Method and system for high pressure die casting
Patent Information
- Application Number
- CN202380029318.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-15
- Filing Date
- 2023-02-15
- Publication Date
- 2024-11-19
AI Technical Summary
The high silicon content in traditional high-pressure die-cast aluminum alloys leads to a decrease in ductility, thermal conductivity and electrical conductivity, and the low-silicon content alloys have poor fluidity, making it difficult to adapt to the high-pressure die-casting process.
A metal alloy with low silicon content modified with nanoparticles is used to disperse nanoparticles such as metal oxides and carbides in the alloy to improve the fluidity and thermal crack resistance of the alloy, making it compatible with the high-pressure die-casting process.
Aluminum alloy die-cast parts with high strength, excellent ductility and high thermal conductivity are achieved, avoiding thermal cracking problems and allowing anodization to a variety of colors, suitable for structural components and thermal management applications.
Smart Images

Figure CN118984882A_ABST
Abstract
Description
Technical Field
[0001] The present invention generally relates to methods and systems for high pressure die casting of metal alloys with low silicon content; more particularly, to methods and systems for high pressure die casting of metal alloys with low silicon content modified with nanoparticles. Background Art
[0002] Die-cast metal alloys have applications in various industries. Die-cast metal alloys generally require high strength and ductility. The metal alloy should also have good castability and thermal cracking resistance in order to be suitable for high-pressure die-casting processes. Traditionally, silicon is added to metal alloys (such as aluminum alloys) in order to improve the fluidity of the metal alloy so that it is compatible with high-pressure die-casting. However, high silicon content may degrade the ductility, thermal conductivity, electrical conductivity and anodization ability of the metal alloy. It may be desirable to have a metal alloy with uncompromising ductility and electrical conductivity that is also suitable for high-pressure die-casting processes. Summary of the invention
[0003] Methods and systems for high pressure die casting of low silicon content metal alloys modified with nanoparticles are described.
[0004] One embodiment of the present invention includes a metal alloy for high pressure die casting, comprising: a metal alloy selected from the group consisting of aluminum alloys, magnesium alloys, copper alloys and zinc alloys; and at least one type of nanoparticles dispersed in the metal alloy; wherein the metal alloy comprises less than 4.0 weight percent silicon; and wherein the metal alloy is compatible with a high pressure die casting process.
[0005] In another embodiment, the metal alloy is selected from the group consisting of A201, AA2024, A206, AA2618, AA5083, AA6013, AA6061, AA6063, AA6069, AA7034, AA7050, AA7075, and AA7068.
[0006] In further embodiments, the at least one type of nanoparticles is selected from metal oxides, non-metal oxides, metal carbides, non-metal carbides, metal silicides, metal borides, metal nitrides, and any combination thereof.
[0007] In yet another embodiment, the at least one type of nanoparticles has a core-shell particle structure.
[0008] In another embodiment, the nanoparticles comprise less than 30 volume % of the metal alloy.
[0009] In yet another embodiment, the nanoparticles comprise 0.1 vol. % to 2 vol. % of the metal alloy.
[0010] In yet another embodiment, the metal alloy comprises AA6061, the nanoparticles comprise TiC, and the TiC nanoparticles comprise 1.0 volume % of the metal alloy.
[0011] In further embodiments, the high pressure die casting process uses a pressure between 30 MPa and 100 MPa.
[0012] In other embodiments, the high pressure die casting process uses a pressure greater than 100 MPa.
[0013] In another embodiment, the high pressure die casting process comprises a cooling step, and the cooling rate is between 100° C. / s and 300° C. / s.
[0014] Another embodiment includes a high pressure die casting method comprising:
[0015] Providing a metal alloy modified with at least one type of nanoparticles, wherein the metal alloy comprises a silicon weight concentration of less than 4.0%;
[0016] melting the metal alloy and filling the die with the molten metal alloy under pressure, wherein the pressure is compatible with a high pressure die casting process; and
[0017] The die is cooled to solidify the molten metal alloy.
[0018] In yet another embodiment, the method further comprises anodizing the die cast metal alloy to at least one color.
[0019] In another embodiment, the metal alloy is selected from the group consisting of aluminum alloys, magnesium alloys, copper alloys, and zinc alloys.
[0020] In further embodiments, the metal alloy is selected from the group consisting of A201, AA2024, A206, AA2618, AA5083, AA6013, AA6061, AA6063, AA6069, AA7034, AA7050, AA7075, and AA7068.
[0021] In another embodiment, the at least one type of nanoparticles is selected from metal oxides, non-metal oxides, metal carbides, non-metal carbides, metal silicides, metal borides, metal nitrides, and any combination thereof.
[0022] In yet another embodiment, the at least one type of nanoparticles has a core-shell particle structure.
[0023] In further embodiments, the at least one type of nanoparticles comprises less than 30 volume % of the metal alloy.
[0024] In another embodiment, the nanoparticles comprise 0.1 vol. % to 2 vol. % of the metal alloy.
[0025] In yet another embodiment, the metal alloy comprises AA6061, the nanoparticles comprise TiC, and the TiC nanoparticles comprise 1.0 volume % of the metal alloy.
[0026] In another embodiment, the die cast metal alloy formed has an elongation equal to or less than 30% and an ultimate tensile strength greater than 500 MPa.
[0027] In further embodiments, the die cast metal alloy has a thickness of at least 0.2 mm.
[0028] In yet another embodiment, the pressure is between 30 MPa and 100 MPa.
[0029] In another embodiment, the pressure is greater than 100 MPa.
[0030] In another embodiment, the die is cooled at a cooling rate between 100° C. / s and 300° C. / s.
[0031] In yet another embodiment, the method further comprises post-processing the die cast metal alloy.
[0032] In further embodiments, the post-treatment is selected from the group consisting of a T5 treatment, a natural aging treatment, and a T6 treatment.
[0033] Another embodiment includes a high pressure die cast metal part comprising: a metal alloy; and at least one type of nanoparticles dispersed in the metal alloy; wherein the metal alloy comprises less than 4.0 weight percent silicon; wherein the metal part is produced via a high pressure die casting process; and wherein the die cast metal part has a thickness of at least 0.2 mm.
[0034] In yet another embodiment, the metal alloy is selected from the group consisting of aluminum alloys, magnesium alloys, copper alloys, and zinc alloys.
[0035] In further embodiments, the metal alloy is selected from the group consisting of A201, AA2024, A206, AA2618, AA5083, AA6013, AA6061, AA6063, AA6069, AA7034, AA7050, AA7075, and AA7068.
[0036] In another embodiment, the at least one type of nanoparticles is selected from metal oxides, non-metal oxides, metal carbides, non-metal carbides, metal silicides, metal borides, metal nitrides, and any combination thereof.
[0037] In yet another embodiment, the at least one type of nanoparticles has a core-shell particle structure.
[0038] In yet another embodiment, the nanoparticles comprise less than 30 volume % of the metal alloy.
[0039] In another embodiment, the nanoparticles comprise 0.1 vol. % to 2 vol. % of the metal alloy.
[0040] In yet another embodiment, the metal alloy comprises AA6061, the nanoparticles comprise TiC, and the TiC nanoparticles comprise 1.0 volume % of the metal alloy.
[0041] In another embodiment, the high pressure die casting process uses a pressure between 30 MPa and 100 MPa.
[0042] In another embodiment, the high pressure die casting process uses a pressure greater than 100 MPa.
[0043] In yet another embodiment, the high pressure die casting process includes a cooling step, and the cooling rate is between 100° C. / s and 300° C. / s.
[0044] In other embodiments, the metal part is anodized to at least one color.
[0045] Another embodiment includes a method of improving the castability of a metal alloy, the method comprising: incorporating at least one type of nanoparticles into the metal alloy; wherein the metal alloy comprises less than 4.0 weight percent silicon; wherein the nanoparticles constitute less than 30 volume percent of the metal alloy; and wherein the metal alloy is compatible with a high pressure die casting process.
[0046] In yet another embodiment, the metal alloy is selected from the group consisting of aluminum alloys, magnesium alloys, copper alloys, and zinc alloys.
[0047] In further embodiments, the metal alloy is selected from the group consisting of A201, AA2024, A206, AA2618, AA5083, AA6013, AA6061, AA6063, AA6069, AA7034, AA7050, AA7075, and AA7068.
[0048] In another embodiment, the at least one type of nanoparticles is selected from metal oxides, non-metal oxides, metal carbides, non-metal carbides, metal silicides, metal borides, metal nitrides, and any combination thereof.
[0049] In yet another embodiment, the at least one type of nanoparticles has a core-shell particle structure.
[0050] In yet another embodiment, the nanoparticles comprise 0.1 vol. % to 2 vol. % of the metal alloy.
[0051] In another embodiment, the metal alloy comprises AA6061, the nanoparticles comprise TiC, and the TiC nanoparticles comprise 1.0 volume % of the metal alloy.
[0052] In another embodiment, the high pressure die casting process uses a pressure between 30 MPa and 100 MPa.
[0053] In other embodiments, the high pressure die casting process uses a pressure greater than 100 MPa.
[0054] In another embodiment, the high pressure die casting process includes a cooling step, and the cooling rate is between 100° C. / s and 300° C. / s.
[0055] Other embodiments and features are described in part in the following description, and in part will become clear to those skilled in the art when reading the description, or may be known by practicing the present disclosure. The nature and advantages of the present disclosure may be further understood by reference to the remainder of the description and the accompanying drawings, which form a part of the present disclosure. BRIEF DESCRIPTION OF THE DRAWINGS
[0056] This specification will be more fully understood with reference to the following drawings, which are presented as exemplary embodiments of the invention and are not to be construed as a complete statement of the scope of the invention. It should be noted that the patent or application file contains at least one color drawing. Copies of this patent or patent application publication with color drawings will be provided by the Patent Office upon request and payment of the necessary fee.
[0057] Figure 1 A high pressure die casting process according to an embodiment of the present invention is shown.
[0058] Figure 2A A high pressure die cast AA6061 part without nanoparticles according to an embodiment of the present invention is shown.
[0059] Figure 2B A high pressure die cast AA6061 part with 1.0 volume % TiC nanoparticles according to an embodiment of the present invention is shown.
[0060] Figures 3A to 3B A non-ferrous die cast AA6061 part with 1.0 volume % nanoparticles after anodizing is shown. DETAILED DESCRIPTION
[0061] Turning now to the accompanying drawings, methods and systems for high pressure die casting using low silicon content metal alloys are described. Many embodiments provide metal alloys with low silicon content for high pressure die casting processes, including (but not limited to) aluminum alloys modified with nanoparticles. The die casting process according to some embodiments produces metal parts with high strength, high ductility and high thermal conductivity. Certain embodiments show that die cast metal parts can be anodized to produce parts of desired colors. Several embodiments show that nanoparticles can enhance the fluidity of aluminum alloys under high pressure and avoid problems including (but not limited to) die-sticking and hot cracking during die casting. Metal alloys modified by nanoparticles according to certain embodiments allow die casting of high performance metal alloys containing low silicon content or no silicon content. Traditionally, high performance aluminum alloys with low silicon content cannot be die cast due to problems such as hot cracking. Die casting metal alloys with low silicon content according to some embodiments can produce aluminum alloys with high strength, excellent ductility and thermal conductivity on a large scale. Many embodiments show that aluminum alloys with low silicon content will allow good anodizing capabilities, thereby providing colored parts. In several embodiments, the combination of strength and ductility can enable die cast metal parts to be used for structural components. In certain embodiments, the high thermal conductivity of die cast aluminum parts, in addition to good strength and ductility, can also allow for effective thermal management in applications including (but not limited to) radiators and heat exchangers.
[0062] Typically, nanoparticles can increase the viscosity of molten metal alloys, which may not be ideal for high pressure die filling and rapid cooling processes during die casting. However, nanoparticles according to many embodiments enable die casting of high performance alloys, including (but not limited to) high performance deformation and casting aluminum alloys having a silicon content of about 0 weight % to about 4.0 weight %, suitable for structural applications. Several embodiments show that nanoparticles can simultaneously enhance the fluidity of the alloy and eliminate hot cracking during rapid cooling. The enhanced fluidity of metal alloys according to certain embodiments can be compatible with die filling processes under high pressure. In various embodiments, the pressure range of the die casting process can be about 30 MPa to about 100 MPa; or less than about 30 MPa; or greater than about 100 MPa. It is readily understood that according to various embodiments of the present invention, any of the various pressures can be utilized as required by the specific application.
[0063] Many embodiments show that the metal alloy resistant to hot cracking can withstand a cooling process with a high cooling rate. In several embodiments, the cooling rate can be from about 100°C / s to about 300°C / s; or less than about 100°C / s; or greater than about 300°C / s. It is readily understood that according to various embodiments of the present invention, any of a variety of cooling rates can be utilized depending on the requirements of a specific application.
[0064] According to certain embodiments, the improved fluidity and castability of the metal alloy by the nanoparticles enables die casting of metal parts having a thickness of about 0.2 mm to about 0.5 mm; or a thickness greater than about 0.5 mm.
[0065] In several embodiments, the ductility and / or elongation of the die cast metal alloy is less than or equal to about 20%; or less than or equal to about 30%. In some embodiments, the strength of the die cast metal alloy may be greater than or equal to about 500 MPa. According to various embodiments, the thermal conductivity of the die cast metal alloy may be less than or equal to about 230 W / mw; or greater than about 230 W / mw. Ductility, strength, and thermal conductivity measurements were performed on the as-cast metal alloy without post-treatment.
[0066] In several embodiments, the die cast metal parts can be anodized to add any desired color. Examples of anodized colors include (but are not limited to): red, blue, pink, gold, yellow, green, and any combination thereof. It is readily understood that according to various embodiments of the present invention, any of a variety of colors may be utilized as required by a particular application.
[0067] For the purposes of the present invention, the term "die casting" may also be interpreted as "high pressure die casting" unless otherwise specified.
[0068] The high pressure die casting process according to various embodiments of the present invention is discussed further below.
[0069] High pressure die casting
[0070] Die casting can be an economical method for mass production of metal parts. During the die casting process, molten metal can be injected into a die under high pressure and then solidified at a high cooling rate (ranging from about tens of degrees Celsius per second to about hundreds of degrees Celsius per second). The applied pressure can be hydraulic or pneumatic pressure. The pressure can be maintained until the casting solidifies. These molds (called die) can be made of high-quality tool steel, can produce parts with complex geometric shapes, and result in high precision and process repeatability. The high-pressure filling of the die in high-pressure die casting allows the molten alloy to be injected quickly, thereby achieving a highly productive automated process.
[0071] In contrast to gravity die casting (also known as permanent mold casting), the molten metal is poured into the mold from above entirely under the force of gravity. Because gravity die casting relies on gravity to fill the mold, the process can be slow and therefore less suitable for large-scale production runs.
[0072] High pressure die casting may have advantages including (but not limited to): high dimensional accuracy, smooth casting surface, reduction or elimination of secondary machining operations, fast production rate, etc. However, one disadvantage of high pressure die casting is that the process is limited to metals with high fluidity. Since the die casting process is under high pressure (about 30 MPa to about 100 MPa) and the molten alloy solidifies at a high cooling rate (about tens to hundreds of degrees Celsius per second), low fluidity molten alloys and / or high viscosity molten alloys may block the mold cavity and affect the accuracy of the cast parts. In addition to high fluidity, alloys suitable for high pressure die casting should also have good crack resistance under high pressure and high cooling rate.
[0073] Anodizing is a process that uses alloy parts as anodes and stainless steel, chrome or conductive electrolytes as cathodes in a suitable electrolyte. Under certain voltage and current conditions, the anode is oxidized to obtain an anodic oxide film on the surface of the workpiece. Sulfuric acid anodizing can be used in the anodizing and coloring process. Anodizing can provide color and / or protective film for die casting alloys.
[0074] Metal alloys for high pressure die casting
[0075] Various types of metal alloys can be used for high pressure die casting, including (but not limited to) zinc alloys, aluminum alloys, copper alloys and tin alloys. Aluminum alloys have been widely used in consumer electronics, automobiles, aerospace, shipbuilding and other fields due to their plasticity, corrosion resistance and light weight. Die-cast aluminum parts are widely used in industries including computer devices, communication devices, consumer electronics, automobiles, construction, windows, aerospace and sports. Since high pressure die casting usually operates on metals at high cooling rates of tens to hundreds of degrees Celsius per second, the fluidity and resistance to hot cracking of the alloy are critical to the integrity of the parts, especially for thin-walled structures. Traditional high-performance aluminum alloys, including (but not limited to) A201, AA2024, A206, AA2618, AA5083, AA6013, AA6061, AA6063, AA6069, AA7034, AA7050, AA7075 and AA7068 provide good strength, ductility and fatigue life, as well as anodizing ability and thermal conductivity. Unfortunately, these alloys are not suitable for die casting due to low fluidity and hot cracking problems.
[0076] Al-Si alloy is one of the most popular aluminum alloys for die casting. Silicon can contribute to the fluidity of the alloy, largely due to its high heat of crystallization. When silicon solidifies, a large amount of heat can be released to reheat the liquid aluminum, thereby enhancing the fluidity of the melt. For die casting alloys, a silicon content of more than 4.5 wt. % (usually in the range of about 8 wt. % to about 13 wt. %) and sufficient alloying elements, including (but not limited to) Fe and / or Mn, are added to ensure high fluidity and resistance to hot cracking. Therefore, die casting aluminum alloys and die casting parts generally contain a silicon content of more than about 4.5 wt. %. Examples of Al-Si alloys suitable for die casting include (but are not limited to): AA360, A360, AA380, AA383, AA384, B390, AA413, A413 and C443.
[0077] However, the silicon phase in the Al-Si alloy will appear gray or black after anodizing, and the anodized alloy and / or parts may appear dark, which may be undesirable in many applications with aesthetic requirements. As the silicon content increases, the color of the anodized film changes as follows: from light gray to dark gray to black gray. Therefore, cast aluminum alloys with high silicon content may not be suitable for anodizing. In addition, the high content of silicon and other elements used to solve the fluidity and hot cracking problems in aluminum die casting alloys will deteriorate the ductility and thermal conductivity and / or electrical conductivity of the aluminum alloy after die casting.
[0078] There are some aluminum alloy systems with low silicon content. An example of an aluminum alloy with low silicon content includes Al-Mg system, such as AA 518, Al-8Mg. Another example of low silicon aluminum alloy includes Al-Mg-Si system. Al-Mg-Si system can include 2 wt%-5.5 wt% Mg, 1.5 wt%-3 wt% Si, trace Mn, trace Fe, and the balance is Al. Examples of Al-Mg-Si system alloys include (but are not limited to) Magsimal-59, C446, Aural-11, Calypso 53 and 54SM. However, these aluminum alloys with low silicon content are difficult to die cast due to low fluidity and high cracking tendency. In addition, such alloys are very sensitive to wall thickness, especially thin walls. In addition, low silicon aluminum alloys may require toxic Be as an additive and may be susceptible to hot tearing and stress corrosion cracking. In addition, due to the alloy content, their thermal conductivity may be low.
[0079] Table 1, reproduced below from the North American Die Casting Association (NADCA), includes the chemical compositions of various Al-Si alloys and Al-8Mg alloys used in high pressure die casting. All individual values are maximum composition percentages unless otherwise noted.
[0080] Table 1. Aluminum die casting alloy composition Aluminum die casting alloy
[0081]
[0082] Table 2, reproduced below from NADCA, includes mechanical properties of aluminum alloys used in high pressure die casting. The typical values are based on "as-cast" properties of individual die cast specimens, rather than specimens cut from production die castings.
[0083] Table 2. Aluminum die casting alloy properties
[0084]
[0085] Table 3, reproduced below from NADCA, includes mechanical properties of magnesium alloys used in high pressure die casting, Zamak die casting alloys, and ZA die casting alloys.
[0086] Table 3. Die casting alloy properties
[0087]
[0088] High-pressure die casting of metal alloys modified with nanoparticles
[0089] In many embodiments, metal alloys modified with nanoparticles can achieve die casting of high-performance metal alloys. In several embodiments, aluminum alloys modified with nanoparticles have low silicon content or no silicon content. Some embodiments show that modified nanoparticles in metal alloys can achieve high-performance deformation and casting alloys, including, but not limited to, aluminum alloys, with low silicon content, suitable for structural applications. In certain embodiments, the silicon content of the metal alloy modified by nanoparticles is from about 0 weight % to about 4.0 weight %. It is easy to understand that according to various embodiments of the present invention, any of the various silicon contents less than about 4.0 weight % can be utilized according to the requirements of specific applications. Many embodiments show that nanoparticles can simultaneously enhance the fluidity (die filling) of the alloy and eliminate hot cracking under high cooling rates without adding a silicon content higher than about 4.0 weight %.
[0090] Several embodiments show that the metal alloys that can be modified with nanoparticles include at least one metal element, including (but not limited to) aluminum (Al), magnesium (Mg), iron (Fe), silver (Ag), copper (Cu), manganese (Mn), nickel (Ni), titanium (Ti), chromium (Cr), cobalt (Co), zinc (Zn) and alloys, mixtures or other combinations of two or more of the above metals, Al alloys, Mg alloys, Zn alloys, Ti-Al alloys, Al-Mg alloys and Mg-Zn alloys, and alloys, mixtures or other combinations of one or more of the above metals with other elements, such as steel (e.g., iron-carbon alloys or iron-chromium-carbon alloys). It is easy to understand that according to various embodiments of the present invention, any of the various metal alloys can be utilized according to the requirements of a specific application. Many embodiments make alloy systems that are traditionally difficult to die cast suitable for die casting after modification with nanoparticles. In several embodiments, aluminum alloys, magnesium alloys and zinc alloys can be modified with nanoparticles to adapt to high pressure die casting. Many embodiments show that the alloy systems modified by nanoparticles for die casting also have desired mechanical properties, thermal conductivity and electrical conductivity. Examples of alloy systems include, but are not limited to, A201, AA2024, A206, AA2618, AA5083, AA6013, AA6061, AA6063, AA6069, AA7034, AA7050, AA7075, and AA7068. It will be readily appreciated that any of a variety of alloy systems may be utilized according to the requirements of a particular application in accordance with various embodiments of the present invention.
[0091] Many embodiments show that nanoparticles are uniformly dispersed in a metal alloy matrix. Many embodiments show that materials that can make nanoparticles include, but are not limited to, ceramics, oxides, nitrides, borides, carbides and other carbon-based particles, metals and metal alloys, and core-shell particles. Specific examples of nanoparticle types that can be dispersed in a metal matrix include aluminum oxide nanoparticles, aluminum nitride nanoparticles, carbon nanotubes, silicon carbide nanoparticles, silicon nitride nanoparticles, titanium carbide nanoparticles, titanium boride nanoparticles, titanium carbonitride nanoparticles, tungsten carbide nanoparticles, and core-shell particles. In addition, nanoparticles can be core-shell nanoparticles including a core material and a coating. Examples include SiC nanoparticles coated with SiO and ceramic nanoparticles coated with metals such as nickel or silver. (For example, see U.S. Pat. No. 9,023,128 B2 of Li et al., the disclosure of which is incorporated herein by reference in its entirety).
[0092] In some embodiments, the nanoparticles may include one or more ceramics, but other nanoparticle materials are also contemplated, including metals or other conductive materials. Examples of suitable nanoparticle materials include metal oxides (e.g., alkaline earth metal oxides, post-transition metal oxides, and transition metal oxides, such as aluminum oxide (Al2O3), magnesium oxide (MgO), titanium oxide (TiO2), yttrium oxide (Y2O3), magnesium aluminate (MgAl2O4), and zirconium oxide (ZrO2)), non-metallic oxides (e.g., silicon oxide (SiO2)), metal carbides (e.g., transition metal carbides, such as titanium carbide (TiC), niobium carbide (NbC), chromium carbide (Cr3C2), nickel carbide (NiC), hafnium carbide (HfC), vanadium carbide (VC), tungsten carbide (WC), and zirconium carbide (ZrO2)). rC)), non-metal carbides (such as silicon carbide (SiC)), metal silicides (such as transition metal silicides, such as titanium silicide (Ti5Si3)), metal borides (such as transition metal borides, such as titanium boride (TiB2), zirconium boride (ZrB2), hafnium boride (HfB2), vanadium boride (VB2) and tungsten boride (W2B5)), metal nitrides (such as transition metal nitrides), core-shell particles, metals (such as transition metals in elemental form, such as tungsten (W)), alloys, mixtures or other combinations of two or more of the above, and alloys, mixtures or other combinations of one or more of the above with other elements. Specific examples of suitable nanoparticle materials include transition metal-containing ceramics, wherein the presence of the transition metal can impart a larger Hamaker constant, a Hamaker constant of a metal matrix that is closer to a reduced van der Waals potential well, such as transition metal carbides, transition metal silicides, transition metal borides, transition metal nitrides and other non-oxides, transition metal-containing ceramics. (See, for example, US Pat. No. 11,040,395 B2 to Li et al., the disclosure of which is incorporated herein by reference in its entirety).
[0093] In many embodiments, the nanoparticles may have an average diameter of less than about 500nm. In some embodiments, the average diameter of the nanoparticles may be between about 1nm and about 500nm; between about 1nm and about 400nm; between about 1nm and about 300nm; between about 1nm and about 200nm; between about 1nm and about 100nm; between about 1nm and about 70nm; between about 1nm and about 50nm; between about 1nm and about 30nm. Several embodiments show that the size distribution of the nanoparticles can be characterized by a standard deviation relative to the average diameter, which is at most about 100%, at most about 90%, at most about 80%, at most about 70%, at most about 60%, or at most about 50% of the average diameter. In certain embodiments, the nanoparticles may have a generally spherical or spheroidal shape, but other shapes and configurations of nanoparticles are also contemplated.
[0094] Many embodiments show that the metal alloy can include nanoparticles in the following volume percentage ranges: about 0.1% to 2%, about 0.25% to 2%, about 0.5% or more, about 1% or more, about 2% or more, about 3% or more, about 5% or more, about 6% or more, about 7% or more, about 8% or more, about 9% or more, about 10% or more, about 15% or more, about 20% or more, about 25% or more, and up to about 30% or more. It is readily understood that any of the various nanoparticle concentrations can be utilized according to the various embodiments of the present invention, depending on the requirements of a particular application.
[0095] Several embodiments show that die-cast metal alloys, including (but not limited to) aluminum alloys with less than 4% silicon content, exhibit desirable mechanical properties, thermal conductivity, and electrical conductivity. The mechanical properties, thermal conductivity, and electrical conductivity of the cast metal alloys without post-treatment were measured. Some embodiments show that low volume percentages of nanoparticles (about 0.1% to about 2%) can be successfully applied to die-cast aluminum alloys that are traditionally difficult or impossible to cast. Examples of such alloys include (but are not limited to) AA6061 (Al-1.0Mg-0.6Si-0.25Cu), AA6063 (Al-0.7Mg-0.4Si), A206 (Al-4.5Cu-0.3Mg), AA7075 (Al-5.6Zn-2.6Mg-1.6Cu), and modified AA7075 (Al-5.6Zn-2.6Mg-0.65Cu) for natural aging. These die casting alloys according to several embodiments show good die casting ability, while achieving high strength and good ductility. Strength and ductility are measured for cast alloys (without post-treatment). In many embodiments, die casting AA6061 and other 6000s aluminum alloys can provide ductility and / or elongation of less than or equal to about 30%, or about 20% to about 30%, or less than or equal to about 20%, or about 10% to about 20%, or less than or equal to about 10%; and less than or equal to about 230W / mw, or about 200W / mw to about 230W / mw, or about 100W / mw to about 200W / mw, or less than or equal to about 100W / mw thermal conductivity, which is better than other commercially available die casting Al-Si alloys (see Table 2 above).
[0096] Many embodiments provide high pressure die casting of 7000 series aluminum alloys. Die casting of 7000 series aluminum alloys can open up application space for die casting high strength aluminum alloys. According to embodiments, modified AA7075 alloy can provide extremely high strength through natural aging after die casting.
[0097] Due to the low silicon content of the die casting metal alloy, the enhanced fluidity and hot cracking resistance of the nanoparticle modified metal alloy according to some embodiments enables the production of thin-walled structures using high pressure die casting processes. Many embodiments produce die cast metal parts having a thickness between about 0.2 mm and about 0.5 mm, or greater than or equal to about 0.5 mm.
[0098] Some embodiments indicate that the thermal conductivity of die cast metal alloys can be affected by porosity. Typically, high pressure die cast aluminum parts have a porosity of about 3% to about 5%. Certain embodiments indicate that the porosity of die cast nanoparticle infused metal alloys may vary from part to part. The porosity of die cast parts can be improved in vacuum die casting or process optimization.
[0099] Many embodiments provide good anodizing ability and quality of die-cast metal alloys with nanoparticles. Traditionally, die-cast aluminum alloys have high Si content. Anodizing high Si content alloys can make Si stand out and turn metal parts gray or black. Therefore, high Si content alloys may not be able to produce different colors via anodization. In several embodiments, the Si content of the metal alloy with nanoparticles is less than 4 weight % and can be anodized to produce parts of various colors. The color can be determined by the dye used to color the surface porous oxide after chemical treatment. Some embodiments show that any color can be applied to the die-cast metal alloy. Due to the effect of low silicon or no silicon, the metal alloy with nanoparticles can also be successfully anodized into various colors.
[0100] Several embodiments show that post-treatment can be applied to the die-cast metal alloy with nanoparticles, but this is not necessary. Typically, high pressure die-cast alloys do not require any solution treatment due to the blistering effect. In some embodiments, post-treatments including (but not limited to) T5 or natural aging can be applied. In certain embodiments, post-treatments including (but not limited to) T6 can be applied to die-cast metal parts with low porosity or no porosity (for example, after vacuum high pressure die casting). It is easy to understand that according to various embodiments of the present invention, any of the various post-processing treatments can be utilized according to the requirements of the specific application.
[0101] Many embodiments provide high pressure die casting processes of metal alloys with infused nanoparticles.In several embodiments, metal alloys including, but not limited to, aluminum alloys, magnesium alloys, and zinc alloys have a silicon content of less than about 4 weight percent. Figure 11 shows a high pressure die casting process according to an embodiment of the present invention. Process 100 starts with preparing a metal and / or metal alloy 101 having nanoparticles. In some embodiments, the nanoparticles can be uniformly incorporated and dispersed in a metal matrix. In several embodiments, the content of the nanoparticles in the metal alloy can be about 0.1 volume % to about 2 volume %. Certain embodiments show that the nanoparticles can be made of materials including (but not limited to) the following: metal oxides (e.g., alkaline earth metal oxides, post-transition metal oxides and transition metal oxides, such as aluminum oxide (Al2O3), magnesium oxide (MgO), titanium oxide (TiO2), yttrium oxide (Y2O3), magnesium aluminate (MgAl2O4) and zirconium oxide (ZrO2)), non-metallic oxides (e.g., silicon oxide (SiO2)), metal carbides (e.g., transition metal carbides, such as titanium carbide (TiC), niobium carbide (NbC), chromium carbide (Cr3C2), nickel carbide (NbC), etc. iC), hafnium carbide (HfC), vanadium carbide (VC), tungsten carbide (WC) and zirconium carbide (ZrC)), non-metal carbides (such as silicon carbide (SiC)), metal silicides (such as transition metal silicides, such as titanium silicide (Ti5Si3)), metal borides (such as transition metal borides, such as titanium boride (TiB2), zirconium boride (ZrB2), hafnium boride (HfB2), vanadium boride (VB2) and tungsten boride (W2B5)), metal nitrides (such as transition metal nitrides), core-shell particles, metals (such as transition metals in elemental form, such as tungsten (W)). Previous work has described in detail the preparation of nanoparticles mixed with metal alloys (see, e.g., PCT Application No. PCT / US20 / 27775 to Li et al.; U.S. Pat. No. 9,322,084 B2 to Li et al.; U.S. Pat. No. 9,023,128 B2 to Li et al.; the disclosures of which are incorporated herein by reference in their entireties.)
[0102] The metal mixed with the nanoparticles can be melted and further alloyed to form a molten metal alloy 102 having a certain composition. Aluminum alloys including, but not limited to, AA6061, AA6063, AA6069, AA2024, AA5083, AA7075, A206, A201, AA6013, AA2024, AA7034, AA7050, and AA7068 can be prepared for high pressure die casting. Many embodiments show that the metal alloy mixed with the nanoparticles has less than about 4 weight percent silicon in order to improve the mechanical properties, thermal conductivity, and anodizing ability of such alloys.
[0103] The die cavity 103 may be prepared before the molten metal alloy is injected. A layer of lubricant may be sprayed inside the die mold to facilitate demolding of the cast metal part. The molten metal alloy may be injected into the die mold 104 under high pressure. Many embodiments show that the pressure at which the molten metal alloy is injected is in the range of about 30 MPa to about 100 MPa. In certain embodiments, the pressure may be lower than about 30 MPa, or higher than about 100 MPa. In some embodiments, the pressure may be higher than 100 MPa. The pressure is maintained until the casting solidifies. The die 105 is then cooled at a high cooling rate. In several embodiments, the cooling rate may be in the range of about 100°C / s to about 300°C / s to solidify the molten metal alloy. In multiple embodiments, the cooling rate may be lower than about 100°C / s, or higher than about 300°C / s. Nanoparticles may improve the fluidity and hot cracking resistance of metal alloys with low silicon content and reduce sticking, thereby making alloys with less than 4 wt% silicon compatible with high pressure injection processes and rapid cooling processes. Once the metal alloy solidifies, the metal part can be removed (not shown).
[0104] The die cast metal part can be anodized to add the desired color 106. Anodizing can be optional. High silicon content in the metal alloy can appear gray or black after anodizing. In contrast, the nanoparticle modified metal alloy has less than 4 weight % silicon, while the normal silicon content is 8 weight % to 10 weight %. Low silicon metal alloys according to many embodiments do not appear gray or black after anodizing. Therefore, die cast metal parts using nanoparticle modified metal alloys can be anodized to add any selected color, including (but not limited to) red, blue, green, yellow, silver, gold.
[0105] Figure 2A and Figure 2B A die-cast aluminum alloy sample according to an embodiment of the present invention is shown in FIG. Figure 2A A die cast AA6061 alloy sample is shown. Figure 2A The AA6061 alloy used in was not modified with nanoparticles. The die cast sample showed multiple crack lines 201. Figure 2B A die cast AA6061 alloy modified with about 1.0 vol% TiC nanoparticles is shown. The die cast sample has a smooth surface. The sample is anodized to obtain a red color.
[0106] Exemplary embodiments
[0107] Although specific embodiments of the systems and methods are discussed in the following sections, it should be understood that these embodiments are provided by way of example and are not intended to be limiting.
[0108] Example 1: High pressure die casting of AA6061 alloy
[0109] Many embodiments provide high pressure die casting of aluminum alloys, including (but not limited to) high performance AA6061 alloys. In several embodiments, the AA6061 alloy can be modified with about 1.0 volume % of nanoparticles, including (but not limited to) TiC nanoparticles. Table 4 below lists the properties of die-cast AA6061 alloys containing about 1.0 volume % of nanoparticles. The nanoparticle-modified AA6061 alloy has an as-cast ultimate tensile strength of about 205 MPa, a yield strength of about 125 MPa, an elongation of about 16%, and a thermal conductivity of about 140 W / mk). Post-treatment can further improve mechanical properties. After T5 treatment, the AA6061 alloy has an ultimate tensile strength of about 226 MPa, a yield strength of about 165 MPa, an elongation of about 10%, and a thermal conductivity of about 142 W / mk). After T6 treatment, the AA6061 alloy has an ultimate tensile strength of about 353 MPa, a yield strength of about 305 MPa, an elongation of about 9%, and a thermal conductivity of about 145 W / mk).
[0110] Table 4. Typical properties of die cast AA6061 containing 1.0 vol% nanoparticles
[0111]
[0112] Die cast aluminum alloys including, but not limited to, AA6061 alloy may be anodized to add any selected color. Figures 3A-3D FIG. 4 shows a die-cast part of AA6061 showing various colors according to an embodiment of the present invention. Figures 3A-3D The die cast AA6061 parts contained about 1.0 vol% TiC nanoparticles. Figure 3A Display die cast parts can be anodized to have a gold color. Figure 3B Display die cast aluminum parts can be anodized to have a red color. Figure 3C Display die cast parts can be anodized to have a silver color. Figure 3D Display die cast alloy can be anodized blue. Die cast metal parts show smooth surface without cracks.
[0113] Example 2: High pressure die casting of A206 alloy
[0114] Several embodiments provide high pressure die casting of aluminum alloys, including (but not limited to) high performance A206 alloys. For A206 alloys, according to many embodiments, nanoparticles allow better fluidity and eliminate hot cracking so that this traditionally difficult to die cast alloy can be reliably die cast. The addition of nanoparticles also improves die filling, part pressure sealing, strength and ductility. Die casting A206 alloys with nanoparticles can provide strengths up to about 450 MPa and elongations up to 15%.
[0115] Principle of Equivalence
[0116] The description of the present invention is given for the purpose of illustration and description. It is not intended to be exhaustive or to limit the invention to the precise form described, and many modifications and variations are possible in light of the above teachings. The embodiments are selected and described in order to best explain the principles of the invention and its practical application. This description will enable others skilled in the art to best utilize and practice the invention in various embodiments and various modifications suitable for a particular use. The scope of the invention is defined by the following claims.
[0117] As used herein, the singular terms "a", "an", and "the" may include plural referents unless the context clearly dictates otherwise. Reference to an object in the singular is not intended to mean "one and only one", but rather "one or more", unless the context clearly dictates otherwise.
[0118] As used herein, the terms "about" and "approximately" are used to describe and explain small variations. When used in conjunction with an event or circumstance, these terms can refer to situations where the event or circumstance occurs exactly, as well as situations where the event or circumstance occurs approximately. When used in conjunction with a numerical value, these terms can refer to a range of variation of less than or equal to ±10% of the numerical value, such as less than or equal to ±5%, less than or equal to ±4%, less than or equal to ±3%, less than or equal to ±2%, less than or equal to ±1%, less than or equal to ±0.5%, less than or equal to ±0.1%, or less than or equal to ±0.05%.
[0119] In addition, quantities, ratios and other numerical values may sometimes be presented in the form of ranges herein. It should be understood that the use of such ranges is for convenience and brevity, and should be flexibly understood to include numerical values clearly specified with range limits, and also include all individual numerical values or subranges contained within the range, as if each numerical value and subrange were clearly specified. For example, a ratio within the range of about 1 to about 200 should be understood to include the clearly mentioned limits of about 1 and about 200, and include individual ratios, such as about 2, about 3, and about 4, and include subranges, such as about 10 to about 50, about 20 to about 100, etc.
Claims
1. A metal alloy for high pressure die casting, comprising: a metal alloy selected from the group consisting of aluminum alloys, magnesium alloys, copper alloys, and zinc alloys; and at least one type of nanoparticles dispersed in the metal alloy; wherein the metal alloy comprises less than 4.0 wt. % silicon; and The metal alloy is compatible with high pressure die casting processes.
2. The metal alloy of claim 1, wherein the metal alloy is selected from the group consisting of A201, AA2024, A206, AA2618, AA5083, AA6013, AA6061, AA6063, AA6069, AA7034, AA7050, AA7075, and AA7068.
3. The metal alloy of claim 1, wherein the at least one type of nanoparticles is selected from the group consisting of metal oxides, non-metal oxides, metal carbides, non-metal carbides, metal silicides, metal borides, metal nitrides, and any combination thereof. The metal alloy of claim 1 , wherein the at least one type of nanoparticles has a core-shell particle structure.
5. The metal alloy of claim 1, wherein the nanoparticles comprise less than 30 volume % of the metal alloy.
6. The metal alloy of claim 1, wherein the nanoparticles comprise 0.1 volume % to 2 volume % of the metal alloy.
7. The metal alloy of claim 1, wherein the metal alloy comprises AA6061, the nanoparticles comprise TiC, and the TiC nanoparticles comprise 1.0 volume % of the metal alloy.
8. The metal alloy of claim 1, wherein the high pressure die casting process uses a pressure between 30 MPa and 100 MPa.
9. The metal alloy of claim 1, wherein the high pressure die casting process uses a pressure greater than 100 MPa.
10. The metal alloy of claim 1, wherein the high pressure die casting process comprises a cooling step, the cooling rate being between 100°C / s and 300°C / s.
11. A method for high pressure die casting, include: Providing a metal alloy modified with at least one type of nanoparticles, wherein the metal alloy comprises a silicon weight concentration of less than 4.0%; melting the metal alloy and filling a die with the molten metal alloy under pressure, wherein the pressure is compatible with a high pressure die casting process; and The die is cooled to solidify the molten metal alloy.
12. The method of claim 11 further comprising anodizing the die cast metal to have at least one color.
13. The method of claim 11, wherein the metal alloy is selected from the group consisting of aluminum alloys, magnesium alloys, copper alloys, and zinc alloys.
14. The method of claim 11, wherein the metal alloy is selected from the group consisting of A201, AA2024, A206, AA2618, AA5083, AA6013, AA6061, AA6063, AA6069, AA7034, AA7050, AA7075, and AA7068.
15. The method of claim 11, wherein the at least one type of nanoparticles is selected from metal oxides, non-metal oxides, metal carbides, non-metal carbides, metal silicides, metal borides, metal nitrides, and any combination thereof.
16. The method of claim 11, wherein the at least one type of nanoparticles has a core-shell particle structure.
17. The method of claim 11, wherein the at least one type of nanoparticles comprises less than 30 volume percent of the metal alloy.
18. The method of claim 11, wherein the nanoparticles comprise 0.1 volume % to 2 volume % of the metal alloy.
19. The method of claim 11, wherein the metal alloy comprises AA6061, the nanoparticles comprise TiC, and the TiC nanoparticles comprise 1.0 volume % of the metal alloy.
20. The method of claim 11, wherein the formed die cast metal alloy has an elongation equal to or less than 30% and an ultimate tensile strength greater than 500 MPa.
21. The method of claim 11, wherein the die cast metal alloy has a thickness of at least 0.2 mm.
22. The method of claim 11, wherein the pressure is between 30 MPa and 100 MPa.
23. The method of claim 11, wherein the pressure is greater than 100 MPa.
24. The method of claim 11, wherein the die is cooled at a cooling rate between 100°C / s and 300°C / s.
25. The method of claim 11, further comprising post-processing the die cast metal alloy.
26. The method according to claim 25, wherein the post-treatment is selected from the group consisting of a T5 treatment, a natural aging treatment, and a T6 treatment.
27. A high pressure die casting metal part comprising: Metal alloys; and at least one type of nanoparticles dispersed in the metal alloy; wherein the metal alloy comprises less than 4.0 weight percent silicon; wherein the metal part is produced via a high pressure die casting process; and The die-cast metal part has a thickness of at least 0.2 mm.
28. The die cast metal part of claim 27, wherein the metal alloy is selected from the group consisting of aluminum alloys, magnesium alloys, copper alloys, and zinc alloys.
29. The die cast metal part of claim 27, wherein the metal alloy is selected from the group consisting of A201, AA2024, A206, AA2618, AA5083, AA6013, AA6061, AA6063, AA6069, AA7034, AA7050, AA7075, and AA7068.
30. The die cast metal part of claim 27, wherein the at least one type of nanoparticles is selected from the group consisting of metal oxides, non-metal oxides, metal carbides, non-metal carbides, metal silicides, metal borides, metal nitrides, and any combination thereof.
31. The die cast metal part of claim 27, wherein the at least one type of nanoparticles has a core-shell particle structure.
32. The die cast metal part of claim 27, wherein the nanoparticles comprise less than 30 volume percent of the metal alloy.
33. The die cast metal part of claim 27, wherein the nanoparticles comprise 0.1 volume % to 2 volume % of the metal alloy.
34. The die cast metal part of claim 27, wherein the metal alloy comprises AA6061, the nanoparticles comprise TiC, and the TiC nanoparticles comprise 1.0 volume % of the metal alloy.
35. The die cast metal part of claim 27, wherein the high pressure die casting process uses a pressure between 30 MPa and 100 MPa.
36. The die cast metal part of claim 27, wherein the high pressure die casting process uses a pressure greater than 100 MPa.
37. The die cast metal part of claim 27, wherein the high pressure die casting process includes a cooling step, the cooling rate being between 100°C / s and 300°C / s.
38. The die cast metal part of claim 27, wherein the metal part is anodized to have at least one color.
39. A method for improving the castability of a metal alloy, include: incorporating at least one type of nanoparticles into the metal alloy; wherein the metal alloy comprises less than 4.0 weight percent silicon; wherein the nanoparticles comprise less than 30 volume % of the metal alloy; and The metal alloy is compatible with high pressure die casting processes.
40. The method of claim 39, wherein the metal alloy is selected from the group consisting of aluminum alloys, magnesium alloys, copper alloys, and zinc alloys.
41. The method of claim 39, wherein the metal alloy is selected from the group consisting of A201, AA2024, A206, AA2618, AA5083, AA6013, AA6061, AA6063, AA6069, AA7034, AA7050, AA7075, and AA7068.
42. The method of claim 39, wherein the at least one type of nanoparticles is selected from the group consisting of metal oxides, non-metal oxides, metal carbides, non-metal carbides, metal silicides, metal borides, metal nitrides, and any combination thereof.
43. The method of claim 39, wherein the at least one type of nanoparticles has a core-shell particle structure.
44. The method of claim 39, wherein the nanoparticles comprise 0.1 volume % to 2 volume % of the metal alloy.
45. The method of claim 39, wherein the metal alloy comprises AA6061, the nanoparticles comprise TiC, and the TiC nanoparticles comprise 1.0 volume % of the metal alloy.
46. The method of claim 39, wherein the high pressure die casting process uses a pressure between 30 MPa and 100 MPa.
47. The method of claim 39, wherein the high pressure die casting process uses a pressure greater than 100 MPa.
48. The method of claim 39, wherein the high pressure die casting process comprises a cooling step, the cooling rate being between 100°C / s and 300°C / s.
Citation Information
Cited By
Methods and systems for die casting
US12698547B2