Non-oriented electromagnetic steel plate and motor iron core

By optimizing the chemical composition and crystal orientation structure in the non-oriented electromagnetic steel plate, the problem of large iron loss deterioration under compression stress is solved, and efficient performance suitable for the motor core is achieved.

CN118984884APending Publication Date: 2024-11-19NIPPON STEEL CORPORATION
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202380031461.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-08-23
Filing Date
2023-03-28
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing non-oriented electromagnetic steel plates have a greater deterioration of iron losses when imparting compression stress, which affects the motor efficiency.

Method used

The non-oriented electromagnetic steel plate adopts a specific chemical composition and crystal-oriented structure, contains elements such as Si, Al, Mn, etc., and the average crystal particle size is more than 30μm and less than 200μm. {111}<011> The aggregation degree is at 1/4 of the plate thickness. 2.00 or above 8.00, the iron loss deterioration under compressive stress is ensured to be small.

Benefits of technology

When used as the raw material for the stator or rotor core in the motor, the iron loss deteriorates under compression stress, which improves the efficiency and performance of the motor.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005064628980000211
    Figure BDA0005064628980000211
  • Figure BDA0005064628980000221
    Figure BDA0005064628980000221
  • Figure BDA0005064628980000241
    Figure BDA0005064628980000241
Patent Text Reader

Abstract

A non-oriented electrical steel sheet having a chemical composition containing, in mass%, 0.006% or less of C, 1.0% to 5.0% (inclusive) of Si, less than 2.5% of sol.Al, 3.0% or less of Mn, 0.30% or less of P, 0.010% or less of S, 0.010% or less of N, and 0.10% or less of O, and optionally containing other elements, and a motor core comprising the non-oriented electrical steel sheet, the non-oriented electrical steel sheet having a chemical composition containing, in mass%, 0.006% or less of C, 1.0% to 5.0% or less of Si, less than 2.5% of sol.Al, 3.0% or less of Mn, 0.30% or less of P, 0.010% or less of S, 0.010% or less of N, and 0.10% or less of O, the average crystal grain size is 30 [mu] m or more and 200 [mu] m or less, and the {111} < 011 > aggregation degree is 2.00 or more and 8.00 or less at a position 1 / 4 of the sheet thickness in the sheet thickness direction from the surface of the steel sheet.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a non-oriented electromagnetic steel sheet and a motor core. Background Art

[0002] In order to reduce greenhouse gases, the industrial field has developed products that consume less energy. For example, in the automotive field, there are low-fuel-consumption vehicles such as hybrid vehicles that combine gasoline engines and motors, and electric vehicles driven by motors. The common technology of these low-fuel-consumption vehicles is the motor, and the efficiency of the motor has become an important technology.

[0003] Generally, a motor is composed of a stator and a rotor. Non-oriented electromagnetic steel sheets used for the iron cores of the stator and the rotor are required to have a small iron loss in order to improve efficiency.

[0004] However, in practical terms, it is necessary to consider the compressive stress applied to the stator and the rotor when the motor is running. This compressive stress generally deteriorates the iron loss of the non-oriented electromagnetic steel sheet. Therefore, for the non-oriented electromagnetic steel sheet used for the stator, it is preferred that the iron loss when the compressive stress is applied is better.

[0005] For example, Patent Document 1 discloses a technology related to a non-oriented electromagnetic steel sheet having excellent magnetic properties. Patent Document 2 discloses a technology related to a non-oriented electromagnetic steel sheet capable of improving motor efficiency. Patent Document 3 discloses a technology related to a non-oriented electromagnetic steel sheet having excellent magnetic properties.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent No. 5447167

[0009] Patent Document 2: Japanese Patent No. 5716315

[0010] Patent Document 3: International Publication No. 2013 / 069754 Summary of the invention

[0011] Technical problem to be solved by the invention

[0012] The present disclosure has been made in view of the above-mentioned problems, and an object of the present disclosure is to provide a non-oriented electromagnetic steel sheet and a motor core which are suitable as materials for stator cores and rotor cores of motors, for example, and which have less degradation in iron loss when compressive stress is applied.

[0013] Technical means for solving technical problems

[0014] The gist of the present disclosure is as follows.

[0015] [1] A non-oriented electromagnetic steel sheet having the following chemical composition, wherein the chemical composition is as follows, in mass %,

[0016] C: 0.006% or less,

[0017] Si: 1.0% to 5.0%

[0018] Sol.Al: less than 2.5%,

[0019] Mn: 3.0% or less,

[0020] P: 0.30% or less,

[0021] S: 0.010% or less,

[0022] N: 0.010% or less,

[0023] O: 0.10% or less,

[0024] Sn: 0~0.20%,

[0025] Sb: 0~0.20%,

[0026] Ca: 0~0.01%,

[0027] Cr: 0~5.0%,

[0028] Ni: 0-5.0%,

[0029] Cu: 0-5.0%,

[0030] Ce: 0~0.10%,

[0031] B: 0~0.10%,

[0032] Mg: 0~0.10%,

[0033] Ti: 0~0.10%,

[0034] V: 0~0.10%,

[0035] Zr: 0~0.10%,

[0036] Nd: 0~0.10%,

[0037] Bi: 0~0.10%,

[0038] W: 0~0.10%,

[0039] Mo: 0~0.10%

[0040] Nb: 0~0.10%,

[0041] Y: 0~0.10%,

[0042] The rest: Fe and impurities,

[0043] The average crystal grain size is 30 μm or more and 200 μm or less;

[0044] At a position of 1 / 4 of the plate thickness in the plate thickness direction from the surface of the steel plate, the degree of aggregation of {111}<011> is 2.00 or more and 8.00 or less.

[0045] [2] The non-oriented electromagnetic steel sheet according to [1], comprising one or more selected from the group consisting of:

[0046] Sn: 0.0010%, above 0.20% and below,

[0047] Sb: 0.0010%, above 0.20% and below,

[0048] Ca: 0.0003%, above 0.01% and below,

[0049] Cr: 0.0010% or more, 5.0% or less,

[0050] Ni: 0.0010% or more, 5.0% or less,

[0051] Cu: 0.0010% or more, 5.0% or less,

[0052] Ce: 0.001% or more, 0.10% or less,

[0053] B: 0.0001% or more, 0.10% or less,

[0054] Mg: 0.0001% or more, 0.10% or less,

[0055] Ti: 0.0001% or more, 0.10% or less,

[0056] V: 0.0001% or more, 0.10% or less,

[0057] Zr: 0.0002% or more, 0.10% or less,

[0058] Nd: 0.002% or more, 0.10% or less,

[0059] Bi: 0.002% or more, 0.10% or less,

[0060] W: 0.002% or more, 0.10% or less,

[0061] Mo: 0.002% or more, 0.10% or less,

[0062] Nb: 0.0001% or more and 0.10% or less, and

[0063] Y: 0.002% or more and 0.10% or less.

[0064] [3] The nonoriented electrical steel sheet according to [1] or [2], wherein the degree of {110}<001> aggregation is 1.00 or more at a position ¼ of the thickness in the thickness direction from the surface of the steel sheet.

[0065] [4] The nonoriented electrical steel sheet according to any one of [1] to [3], wherein at a position 1 / 4 of the thickness in the thickness direction from the surface of the steel sheet, the value of {111}<112> aggregation / {111}<011> aggregation is 1.00 or less.

[0066] [5] The nonoriented electrical steel sheet according to any one of [1] to [4], wherein the degree of aggregation of {411}<148> is 2.00 or less at a position of 1 / 4 of the sheet thickness in the sheet thickness direction from the surface of the steel sheet.

[0067] [6] The nonoriented electrical steel sheet according to any one of [1] to [5], wherein the degree of aggregation of {411}<011> is 2.00 or less at a position of 1 / 4 of the sheet thickness in the sheet thickness direction from the surface of the steel sheet.

[0068] [7] The nonoriented electrical steel sheet according to any one of [1] to [6], wherein the sheet thickness at a position of 1 / 4 of the sheet thickness in the sheet thickness direction from the surface of the steel sheet is 0.10 mm to 0.35 mm.

[0069] [8] A motor core having a structure in which a plurality of non-oriented electromagnetic steel sheets according to any one of [1] to [7] are stacked.

[0070] Effects of the Invention

[0071] According to the above aspects of the present disclosure, for example, a non-oriented electromagnetic steel sheet and a motor core which can be suitably used as a material of a stator core and a rotor core of a motor and which have less degradation in iron loss when a compressive stress is applied can be provided. DETAILED DESCRIPTION

[0072] Hereinafter, a preferred embodiment of the non-oriented electromagnetic steel sheet of the present disclosure will be described in detail. However, the present disclosure is not limited to the configuration disclosed in the following embodiment, and various changes can be made without departing from the main purpose of the present disclosure. In addition, for the numerical ranges limited in the present disclosure, unless otherwise specified, the numerical values ​​recorded as the lower limit and the upper limit are included in the range. However, for numerical values ​​expressed as "exceeding" or "less than", their values ​​are not included in the numerical range. "%" related to the content of each element means "mass %".

[0073] In addition, in the numerical ranges described stepwise in the present specification, the upper limit value of a numerical range in a certain step may be replaced by the upper limit value of a numerical range described in another stepwise manner, or may be replaced by a value described in the Examples.

[0074] In the numerical ranges described stepwise in the present specification, the lower limit value of a numerical range in a certain step may be replaced by the lower limit value of a numerical range described in another stepwise manner, or may be replaced by a value described in the Examples.

[0075] When a preferred lower limit value and an upper limit value are described separately for the content of each element, a numerical range in which the lower limit value and the upper limit value are arbitrarily combined may be used as the preferred content of the element.

[0076] When “0 to” or “0% or more” is described for the content of an element and the lower limit is 0%, or when only the upper limit is described, it means that the element may not be contained.

[0077] [Non-oriented electrical steel sheet]

[0078] The non-oriented electromagnetic steel sheet of the present disclosure can be suitably used as an iron core of a motor of an electric vehicle, a hybrid vehicle, etc. Here, the non-oriented electromagnetic steel sheet refers not only to coil products but also to steel sheets constituting the iron core (iron core material).

[0079] That is, the so-called "non-oriented electromagnetic steel sheet" in each scheme of the present disclosure can include not only the "steel sheet" in the form of a coil or a cut plate manufactured by a steel sheet manufacturer, but also, for example, can include the "steel sheet" processed by the user into the shape of a motor core through punching, lamination, etc., and constituting the motor core.

[0080] (Chemical Composition)

[0081] First, the reasons for limiting the chemical composition of the non-oriented electrical steel sheet of the present disclosure will be described.

[0082] The non-oriented electrical steel sheet of the present disclosure contains Si and, if necessary, a selected element as a chemical composition, and the balance is Fe and impurities. Hereinafter, each element will be described.

[0083] C: 0% or more and 0.006% or less

[0084] C (carbon) is an element contained as an impurity and deteriorates the magnetic properties. Therefore, the C content is set to 0.006% or less. Preferably, it is 0.003% or less. Regarding the C content, it is preferably less, so there is no need to limit the lower limit, and the lower limit may also be 0%. However, it is not easy to make the content 0% in industry, so the lower limit may also be 0.0005%, or it may be 0.0010%.

[0085] Si: 1.0% or more and 5.0% or less

[0086] Si (silicon) is an element effective in increasing the resistivity of the steel sheet to reduce the iron loss. Therefore, the Si content is set to 1.0% or more. In addition, Si is an element effective in reducing the anisotropy in the magnetic plate surface and reducing the anisotropy in the mechanical plate surface in the non-oriented electromagnetic steel sheet used as the iron core of the motor. In this case, the Si content is preferably greater than 2.0% and less than 5.0%, more preferably greater than 2.5% and less than 5.0%, more preferably greater than 3.0% and less than 5.0%, and more preferably greater than 3.2% and less than 5.0%. On the other hand, when it is excessively contained, the magnetic flux density will be significantly reduced. Therefore, the Si content is set to less than 5.0%. From the viewpoint of suppressing the reduction in magnetic flux density, the Si content is preferably greater than 1.0% and less than 4.5%, more preferably greater than 1.0% and less than 4.0%, and more preferably greater than 1.0% and less than 3.5%.

[0087] Sol.Al: 0% or more but less than 2.5%

[0088] Al (aluminum) is a selective element that is effective in increasing the resistivity of the steel sheet to reduce the iron loss, but when it is contained excessively, the magnetic flux density will be significantly reduced. Therefore, the sol.Al content is set to less than 2.5%. Regarding the sol.Al content, there is no need to limit the lower limit, and the lower limit can also be 0%. However, in order to more reliably obtain the effect based on the above-mentioned action, it is preferred that the sol.Al content is set to 0.03% or more, and more preferably, it is set to 0.10% or more. In addition, sol.Al means acid-soluble aluminum.

[0089] Here, Si and Al are elements effective in reducing the anisotropy in the magnetic plate surface and reducing the anisotropy in the mechanical plate surface. Therefore, the total content of Si and sol.Al is preferably more than 2.0%, more preferably more than 3.0%, and more preferably more than 4.0%. On the other hand, Si and Al have high solid solution strengthening ability, so when they are excessively contained, cold rolling becomes difficult. Therefore, it is preferred that the total content of Si and sol.Al is less than 5.5%.

[0090] Mn: 0% or more and 3.0% or less

[0091] Mn (manganese) is a selective element that is effective in reducing iron loss by increasing the resistivity of steel plates. However, Mn has a higher alloy cost than Si and Al, so when the Mn content increases, it will be economically disadvantageous. Therefore, the Mn content is set to 3.0% or less. Regarding the Mn content, it is preferably 2.7% or less, and more preferably 2.5% or less. Regarding the Mn content, there is no need to limit the lower limit, and the lower limit may also be 0%. However, in order to more reliably obtain the effect based on the above-mentioned action, regarding the Mn content, it is preferably 0.0010% or more, more preferably 0.0030% or more, and further preferably 0.010% or more.

[0092] P: 0% or more and 0.30% or less

[0093] P (phosphorus) is an element generally contained as an impurity. However, since P has the effect of improving the texture of the non-oriented electromagnetic steel sheet to improve the magnetic properties, it can also be contained as needed. However, since P is also a solid solution strengthening element, when the P content becomes excessive, the steel sheet will harden and cold rolling will become difficult. Therefore, the P content is set to 0.30% or less. Regarding the P content, it is preferably 0.20% or less. Regarding the P content, there is no need to limit the lower limit value, and the lower limit value can also be 0%. However, in order to more reliably obtain the effect based on the above-mentioned effect, regarding the P content, it is preferably 0.0010% or more, more preferably 0.010% or more, and further preferably 0.015% or more.

[0094] S: 0% or more, 0.010% or less

[0095] S (sulfur) is contained as an impurity, and combines with Mn in steel to form fine MnS, which inhibits the growth of grains during annealing and deteriorates the magnetic properties of the non-oriented electrical steel sheet. Therefore, the S content is set to 0.010% or less. The S content is preferably 0.005% or less, and more preferably 0.003% or less. The S content is preferably less, so there is no need to limit the lower limit, and the lower limit may be 0%. However, it is not easy to make the content 0% in industry, so the lower limit may be 0.0001%, or 0.001%.

[0096] N: 0% or more, 0.010% or less

[0097] N (nitrogen) is contained as an impurity, and combines with Al to form fine AlN, which hinders the growth of grains during annealing and deteriorates the magnetic properties. Therefore, the N content is set to less than 0.010%. Regarding the N content, it is preferably less than 0.005%, and more preferably less than 0.003%. Regarding the N content, it is preferably less, so there is no need to limit the lower limit, and the lower limit can also be 0%. However, it is not easy to make the content 0% in industry, so the lower limit can also be set to more than 0.0001%, or it can be set to more than 0.0010%, or it can be set to more than 0.0015%.

[0098] O: 0% or more, 0.10% or less

[0099] O (oxygen) is contained as an impurity, forming oxides and deteriorating the magnetic properties. Therefore, the O content is set to 0.10% or less. Regarding the O content, it is preferably 0.08% or less, more preferably 0.05% or less, further preferably 0.010% or less, and particularly preferably 0.008% or less. Regarding the O content, it is preferably less, so there is no need to limit the lower limit, and the lower limit can also be 0%. However, it is not easy to make the content 0% in industry, so the lower limit can also be set to 0.0001% or more, or 0.0005% or more, or 0.0008% or more.

[0100] In addition to the above-mentioned elements, the chemical composition of the non-oriented electrical steel sheet of the present disclosure may contain at least one of Sn, Sb, Ca, Cr, Ni, Cu and Ce as a selective element. For example, the contents of these selective elements may be as follows.

[0101] Sn: 0% or more and 0.20% or less

[0102] Sb: 0% or more and 0.20% or less

[0103] Sn (tin) and Sb (antimony) are selective elements that have the effect of improving the texture of the non-oriented electromagnetic steel sheet to improve the magnetic properties (for example, magnetic flux density), so they can also be contained as needed. However, when Sn and / or Sb are contained excessively, the steel may become brittle and cause cold rolling fracture, and the magnetic properties may sometimes be deteriorated. Therefore, the contents of Sn and Sb are respectively set to less than 0.20%. There is no need to limit the lower limit of each content of Sn and Sb, and the lower limit may also be 0%. However, in order to more reliably obtain the effect based on the above-mentioned effect, the Sn content is preferably 0.0010% or more, and more preferably 0.01% or more. In addition, with regard to the Sb content, it is preferably 0.0010% or more, preferably 0.002% or more, and more preferably 0.01% or more.

[0104] Ca: 0% or more and 0.01% or less

[0105] Ca (calcium) is an effective selective element for inclusion control because it suppresses the precipitation of fine sulfides (MnS, Cu2S, etc.) by generating coarse sulfides. When added moderately, it has the effect of improving grain growth to improve magnetic properties (for example, iron loss). However, when Ca is excessively contained, the effect based on the above effect will be saturated and cost increase will be incurred. Therefore, the Ca content is set to 0.01% or less. Regarding the Ca content, it is preferably 0.008% or less, and more preferably 0.005% or less. Regarding the Ca content, there is no need to limit the lower limit value, and the lower limit value can also be 0%. However, in order to more reliably obtain the effect based on the above effect, it is preferred that the Ca content is set to 0.0003% or more. Regarding the Ca content, it is preferably 0.001% or more, and more preferably 0.002% or more.

[0106] Cr: 0% or more but less than 5.0%

[0107] Cr (chromium) is a selective element that improves magnetic properties (for example, iron loss) by increasing intrinsic resistance. However, when it is contained excessively, the saturation flux density is sometimes reduced. In addition, the effect based on the above action will be saturated and the cost will be increased. Therefore, the Cr content is set to 5.0% or less. The Cr content may also be less than 4.0%, preferably less than 0.5%, and more preferably less than 0.1%. Regarding the Cr content, there is no need to limit the lower limit value, and the lower limit value may also be 0%. However, in order to more reliably obtain the effect based on the above action, it is preferred that the Cr content is 0.0010% or more.

[0108] Ni: 0% or more and 5.0% or less

[0109] Ni (nickel) is a selective element that improves magnetic properties (for example, saturation magnetic flux density). However, when Ni is contained excessively, the effect based on the above-mentioned action will be saturated and cost increase will be incurred. Therefore, the Ni content is set to 5.0% or less. The Ni content may also be less than 4.0%, preferably less than 0.5%, and more preferably less than 0.1%. Regarding the Ni content, there is no need to limit the lower limit value, and the lower limit value may also be 0%. However, in order to more reliably obtain the effect based on the above-mentioned action, it is preferred that the Ni content is 0.0010% or more.

[0110] Cu: 0% or more and 5.0% or less,

[0111] Cu (copper) is a selective element that improves the strength of the steel plate. However, when Cu is excessively contained, the saturation magnetic flux density may be reduced. In addition, the effect based on the above action may be saturated, resulting in an increase in cost. Therefore, the Cu content is set to 5.0% or less. The Cu content may also be 4.0% or less, preferably 0.1% or less. Regarding the Cu content, there is no need to limit the lower limit, and the lower limit may also be 0%. However, in order to more reliably obtain the effect based on the above action, it is preferred that the Cu content is 0.0010% or more.

[0112] Ce: 0% or more, 0.10% or less

[0113] Ce (cerium) is a selective element that reduces iron loss by generating coarse sulfides and oxysulfides, thereby inhibiting the precipitation of fine sulfides (MnS, Cu2S, etc.) and improving grain growth. However, when it is contained excessively, in addition to sulfides and oxysulfides, oxides are also generated, which sometimes deteriorates iron loss. In addition, the effect based on the above action will be saturated, resulting in an increase in cost. Therefore, the Ce content is set to 0.10% or less. Preferably, the Ce content is 0.01% or less. Regarding the Ce content, there is no need to limit the lower limit value, and the lower limit value may also be 0%. However, in order to more reliably obtain the effect based on the above action, it is preferred that the Ce content is 0.001% or more. It is further preferred that the Ce content is 0.002% or more, further preferred that it is 0.003% or more, and further preferred that it is 0.005% or more.

[0114] The chemical composition of the non-oriented electrical steel sheet of the present disclosure may further contain, as a selective element, at least one of B, Mg, Ti, V, Zr, Nd, Bi, W, Mo, Nb and Y. The contents of these selective elements may be controlled based on known knowledge. For example, the contents of these selective elements may be as follows.

[0115] B: 0% or more but less than 0.10%

[0116] Mg: 0% or more and 0.10% or less,

[0117] Ti: 0% or more and 0.10% or less,

[0118] V: 0% or more and 0.10% or less,

[0119] Zr: 0% or more and 0.10% or less

[0120] Nd: 0% or more and 0.10% or less,

[0121] Bi: 0% or more and 0.10% or less,

[0122] W: 0% or more and 0.10% or less,

[0123] Mo: 0% or more and 0.10% or less,

[0124] Nb: 0% or more and 0.10% or less,

[0125] Y: 0% to 0.10%.

[0126] Furthermore, it is preferred that the non-oriented electrical steel sheet of the present disclosure contains, in addition to 1.0% to 5.0% Si, the chemical composition further contains, by mass %,

[0127] C: 0.0010% or more and 0.006% or less,

[0128] Sol.Al: 0.10% or more but less than 2.5%,

[0129] Mn: 0.0010% or more and 3.0% or less,

[0130] P: 0.0010% or more and 0.30% or less,

[0131] S: 0.0001% or more and 0.010% or less,

[0132] N: more than 0.0015% and less than 0.010%,

[0133] O: 0.0001% or more and 0.10% or less,

[0134] Sn: 0.0010% or more and 0.20% or less,

[0135] Sb: 0.0010% or more and 0.20% or less,

[0136] Ca: 0.0003% or more and 0.01% or less,

[0137] Cr: 0.0010% or more and 5.0% or less,

[0138] Ni: 0.0010% to 5.0%,

[0139] Cu: 0.0010% or more and 5.0% or less,

[0140] Ce: 0.001% or more and 0.10% or less,

[0141] B: 0.0001% or more and 0.10% or less,

[0142] Mg: 0.0001% or more and 0.10% or less,

[0143] Ti: 0.0001% or more and 0.10% or less,

[0144] V: 0.0001% or more and 0.10% or less,

[0145] Zr: 0.0002% or more and 0.10% or less

[0146] Nd: 0.002% or more and 0.10% or less,

[0147] Bi: 0.002% or more and 0.10% or less,

[0148] W: 0.002% or more and 0.10% or less,

[0149] Mo: 0.002% or more and 0.10% or less,

[0150] Nb: 0.0001% or more and 0.10% or less, and

[0151] Y: at least one of 0.002% to 0.10%.

[0152] The B content is preferably 0.02% or less, more preferably 0.01% or less.

[0153] Preferably, the Mg content is 0.01% or less, more preferably 0.005% or less. Preferably, the Ti content is 0.100% or less, more preferably 0.002% or less. Preferably, the V content is 0.05% or less, more preferably 0.04% or less.

[0154] The Zr content is preferably 0.08% or less, more preferably 0.06% or less.

[0155] The Nd content is preferably 0.05% or less, more preferably 0.01% or less.

[0156] The Bi content is preferably 0.05% or less, more preferably 0.01% or less.

[0157] The W content is preferably 0.05% or less, more preferably 0.01% or less.

[0158] The Mo content is preferably 0.05% or less, more preferably 0.01% or less.

[0159] The Nb content is preferably 0.05% or less, more preferably 0.03% or less.

[0160] The Y content is more preferably 0.05% or less, and even more preferably 0.01% or less.

[0161] In addition, from the viewpoint of achieving the effects described later, the preferred lower limits of the contents of the respective elements are as follows.

[0162] Preferably, the B content is 0.0002% or more.

[0163] Preferably, the Mg content is 0.0004% or more.

[0164] Preferably, the Ti content is 0.001% or more.

[0165] Preferably, the V content is 0.002% or more.

[0166] Preferably, the Zr content is 0.002% or more.

[0167] Preferably, the Nd content is 0.002% or more.

[0168] Preferably, the Bi content is 0.002% or more.

[0169] Preferably, the W content is 0.002% or more.

[0170] Preferably, the Mo content is 0.002% or more.

[0171] Preferably, the Nb content is 0.002% or more.

[0172] Preferably, the Y content is 0.002% or more.

[0173] The above-mentioned optional elements are divided into the following groups A to E according to the difference in the effects exerted by each element.

[0174] [Group A]Sn, Sb, Ca, Cr, Ni, Cu, Ce

[0175] Elements that can improve magnetic and / or mechanical properties through texture, inclusion control, intrinsic resistance, saturation magnetic flux density, solid solution strengthening, etc.

[0176] [Group B] Ti, V, Zr, Nb

[0177] Elements that improve grain growth by coarsening precipitates

[0178] [Group C] Mg, Nd, Bi, Y

[0179] Elements that can control inclusions such as sulfides and oxides

[0180] [Group D]B

[0181] Elements that can exert more preferable effects through nitride control

[0182] [Group E]

[0183] Elements that have a preferred effect by improving mechanical properties

[0184] W.Mo

[0185] The non-oriented electrical steel sheet of the present disclosure may contain one or more elements selected from the group consisting of the above-mentioned groups A to E. For example, it may contain one or more elements of group A, group B, group C, group D and / or group E.

[0186] The chemical composition mentioned above can be measured by general analysis methods for steel. For example, the chemical composition can be measured by ICP-AES (Inductively Coupled Plasma-Atomic Emission Spectrometry). In addition, sol.Al can be measured by ICP-AES using the filtrate after the sample is heated and decomposed with acid. In addition, Si can be measured by ICP emission spectrometry, C and S can be measured by combustion-infrared absorption, N can be measured by inert gas melting thermal conductivity, and O can be measured by inert gas melting-non-dispersive infrared absorption.

[0187] In addition, the above chemical composition is the composition of the non-oriented electromagnetic steel sheet that does not include an insulating film or the like. In the case where the non-oriented electromagnetic steel sheet used as the measurement sample has an insulating film or the like on the surface, the measurement is performed after it is removed. For example, the insulating film or the like can be removed by the following method. First, the non-oriented electromagnetic steel sheet having the insulating film or the like is immersed in a sodium hydroxide aqueous solution, a sulfuric acid aqueous solution, and a nitric acid aqueous solution in sequence, and then washed. Finally, it is dried with warm air. In this way, a non-oriented electromagnetic steel sheet with the insulating film removed can be obtained. In addition, the insulating film or the like can also be removed by grinding.

[0188] (Characteristics of crystal orientation)

[0189] Regarding the non-oriented electrical steel sheet disclosed in the present invention, at a position of 1 / 4 of the thickness in the thickness direction from the surface of the steel sheet, the degree of {111}<011> aggregation is 2.00 or more and 8.00 or less (hereinafter, the description of "a position of 1 / 4 of the thickness in the thickness direction from the surface of the steel sheet" may be omitted).

[0190] In addition, the so-called "aggregation degree" of crystal orientation in the present disclosure refers to an index generally used when displaying texture. For example, the so-called {111}<011>aggregation degree refers to an index indicating how many times the frequency of existence of grains having the crystal orientation {111}<011> is relative to a structure having a random orientation distribution (in this case, the aggregation degree is 1).

[0191] Regarding the non-oriented electrical steel sheet disclosed in the present invention, at a position 1 / 4 of the sheet thickness in the sheet thickness direction from the surface of the steel sheet, in addition to the {111}<011> aggregation being 2.00 or more and 8.00 or less, it is preferred that at least one of the following conditions is satisfied: the {110}<001> aggregation being 1.00 or more, the value of the {111}<112> aggregation / {111}<011> aggregation being 1.00 or less, the {411}<148> aggregation being 2.00 or less, and the {411}<011> aggregation being 2.00 or less.

[0192] The {111}<011> aggregation degree of 2.00 or more and 8.00 or less is an important feature of the non-oriented electrical steel sheet of the present disclosure. The {111}<011> orientation is an orientation with good magnetic properties when stress is applied.

[0193] Furthermore, the present inventors have succeeded in achieving both high levels of magnetic properties both under normal conditions and when stress is applied by appropriately controlling at least any one of the concentrations of {110}<001>, {111}<112>, {411}<148> and {411}<011> orientations simultaneously with {111}<011> as shown below.

[0194] The {110}<001> orientation is an orientation excellent in magnetic properties, and it is preferable that the degree of aggregation be 1.00 or more.

[0195] Although the {111}<112> orientation is an orientation that can minimize the deterioration of magnetic properties when stress is applied, when the aggregation degree is too high, the magnetic properties in a state where no compressive stress is applied deteriorate. Therefore, in view of the balance of aggregation between {111}<011> orientations having the same plane index and having substantially the same influence on magnetic properties, it is preferred that the value of {111}<112> aggregation / {111}<011> aggregation (aggregation ratio) be set to 1.00 or less.

[0196] The {411}<148> orientation is an orientation in which magnetic properties tend to deteriorate when compressive stress is applied, and it is preferable that the degree of aggregation be 2.00 or less.

[0197] The {411}<011> orientation is an orientation in which magnetic properties tend to deteriorate when compressive stress is applied, and it is preferable that the degree of aggregation be 2.00 or less.

[0198] The crystal orientation can be measured by the following method. A steel plate sample of about 30 mm × 30 mm cut out from a steel plate is subjected to mechanical grinding and chemical grinding to remove the surface layer from the surface of the steel plate to 1 / 4t on one side. Here, the so-called 1 / 4t portion means a portion corresponding to a depth of t×1 / 4 from the surface when the thickness of the steel plate is recorded as t. When removing the surface layer, a test piece for measurement with a reduced thickness is made until the 1 / 4t portion of the original steel plate becomes the surface. In addition, when the surface layer from the surface to 1 / 4t on one side of the steel plate is removed by mechanical grinding and chemical grinding, there may be a situation where it is difficult to strictly appear the surface of the 1 / 4t portion, and the removal margin is allowed to a certain extent. Considering the average crystal grain size (30 μm or more and 200 μm or less) of the non-oriented electromagnetic steel sheet disclosed in the present invention, the concentration of the crystal orientation of the region of the average crystal grain size of the steel plate in the depth direction can be regarded as the same degree relative to the depth 1 / 4t portion from the surface of the steel plate. Considering the preferred plate thickness (above 0.10 mm and below 0.35 mm), mechanical grinding and chemical grinding can be used to produce a surface with a depth of 1 / 4t±1 / 8t from the surface of the steel plate, that is, in the range of 1 / 8t to 3 / 8t, to measure the crystal orientation.

[0199] After grinding the sample extracted from the steel plate and removing 1 / 4t of the surface layer, the crystal orientation can be determined by the electron backscatter diffraction (EBSD) method. The observation field is preferably 2400 μm per field of view. 2 Above 2.5mm 2 In the following, it is preferred to use the average value of each value calculated for multiple fields of view of more than 2 and less than 5. According to the above observation results, a crystal orientation distribution function ODF (Orientation Determination Function) is prepared. Based on the crystal orientation distribution function, the aggregation degree of each orientation in the surface is obtained. In addition, in order to ensure the accuracy of the value of the aggregation degree, it is preferred that the number of expansions of ODF is more than 18.

[0200] (magnetic properties)

[0201] In the present disclosure, the effect of the invention (deterioration suppression of iron loss when compressive stress is applied) can be confirmed by the iron loss W10 / 400 [W / kg] when the magnetic flux density is 1.0T and the frequency is 400Hz. Regarding the iron loss, the iron loss when the excitation direction is the rolling direction (L direction), the rolling right angle direction (C direction) and the 45° direction (D direction) of the steel plate is recorded as WL, WC and WD respectively, and the average value of the characteristics within the plate surface obtained by (WL+WC+2×WD) / 4 is used. In this specification, this characteristic is sometimes referred to as "whole-week average (iron loss)". Regarding the rolling direction, it is clear as long as the non-oriented electromagnetic steel sheet is provided in the form of a coil, but in the case of a cut plate or in the state of being taken out from the motor core, it cannot be judged only by the shape. In this case, the rolling direction can be determined by the grooves on the surface of the steel plate formed during cold rolling. Regarding this method, it is a method that is used in daily life as long as it is a person skilled in the art, and its judgment is not difficult.

[0202] In the present disclosure, the effect of the invention is confirmed by the degradation amount Ws-Wn of the whole-cycle average iron loss Wn [W / kg] calculated from the iron loss value in each in-plane direction under no-load condition and the whole-cycle average iron loss Ws [W / kg] calculated from the iron loss value in each in-plane direction under the condition of applying 20MPa of compressive stress to each excitation direction. With regard to the non-oriented electromagnetic steel sheet of the present disclosure, Ws-Wn is preferably set to a form of 8.50 or less. With regard to Ws-Wn, it is further preferred that it is 8.25 or less, and it is further preferred that it is 8.00 or less.

[0203] Each magnetic property can be measured by the single sheet magnetic property test method (Single Sheet Tester: SST) specified in JIS C2556: 2015. In addition, in the case where it is difficult to extract a test piece of the size specified in JIS, for example, a test piece of width 55 mm × length 55 mm can be extracted to perform measurement in accordance with the single sheet magnetic property test method. At this time, it is preferred to use the Epstein equivalent value converted to the Epstein tester specified in JIS C2550: 2011.

[0204] (Average crystal size)

[0205] Whether the crystal grain size is too large or too small, the iron loss under high frequency conditions may deteriorate. Therefore, the average crystal grain size may be set within a general practical range, which is 30 μm or more and 200 μm or less.

[0206] The average crystal grain size can be measured by the cutting method specified in JIS G0551: 2020. For example, in a longitudinal cross-sectional structure photograph in the plate thickness direction, the average value of the crystal grain size measured by the cutting method can be used for the plate thickness direction and the rolling direction. As the longitudinal cross-sectional structure photograph, an optical microscope photograph can be used, for example, a photograph taken at a magnification of 50 times can be used.

[0207] (plate thickness)

[0208] As for the plate thickness, the thinner it is, the lower the iron loss will be. It can be set to a general practical range, preferably, it is set to 0.35mm or less. More preferably, it is 0.30mm or less. On the other hand, excessive thinning will significantly reduce the productivity of the steel plate or the motor, so it is preferred to set the plate thickness to 0.10mm or more. More preferably, it is 0.15mm or more.

[0209] The sheet thickness can be measured by a micrometer. In addition, when the non-oriented electrical steel sheet as the measurement sample has an insulating film or the like on the surface, the measurement is performed after removing it. The method of removing the insulating film is as described above.

[0210] [Method for producing non-oriented electrical steel sheet]

[0211] An example of a method for manufacturing the non-oriented electromagnetic steel sheet of the present invention is described below. In addition, as long as the non-oriented electromagnetic steel sheet of the present invention has the above-mentioned structure, the manufacturing method is not particularly limited. The following manufacturing method is an example for manufacturing the non-oriented electromagnetic steel sheet of the present invention, and is a preferred example of the manufacturing method of the non-oriented electromagnetic steel sheet of the present invention.

[0212] The method for producing a non-oriented electrical steel sheet disclosed in the present invention sequentially comprises a hot rolling step, a first cold rolling step, an intermediate annealing step, a second cold rolling step, and a final annealing step. In these steps, it is particularly effective to apply the following conditions (A) to (E). In addition, the temperature in the following description means the surface temperature of the steel sheet.

[0213] (A) Heat treatment after hot rolling: After the hot finish rolling, no heat treatment at 900° C. or higher is performed until the first cold rolling starts.

[0214] (B) First cold rolling step: the reduction ratio is set to 30% to 85%.

[0215] (C) Intermediate annealing step: the average heating rate from 500°C to 650°C is set to 300°C / s to 1000°C / s, the holding temperature is set to 700°C to 1100°C, the holding time is set to 10 seconds to 300 seconds, and the average cooling rate from 700°C to 500°C is set to 25°C / s or more.

[0216] (D) Second cold rolling step: the reduction ratio is set to 30% to 75%, and the final sheet thickness is set to 0.10 mm to 0.35 mm.

[0217] (E) Final annealing step: the holding temperature is set to 900° C. or higher and 1200° C. or lower.

[0218] Hereinafter, each step will be described.

[0219] (Hot rolling process)

[0220] The hot-rolled steel sheet to be subjected to the first cold rolling step can be obtained by hot-rolling a steel block or steel sheet (hereinafter also referred to as a “slab”) having the above-mentioned chemical composition.

[0221] In hot rolling, the steel having the above chemical composition is made into a slab by a common method such as continuous casting or a method of splitting and rolling a steel block, and then loaded into a heating furnace for hot rolling. At this time, if the slab temperature is high, hot rolling can be performed without loading it into a heating furnace.

[0222] The various conditions of hot rolling are not particularly limited, but generally, the conditions of setting the slab heating temperature to 950 to 1250° C., the final temperature to 700 to 1000° C., and the final slab thickness to about 1.0 to 4.0 mm are adopted.

[0223] (Heat treatment of hot rolled plates)

[0224] The first cold rolling is continued for the hot-rolled sheet that has finished the hot rolling. At this time, the hot-rolled steel sheet supplied to the first cold rolling process will not be subjected to a heat treatment of 900°C or more after the final rolling under hot conditions. The purpose of this restriction is to prevent the structure formed by hot working from changing significantly before the first cold rolling. When the outlet temperature of the final pass of hot rolling becomes 900°C or more, the sheet will stay in a temperature range of 900°C or more during the period from cooling from the outlet of the final pass to reaching less than 900°C, but generally, it will be cooled to less than 900°C within a few seconds, so in the present disclosure, the retention during this period can be ignored. Therefore, with regard to the heat treatment in the present disclosure, the thermal history implemented by hot-rolled sheet coiling or hot-rolled sheet annealing will be the subject. After the hot final rolling is completed, when a heat treatment of 900°C or more is performed, the grain size of the hot-rolled sheet will increase, and the structure after the intermediate annealing process will change, and the {111}<011> aggregation after the final annealing specified in the above content will not be satisfied. Therefore, it is not preferred to keep the hot rolled sheet hot after coiling. In particular, the hot rolling coiling temperature, which is maintained for a long time, is preferably 850°C or lower, and more preferably 800°C or lower.

[0225] (1st cold rolling process)

[0226] In the first cold rolling step, the hot-rolled steel sheet having the above-mentioned chemical composition is cold rolled at a reduction ratio (cumulative reduction ratio) of 30% to 85%.

[0227] When the reduction ratio in the first cold rolling step is less than 30% or exceeds 85%, the target magnetic properties may not be obtained. Therefore, the reduction ratio in the first cold rolling step is set to 30% to 85%.

[0228] The conditions other than the above in cold rolling, such as the steel sheet temperature during cold rolling and the roll diameter, are not particularly limited and are appropriately selected according to the chemical composition of the hot-rolled steel sheet, the target steel sheet thickness, and the like.

[0229] (Intermediate annealing process)

[0230] In the intermediate annealing process, the cold-rolled steel sheet obtained by the above-mentioned first cold rolling process is subjected to intermediate annealing, and the average heating rate from 500°C to 650°C is set to 300°C / second or more and 1000°C / second or less, the holding temperature is set to 700°C or more and 1100°C or less, the holding time is set to 10 seconds or more and 300 seconds or less, and the average cooling rate from 700°C to 500°C is set to 25°C / second or more.

[0231] When the above-mentioned conditions in the intermediate annealing step are not satisfied, the target magnetic properties may not be obtained. The conditions other than the above-mentioned conditions in the intermediate annealing step are not particularly limited.

[0232] In addition, there is no need to set an upper limit value for the average cooling rate from 700° C. to 500° C., but the upper limit value may be set to 70° C. / sec as necessary.

[0233] Preferably, the holding temperature is 850°C or higher. In addition, it is preferred that the holding time is 180 seconds or less. Furthermore, it is preferred that the average cooling rate from 700°C to 500°C is set to 28°C / second or more. In particular, if, on the basis of satisfying the conditions of the present disclosure, all of the following conditions are satisfied: Si content: more than 2.0%, average heating rate from 500°C to 650°C: 300°C / second or more, holding temperature: 850°C or more, holding time: 180 seconds or less, average cooling rate from 700°C to 500°C: 33°C / second or more, then a non-oriented electromagnetic steel sheet having good magnetic properties when stress is applied can be obtained.

[0234] (Second cold rolling process)

[0235] In the second cold rolling step, the intermediate annealed steel sheet obtained in the intermediate annealing step is cold rolled at a reduction ratio (cumulative reduction ratio) of 30% to 75% to a sheet thickness of 0.10 mm to 0.35 mm.

[0236] When the reduction ratio in the second cold rolling step is less than 30% or exceeds 75%, the target magnetic properties may not be obtained. Therefore, the reduction ratio in the second cold rolling step is set to 30% to 75%.

[0237] Preferably, the plate thickness is set to be 0.10 mm or more and 0.35 mm or less. More preferably, the plate thickness is set to be 0.15 mm or more and 0.30 mm or less.

[0238] The conditions other than the above-mentioned cold rolling conditions such as the steel sheet temperature during cold rolling and the roll diameter are not particularly limited and are appropriately selected according to the chemical composition of the steel sheet, the target steel sheet thickness, and the like.

[0239] (Final annealing process)

[0240] In the final annealing step, the cold rolled steel sheet obtained in the second cold rolling step is subjected to final annealing in a temperature range of 900° C. to 1200° C. This condition is not special and is adopted in the production of general non-oriented electrical steel sheets.

[0241] When the final annealing temperature in the final annealing process is less than 900°C, the average crystal grain size will be less than 30μm due to insufficient grain growth, and sufficient magnetic properties cannot be obtained. Therefore, the final annealing temperature is set to 900°C or more. On the other hand, when the final annealing temperature exceeds 1200°C, the grain growth other than the {111}<011> orientation that is a characteristic of the non-oriented electromagnetic steel sheet disclosed in the present invention will become dominant, the grain growth will proceed excessively, the average crystal grain size will exceed 200μm, and sufficient magnetic properties cannot be obtained. Therefore, the final annealing temperature is set to 1200°C or less.

[0242] The final annealing time in the temperature range of 900°C to 1200°C may not be particularly specified, but is preferably set to 1 second or longer in order to more reliably obtain good magnetic properties. On the other hand, from the perspective of productivity, the final annealing time is preferably set to 120 seconds or shorter.

[0243] The conditions of the final annealing other than those described above are not particularly limited.

[0244] In addition, the final annealing can be performed by the steel plate manufacturer after the second cold rolling. Alternatively, the steel plate after the second cold rolling is shipped and can be performed as a heat treatment in the core shape, so-called stress relief annealing, at the user's site of the steel plate, for example, after the punching process and the steel plate lamination.

[0245] (Other processes)

[0246] During the hot rolling, after the scale formed on the surface of the steel sheet is removed, the steel sheet is subjected to cold rolling. Therefore, it is preferable to perform pickling on the hot-rolled steel sheet.

[0247] Alternatively, after the second cold rolling step or the final annealing step, a coating step is performed according to a general method, and the coating step forms an insulating film composed of only organic components, only inorganic components, or an organic-inorganic composite on the surface of the steel sheet. From the viewpoint of reducing the environmental burden, an insulating film that does not contain chromium may also be formed by coating. In addition, the coating step may be a step in which an insulating coating that exerts adhesive ability is applied by heating and pressurizing. As a coating material that exerts adhesive ability, acrylic resin, phenolic resin, epoxy resin or melamine resin, etc., can be used.

[0248] [use]

[0249] The use of the non-oriented electromagnetic steel sheet disclosed in the present invention is not particularly limited, but is preferably used as a raw material for the stator core and rotor core of a motor. The non-oriented electromagnetic steel sheet disclosed in the present invention can be punched into a predetermined shape and made into a motor core having a structure of stacking multiple sheets. The deterioration of the iron loss of such a motor core when a compressive stress is applied is small, which can contribute to the efficiency of the motor.

[0250] [Example]

[0251] Hereinafter, although an Example is demonstrated, the non-oriented electrical steel sheet of this indication is not limited to the following Example.

[0252] In a vacuum melting furnace, slabs (ingots) adjusted to the chemical compositions shown in Table 1-1 and Table 1-2 were produced. In addition, the underlined contents in the components shown in Table 1-1 and Table 1-2 mean that they are outside the scope of the present disclosure, and the remainder is Fe and impurities. Blank columns mean that the component (element) is not intentionally added.

[0253]

Table 1-1

[0254] Table 1-1

[0255]

[0256]

Table 1-2

[0257] Table 1-2

[0258]

[0259] After the slabs (steel types A to B7) having the chemical compositions shown in Tables 1-1 and 1-2 were inserted into a heating furnace and heated to 1100°C, hot rolling was performed to obtain a plate thickness of 2.0 mm to produce hot-rolled steel plates. The final temperature was 850°C and the coiling temperature was 600°C as the basis. However, for some steel plates, any one of the conditions such as the plate thickness, final temperature, and coiling temperature was changed. For example, No.a16 was set to a final temperature of 930°C and a coiling temperature of 900°C. In addition, No.k1 and v1 were set to a final temperature of 1000°C and a coiling temperature of 800°C, and No.n1 was set to a final temperature of 800°C and a coiling temperature of 300°C.

[0260] These hot-rolled steel sheets were subjected to hot-rolled sheet annealing, first cold rolling, intermediate annealing, second cold rolling, and final annealing in this order. The respective conditions are shown in Table 2-1, Table 3-1, Table 4-1, and Table 5-1.

[0261] In addition, this Example was implemented without forming an insulating film on the surface of the steel plate.

[0262] [Measurement of average crystal particle size]

[0263] For each steel plate, after final annealing, the crystal grain size was measured using an optical microscope photograph obtained by observing a longitudinal section in the plate thickness direction and the rolling direction at 50 times by the above-mentioned cutting method, and the average crystal grain size was determined.

[0264] [Texture measurement]

[0265] The steel plate samples of about 30mm×30mm cut from each steel plate were subjected to mechanical grinding and chemical grinding until the 1 / 4t part of the original steel plate became the surface, and the test pieces for measuring the reduced thickness were made respectively. For the obtained test pieces, EBSD was used to observe in each field of view of 900μm×2500μm, and 5 places were observed. According to the observation results, the crystal orientation distribution function ODF was made, and the aggregation degree of each orientation in the surface was obtained based on the crystal orientation distribution function. The aggregation degree of each orientation adopted the average value of the values ​​calculated for each field of view.

[0266] [Measurement of magnetic properties]

[0267] The magnetic properties of each steel plate were measured by SST. As the iron loss W10 / 400 [W / kg] when excited at a magnetic flux density of 1.0T and a frequency of 400Hz, the iron loss Wn [W / kg] in the no-load state and the iron loss Ws [W / kg] in the state where a compressive stress of 20MPa was applied in the excitation direction were measured, and Ws-Wn was obtained. When Ws-Wn was 8.50 or less, it was judged that the iron loss when the compressive stress was applied was good.

[0268] The manufacturing conditions of each steel plate are shown in Table 2-1, Table 3-1, Table 4-1, and Table 5-1, and the texture, average grain size, and magnetic properties are shown in Table 2-2, Table 3-2, Table 4-2, and Table 5-2. In addition, underlines mean outside the scope of the present disclosure or outside the scope of the above-mentioned preferred manufacturing method.

[0269]

Table 2-1

[0270]

[0271]

Table 2-2

[0272]

[0273]

Table 3-1

[0274]

[0275]

Table 3-2

[0276]

[0277]

Table 4-1

[0278]

[0279]

Table 4-2

[0280]

[0281]

Table 5-1

[0282]

[0283]

Table 5-2

[0284]

[0285] The steel plates of the embodiments produced by the chemical composition and preferred production method disclosed in the present invention, with an average grain size of 30 μm to 200 μm and a {111}<011> aggregation degree of 2.00 to 8.00, have an iron loss degradation (Ws-Wn) of 8.50 W / kg or less and are relatively good in iron loss when compressive stress is applied.

[0286] On the other hand, the steel sheets of the comparative examples whose chemical composition, average grain size or {111}<011> aggregation degree are outside the range of the present disclosure have iron loss degradation (Ws-Wn) exceeding 8.50 W / kg, and the iron loss when compressive stress is applied is larger than that of the examples.

[0287] In addition, No. a20 and a23 in Table 2-2 and No. ab2 and ac2 in Table 5-2 all had cracks generated during the first cold rolling, and the steel sheet properties were not measured.

[0288] The disclosures of Japanese Patent Application No. 2022-057541 filed on March 30, 2022 and Japanese Patent Application No. 2022-132805 filed on August 23, 2022 are incorporated herein by reference in their entirety. All documents, patent applications, and technical standards described in this specification are incorporated herein by reference to the same extent as if each document, patent application, and technical standard were specifically and separately described.

Claims

1. A non-oriented electromagnetic steel sheet having the following chemical composition, wherein the chemical composition is as follows, in mass %, C: 0.006% or less, Si: 1.0% to 5.0% Sol.Al: less than 2.5%, Mn: 3.0% or less, P: 0.30% or less, S: 0.010% or less, N: 0.010% or less, O: 0.10% or less, Sn: 0~0.20%, Sb: 0~0.20%, Ca: 0~0.01%, Cr: 0~5.0%, Ni: 0-5.0%, Cu: 0-5.0%, Ce: 0~0.10%, B: 0~0.10%, Mg: 0~0.10% Ti: 0~0.10%, V: 0~0.10%, Zr: 0~0.10%, Nd: 0~0.10%, Bi: 0~0.10%, W: 0~0.10%, Mo: 0~0.10% Nb: 0-0.10%, Y: 0~0.10%, The rest: Fe and impurities, The average crystal grain size is 30 μm or more and 200 μm or less. At a position of 1 / 4 of the plate thickness in the plate thickness direction from the surface of the steel plate, the degree of aggregation of {111}<011> is 2.00 or more and 8.00 or less.

2. The non-oriented electromagnetic steel sheet according to claim 1, comprising one or more selected from the group consisting of: Sn: 0.0010% or more and 0.20% or less, Sb: 0.0010% or more and 0.20% or less, Ca: 0.0003% or more and 0.01% or less, Cr: 0.0010% or more and 5.0% or less, Ni: 0.0010% to 5.0%, Cu: 0.0010% or more and 5.0% or less, Ce: 0.001% or more and 0.10% or less, B: 0.0001% or more and 0.10% or less, Mg: 0.0001% or more and 0.10% or less, Ti: 0.0001% or more and 0.10% or less, V: 0.0001% or more and 0.10% or less, Zr: 0.0002% or more and 0.10% or less Nd: 0.002% or more and 0.10% or less, Bi: 0.002% or more and 0.10% or less, W: 0.002% or more and 0.10% or less, Mo: 0.002% or more and 0.10% or less, Nb: 0.0001% or more and 0.10% or less, and Y: 0.002% or more and 0.10% or less.

3. The non-oriented electrical steel sheet according to claim 1 or 2, wherein: At a position of 1 / 4 of the plate thickness in the plate thickness direction from the surface of the steel plate, the degree of aggregation of {110}<001> is 1.00 or more.

4. The non-oriented electrical steel sheet according to any one of claims 1 to 3, wherein: At a position ¼ of the plate thickness in the plate thickness direction from the surface of the steel plate, a value of {111}<112> aggregation / {111}<011> aggregation is 1.00 or less.

5. The non-oriented electrical steel sheet according to any one of claims 1 to 4, wherein: At a position of 1 / 4 of the plate thickness in the plate thickness direction from the surface of the steel plate, the degree of aggregation of {411}<148> is 2.00 or less.

6. The non-oriented electrical steel sheet according to any one of claims 1 to 5, wherein: At a position of 1 / 4 of the plate thickness in the plate thickness direction from the surface of the steel plate, the degree of aggregation of {411}<011> is 2.00 or less.

7. The non-oriented electrical steel sheet according to any one of claims 1 to 6, wherein: The plate thickness is not less than 0.10 mm and not more than 0.35 mm.

8. A motor core having a structure in which a plurality of non-oriented electromagnetic steel sheets according to any one of claims 1 to 7 are stacked.

Citation Information

Patent Citations

  • Anisotropic electromagnetic steel sheet and method for producing same

    WO2013069754A1

  • JP特许2022-057541

  • JP特许2022-132805