Treatment agent for manufacturing carbon fiber textile yarn, and carbon fiber textile yarn
By using specific (poly)oxyalkylene derivatives and ester compounds in the manufacture of carbon fiber textile yarns, the problem of direct spinning of carbon fibers is solved, and the yarn wrapping and staple fiber falls are suppressed, and the production efficiency and dimensional accuracy are improved. The efficient manufacturing of carbon fiber textile yarns is achieved.
Patent Information
- Application Number
- CN202380033161.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-15
- Filing Date
- 2023-04-10
- Publication Date
- 2024-11-19
AI Technical Summary
The prior art is difficult to directly spin carbon fibers into textile yarns, resulting in a decrease in operability, and it is necessary to pass the process of flame-resistant fiber spinning and carbonization, and the recycling of carbon fibers is limited.
The treatment agent for manufacturing a carbon fiber textile yarn containing (poly)oxyalkylene derivatives with a number average molecular weight of 30,000 or less is used, and the (poly)oxyalkylene derivatives and ester compounds of 20% or less are used in a stripping machine. The combination of the carbon fiber yarn strips is inhibited from winding and falling off of the staple fibers, and improves the bundling and drafting properties of the yarn strips.
Effectively inhibit the winding of carbon fiber yarns to the strip roll, improve the anti-falling properties of short fibers and the drafting properties of yarns, simplify the production process of carbon fiber textile yarns, reduce the carbonization steps, improve dimensional accuracy and save resources.
Smart Images

Figure BDA0005075539290000081
Abstract
Description
Technical Field
[0001] The present invention relates to a treating agent for producing carbon fiber textile yarn and carbon fiber textile yarn. Background Art
[0002] Generally, carbon fiber cloth composed of carbon fiber is known. Carbon fiber cloth is used in composite materials together with matrix resin, for example. Composite materials are used in various fields such as medical equipment, precision equipment and industrial machinery, construction materials, energy, transmission equipment, aerospace, sports and leisure.
[0003] Patent Document 1 describes a technique for producing a flame resistant fabric by spinning flame resistant fibers in advance and then weaving the fibers. The flame resistant fabric is carbonized to produce a carbon fiber fabric. Prior art literature Patent Literature
[0004] Patent Document 1: Japanese Patent Application Publication No. 2006-274507 Summary of the invention Problems to be solved by the invention
[0005] However, it has been difficult to directly spin carbon fibers to produce carbon fiber textile yarns. One of the reasons for this is that the carbon fiber yarns are wound around the rollers of the drawing frame, which reduces the operability. Therefore, in the past, as shown in Patent Document 1, flame resistant fibers were spun to produce flame resistant fabrics, and then the flame resistant fabrics were carbonized to produce carbon fiber fabrics. Directly spinning carbon fibers to produce carbon fiber textile yarns is also one of the carbon fiber recycling methods. Therefore, research on directly spinning carbon fibers to produce carbon fiber textile yarns has been actively conducted. Means for solving problems
[0006] A treatment agent for producing a carbon fiber spun yarn according to one embodiment of the present invention for solving the above-mentioned problems is characterized in that the treatment agent contains a (poly)oxyalkylene derivative (A), and the number average molecular weight of the (poly)oxyalkylene derivative (A) is 30,000 or less.
[0007] The treatment agent for producing a carbon fiber spun yarn preferably contains the (poly)oxyalkylene derivative (A) in a ratio of 20% by mass or more and 60% by mass or less. In the above-mentioned treatment agent for producing a carbon fiber spun yarn, the number average molecular weight of the above-mentioned (poly)oxyalkylene derivative (A) is preferably 500 or more and 1200 or less.
[0008] The above-mentioned carbon fiber textile yarn manufacturing treatment agent may further contain an ester compound (B). When the total content ratio of the above-mentioned (poly)oxyalkylene derivative (A) and the above-mentioned ester compound (B) is set to 100 mass%, it is preferred that the above-mentioned (poly)oxyalkylene derivative (A) is contained in a ratio of 30 mass% to 60 mass%, and the above-mentioned ester compound (B) is contained in a ratio of 40 mass% to 70 mass%.
[0009] A carbon fiber spun yarn according to another aspect of the present invention for solving the above-mentioned problems is characterized in that the above-mentioned carbon fiber spun yarn producing treatment agent is adhered thereto. Effects of the Invention
[0010] According to the treating agent for producing a carbon fiber spun yarn of the present invention, it is possible to suppress the carbon fiber sliver from being entangled with the rollers of a drawing frame. DETAILED DESCRIPTION
[0011] <First Embodiment> A first embodiment that embodies the treating agent for producing a carbon fiber spun yarn (hereinafter also referred to as a treating agent) of the present invention will be described.
[0012] The treatment agent of the present embodiment contains a (poly)oxyalkylene derivative (A), and the number average molecular weight of the (poly)oxyalkylene derivative (A) is 30,000 or less. By containing the (poly)oxyalkylene derivative (A) described above in the treatment agent, when carbon fiber is directly spun to produce a carbon fiber spun yarn, it is possible to suppress the carbon fiber sliver from being entangled with the rollers of a drawing frame.
[0013] The components constituting the treatment agent are described below. ((Poly)oxyalkylene derivative (A)) As the (poly)oxyalkylene derivative (A), a known (poly)oxyalkylene derivative (A) having a number average molecular weight of 30,000 or less can be used. As the above-mentioned known (poly)oxyalkylene derivative (A), for example, a compound formed by adding alkylene oxide to alcohols or carboxylic acids can be mentioned. In addition, an ether·ester compound formed by adding alkylene oxide to an ester compound of carboxylic acids and polyols can also be mentioned. As alcohols or carboxylic acids, linear or branched aliphatic alcohols or carboxylic acids can be used, and aromatic alcohols or carboxylic acids can also be used. In addition, saturated alcohols or carboxylic acids can be used, and unsaturated alcohols or carboxylic acids can be used. In addition, monovalent or divalent or higher alcohols or carboxylic acids can be used.
[0014] Specific examples of the (poly)oxyalkylene derivative (A) include ethylene oxide adducts of butanol, ethylene oxide adducts of glycerol, ethylene oxide adducts of oleic acid, ethylene oxide adducts of laurylamine, ethylene oxide adducts of 3,5,5-trimethyl-1-hexanol, ethylene oxide adducts of stearyl alcohol, ethylene oxide adducts of lauric acid, ethylene oxide adducts of diethylenetriamine dioleamide, ethylene oxide adducts of diethyleneamine monolauramide, ethylene oxide adducts of sorbitan monooleate, ethylene oxide adducts of hydrogenated castor oil, and ethylene oxide-propylene oxide adducts of glycerol.
[0015] These (poly)oxyalkylene derivatives (A) may be used alone or in combination of two or more. In addition, as long as it is a compound containing a (poly)oxyalkylene, even if it contains an ester bond in the molecular skeleton, it is included in the (poly)oxyalkylene derivative (A).
[0016] The number average molecular weight of the (poly)oxyalkylene derivative (A) is preferably 500 or more and 1200 or less. If the number average molecular weight of the (poly)oxyalkylene derivative (A) is within the above numerical range, it is possible to appropriately suppress the situation where the carbon fiber sliver is wound around the roller of the drawing machine. Specifically, if the number average molecular weight of the (poly)oxyalkylene derivative (A) is 500 or more, the monofilaments of the carbon fiber are not easy to spread out from each other. Therefore, it is possible to suppress the monofilaments contained in the sliver from being wound around the roller. If the number average molecular weight of the (poly)oxyalkylene derivative (A) is 1200 or less, it is possible to suppress the adhesion of the surface of the sliver from becoming too high. Therefore, it is possible to suppress the entire sliver from being wound around the roller.
[0017] The method for measuring the number average molecular weight of the (poly)oxyalkylene derivative (A) is not particularly limited, and a known measurement method can be used. The method for measuring the number average molecular weight is as follows. The content ratio of the (poly)oxyalkylene derivative (A) in the treatment agent is not particularly limited, but is preferably 20% by mass or more and 60% by mass or less.
[0018] If the content ratio of the (poly)oxyalkylene derivative (A) in the treatment agent is within the above numerical range, short fibers can be prevented from falling off when the carbon fiber sliver is stretched using a drawing machine. Specifically, if the content ratio of the (poly)oxyalkylene derivative (A) in the treatment agent is 20% by mass or more, the bundling of the sliver is improved, so the monofilaments contained in the sliver are not easy to spread out. Therefore, the monofilaments contained in the sliver can be suppressed from falling off. If the content ratio of the (poly)oxyalkylene derivative (A) in the treatment agent is 60% by mass or less, the monofilaments contained in the sliver can be suppressed from excessively adhering to each other. Therefore, it is possible to suppress the situation where the monofilaments are excessively attached to each other and fall off in blocks.
[0019] It should be noted that the performance of preventing the short fibers from falling off is referred to as short fiber falling prevention property. (Ester compound (B)) The treatment agent preferably contains an ester compound (B).
[0020] The ester compound (B) is a compound having an ester bond in the molecular skeleton, which is formed by dehydration condensation between a compound having a carboxyl group and a compound having a hydroxyl group. Examples of the compound having a carboxyl group include carboxylic acids. Examples of the compound having a hydroxyl group include alcohols.
[0021] The carboxylic acid and alcohol may be monovalent or polyvalent. In addition, they may have a saturated hydrocarbon group or an unsaturated hydrocarbon group. In addition, they may have a branched chain or a straight chain. They may be a fully esterified compound in which the carboxylic acid and all the hydroxyl groups of the polyol are ester-bonded, or they may be a partially esterified compound in which the carboxylic acid and a part of the hydroxyl groups of the polyol are ester-bonded.
[0022] Specific examples of the ester compound (B) include oleic acid esters of alcohols having 12 to 13 carbon atoms, sorbitan monooleate, and hydrogenated castor oil. These ester compounds (B) may be used alone or in combination of two or more.
[0023] In addition, even if it is a compound containing an ester bond, the compound containing a (poly)oxyalkylene is not included in the ester compound (B) but is included in the (poly)oxyalkylene derivative (A).
[0024] The content ratio of the (poly)oxyalkylene derivative (A) and the ester compound (B) in the treatment agent is not particularly limited. In the treatment agent, when the total content ratio of the (poly)oxyalkylene derivative (A) and the ester compound (B) is set to 100 mass%, it is preferred that the (poly)oxyalkylene derivative (A) is contained in an amount of 30 mass% or more and 60 mass% or less. In addition, it is preferred that the ester compound (B) is contained in an amount of 40 mass% or more and 70 mass% or less.
[0025] By making the content ratio of the (poly)oxyalkylene derivative (A) and the above-mentioned ester compound (B) within the above-mentioned numerical range, when the sliver is stretched in the drawing machine, the cutting of the sliver can be appropriately suppressed. Specifically, if the ester compound (B) is 40% by mass or more, the monofilaments contained in the sliver are easy to slide against each other, so it is possible to suppress the monofilaments from being cut in blocks. If the ester compound (B) is 70% by mass or less, it is possible to suppress the monofilaments contained in the sliver from becoming too easy to slide against each other. Therefore, it is possible to suppress the monofilaments contained in the sliver from falling off.
[0026] In addition, the performance of being able to stretch the yarn while suppressing the cutting of the yarn is called drafting property. (Other ingredients (C)) The treatment agent may contain other components (C) in addition to the (poly)oxyalkylene derivative (A) and the ester compound (B). Examples of other components (C) include stabilizers for maintaining the quality of the treatment agent, charge control agents, antistatic agents, thickeners, antioxidants, ultraviolet absorbers, defoamers (silicone compounds), surfactants, smoothing agents, and other components commonly used in treatment agents.
[0027] It should be noted that the treatment agent is composed of non-volatile components. Non-volatile components refer to absolutely dry products after volatile diluents and the like are fully removed by heat treatment at 105°C for 2 hours. Therefore, water, organic solvents, and the like are not included in other components (C).
[0028] Specific examples of the other component (C) include a 40° C. kinematic viscosity of 9.5 (mm 2 / s) of mineral oil as a lubricant. The content of other components (C) in the treatment agent is not particularly limited, but is preferably 80% by mass or less, more preferably 60% by mass or less, further preferably 30% by mass or less, and most preferably 10% by mass or less.
[0029] <Second Embodiment> A second embodiment of the carbon fiber textile yarn of the present invention is described. The carbon fiber textile yarn of this embodiment is attached with the treatment agent of the first embodiment. The amount of the treatment agent (containing no solvent) of the first embodiment attached to the carbon fiber textile yarn is not particularly limited, but from the perspective of further improving the effect of the present invention, it is preferably attached at a ratio of 0.1% by mass or more and 10% by mass or less.
[0030] There is no particular limitation on the carbon fibers constituting the carbon fiber textile yarn, and examples thereof include PAN-based carbon fibers obtained using acrylic fibers as raw materials, asphalt-based carbon fibers obtained using asphalt as raw materials, recycled carbon fibers, polyester fibers, and carbon fibers obtained using polyethylene resins, phenol resins, cellulose resins, lignin resins, etc. as raw materials.
[0031] The length of the carbon fiber is not particularly limited, and may be short fibers of a length of less than 1 cm, also known as chopped fibers, or short fibers of a length of about 3 cm to 7 cm, also known as short fibers. In addition, it may be long fibers of a length of more than 10 cm, also known as filaments. When carbon fibers are recovered from carbon fiber cloth used in composite materials, a large amount of short fibers are included.
[0032] The method for manufacturing a carbon fiber textile yarn of the present embodiment has the following steps: an imparting step of imparting the treatment agent of the first embodiment to the carbon fiber; and a combing step of aligning the fiber direction of the carbon fiber that has undergone the imparting step to form a rope-shaped yarn. There is also a drawing step of gathering and stretching a plurality of yarn strips. The drawing step is performed by gathering a plurality of yarn strips into one yarn strip while conveying it using the rollers of a drawing frame and stretching it. There is further a spun step of stretching the yarn strip that has undergone the drawing step and winding it around a roving; a ring spinning step of stretching the roving and winding it around a worsted yarn; and a winding step of winding it into a package while adjusting the quality of the worsted yarn. By performing these steps in sequence, a carbon fiber textile yarn can be manufactured.
[0033] In the application step, the treatment agent of the first embodiment is applied to the carbon fibers by oiling them and making them adhere. As a method of applying oil, for example, an aqueous liquid containing the treatment agent of the first embodiment and water, or an aqueous solution obtained by further diluting the aqueous liquid, can be used, and a known oiling method can be applied. As a known oiling method, for example, an immersion method, a spray method, a roller method, a guided oiling method using a metering pump, etc. can be cited.
[0034] In addition, in preparation of an aqueous liquid, a well-known mechanical emulsification method using a homomixer, a homogenizer, etc. can be applied. The timing of performing the providing step is not particularly limited as long as it is before the drawing step.
[0035] The use of carbon fiber textile yarn is not particularly limited. For example, it can be used to make carbon fiber cloth and used in composite materials together with matrix resin. In addition, it can also be used for gas diffusion electrodes of fuel cells.
[0036] <Function and Effect> According to the treatment agent of the first embodiment and the carbon fiber spun yarn of the second embodiment, the following actions and effects can be obtained.
[0037] (1) The treatment agent contains a (poly)oxyalkylene derivative (A), and the number average molecular weight of the (poly)oxyalkylene derivative (A) is 30,000 or less. Therefore, when the carbon fiber is directly spun to produce a carbon fiber textile yarn, it is possible to suppress the carbon fiber yarn from being entangled with the rollers of the drawing frame. It is not necessary to stop the operation in order to remove the yarn entangled with the rollers of the drawing frame. Therefore, the carbon fiber can be directly spun to produce a carbon fiber textile yarn without reducing the operability.
[0038] (2) The treatment agent contains the (poly)oxyalkylene derivative (A) in a ratio of 20% by mass to 60% by mass. Therefore, when the carbon fiber yarn is stretched using a drawing machine, the short fibers can be properly prevented from falling off. In other words, the anti-falling property of the short fibers in the carbon fiber can be improved.
[0039] (3) The number average molecular weight of the (poly)oxyalkylene derivative (A) is 500 or more and 1200 or less. Therefore, it is possible to appropriately suppress the sliver of carbon fiber from being entangled with the rollers of the drawing frame.
[0040] (4) The treatment agent contains an ester compound (B), and when the total content ratio of the (poly)oxyalkylene derivative (A) and the ester compound (B) is set to 100 mass%, the (poly)oxyalkylene derivative (A) is contained in an amount of 30 mass% to 60 mass%. In addition, the ester compound (B) is contained in an amount of 40 mass% to 70 mass%. Therefore, when the sliver in the drawing machine is stretched, the cutting of the sliver can be appropriately suppressed. In other words, the drafting property can be improved.
[0041] (5) Carbon fiber textile yarn is produced by directly spinning carbon fiber. Therefore, carbon fiber cloth can be simply produced by only weaving carbon fiber textile yarn. In the prior art, carbon fiber cloth is produced by carbonizing flame-resistant cloth made of flame-resistant fiber, so that relatively large dimensional changes occur during carbonization. In contrast, according to the carbon fiber textile yarn of the present invention, carbon fiber cloth can be produced without carbonization, so the dimensional change is relatively reduced. Therefore, the dimensional accuracy of the carbon fiber cloth can be improved.
[0042] (6) The recycled carbon fiber can be used as a raw material for carbon fiber textile yarn. This can effectively utilize resources and eliminate the need to carbonize synthetic fibers to produce carbon fiber, which helps reduce costs. Example
[0043] In order to more specifically describe the configuration and effects of the present invention, examples and the like are given below, but the present invention is not limited to these examples. It should be noted that in the description of the following examples and comparative examples, % means mass %.
[0044] Test group 1 (preparation of treatment agent) (Example 1) The (poly)oxyalkylene derivative (A-1) and the ester compound (B-1) shown in Table 1 were weighed so as to be 60% by mass and 40% by mass, and added to a container. These were stirred and uniformly mixed at a temperature of about 80°C to prepare a treatment agent. Further, 20°C water was added to the container while being stirred and uniformly mixed. Thereafter, emulsification was performed using a homogenizer to prepare a 20% aqueous solution of the treatment agent.
[0045] (Examples 2 to 33 and Comparative Examples 1 to 3) The treatment agents of Examples 2 to 33 and Comparative Examples 1 to 3 were prepared by the same method as in Example 1 using the components shown in Table 1.
[0046] The (poly)oxyalkylene derivative (A) and the ester compound (B) in the treatment agent of each example are shown in the "(poly)oxyalkylene derivative (A)" column and the "ester compound (B)" column of Table 1, respectively. The type and content ratio of other components (C) are shown in the "other components (C)" column of Table 1.
[0047] When the total content of the (poly)oxyalkylene derivative (A) and the ester compound (B) is 100 mass %, the content of the (poly)oxyalkylene derivative (A) is shown in the column "(A) / ((A)+(B))".
[0048] [Table 1]
[0049] The details of each component A-1 to A-15, a-16, B-1 to B-3, and C-1 described in the category column of Table 1 are as follows. ((Poly)oxyalkylene derivative (A)) The type and number average molecular weight of the (poly)oxyalkylene derivative (A) are shown in the "Compound Name" column and the "Number Average Molecular Weight" column in Table 2, respectively.
[0050] [Table 2] type Compound Name Number average molecular weight A-1 Butanol ethylene oxide adduct 1178 A-2 Glycerol ethylene oxide adduct 972 A-3 Oleic acid ethylene oxide adduct 895 A-4 Laurylamine ethylene oxide adduct 1065 A-5 3,5,5-Trimethyl-1-hexanol ethylene oxide adduct 738 A-6 Ethylene oxide adduct of stearyl alcohol 787 A-7 Lauric acid ethylene oxide adduct 1132 A-8 Ethylene oxide adduct of diethylenetriamine dioleamide 1158 A-9 Diethyleneamine monolauroamide ethylene oxide adduct 1015 A-10 Sorbitan monooleate ethylene oxide adduct 1000 A-11 Hydrogenated castor oil ethylene oxide adduct 1196 A-12 Butanol ethylene oxide adduct 3800 A-13 Butanol ethylene oxide adduct 2300 A-14 Butanol ethylene oxide adduct 474 A-15 Glycerol ethylene oxide propylene oxide adduct 24192 a-16 Glycerol ethylene oxide propylene oxide adduct 39492
[0051] The number average molecular weight (Mn) of the (poly)oxyalkylene derivative (A) is measured by the GPC method under the following measurement conditions. Device: HLC-8320GPC manufactured by Tosoh Corporation Column: TSK gel Super H4000 :TSK gel Super H3000 :TSK gel Super H2000 (both manufactured by Tosoh Corporation) Column temperature: 40°C Detection device: Differential refractive index detector Sample solution: 0.25 mass% tetrahydrofuran solution Solution flow rate: 0.5mL / min Solution injection volume: 10μL Standard sample: Polystyrene (TSK STANDARD POLYSTYRENE manufactured by Tosoh Corporation) A calibration curve is prepared using standard samples to determine the number average molecular weight (Mn) of the (poly)oxyalkylene derivative (A).
[0052] (Ester compound (B)) B-1: Oleic acid ester of alcohol having 12 to 13 carbon atoms B-2: Sorbitan monooleate B-3: Hydrogenated castor oil (Other ingredients (C)) C-1: Kinematic viscosity at 40°C is 9.5 (mm 2 / s) mineral oil Test Group 2 (Manufacture of Carbon Fiber Textile Yarn) Using the treating agent prepared in Test Group 1, carbon fiber textile yarn was produced.
[0053] As the carbon fiber, staple fibers with an average length of 50 mm obtained from a composite material in the form of recycled materials were used. For the carbon fiber, as an imparting process, the 20% aqueous solution of the treatment agent prepared in test group 1 was further diluted to make a 0.4% aqueous solution, and it was attached by spraying. The amount of the treatment agent attached to the solid content of the short fiber was 0.4% by mass (without solvent). The carbon fiber attached with the treatment agent was dried in a hot air dryer at 80°C for 1 hour.
[0054] Next, the carbon fiber that has undergone the imparting step is subjected to a carding step, a drawing step, a spun spinning step, a ring spinning step, and a winding step in order to produce a carbon fiber spun yarn. In the drawing step, two slivers are combined using a drawing frame and stretched to 3.9 times.
[0055] Test Group 3 (Evaluation) For each treatment agent described in Examples 1 to 33 and Comparative Examples 1 to 3, the anti-rolling property, drafting property, and anti-short fiber falling property were evaluated as evaluation items for processability when manufacturing carbon fiber textile yarns. The process of each test is as follows. In addition, the evaluation results based on each test are shown in the "Anti-rolling Property" column, "Drafting Property" column, and "Anti-short fiber falling property" column of Table 1, respectively.
[0056] (Anti-rolling property) In the drawing process of test group 2, visual observation was made to see whether the yarn was wrapped around the roller of the drawing machine. The time from the start of drawing to the winding of the yarn around the roller of the drawing machine was measured and evaluated according to the following evaluation criteria. It should be noted that the winding of the yarn includes two methods: the method in which the entire yarn is wound around the roller, and the method in which the monofilament contained in the yarn is wound around the roller.
[0057] · Evaluation criteria for anti-rolling performance ◎ (good): The yarn is not wound around the roller even after 10 minutes from the start of drawing. ○ (Pass): The yarn is wound around the roller within more than 5 minutes and within 10 minutes. × (failed): The yarn was entangled with the roller within 5 minutes. (Stretchability) The tensile strength elongation test was performed using the yarn produced in the combing process of test group 2. The conditions of the tensile strength elongation test were as follows: the clamping length of the yarn was 10 cm, the stretching speed was 10 cm / min and the yarn was stretched for 1 minute. The time until the yarn bundle constituting the yarn was cut was measured and evaluated according to the following evaluation criteria. It should be noted that the cutting of the yarn bundle constituting the yarn includes two methods: the monofilaments contained in the yarn are cut into blocks, and the monofilaments contained in the yarn fall off.
[0058] ·Evaluation criteria for draftability ◎ (Good): The yarn bundle was not cut during the 1-minute stretching. ○ (Pass): The time until the tow was cut was 50 seconds or more and less than 1 minute. × (failure): The time until the tow was cut was less than 50 seconds. (Preventing short fibers from falling off) In the drawing process of test group 2, after 10 minutes from the start of drawing, visually observe whether there is any falling of short fibers in the drawing frame. In addition, as a comparative test, the carbon fiber used in test group 2 was used, and the imparting process was omitted, and the drawing process was carried out without attaching a treatment agent. Visually observe whether there is any falling of short fibers after 10 minutes from the start of drawing, and evaluate according to the following evaluation criteria. It should be noted that the falling of short fibers includes two ways: the monofilaments contained in the yarn are scattered and fall off, and the monofilaments fall off in blocks.
[0059] Evaluation criteria for preventing short fiber shedding ◎ (Good): No short fibers are falling off ○ (Pass): Although a small amount of short fibers fell off, the amount was less than that in the comparative test. × (failed): A large amount of short fibers fell off, which was equal to or more than that in the comparative test. According to Table 1, in the treatment agent of Comparative Example 1, the number average molecular weight of the (poly)oxyalkylene derivative (A) exceeded 30,000, and thus the anti-rolling property was unacceptable.
[0060] The treatment agent of Comparative Example 2 did not contain the (poly)oxyalkylene derivative (A), and the content of the ester compound (B) was 100 mass %. Therefore, the anti-rolling property, drafting property, and short fiber falling prevention property were all unacceptable.
[0061] In Comparative Example 3, since the treatment agent itself was not used, the anti-rolling property and the short fiber falling-off prevention property were unacceptable. In addition, since the tow was very easily cut, the drafting property could not be evaluated.
[0062] On the other hand, in the treatment agents of Examples 1 to 33, the roll-wrapping prevention property, drafting property, and short fiber-falling prevention property were all acceptable or good. According to the treatment agent of the present invention, it is possible to suppress the sliver of carbon fiber from being entangled with the rollers of the drawing frame, and to suppress the sliver from being cut and the falling of short fibers when the sliver is stretched in the drawing frame.
Claims
1. A treatment agent for manufacturing carbon fiber textile yarn, characterized in that: It contains a (poly)oxyalkylene derivative (A) having a number average molecular weight of 30,000 or less.
2. The treating agent for producing carbon fiber textile yarn according to claim 1, wherein The (poly)oxyalkylene derivative (A) is contained in a ratio of 20 mass % or more and 60 mass % or less.
3. The treating agent for producing carbon fiber textile yarn according to claim 1, wherein The number average molecular weight of the (poly)oxyalkylene derivative (A) is 500 or more and 1200 or less.
4. The treating agent for producing carbon fiber textile yarn according to claim 1, wherein The treatment agent further contains an ester compound (B), When the total content ratio of the (poly)oxyalkylene derivative (A) and the ester compound (B) is 100 mass %, the (poly)oxyalkylene derivative (A) is contained in a ratio of 30 mass % to 60 mass %, and the ester compound (B) is contained in a ratio of 40 mass % to 70 mass %.
5. A carbon fiber textile yarn, characterized in that: The treating agent for producing a carbon fiber spun yarn according to any one of claims 1 to 4 is adhered thereto.
Citation Information
Patent Citations
JP1973033193A
Method of spinning carbon fiber
JP1978031828A
Fire-resistant spun yarn and method for producing the same
JP2004124309A
Manufacturing method of synthetic fiber treatment agent, synthetic fiber treatment agent, synthetic fiber, and manufacturing method of synthetic fiber
JP6795238B1
Treatment agent for synthetic fibers, and synthetic fibers
JP6844881B1