to a direct reduction facility for use as a reducing agent under fluctuating conditions, such as during summer.

[0638] During spring and autumn, renewable electricity can be generated by a wind energy device connected to and used by an electrolysis unit and / or a high-temperature electrolysis unit. During spring and autumn, the hydrogen and / or the hydrogen-containing reducing agent generated in this way from renewable energy sources is preferably temporarily stored in a storage facility in a gas tank and / or a geological reservoir.

[0639] In this way, efficient storage of renewable energy (in the form of hydrogen and / or hydrogen-containing reducing agents) is achieved, which renewable energy can later be used as reducing agent by the direct reduction facility during the summer when the generation of renewable electricity is low, i.e. when sufficient regeneratively generated electrical energy is not available.

[0640] Alternatively, the reducing agent may be preheated to some extent prior to introduction into the direct reduction facility.

[0641] Alternatively, the temperature of the iron ore oxide material to be charged to the direct reduction facility may be higher than the temperature of the reducing agent to be introduced and / or being introduced into the direct reduction facility.

[0642] Alternatively, the temperature of the iron ore oxide material to be charged to the direct reduction facility may be lower than the temperature of the reducing agent to be and / or being introduced into the direct reduction facility.

[0643] The temperature of the iron ore oxide material to be charged into the direct reduction facility may have a temperature of about 50°C to about 350°C, or about 100°C to about 400°C, or about 200°C to about 500°C, or about 300°C to about 600°C, or about 400°C to about 700°C, or about 500°C to about 800°C, or about 600°C to about 900°C, or about 700°C to about 1000°C, or about 800°C to about 1100°C, or about 900°C to about 1200°C, or more.

[0644] The reducing agent may be preheated prior to introduction into the direct reduction facility, wherein the introduced reducing agent may be preheated to a temperature of about 200°C to about 500°C, or about 300°C to about 600°C, or about 400°C to about 700°C, or about 500°C to about 800°C, or about 600°C to about 900°C, or about 700°C to about 1000°C, or about 800°C to about 1100°C, or about 900°C to about 1200°C, or more.

[0645] Alternatively, by introducing relatively warm reducing agent (e.g., about 600°C to 900°C) into the direct reduction facility, it is achieved that the iron ore oxide material that retains heat energy, reaches the middle portion and / or lower interior portion of the direct reduction facility and undergoes direct reduction and / or heat treatment does not cool rapidly in the direct reduction facility.

[0646] Thus, the heat treatment can be carried out efficiently. The passivated and reduced iron material will have a compact and dense structure for achieving an intermediate product that is resistant to reoxidation.

[0647] The intermediate product may be defined as a small, round, pear-shaped, drop-shaped, pellet-shaped, bead-shaped, sphere-shaped or ellipsoidal object of the passivated reduced iron ore material having a compact and dense structure for producing a reoxidation resistant intermediate product.

[0648] Alternatively, the direct reduction facility is configured to allow the reduced iron ore material to descend into the lower inner portion and / or the middle inner portion to provide a heat treatment process for heat treating the reduced iron ore material using a relatively warm reducing agent providing thermal energy to avoid rapid cooling of the iron ore material undergoing direct reduction and / or heat treatment.

[0649] Alternatively, the control circuit is connected to the iron ore oxide preheating device and / or the heating device and is configured to control the temperature of the iron ore oxide material to be loaded so that the iron ore oxide material undergoing reduction and / or heat treatment will strive towards a predetermined temperature of about 200°C to 600°C, preferably about 300°C to 500°C during a predetermined period of time long enough to enable the heat treatment process to provide the desired passivation parameter value of the reduced iron ore material and thereby provide an intermediate product that is resistant to reoxidation.

[0650] Alternatively, the predetermined temperature is about 400°C to 800°C, preferably about 500°C to 700°C.

[0651] Alternatively, the predetermined temperature is about 600°C to 1000°C, preferably about 700°C to 900°C.

[0652] Alternatively, the control circuit is further connected to a reductant preheating device configured to preheat the reductant before introduction into the direct reduction facility, and configured to control the temperature of the reductant so that the iron ore oxide material undergoing reduction and / or heat treatment will strive towards a predetermined temperature of about 200°C to 600°C, preferably about 300°C to 500°C during a predetermined period of time long enough to enable the thermal treatment process to provide the desired passivation parameter value of the reduced iron ore material and thereby provide an intermediate product that is resistant to reoxidation.

[0653] Alternatively, the control circuitry may be adapted to provide a heat treatment process in a direct reduction facility for heat treating the iron ore oxide material undergoing reduction during a predetermined time period by controlling the temperature of the iron ore oxide material retaining thermal energy towards a predetermined temperature so as to achieve desired passivation parameter values ​​with respect to porosity and / or sponge iron size and / or weight per volume of sponge iron produced and / or iron ore particle structure and / or sample cut uniformity and / or shrinkage and / or sintering and / or cold crushing strength etc.

[0654] Alternatively, the desired passivation parameter value may be defined as a value for the rate and / or extent and / or grade and / or portion and / or proportion of reoxidation of the intermediate product (sponge iron and / or reduced iron ore material).

[0655] Alternatively, the desired passivation parameter value for porosity, its definition can be expressed as the ratio of the pore volume of the sponge iron produced to its total volume. The sponge iron size can be expressed as the average diameter of the sponge iron agglomerates typically produced. The weight per volume can be defined as a measure of the iron concentration of the sponge iron agglomerates typically produced. The iron ore particle structure can be defined as the final microstructure of the sponge iron agglomerates produced and the distribution of dense and porous areas. The sample cutting uniformity can define the density of the sponge iron agglomerates produced.

[0656] Alternatively, a heat treatment process provided by a control circuit during a predetermined time period so as to achieve a desired passivation parameter value for the sponge iron produced produces a sponge iron or intermediate product having a highly uniform chemical composition for cost-effective and energy-efficient production in subsequent steel production in a steel plant and / or a high uniformity of final porosity in specific areas (e.g. central areas of sponge iron agglomerates) and / or a dense structure, is resistant to reoxidation, and is produced with low carbon dioxide emissions.

[0657] The present disclosure may not be limited to the examples described above, but many possibilities of modifications or combinations of the examples described herewith will be apparent to a person skilled in the art without departing from the basic idea as defined in the appended claims.

Claims

1. A method for producing steel, whereby an iron ore oxide material (5) is reduced with a reducing agent (H) in a direct reduction facility (7), and the intermediate product (RM) of the direct reduced iron ore material thus obtained and eventually accompanying substances are metallurgically processed; - the reducing agent (H) is produced by electrolysis of water by means of an electrolysis unit (17); - the electric energy required for electrolysis can be renewable energy from hydropower and / or wind power and / or photovoltaic or other renewable energy forms (2), - if sufficient reducing agent is available, the intermediate product (RM) is produced independently of the current demand; Features include: - the iron ore oxide material (5) is transported from the iron ore oxide material supply device (3, 4) to the direct reduction facility (7) and retains the heat energy originating from the iron ore oxide material supply device (3, 4), - The direct reduction facility (7) is configured to introduce the reducing agent (H), which is suitable for reacting with the iron ore oxide material (5) retaining thermal energy, thereby heating or further heating the introduced reducing agent (H) by utilizing the thermal energy of the iron ore oxide material (5) to achieve a chemical reaction between the iron ore oxide material (5) and the reducing agent (H), thereby reducing the iron ore oxide material (5) to the intermediate product (RM), thereby providing an energy-saving and time-saving process for producing steel using renewable energy on an industrial scale, and for conserving renewable energy to cope with fluctuations in the production of regeneratively generated electrical energy.

2. The method according to claim 1, wherein if sufficient regeneratively generated electrical energy is available, the reducing agent (H) is produced independently of the current demand, and the produced reducing agent (H) is temporarily stored to cope with fluctuations in the renewable energy production.

3. The method according to claim 1 or 2, in: - if sufficient regeneratively produced electrical energy is available, the reducing agent (H) and / or the intermediate product (RM) are always produced independently of the current demand; - storing said intermediate products (RM) which are not needed until they are needed / used, so that said renewable energy stored therein is also stored; - during the reduction of the iron ore oxide material (5) to the intermediate product (RM), adding a carbon-containing gas (CG) or a hydrogen-containing gas to the reducing agent (H) to incorporate carbon into the intermediate product; - the amount of the carbon-containing gas (CG) or hydrogen-containing gas added to the reducing agent (H) used for reduction is at least such that the carbon content in the intermediate product is 0.0005 mass % to 6.3 mass %; and The carbon-containing gas is methane or another carbon-containing gas from biogas production or from the pyrolysis of renewable raw materials, or is synthesis gas from biomass.

4. The method according to any one of claims 1 to 3, in: - The iron ore oxide material providing device comprises an iron ore oxide material production unit (3), wherein the iron ore oxide material production unit (3) is configured to produce the iron ore oxide material (5) retaining the thermal energy, and to transport the iron ore oxide material (5) retaining the thermal energy to the direct reduction facility (7).

5. The method according to claim 4, wherein the iron ore oxide material (5) retains thermal energy originating from a manufacturing heat process of the iron ore oxide material production unit (3).

6. The method according to any one of claims 1 to 3, in: - The iron ore oxide material providing apparatus comprises a preheating device (4) configured to preheat the iron ore oxide material (5) before conveying the iron ore oxide material (5) to the direct reduction facility (7).

7. The method according to any one of the preceding claims, wherein the electrolysis unit (19) also produces oxygen (10) which is used by the iron ore oxide material production unit (3) to produce the iron ore oxide material (5).

8. A method according to claim 7, wherein the oxygen (10) is produced independently of current demand if sufficient regeneratively generated electrical energy is available; whereas the intermediate products (RM) not required are stored until required / used, so that the renewable energy stored therein is also stored.

9. A method according to any one of the preceding claims, wherein carbonaceous matter (100) extracted from a carbon source (CS) is added to the direct reduced iron ore material in a carburizing zone (101, 102) integrated with and / or connected to the direct reduction facility (7).

10. The method according to claim 9, wherein the carbon source (CS) include: - Carbon Capture and Utilization Unit (CCU) and / or; - a carbon production unit (CS1) configured for producing non-fossil produced carbon and / or; - a biogas production unit (CS2) configured for producing carbon-containing gas and / or; - A synthesis gas production unit configured for producing a carbon-containing synthesis gas from biomass.

11. The method according to claim 1, wherein the intermediate product (RM) is a carbon-free intermediate product.

12. The method according to claim 11, wherein the intermediate product (RM) is conveyed to the steel industry (17) in a flammable product storage and conveying facility (FL).

13. A method according to any one of the preceding claims, wherein the control circuit (50) is suitable for controlling the iron ore oxide material temperature of the iron ore oxide material (5) delivered to the direct reduction facility (7) and / or controlling the internal gas pressure in the direct reduction facility (7) and / or the reducing agent temperature and / or the reducing agent gas pressure of the introduced reducing agent (H).

14. A method according to any one of the preceding claims, wherein a first control circuit (51) is adapted to control the temperature of the iron ore oxide material (5) delivered to the direct reduction facility (7) by controlling the iron ore oxide material production unit (3) to discharge the iron ore oxide material (5) at a specific temperature, the specific temperature corresponding to a first temperature value determined according to a desired parameter value of the direct reduced iron ore material and / or intermediate product (RM).

15. A method according to any one of the preceding claims, wherein a second control circuit (52) is adapted to control the temperature of the iron ore oxide material (5) conveyed to the direct reduction facility (7) by controlling the preheating device (4) to discharge the iron ore oxide material (5) from the preheating device (4) at a specific temperature, the specific temperature corresponding to a first temperature value determined according to a desired parameter value of the direct reduced iron ore material and / or intermediate product (RM).

16. A method according to any one of the preceding claims, wherein a third control circuit (53) is suitable for controlling the reducing agent gas pressure of the reducing agent delivered to the direct reduction facility (7) by controlling a first pressurizing device (63), wherein the first pressurizing device (63) is suitable for pressurizing the reducing agent entering the direct reduction facility at a specific reducing agent gas pressure corresponding to a first reducing agent gas pressure value determined according to the desired parameter value of the direct reduced iron ore material and / or intermediate product (RM).

17. A method according to any one of the preceding claims, wherein the fourth control circuit (54) is suitable for controlling the internal reduction pressure in the direct reduction facility (7) by controlling a second pressurizing device 64, wherein the second pressurizing device 64 is used to pressurize the interior of the reduction facility (7) with a specific internal reduction pressure, and the specific internal reduction pressure corresponds to a first internal reduction pressure value determined according to the desired parameter value of the direct reduced iron ore material and / or intermediate product (RM).

18. A method according to any of the preceding claims, wherein a fifth control circuit (55) is suitable for controlling the reducing agent temperature of the reducing agent injected into the direct reduction facility (7) by controlling a heating device (74), wherein the heating device (74) is configured to heat the reducing agent at a specific reducing agent temperature corresponding to a first reducing agent temperature value determined according to a desired parameter value of the direct reduced iron ore material and / or intermediate product (RM).

19. A method according to any one of the preceding claims, wherein the control circuit (51, 52, 53, 54, 55) is adapted to adjust the iron ore oxide material temperature and / or the internal reduction pressure and / or the reducing agent temperature and / or reducing agent pressure according to desired properties of the intermediate product (RM).

20. A method according to any one of the preceding claims, wherein the method The following steps are involved: direct reduction of the iron ore oxide material by a reducing agent having a hydrogen content of at least 80% by volume; Therein the carbon content in the direct reduced iron ore material is then increased and / or added by means of a carburizing gas and thereafter the spent carburizing gas is at least partially removed while mixing of the carburizing gas with the reducing agent is largely avoided.

21. A steel production arrangement provided for the production of steel and a method for producing steel, the steel production arrangement being characterized by: - an iron ore oxide material providing device (3, 4), the iron ore oxide material providing device (3, 4) being configured to provide an iron ore oxide material (5) retaining thermal energy; - a direct reduction facility (7) configured to reduce the iron ore oxide material and configured to utilize the thermal energy of the iron ore oxide material (5) to heat or further heat an introduced reducing agent (H); - the direct reduction facility (7) is configured for introducing the reducing agent (H) which is suitable for reacting with the iron ore oxide material (5) retaining thermal energy to achieve a chemical reaction between the iron ore oxide material (5) and the reducing agent (H) for providing an energy-saving and time-saving process for producing steel using renewable energy on an industrial scale, and for conserving renewable energy to cope with fluctuations in the production of regeneratively generated electrical energy; - a control circuit (50, 51, 52, 53, 54, 55) configured to control the iron ore oxide material providing device (3, 4) and to control the reduction of the iron ore oxide material; - an iron ore oxide conveying device (95) adapted to load the iron ore oxide material (5) from the iron ore oxide material supply device (3, 4) into the direct reduction facility (7); and / or - an electrolysis unit (19) configured for electrolyzing water to produce hydrogen and oxygen; and / or - A steel industry (17) configured to produce steel.

22. A steel production arrangement according to claim 21, wherein the control circuit (50, 51, 52, 53, 54, 55) is configured to operate the loading of the iron ore oxide material into the direct reduction facility (7); wherein the control circuit (50, 51, 52, 53, 54, 55) is configured to control the temperature of the iron ore oxide material (5) transported to the direct reduction facility (7) and / or control the internal reduction pressure in the direct reduction facility (7) and / or the reducing agent temperature and / or the reducing agent gas pressure of the introduced reducing agent (H).

23. A data program (P) programmed to cause a steel production arrangement according to claim 21 or 22 to perform a method according to any one of claims 1 to 20, wherein the data program (P) comprises a program code that can be read on a computer of a control circuit (50, 51, 52, 53, 54, 55) to implement the method comprising the following steps: - producing said iron ore oxide material (5); - loading the iron ore oxide material (5) which retains thermal energy and is provided by the iron ore oxide material supply device (3, 4) into the direct reduction facility (7) from the iron ore oxide material supply device (3, 4), - introducing the reducing agent (H) into the direct reduction facility (7); - reducing the iron ore oxide material (5) into an intermediate product (RM) by utilizing the thermal energy of the iron ore oxide material (5) to heat or further heat an introduced reducing agent (H) to achieve a chemical reaction; and - discharging the intermediate product (RM) from the direct reduction plant (7); and / or - The intermediate product (RM) is sent to the steel industry (17).

24. Data program (P) according to claim 23, wherein the method comprises the following further steps: - sending parameter value signals from detector means (DCT1, DCT2) of the direct reduction plant (7) to the control circuit (50, 51, 52, 53; 54; 55); and - Commanding the conveying device (95) of the iron ore oxide material supply device (3, 4) to stop charging the iron ore oxide material (5) retaining thermal energy into the direct reduction facility (7).

25. The method according to any one of claims 1 to 20, whereby the iron ore oxide material (5) retaining thermal energy provided by the iron ore oxide material providing device (3, 4) is loaded into the upper inner part (UP) of the direct reduction facility (7) of the steel production configuration via an iron ore oxide material loading device; a sixth control circuit (56) is electrically connected to a reducing agent temperature regulating device (18), the reducing agent temperature regulating device (18) being configured to regulate the temperature of the reducing agent (H) to be introduced into the middle part (IP) and / or the lower inner part (LP) of the direct reduction facility (7) via a reducing agent inlet device; the method is characterized by the following steps: - reducing the iron ore oxide material (5) in the upper inner portion (UP) by utilizing the thermal energy of the iron ore oxide material (5) to heat or further heat the introduced hydrogen-containing reducing agent (H) to provide a chemical reaction between the hydrogen-containing reducing agent (H) and the iron ore oxide material (5); - providing a thermal treatment process to thermally treat the iron ore oxide material (5) subjected to reduction and / or to thermally treat the reduced iron ore material (16) before it is discharged from the lower inner part (LP); and controlling the temperature of the introduced reducing agent (H) to adjust the chemical reaction and / or the thermal treatment process to achieve at least one desired passivation parameter value (DPPV) of the intermediate product (RM).