Polishing composition
By using silica particles, alkaline compounds and specific water-soluble polymer compositions in the grinding composition, the problem of difficult to balance the grinding rate and surface quality in the prior art is solved, and efficient silicon wafer surface grinding is achieved .
Patent Information
- Application Number
- CN202380028802.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-23
- Filing Date
- 2023-03-08
- Publication Date
- 2024-11-19
AI Technical Summary
While the existing grinding composition improves the surface quality of semiconductor substrates such as silicon wafers, it is difficult to take into account both high processing force and grinding rate, resulting in a reduction in manufacturing efficiency and cost-effectiveness.
By optimizing their content ratio and molecular weight, by optimizing their content ratio and molecular weight, the compositions containing silica particles, alkali compounds and specific three water-soluble polymers (cellulose derivatives, polyvinyl alcohol-based polymers, and polymers containing nitrogen atoms, Balance the grinding rate and surface quality.
It achieves a balance between high-quality surface grinding surfaces and improving grinding rate, improving manufacturing efficiency and cost-effectiveness.
Smart Images

Figure BDA0005050980120000121 
Figure BDA0005050980120000401
Abstract
Description
Technical Field
[0001] The present invention relates to a polishing composition. This application claims priority based on Japanese Patent Application No. 2022-047438 filed on March 23, 2022, the entire contents of which are incorporated herein by reference. Background Art
[0002] The surface of a material such as a metal or semi-metal, non-metal, or its oxide is precisely ground using a grinding composition. For example, the surface of a silicon wafer used as a component of a semiconductor device is generally processed into a high-quality mirror surface through a grinding process (rough grinding process) and a polishing process (precision grinding process). The above-mentioned polishing process typically includes a pre-polishing process (pre-grinding process) and a fine polishing process (final grinding process). Regarding technical documents on grinding compositions mainly used in the use of semiconductor substrates such as grinding silicon wafers, Patent Documents 1 to 5 can be cited.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent No. 5897200
[0006] Patent Document 2: Japanese Patent No. 6037416
[0007] Patent Document 3: Japanese Patent No. 6185432
[0008] Patent Document 4: Japanese Patent No. 6232243
[0009] Patent Document 5: Japanese Patent Application Publication No. 2020-13824 Summary of the invention
[0010] Problem that the invention aims to solve
[0011] In the grinding composition, a composition with a grinding ability that can efficiently grind the grinding object can be used. For example, when grinding substrates such as semiconductor substrates of the above-mentioned silicon wafer, the mechanical grinding effect produced by abrasive particles and the chemical grinding effect (alkali etching) produced by alkaline compounds can be utilized, and through these effects, high processing power can be exerted. The grinding composition with high processing power can improve manufacturing efficiency and cost-effectiveness, which is preferred. In this grinding process, by using silicon dioxide particles as abrasive particles, a grinding surface with good quality can be efficiently achieved.
[0012] In addition, in the polishing composition used for the polishing of the above-mentioned substrate, for example, the polishing composition used in the fine polishing process (especially the fine polishing process of semiconductor substrates such as silicon wafers and other substrates) is required to achieve the performance of high-quality surface after polishing. The improvement of the surface quality of the polished surface can be achieved by making the polishing composition contain a water-soluble polymer and using the above-mentioned water-soluble polymer to protect the substrate. For example, patent documents 1 to 5 disclose a polishing composition, which contains silica particles, an alkaline compound and a water-soluble polymer. By using the above-mentioned water-soluble polymer, it is possible to inhibit excessive alkali etching of the surface of the polished object and prevent the roughness of the polished surface, but on the other hand, due to the above-mentioned alkali etching inhibition, it sometimes leads to a decrease in processing force and even a decrease in manufacturing efficiency. Patent documents 1 to 5 have an evaluation of the surface quality (haze, defects) of the polishing composition containing the above-mentioned water-soluble polymer, but there is no discussion on the processing force. In general, the improvement of the quality of the polished surface is in a trade-off relationship with the polishing rate. If a polishing composition that can take both into account at a high level can be achieved, it is practically beneficial, for example, it is particularly beneficial in the fine polishing process.
[0013] Based on the above background, the present inventors conducted intensive research and found that by selecting and using three specific water-soluble polymers, it is possible to achieve a higher level of both surface quality and polishing rate than when two water-soluble polymers are used in combination, thereby completing the present invention. That is, the object of the present invention is to provide a polishing composition that can obtain high surface quality and improve the polishing rate by selecting three specific water-soluble polymers.
[0014] Solutions for solving problems
[0015] According to the present specification, a polishing composition is provided, which comprises: silica particles as abrasive particles, an alkaline compound, water, a cellulose derivative as a first water-soluble polymer, a polyvinyl alcohol-based polymer as a second water-soluble polymer, and a polymer containing a nitrogen atom as a third water-soluble polymer. In the polishing composition, the ratio of the content C1 of the first water-soluble polymer to the total content of the content C2 of the second water-soluble polymer and the content C3 of the third water-soluble polymer, i.e., C1 / (C2+C3), is 0.1 or more. In the polishing composition comprising silica particles, an alkaline compound and water, by selecting the above-mentioned three specific water-soluble polymers and blending them in a well-balanced manner, a high surface quality can be obtained and a polishing rate can be increased.
[0016] In some embodiments, the ratio of the third water-soluble polymer content C3 to the second water-soluble polymer content C2, i.e., C3 / C2, is 0.05 or more and less than 5. With this composition, the effects of the technology disclosed herein can be preferably achieved.
[0017] In some embodiments, the ratio of the content C3 of the third water-soluble polymer to the total content of the content C1 of the first water-soluble polymer and the content C2 of the second water-soluble polymer, i.e., C3 / (C1+C2), is 0.18 or more and less than 10. According to this composition, the effects of the technology disclosed herein can be preferably achieved.
[0018] In some embodiments, the average aspect ratio of the silicon dioxide particles is greater than or equal to 1.0 and less than or equal to 3.0. By using silicon dioxide particles having the above average aspect ratio, it is easy to balance the polishing rate and the surface quality.
[0019] In some embodiments, the weight average molecular weight (Mw) of the third water-soluble polymer is 50,000 or more. By using a third water-soluble polymer having an Mw of a predetermined value or more, a haze improvement effect tends to be easily obtained.
[0020] In some embodiments, the third water-soluble polymer is an acryloylmorpholine polymer. According to the polishing composition containing the acryloylmorpholine polymer as the third water-soluble polymer, a high-quality polished surface can be easily obtained.
[0021] In some preferred embodiments, the content C1 of the first water-soluble polymer, the content C2 of the second water-soluble polymer, and the content C3 of the third water-soluble polymer satisfy the following relationship on a weight basis: C1<(C2+C3). By limiting the amount of the cellulose derivative used as the first water-soluble polymer relative to the second and third water-soluble polymers, it is easy to achieve both an increase in polishing rate and a decrease in haze.
[0022] The polishing composition disclosed herein is preferably used for polishing a surface formed of a silicon material. By polishing a surface formed of a silicon material using the polishing composition, a high-quality surface composed of a silicon material can be efficiently achieved.
[0023] The polishing composition disclosed herein may be a concentrated liquid. The polishing composition disclosed herein may be produced, distributed, and stored in the form of a concentrated liquid. DETAILED DESCRIPTION
[0024] The following describes a suitable embodiment of the present invention. It should be noted that in this specification, matters other than those specifically mentioned and necessary for implementing the present invention can be grasped by conventional technical means of those skilled in the art based on the prior art in this field. The present invention can be implemented according to the contents disclosed in this specification and the technical common sense in this field.
[0025] <Abrasive Grains>
[0026] The grinding composition disclosed herein contains silica particles as abrasive particles. The silica particles as abrasive particles play a role in mechanically grinding the surface of the grinding object. By making the grinding composition contain abrasive particles, the grinding rate can be increased based on the mechanical grinding effect caused by the abrasive particles. In addition, in the grinding composition that can be used for grinding (e.g., fine polishing) of a grinding object having a surface formed of silicon, such as a silicon wafer described later, it is particularly meaningful to use silica particles as abrasive particles.
[0027] As specific examples of silica particles, colloidal silica, fumed silica, precipitated silica, etc. can be cited. The silica particles can be used alone or in combination of two or more. From the viewpoint of easily obtaining a polished surface with excellent surface quality after grinding, the use of colloidal silica is particularly preferred. As colloidal silica, for example, colloidal silica made from water glass (sodium silicate) as a raw material by an ion exchange method and alkoxide method colloidal silica (colloidal silica manufactured by a hydrolysis condensation reaction of alkoxysilane) can be preferably used. Colloidal silica can be used alone or in combination of two or more.
[0028] The true specific gravity of the silicon dioxide constituting the silicon dioxide particles is preferably 1.5 or more, more preferably 1.6 or more, and further preferably 1.7 or more. The upper limit of the true specific gravity of silicon dioxide is not particularly limited, and is typically 2.3 or less, for example, 2.2 or less. The true specific gravity of the silicon dioxide particles can be a measured value obtained by a liquid substitution method using ethanol as a substitution liquid.
[0029] The average primary particle size of the abrasive (typically silica particles) is not particularly limited, and from the viewpoint of the grinding rate, it is preferably 5 nm or more, more preferably 10 nm or more. From the viewpoint of obtaining a higher grinding effect (such as a reduction in haze, removal of defects, etc.), the above average primary particle size is preferably 15 nm or more, more preferably 20 nm or more (for example, more than 20 nm). In addition, from the viewpoint of preventing scratches, the average primary particle size of the abrasive is preferably 100 nm or less, more preferably 50 nm or less, and further preferably 45 nm or less. From the viewpoint of easily obtaining a surface with lower haze, in some embodiments, the average primary particle size of the abrasive can be 43 nm or less, less than 40 nm, less than 38 nm, less than 35 nm, less than 32 nm, or less than 30 nm.
[0030] It should be noted that in this specification, the average primary particle size refers to the specific surface area (BET value) measured by the BET method, and is calculated according to the formula: average primary particle size (nm) = 6000 / (true density (g / cm 3 )×BET value (m 2 The above-mentioned specific surface area can be measured using, for example, a surface area measuring device manufactured by Micromeritics, trade name "Flow Sorb II 2300".
[0031] The average secondary particle size of the abrasive (typically silica particles) is not particularly limited, and can be appropriately selected from a range of about 15 nm to 300 nm, for example. From the viewpoint of increasing the grinding rate, the average secondary particle size is preferably greater than 30 nm, and more preferably greater than 35 nm. In some embodiments, the average secondary particle size can be, for example, greater than 40 nm, or greater than 42 nm, and preferably greater than 44 nm. In addition, it is generally advantageous for the average secondary particle size to be less than 250 nm, preferably less than 200 nm, and more preferably less than 150 nm. In some preferred embodiments, the average secondary particle size is less than 120 nm, more preferably less than 100 nm, and further preferably less than 70 nm, and can be, for example, less than 60 nm, or less than 50 nm.
[0032] In this specification, the average secondary particle size refers to the particle size (volume average particle size) measured by a dynamic light scattering method. The average secondary particle size of the abrasive can be measured by a dynamic light scattering method using, for example, Nanotrac UPA-UT151 manufactured by Nikkiso Co., Ltd.
[0033] The shape (outer shape) of the silica particles may be spherical or non-spherical. Specific examples of non-spherical particles include peanut-shaped (i.e., the shape of peanut shells), cocoon-shaped, candy-shaped, rugby-shaped, etc. For example, silica particles having mostly peanut-shaped or cocoon-shaped particles are preferably used.
[0034] Although not particularly limited, the average value (average aspect ratio) of the major diameter / minor diameter ratio of the silica particles is in principle 1.0 or more, preferably 1.05 or more, more preferably 1.1 or more, and can be 1.2 or more. With the increase of the average aspect ratio, a higher polishing rate can be achieved. In addition, from the viewpoint of reducing scratches, the average aspect ratio of the silica particles is preferably 3.0 or less, more preferably 2.0 or less, more preferably 1.5 or less, and can be 1.4 or less.
[0035] The shape (outer shape) and average aspect ratio of silica particles can be grasped, for example, by electron microscope observation. As a specific step to grasp the average aspect ratio, for example, a scanning electron microscope (SEM) is used to draw the smallest rectangle circumscribed to each particle image for a specified number (e.g., 200) of silica particles with identifiable independent particle shapes. Then, for the rectangle drawn for each particle image, the value obtained by dividing the length of its long side (the value of the long diameter) by the length of the short side (the value of the short diameter) is calculated and used as the long diameter / short diameter ratio (aspect ratio). The average aspect ratio can be calculated by arithmetically averaging the aspect ratios of the above-mentioned specified number of particles.
[0036] The polishing composition disclosed herein may also contain abrasives other than silica particles (hereinafter also referred to as "non-silica abrasives") within a range that does not significantly hinder the effect of the present invention. Examples of non-silica abrasives include inorganic particles, organic particles, and organic-inorganic composite particles. Specific examples of inorganic particles include: oxide particles such as aluminum oxide particles, cerium oxide particles, chromium oxide particles, titanium dioxide particles, zirconium oxide particles, magnesium oxide particles, manganese dioxide particles, zinc oxide particles, and iron red particles; nitride particles such as silicon nitride particles and boron nitride particles; carbide particles such as silicon carbide particles and boron carbide particles; diamond particles; carbonates such as calcium carbonate and barium carbonate, etc. Specific examples of organic particles include polymethyl methacrylate (PMMA) particles, poly(meth)acrylic acid particles (here (meth)acrylic acid refers to acrylic acid and methacrylic acid), polyacrylonitrile particles, etc. Such abrasives can be used alone or in combination of two or more.
[0037] The technology disclosed herein can be preferably implemented in an embodiment using only silica particles as abrasive particles. From such a viewpoint, it is appropriate that the proportion of silica particles in the total amount of abrasive particles is 90% by weight or more, preferably 95% by weight or more, and more preferably 98% by weight or more (e.g., 99 to 100% by weight).
[0038] <Basic Compounds>
[0039] The grinding composition disclosed herein contains a basic compound. In this specification, a basic compound refers to a compound having a function of being dissolved in water and raising the pH of an aqueous solution. By making the grinding composition contain a basic compound, the grinding object can be efficiently ground by its chemical grinding action (alkali etching). As the basic compound, nitrogen-containing organic or inorganic basic compounds, phosphorus-containing basic compounds, hydroxides of alkali metals, hydroxides of alkaline earth metals, various carbonates, bicarbonates, etc. can be used. As examples of nitrogen-containing basic compounds, quaternary ammonium compounds, ammonia, amines (preferably water-soluble amines) and the like can be listed. As examples of phosphorus-containing basic compounds, quaternary phosphonium compounds can be listed. Such basic compounds can be used alone or in combination of two or more.
[0040] As specific examples of alkali metal hydroxides, potassium hydroxide, sodium hydroxide, etc. can be listed. As specific examples of carbonates or bicarbonates, ammonium bicarbonate, ammonium carbonate, potassium bicarbonate, potassium carbonate, sodium bicarbonate, sodium carbonate, etc. can be listed. As specific examples of amines, methylamine, dimethylamine, trimethylamine, ethylamine, diethylamine, triethylamine, ethylenediamine, monoethanolamine, N-(β-aminoethyl)ethanolamine, hexamethylenediamine, diethylenetriamine, triethylenetetramine, anhydrous piperazine, piperazine hexahydrate, 1-(2-aminoethyl)piperazine, N-methylpiperazine, guanidine, imidazole, triazole and other azoles can be listed. As specific examples of quaternary phosphonium compounds, quaternary phosphonium hydroxides such as tetramethylphosphonium hydroxide and tetraethylphosphonium hydroxide can be listed.
[0041] As the quaternary ammonium compound, a quaternary ammonium salt (typically a strong base) such as a tetraalkylammonium salt or a hydroxyalkyltrialkylammonium salt can be used. The anion component in the quaternary ammonium salt can be, for example, OH - 、F - , Cl - Br - ,I - 、ClO4 - 、BH4 - As examples of the above-mentioned quaternary ammonium compounds, there are exemplified those in which the anion is OH -The quaternary ammonium salt is a quaternary ammonium hydroxide. Specific examples of quaternary ammonium hydroxides include tetraalkylammonium hydroxides such as tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, tetrapentylammonium hydroxide, and tetrahexylammonium hydroxide; and hydroxyalkyltrialkylammonium hydroxides such as 2-hydroxyethyltrimethylammonium hydroxide (also called choline).
[0042] Among these basic compounds, at least one basic compound selected from, for example, alkali metal hydroxides, quaternary ammonium hydroxides, and ammonia can be preferably used. In particular, tetraalkylammonium hydroxides (such as tetramethylammonium hydroxide) and ammonia are more preferred, and ammonia is particularly preferred.
[0043] <Water-soluble polymer>
[0044] The polishing composition disclosed herein is characterized by containing three specific water-soluble polymers as water-soluble polymers. Specifically, the polishing composition contains a cellulose derivative as the first water-soluble polymer, a polyvinyl alcohol-based polymer as the second water-soluble polymer, and a polymer containing a nitrogen atom as the third water-soluble polymer. By selecting and using the above three specific water-soluble polymers, a high surface quality produced by using the above water-soluble polymers can be obtained, and the polishing rate can be increased. The improvement of the polishing rate can be achieved by selecting the above three water-soluble polymers.
[0045] The first water-soluble polymer, the second water-soluble polymer, and the third water-soluble polymer are described in detail below.
[0046] <First water-soluble polymer>
[0047] The polishing composition disclosed herein comprises a cellulose derivative as the first water-soluble polymer. The cellulose derivative is a polymer comprising a β-glucose unit as a main repeating unit and has a structure derived from cellulose. By using a cellulose derivative, a higher polishing rate can be maintained and a high surface quality can be obtained. Although not particularly restrictive, it is believed that the cellulose derivative acts on both the silica particles and the substrate (e.g., silicon wafer) to appropriately protect the substrate surface. In addition, by using a cellulose derivative in combination with a polyvinyl alcohol-based polymer described later, there is a tendency to obtain a substrate protection effect based on a water-soluble polymer and increase the polishing rate.
[0048] Specific examples of cellulose derivatives include hydroxyethyl cellulose (HEC), hydroxypropyl cellulose, hydroxyethyl methyl cellulose, hydroxypropyl methyl cellulose, methyl cellulose, ethyl cellulose, ethyl hydroxyethyl cellulose, carboxymethyl cellulose, etc. In particular, HEC is preferred. Cellulose derivatives may be used alone or in combination of two or more.
[0049] The weight average molecular weight (Mw) of the cellulose derivative can be set to about 200×10 4 Below, 150×10 4 The following are suitable. The above Mw can be approximately 100×10 4 Below, it can be about 50×10 4 Less than (e.g., approximately less than 50×10 4 ), can be approximately 40×10 4 Below, it can also be about 30×10 4 Less than (e.g. less than 30×10 4 ). By using a cellulose derivative having a moderately limited Mw, there is a tendency to easily obtain good surface quality. In addition, from the perspective of the protection of the polished surface, the above Mw is, for example, about 0.2×10 4 Above, about 0.5×10 4 The above is appropriate, preferably about 1.0×10 4 More preferably, about 3.0×10 4 More than 10×10 4 Above, it can also be about 20×10 4 above.
[0050] As the Mw of the water-soluble polymer, the molecular weight calculated by the value (water system, polyethylene oxide conversion) measured by the aqueous gel permeation chromatography (GPC) can be used. The same is true for the Mw of the first water-soluble polymer, the second water-soluble polymer described later, and the third water-soluble polymer. As a GPC measuring device, the model name "HLC-8320GPC" made by Tosoh Corporation can be used. The measurement can be carried out, for example, according to the following conditions. The same method can also be used for the embodiments described later.
[0051] [GPC measurement conditions]
[0052] Sample concentration: 0.1 wt%
[0053] Column: TSKgel GMPW XL
[0054] Detector: Differential Refractometer
[0055] Eluent: 100 mM sodium nitrate aqueous solution / acetonitrile = 10-8 / 0-2
[0056] Flow rate: 1mL / min
[0057] Measuring temperature: 40℃
[0058] Sample injection volume: 200 μL
[0059] Although not particularly limited, in some embodiments, the content of the first water-soluble polymer (specifically, a cellulose derivative) in the polishing composition can be set to, for example, 0.01 parts by weight or more, and it is appropriate to set it to 0.05 parts by weight or more relative to 100 parts by weight of abrasive (typically, silica particles). In some preferred embodiments, from the viewpoint of better exerting the effect of the use of the first water-soluble polymer (such as the haze reduction effect), the above content is 0.1 parts by weight or more, more preferably 0.3 parts by weight or more, and further preferably 0.5 parts by weight or more, and can be 1 part by weight or more, 2 parts by weight or more, or 3 parts by weight or more. In addition, regarding the content of the first water-soluble polymer relative to 100 parts by weight of abrasive, in some embodiments, it can be, for example, 30 parts by weight or less, or 15 parts by weight or less. By limiting the amount of the first water-soluble polymer (specifically, a cellulose derivative) used, the polishing composition can easily obtain good filterability and dispersion stability. In some preferred embodiments, from the viewpoint of improving the polishing rate, the content of the first water-soluble polymer relative to 100 parts by weight of the abrasive is 10 parts by weight or less, more preferably 8 parts by weight or less, further preferably 6 parts by weight or less, 5 parts by weight or less, or 4 parts by weight or less (e.g., 3 parts by weight or less). According to the technology disclosed herein, by appropriately controlling the content of the cellulose derivative used as the water-soluble polymer, it is possible to maintain high surface quality while improving the polishing rate.
[0060] <Second water-soluble polymer>
[0061] The grinding composition disclosed herein comprises a polyvinyl alcohol polymer as the second water-soluble polymer. According to the grinding composition comprising the polyvinyl alcohol polymer, a high-quality grinding surface is easily obtained. Although not particularly restrictive, it is believed that the polyvinyl alcohol polymer protects the substrate surface by acting on the substrate surface, and contributes to improving the grinding surface quality (specifically, reducing the haze) by a different effect from the effect of the first water-soluble polymer. By using the polyvinyl alcohol polymer as the second water-soluble polymer in combination with the first and third water-soluble polymers, the grinding rate can be increased according to the different effects of each water-soluble polymer, and a high surface quality can be effectively achieved.
[0062] In this specification, a polyvinyl alcohol polymer refers to a polymer containing a vinyl alcohol unit (hereinafter also referred to as a "VA unit") as its repeating unit. The polyvinyl alcohol polymer may be used alone or in combination of two or more. The polyvinyl alcohol polymer may contain only VA units as repeating units, or may contain repeating units other than VA units (hereinafter also referred to as "non-VA units") in addition to VA units. The polyvinyl alcohol polymer may be a random copolymer containing VA units and non-VA units, a block copolymer, an alternating copolymer, or a graft copolymer. The polyvinyl alcohol polymer may contain only one non-VA unit, or may contain two or more non-VA units.
[0063] The above-mentioned polyvinyl alcohol-based polymer can be unmodified polyvinyl alcohol (unmodified PVA) or modified polyvinyl alcohol (modified PVA). The unmodified PVA here refers to a polyvinyl alcohol-based polymer produced by hydrolyzing (saponifying) polyvinyl acetate, which does not substantially contain repeating units (-CH2-CH(OCOCH3)-) of a structure formed by vinyl polymerization of vinyl acetate and repeating units other than VA units. The saponification degree of the above-mentioned unmodified PVA can be, for example, 60% or more, and from the viewpoint of water solubility, it can be 70% or more, 80% or more, or 90% or more. In some embodiments, the saponification degree of the unmodified PVA can be 98% or more (completely saponified).
[0064] The polyvinyl alcohol polymer can be a modified PVA comprising a VA unit and a non-VA unit, wherein the non-VA unit has at least one structure selected from an oxyalkylene group, a carboxyl group, a (di) carboxyl group, a (di) carboxyl ester group, a phenyl group, a naphthyl group, a sulfonic acid group, an amino group, a hydroxyl group, an amide group, an imide group, a nitrile group, an ether group, an ester group and their salts. In addition, as a non-VA unit that can be included in the modified PVA, it can be, for example, a repeating unit derived from an N-vinyl monomer, an N-(methyl)acryloyl monomer, a repeating unit derived from ethylene, a repeating unit derived from an alkyl vinyl ether, a repeating unit derived from a vinyl ester of a monocarboxylic acid having more than 3 carbon atoms, a repeating unit derived from a (di) acetone compound, etc., but is not limited thereto. As a suitable example of the above-mentioned N-vinyl monomer, N-vinyl pyrrolidone can be cited. As a suitable example of the above-mentioned N-(methyl)acryloyl monomer, N-(methyl)acryloyl morpholine can be cited. The alkyl vinyl ether may be, for example, a vinyl ether having an alkyl group having 1 to 10 carbon atoms, such as propyl vinyl ether, butyl vinyl ether, and 2-ethylhexyl vinyl ether. The vinyl ester of a monocarboxylic acid having 3 or more carbon atoms may be, for example, a vinyl ester of a monocarboxylic acid having 3 to 7 carbon atoms, such as vinyl propionate, vinyl butyrate, vinyl valerate, and vinyl hexanoate. Suitable examples of the (di)acetone compound include diacetone (meth)acrylamide and acetylacetone.
[0065] In addition, in some preferred embodiments, an acetalized polyvinyl alcohol polymer can be used as the polyvinyl alcohol polymer. As the acetalized polyvinyl alcohol polymer, for example, a modified PVA in which a part of the VA units contained in the polyvinyl alcohol polymer is acetalized can be cited. The modified PVA in which a part of the VA units contained in the above-mentioned polyvinyl alcohol polymer is acetalized (acetalized PVA (ac-PVA)) can be obtained by reacting a part of the hydroxyl groups of the polyvinyl alcohol polymer with an aldehyde compound or a ketone compound for acetalization. Typically, the acetalized polyvinyl alcohol polymer can be obtained by an acetalization reaction of a polyvinyl alcohol polymer with an aldehyde compound. In some preferred embodiments, the carbon number of the above-mentioned aldehyde compound is 1 to 7, and more preferably 2 to 7.
[0066] Examples of the aldehyde compound include: formaldehyde; linear or branched alkyl aldehydes such as acetaldehyde, propionaldehyde, n-butyraldehyde, isobutyraldehyde, tert-butyraldehyde, valeraldehyde, and hexanal; and alicyclic or aromatic aldehydes such as cyclohexanecarboxaldehyde and benzaldehyde. These may be used alone or in combination of two or more. In addition to formaldehyde, an aldehyde compound in which one or more hydrogen atoms are substituted by a halogen or the like may be used. In particular, linear or branched alkyl aldehydes are preferred from the viewpoint of high solubility in water and easy acetalization reaction, and acetaldehyde, propionaldehyde, n-butyraldehyde, and n-valeraldehyde are more preferred.
[0067] As the aldehyde compound, in addition to the above, aldehyde compounds having 8 or more carbon atoms, such as 2-ethylhexanal, nonanal, and decanal, can be used.
[0068] The acetalized polyvinyl alcohol polymer includes a VA unit belonging to the structural part represented by the following chemical formula: -CH2-CH(OH)- and an acetalized structural unit represented by the following general formula (1) (hereinafter also referred to as "VAC unit").
[0069]
[0070] (In formula (1), R is a hydrogen atom, or a straight-chain or branched alkyl group, which may be substituted by a functional group.)
[0071] In some preferred embodiments, R in the above formula (1) is a hydrogen atom or a linear or branched alkyl group having 1 to 6 carbon atoms. R may be one of them or a combination of two or more thereof. From the viewpoint of improving haze reduction performance, R is preferably a linear or branched alkyl group having 1 to 6 carbon atoms.
[0072] From the viewpoint of improving haze reduction performance, the acetalization degree of the acetalized polyvinyl alcohol polymer can be set to 1 mol% or more, can be 5 mol% or more, preferably 10 mol% or more, more preferably 15 mol% or more, further preferably 20 mol% or more, particularly preferably 25 mol% or more (e.g. 27 mol% or more). From the viewpoint of improving hydrophilicity, the acetalization degree of the acetalized polyvinyl alcohol polymer is preferably set to less than 60 mol%, further 50 mol% or less, more preferably 40 mol% or less, particularly preferably 35 mol% or less (e.g. 33 mol% or less). It should be noted that, in this specification, "acetalization degree" refers to the proportion of acetalized structural units (VAC units) in all repeating units constituting the acetalized polyvinyl alcohol polymer.
[0073] In addition, as the polyvinyl alcohol polymer, a cation-modified polyvinyl alcohol into which a cationic group such as a quaternary ammonium structure is introduced can also be used. Examples of the above-mentioned cation-modified polyvinyl alcohol include polyvinyl alcohol into which a cationic group derived from a monomer having a cationic group such as a diallyldialkylammonium salt, an N-(meth)acryloylaminoalkyl-N,N,N-trialkylammonium salt, etc. is introduced. In addition, as the vinyl alcohol polymer, a non-VA unit having a chemical formula of: -CH2-CH(CR 1 (OR 4 )-CR 2 (OR 5 )-R 3 )-represented by the polymer of the structural part. Here R 1 ~R 3Each independently represents a hydrogen atom or an organic group, R 4 and R 5 Each independently represents a hydrogen atom or R 6 -CO-(where R 6 For example, in the above chemical formula, R 1 ~R 3 When at least one of is an organic group, the organic group may be a linear or branched alkyl group having 1 to 8 carbon atoms. 6 The carbon number may be a linear or branched alkyl group having 1 to 8 carbon atoms.
[0074] In some embodiments, as the modified PVA, a modified PVA having a 1,2-diol structure in the side chain can be used. 1 ~R 5 A modified PVA (butene glycol-vinyl alcohol copolymer (BVOH)) containing non-VA units containing hydrogen atoms.
[0075] The proportion of the molar number of VA units in the molar number of all repeating units constituting the polyvinyl alcohol polymer can be, for example, 5% or more, 10% or more, 20% or more, or 30% or more. Although not particularly limited, in some embodiments, the proportion of the molar number of the above-mentioned VA units can be 50% or more, 65% or more, 75% or more, 80% or more, or 90% or more (for example, 95% or more or 98% or more). The repeating units constituting the polyvinyl alcohol polymer can be substantially 100% VA units. Here, "substantially 100%" means that the polyvinyl alcohol polymer is at least not intentionally made to contain non-VA units. Typically, the proportion of the molar number of non-VA units in the molar number of all repeating units is less than 2% (for example, less than 1%), including the case of 0%. In other embodiments, the proportion of the molar number of VA units in the molar number of all repeating units constituting the polyvinyl alcohol polymer can be, for example, less than 95%, less than 90%, less than 80%, or less than 70%.
[0076] The content of VA units in the polyvinyl alcohol polymer (content on a weight basis) can be, for example, 5% by weight or more, 10% by weight or more, 20% by weight or more, or 30% by weight or more. Although not particularly limited, in some embodiments, the content of the above-mentioned VA unit can be 50% by weight or more (for example, more than 50% by weight), 70% by weight or more, or 80% by weight or more (for example, 90% by weight or more, or 95% by weight or more, or 98% by weight or more). The repeating units constituting the polyvinyl alcohol polymer can be substantially 100% by weight VA units. Here, "substantially 100% by weight" means that at least non-VA units are not intentionally contained as repeating units constituting the polyvinyl alcohol polymer. Typically, it means that the content of non-VA units in the polyvinyl alcohol polymer is less than 2% by weight (for example, less than 1% by weight). In other embodiments, the content of VA units in the polyvinyl alcohol polymer can be, for example, less than 95% by weight, less than 90% by weight, less than 80% by weight, or less than 70% by weight.
[0077] The polyvinyl alcohol polymer may contain multiple polymer chains with different contents of VA units in the same molecule. Here, a polymer chain refers to a part (chain segment) that constitutes a part of a molecule of a polymer. For example, the polyvinyl alcohol polymer may contain a polymer chain A with a VA unit content higher than 50% by weight and a polymer chain B with a VA unit content lower than 50% by weight (i.e., a non-VA unit content higher than 50% by weight) in the same molecule.
[0078] The polymer chain A may contain only VA units as repeating units, or may contain non-VA units in addition to VA units. The content of VA units in the polymer chain A may be 60% by weight or more, 70% by weight or more, 80% by weight or more, or 90% by weight or more. In some embodiments, the content of VA units in the polymer chain A may be 95% by weight or more, or 98% by weight or more. The repeating units constituting the polymer chain A may be substantially 100% by weight of VA units.
[0079] The polymer chain B may contain only non-VA units as repeating units, or may contain VA units in addition to non-VA units. The content of non-VA units in the polymer chain B may be 60% by weight or more, 70% by weight or more, 80% by weight or more, or 90% by weight or more. In some embodiments, the content of non-VA units in the polymer chain B may be 95% by weight or more, or 98% by weight or more. The repeating units constituting the polymer chain B may be substantially 100% by weight of non-VA units.
[0080] As examples of polyvinyl alcohol-based polymers containing polymer chain A and polymer chain B in the same molecule, block copolymers and graft copolymers containing these polymer chains can be cited. The above-mentioned graft copolymer can be a graft copolymer having a structure in which polymer chain B (side chain) is grafted onto polymer chain A (main chain), or a graft copolymer having a structure in which polymer chain A (side chain) is grafted onto polymer chain B (main chain). In some embodiments, a polyvinyl alcohol-based polymer having a structure in which polymer chain B is grafted onto polymer chain A can be used.
[0081] Examples of polymer chain B include polymer chains having repeating units derived from N-vinyl monomers as main repeating units; polymer chains having repeating units derived from N-(meth)acryloyl monomers as main repeating units; polymer chains having repeating units derived from vinyl esters of dicarboxylic acids such as fumaric acid, maleic acid, and maleic anhydride as main repeating units; polymer chains having repeating units derived from aromatic vinyl monomers such as styrene and vinylnaphthalene as main repeating units; polymer chains having oxyalkylene units as main repeating units, etc. It should be noted that in this specification, unless otherwise specified, the main repeating unit refers to a repeating unit having a content exceeding 50% by weight.
[0082] As a suitable example of polymer chain B, a polymer chain having N-vinyl monomer as main repeating unit, i.e., N-vinyl polymer chain, can be cited. The content of repeating units derived from N-vinyl monomer in N-vinyl polymer chain is typically more than 50% by weight, and may be more than 70% by weight, more than 85% by weight, or more than 95% by weight. Polymer chain B may be substantially entirely repeating units derived from N-vinyl monomer.
[0083] In this specification, examples of N-vinyl monomers include monomers having nitrogen-containing heterocycles (e.g., lactam rings) and N-vinyl chain amides. As specific examples of N-vinyl lactam monomers, N-vinyl pyrrolidone, N-vinyl piperidone, N-vinyl morpholinone, N-vinyl caprolactam, N-vinyl-1,3-oxazine-2-one, N-vinyl-3,5-morpholinedione, etc. can be cited. As specific examples of N-vinyl chain amides, N-vinyl acetamide, N-vinyl propionamide, N-vinyl butyric acid amide, etc. can be cited. Polymer chain B, for example, can be an N-vinyl polymer chain in which more than 50% by weight (e.g., more than 70% by weight, or more than 85% by weight, or more than 95% by weight) of its repeating units are N-vinyl pyrrolidone units. The repeating units constituting polymer chain B can be substantially all N-vinyl pyrrolidone units.
[0084] As another example of polymer chain B, there can be cited a polymer chain having a repeating unit derived from an N-(meth)acryloyl type monomer as a main repeating unit, that is, an N-(meth)acryloyl polymer chain. The content of the repeating unit derived from the N-(meth)acryloyl type monomer in the N-(meth)acryloyl polymer chain typically exceeds 50% by weight, and may be 70% by weight or more, 85% by weight or more, or 95% by weight or more. The polymer chain B may be substantially entirely composed of repeating units derived from N-(meth)acryloyl type monomers.
[0085] In the present specification, examples of N-(meth)acryloyl-type monomers include chain amides having N-(meth)acryloyl groups and cyclic amides having N-(meth)acryloyl groups. Examples of chain amides having N-(meth)acryloyl groups include (meth)acrylamide; N-alkyl(meth)acrylamide such as N-methyl(meth)acrylamide, N-ethyl(meth)acrylamide, N-propyl(meth)acrylamide, N-isopropyl(meth)acrylamide, and N-n-butyl(meth)acrylamide; and N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N,N-dipropyl(meth)acrylamide, N,N-diisopropyl(meth)acrylamide, and N,N-di(n-butyl)(meth)acrylamide. Examples of the cyclic amide having an N-(meth)acryloyl group include N-(meth)acryloylmorpholine and N-(meth)acryloylpyrrolidine.
[0086] As another example of polymer chain B, there can be mentioned a polymer chain containing an oxyalkylene unit as a main repeating unit, that is, an oxyalkylene polymer chain. The content of the oxyalkylene unit in the oxyalkylene polymer chain is typically more than 50% by weight, and may be 70% by weight or more, 85% by weight or more, or 95% by weight or more. The repeating units contained in polymer chain B may be substantially all oxyalkylene units.
[0087] Examples of oxyalkylene units include oxyethylene units, oxypropylene units, oxybutylene units, etc. Such oxyalkylene units may be repeating units derived from corresponding alkylene oxides. The oxyalkylene units contained in the oxyalkylene polymer chain may be one type or two or more types. For example, it may be an oxyalkylene polymer chain comprising a combination of oxyethylene units and oxypropylene units. In the oxyalkylene polymer chain comprising two or more oxyalkylene units, these oxyalkylene units may be random copolymers of corresponding alkylene oxides, may be block copolymers, may be alternating copolymers, or graft copolymers.
[0088] As other examples of the polymer chain B, there can be listed a polymer chain comprising repeating units derived from an alkyl vinyl ether (e.g., a vinyl ether having an alkyl group having 1 to 10 carbon atoms), a polymer chain comprising repeating units derived from a monocarboxylic acid vinyl ester (e.g., a vinyl ester of a monocarboxylic acid having 3 or more carbon atoms), a polymer chain into which a cationic group (e.g., a cationic group having a quaternary ammonium structure) is introduced, and the like.
[0089] The polyvinyl alcohol-based polymer as the second water-soluble polymer in the technology disclosed herein is preferably a copolymer comprising VA units and non-VA units, i.e., a modified polyvinyl alcohol. In addition, the saponification degree of the modified polyvinyl alcohol-based polymer as the second water-soluble polymer is usually 50 mol% or more, preferably 65 mol% or more, more preferably 70 mol% or more, for example, 75 mol% or more. In the case of using a modified PVA having a 1,2-diol structure as a copolymer comprising VA units and non-VA units, the saponification degree of the polyvinyl alcohol-based polymer can be 95 mol% or more (e.g., more than 95 mol%), or 98 mol% or more. It should be noted that the saponification degree of the polyvinyl alcohol-based polymer is in principle less than 100 mol%.
[0090] Although not particularly limited, in some embodiments, when the non-VA unit contains a nitrogen atom, a polymer having a VA unit content of 50% by weight or more may be used as the second water-soluble polymer (polyvinyl alcohol-based polymer).
[0091] The weight average molecular weight (Mw) of the polyvinyl alcohol polymer can be set to, for example, 100×10 4 Below, 60×10 4 The following are appropriate. From the viewpoint of concentration efficiency, etc., the above Mw can be 30×10 4 Below, preferably 20×10 4 Below, for example, it can be 10×10 4 Below, can be 8×10 4 Below, can be 5×10 4 Below, it can also be 3×10 4 If the Mw of the polyvinyl alcohol polymer decreases, the dispersion stability of the polyvinyl alcohol polymer tends to improve. In addition, from the perspective of appropriately protecting the polished surface and maintaining or improving the surface quality, the Mw may be, for example, 0.2×10 4 Above, usually preferably 0.5×10 4 As the Mw of the polyvinyl alcohol polymer increases, the effect of protecting the polishing object and improving wettability tends to increase. From this point of view, in some embodiments, the Mw is 0.8×10 4The above is appropriate, preferably 1.0×10 4 Above, it can be 2×10 4 Above, can be 3×10 4 Above, for example, it can be 4×10 4 Above, it can also be 5×10 4 above.
[0092] Although not particularly limited, in some embodiments, the content of the second water-soluble polymer (specifically, a polyvinyl alcohol-based polymer) in the polishing composition can be, for example, 0.01 parts by weight or more relative to 100 parts by weight of abrasive grains (typically silica grains). From the viewpoint of reducing haze, etc., it is appropriate to set it to 0.1 parts by weight or more, preferably 0.5 parts by weight or more, more preferably 1 part by weight or more, and it can be 1.5 parts by weight or more, or it can be 2 parts by weight or more. The content of the second water-soluble polymer relative to 100 parts by weight of abrasive grains can be, for example, 50 parts by weight or less, or it can be 30 parts by weight or less. From the viewpoint of the dispersion stability of the polishing composition, in some embodiments, it is appropriate to set the content of the second water-soluble polymer relative to 100 parts by weight of abrasive grains to 15 parts by weight or less, preferably 10 parts by weight or less, more preferably 5 parts by weight or less, and it can be 3 parts by weight or less, or it can be 2 parts by weight or less. By appropriately setting the usage amount of the second water-soluble polymer (specifically, a polyvinyl alcohol polymer) within the above range, it is possible to better balance high surface quality and improved polishing rate. Although not particularly restrictive, it is believed that by controlling the usage amount of the second water-soluble polymer (specifically, a polyvinyl alcohol polymer), the protective effect of the substrate surface produced by the first and third water-soluble polymers (such as inhibiting alkali etching) will be appropriately limited, and high surface quality can be maintained and the polishing rate can be improved.
[0093] <Third Water-Soluble Polymer>
[0094] The grinding composition disclosed herein includes a polymer containing nitrogen atoms (polymer containing nitrogen atoms) as the third water-soluble polymer. Typically, the polymer containing nitrogen atoms can be a polymer containing repeating units (repeating units containing nitrogen atoms) derived from a monomer having a nitrogen atom. According to the grinding composition containing the polymer containing nitrogen atoms, a high-quality grinding surface is easily obtained. Although not particularly restrictive, it is believed that the polymer containing nitrogen atoms protects the substrate surface based on the adsorption of silica particles, and it is believed that it helps to improve the grinding surface quality (specifically, reduce the haze) through a different effect from the effect of the first and second water-soluble polymers. By using a polymer containing nitrogen atoms as the third water-soluble polymer in combination with the first and second water-soluble polymers, based on the different effects of each water-soluble polymer, the grinding rate can be increased and a high surface quality can be achieved.
[0095] As polymers containing nitrogen atoms, polymers containing nitrogen atoms in the main chain and polymers containing nitrogen atoms in the side chain (pendant) can be used. Examples of polymers containing nitrogen atoms in the main chain include alkylene polyoxyalkylene amine polymers and the like. Examples of polymers containing nitrogen atoms in the side chain include N-vinyl type polymers, N-(meth)acryloyl type polymers and the like. Other examples of polymers containing nitrogen atoms include polymers having an alkylene diamine structure such as ethylenediaminetetrapolyoxyethylenepolyoxypropylene (Poloxamine). The polymers containing nitrogen atoms can be used alone or in combination of two or more.
[0096] In some embodiments, an alkylene polyalkylene oxide amine polymer may be used as a polymer containing a nitrogen atom. The alkylene polyalkylene oxide amine polymer includes a polymer having a repeating unit of an alkylene group and a tertiary amine having a polyalkylene oxide bonded to a nitrogen atom.
[0097] Alkylene polyalkylene oxide amine polymers can be manufactured by any method known to those skilled in the art. For example, alkylene polyalkylene oxide amine polymers can be manufactured by addition polymerization of active hydrogen and alkylene oxide of polyamine compounds having two or more primary and / or secondary amino groups and containing 4 to 100 nitrogen atoms in the molecule. As examples of polyamine compounds providing a main chain structure, polyethylene polyamines such as triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, and hexaethyleneheptamine, and polyalkyleneimines such as polyethyleneimine obtained by polymerization of ethyleneimine can be cited. These compounds can be used alone or in combination of two or more, and can also form a main chain structure. As examples of alkylene oxides added to the main chain structure, ethylene oxide, propylene oxide, and butylene oxide can be cited. These alkylene oxides can be used alone or in combination of two or more. In some embodiments, as a polymer containing nitrogen atoms, an N-vinyl polymer can be used. Examples of N-vinyl polymers include polymers containing repeating units derived from monomers having nitrogen-containing heterocycles (e.g., lactam rings). Examples of such polymers include homopolymers and copolymers of N-vinyl lactam type monomers (for example, copolymers in which the copolymerization ratio of N-vinyl lactam type monomers exceeds 50% by weight), homopolymers and copolymers of N-vinyl chain amides (for example, copolymers in which the copolymerization ratio of N-vinyl chain amides exceeds 50% by weight), etc.
[0098] Specific examples of N-vinyl lactam monomers (i.e., compounds having a lactam structure and an N-vinyl group in one molecule) include N-vinyl pyrrolidone (VP), N-vinyl piperidone, N-vinyl morpholinone, N-vinyl caprolactam (VC), N-vinyl-1,3-oxazine-2-one, N-vinyl-3,5-morpholinedione, etc. Specific examples of polymers containing N-vinyl lactam monomer units include polyvinyl pyrrolidone, polyvinyl caprolactam, random copolymers of VP and VC, random copolymers of one or both of VP and VC and other vinyl monomers (e.g., acrylic monomers, vinyl ester monomers, etc.), block copolymers containing polymer chains containing one or both of VP and VC, alternating copolymers, graft copolymers, etc.
[0099] Specific examples of the N-vinyl chain amide include N-vinylacetamide, N-vinylpropionic acid amide, and N-vinylbutyric acid amide.
[0100] In some embodiments, as the third water-soluble polymer (polymer containing nitrogen atoms), an N-(meth)acryloyl type polymer can be preferably used. The effect produced by the technology disclosed herein can be more preferably achieved in a composition containing an N-(meth)acryloyl type polymer. Examples of N-(meth)acryloyl type polymers include homopolymers and copolymers of N-(meth)acryloyl type monomers (typically copolymers in which the copolymerization ratio of N-(meth)acryloyl type monomers exceeds 50 weight %). Examples of N-(meth)acryloyl type monomers include chain amides having an N-(meth)acryloyl group and cyclic amides having an N-(meth)acryloyl group.
[0101] Examples of chain amides having N-(meth)acryloyl groups include (meth)acrylamide; N-alkyl(meth)acrylamide such as N-methyl(meth)acrylamide, N-ethyl(meth)acrylamide, N-propyl(meth)acrylamide, N-isopropyl(meth)acrylamide, and N-n-butyl(meth)acrylamide; and N,N-dialkyl(meth)acrylamide such as N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N,N-dipropyl(meth)acrylamide, N,N-diisopropyl(meth)acrylamide, and N,N-di(n-butyl)(meth)acrylamide. Examples of polymers containing chain amides having N-(meth)acryloyl groups as monomer units include homopolymers of N-isopropylacrylamide and copolymers of N-isopropylacrylamide (e.g., copolymers in which the copolymerization ratio of N-isopropylacrylamide exceeds 50% by weight).
[0102] As examples of cyclic amides with N-(meth)acryloyl groups, N-acryloyl morpholine, N-acryloyl thiomorpholine, N-acryloyl piperidine, N-acryloyl pyrrolidine, N-methacryloyl morpholine, N-methacryloyl piperidine, N-methacryloyl pyrrolidine, etc. can be cited. As examples of polymers containing cyclic amides with N-(meth)acryloyl groups as monomer units, acryloyl morpholine polymers (PACMO) can be cited. As typical examples of acryloyl morpholine polymers, homopolymers of N-acryloyl morpholine (ACMO) and copolymers of ACMO (e.g., copolymers with a copolymerization ratio of ACMO exceeding 50% by weight) can be cited. In acryloyl morpholine polymers, the proportion of the number of moles of ACMO units in the number of moles of all repeating units is usually 50% or more, and it is appropriate to be 80% or more (e.g., 90% or more, typically 95% or more). The water-soluble polymer may be one in which all repeating units are substantially composed of ACMO units.
[0103] It should be noted that, although not particularly limited, in some embodiments, as the third water-soluble polymer (nitrogen atom-containing polymer), a polymer having a VA unit content of less than 50% by weight may be used.
[0104] The weight average molecular weight (Mw) of the nitrogen-containing polymer (for example, N-(meth)acryloyl polymer, preferably PACMO) can be set to, for example, 100×10 4 Below, 70×10 4 The following are appropriate. From the viewpoint of concentration efficiency, etc., the above Mw can be 60×10 4 Below, 50×10 4 In addition, from the viewpoint of maintaining or improving the surface quality, the Mw may be, for example, 1.0×10 4 Above, can be 5×10 4 Above, it can also be 10×10 4 More than (for example, more than 10×10 4 In some embodiments, the Mw is 20×10 4 The above is appropriate, preferably 30×10 4 More preferably 35×10 4 More than 40×10 4 More than (for example, more than 40×10 4). By using a nitrogen-containing polymer with a high Mw, a high surface quality can be easily obtained. In addition, although not particularly limited, in some embodiments, as the third water-soluble polymer (specifically, a nitrogen-containing polymer), a polymer having a higher Mw than the Mw of the second water-soluble polymer can be preferably used. By using two water-soluble polymers having the above relative Mw, it is possible to preferably achieve a balance between polishing rate and surface quality.
[0105] Although not particularly limited, in some embodiments, the content of the third water-soluble polymer (specifically, a polymer containing a nitrogen atom) in the polishing composition can be set to, for example, 0.01 parts by weight or more relative to 100 parts by weight of abrasive (typically, silica particles). From the viewpoint of reducing haze, it is appropriate to set it to 0.1 parts by weight or more, preferably 0.5 parts by weight or more, more preferably 1 part by weight or more, and it can also be 2 parts by weight or more. In addition, the content of the polymer containing a nitrogen atom can be, for example, 50 parts by weight or less, or 30 parts by weight or less relative to 100 parts by weight of abrasive. From the viewpoint of the dispersion stability of the polishing composition, in some embodiments, the content of the polymer containing a nitrogen atom is set to 15 parts by weight or less relative to 100 parts by weight of abrasive, preferably 10 parts by weight or less, more preferably 5 parts by weight or less, for example, 3.5 parts by weight or less. By appropriately setting the usage amount of the third water-soluble polymer (specifically, a polymer containing a nitrogen atom) from the above range, a high surface quality can be obtained.
[0106] Although not particularly limited, in some embodiments, the total content of the three water-soluble polymers (the first, second and third water-soluble polymers) contained in the polishing composition can be set to, for example, 0.01 parts by weight or more relative to 100 parts by weight of abrasive (typically silica particles). From the viewpoint of reducing haze, it is appropriate to set it to 0.1 parts by weight or more, preferably 0.5 parts by weight or more, more preferably 1 part by weight or more, further preferably 2 parts by weight or more, particularly preferably 4 parts by weight or more, and it can also be 6 parts by weight or more. In addition, the total content of the above-mentioned water-soluble polymers can be, for example, 50 parts by weight or less, or 30 parts by weight or less relative to 100 parts by weight of abrasive. From the viewpoint of the dispersion stability of the polishing composition, in some embodiments, it is appropriate to set the total content of the above-mentioned water-soluble polymers to 15 parts by weight or less relative to 100 parts by weight of abrasive, preferably 12 parts by weight or less, and it can also be 10 parts by weight or less (for example, less than 10 parts by weight).
[0107] In the polishing composition disclosed herein, the ratio of the content C1 of the first water-soluble polymer to the total content of the content C2 of the second water-soluble polymer and the content C3 of the third water-soluble polymer (C1 / (C2+C3)) is 0.1 or more on a weight basis. The effect produced by the technology disclosed herein can be achieved in a composition containing the first, second and third water-soluble polymers in the above ratio. In some embodiments, the above ratio (C1 / (C2+C3)) can be, for example, 0.2 or more, 0.4 or more, 0.5 or more, or 0.6 or more on a weight basis. By increasing the above ratio (C1 / (C2+C3)), the role of the cellulose derivative as the first water-soluble polymer can be effectively exerted. The upper limit of the above ratio (C1 / (C2+C3)) is not particularly limited, and can be, for example, 10 or less, or 5 or less on a weight basis. From the viewpoint of properly exerting the effects of the technology disclosed herein (especially improving the polishing rate), the above-mentioned ratio (C1 / (C2+C3)) is, in some embodiments, for example, 4.5 or less, preferably 4 or less, more preferably 3 or less, and further preferably 2 or less, on a weight basis. In some preferred embodiments, a composition in which the content C1 of the above-mentioned first water-soluble polymer is lower than the total content of the content C2 of the above-mentioned second water-soluble polymer and the content C3 of the above-mentioned third water-soluble polymer can be adopted. That is, a composition satisfying the following relationship: C1<(C2+C3) can be adopted. In this way, according to the composition in which the above-mentioned ratio (C1 / (C2+C3)) is less than 1 (weight basis), it is possible to achieve both high surface quality (for example, a reduction in haze value) and an increase in polishing rate at a higher level. The above-mentioned ratio (C1 / (C2+C3)) can be less than 0.9, less than 0.7, or less than 0.5 on a weight basis.
[0108] Although not particularly limited, in some embodiments, the ratio of the content C3 of the third water-soluble polymer to the total content of the content C1 of the first water-soluble polymer and the content C2 of the second water-soluble polymer (C3 / (C1+C2)) is, for example, greater than 0.1 on a weight basis, and it is appropriate to set it to be greater than 0.15. In some preferred embodiments, the above ratio (C3 / (C1+C2)) is greater than 0.18, and can be greater than 0.30, can be greater than 0.40, can be greater than 0.50, or can be greater than 0.60. By setting the above ratio (C3 / (C1+C2)) to a value greater than a specified value, it is easy to obtain a high surface quality. The upper limit value of the above ratio (C3 / (C1+C2)) is, for example, less than 10 (for example, less than 10) on a weight basis, and it is appropriate to set it to be less than 5. In some preferred embodiments, the ratio (C3 / (C1+C2)) is, for example, 1 or less (e.g., less than 1) on a weight basis, and may be 0.8 or less, 0.7 or less, or 0.6 or less. By limiting the ratio (C3 / (C1+C2)) to a value below a specified value, it tends to be easier to obtain an effect of increasing the polishing rate.
[0109] Although not particularly limited, in some embodiments, the ratio C2 / (C1+C3) of the content C2 of the second water-soluble polymer relative to the total content of the content C1 of the first water-soluble polymer and the content C3 of the third water-soluble polymer is, for example, 0.1 or more, and 0.2 or more is appropriate, and may be 0.3 or more, 0.5 or more, 0.7 or more, or 1 or more. By setting the above ratio C2 / (C1+C3) to a value greater than or equal to a specified value, the role of the polyvinyl alcohol-based polymer as the second water-soluble polymer can be effectively exerted. The upper limit of the above ratio C2 / (C1+C3) is, for example, 10 or less, 5 or less, 3 or less, or 1 or less, on a weight basis. By appropriately setting the above ratio C2 / (C1+C3) within the above range, the effect of the technology disclosed herein can be preferentially exerted.
[0110] Although not particularly limited, in some embodiments, the ratio (C3 / C2) of the content C3 of the third water-soluble polymer relative to the content C2 of the second water-soluble polymer is, for example, 0.01 or more on a weight basis. In some preferred embodiments, the above ratio (C3 / C2) is 0.05 or more on a weight basis, more preferably 0.1 or more, further preferably 0.3 or more, can be 0.5 or more, and can also be 0.7 or more. By setting the above ratio (C3 / C2) to a value above a specified value, it is easy to obtain a high surface quality. The upper limit of the above ratio (C3 / C2) is, for example, 10 or less on a weight basis, and it is appropriate to be 5 or less (for example, less than 5). In some preferred embodiments, the above ratio (C3 / C2) is 3 or less, more preferably 2 or less, and can be 1 or less. By setting the above ratio (C3 / C2) to be low within a specified range, a high surface quality can be maintained, and a higher polishing rate can be easily obtained.
[0111] Although not particularly limited, in some embodiments, the ratio (C1 / C3) of the content C1 of the first water-soluble polymer to the content C3 of the third water-soluble polymer is, for example, 0.1 or more, and appropriately 0.3 or more, on a weight basis. In some preferred embodiments, the above ratio (C1 / C3) is 0.5 or more, and may be 0.8 or more, or 1 or more. The upper limit of the above ratio (C1 / C3) is, for example, 10 or less on a weight basis, and in some preferred embodiments, 5 or less, and may be 3 or less, or 1.5 or less. By appropriately setting the above ratio (C1 / C3) within the above range, the effect produced by the technology disclosed herein can be preferably exerted.
[0112] Although not particularly limited, in some embodiments, the ratio (C1 / C2) of the content C1 of the first water-soluble polymer relative to the content C2 of the second water-soluble polymer is, for example, 0.01 or more on a weight basis, 0.1 or more is appropriate, preferably 0.2 or more, 0.4 or more, 0.6 or more, or 0.8 or more. In addition, the upper limit of the above ratio (C1 / C2) is, for example, 10 or less on a weight basis, 5 or less is appropriate, preferably 3 or less, or 1 or less (less than 1). By appropriately setting the above ratio (C1 / C2) within the above range, the effect of the technology disclosed herein can be preferably exerted.
[0113] Although not particularly limited, the contents and ratios of the first, second and third water-soluble polymers (eg, ratio (C1 / (C2+C3)) are preferably used in a silicon wafer polishing composition, and are particularly suitable for a silicon wafer fine polishing composition.
[0114] <Optional water-soluble polymer>
[0115] The polishing composition disclosed herein may also include water-soluble polymers other than the first water-soluble polymer, the second water-soluble polymer and the third water-soluble polymer as optional components (hereinafter also referred to as optional water-soluble polymers) within the scope that does not significantly hinder the effect of the present invention. As such optional water-soluble polymers, for example, starch derivatives, polymers comprising oxyalkylene units, etc. may be used.
[0116] Examples of starch derivatives include α-starch, pullulan, carboxymethyl starch, and cyclodextrin.
[0117] As the example of the polymer comprising oxyalkylene units, block copolymers of polyethylene oxide (PEO), ethylene oxide (EO) and propylene oxide (PO) or butylene oxide (BO), random copolymers of EO and PO or BO, etc. can be exemplified. Among them, preferably a block copolymer of EO and PO or a random copolymer of EO and PO. The block copolymer of EO and PO can be a diblock copolymer or a triblock copolymer comprising a PEO block and a polypropylene oxide (PPO) block, etc. The example of the above-mentioned triblock copolymer includes a PEO-PPO-PEO type triblock copolymer and a PPO-PEO-PPO type triblock copolymer. Usually more preferably a PEO-PPO-PEO type triblock copolymer.
[0118] In addition, in this specification, unless otherwise specified, the term "copolymer" means various copolymers including random copolymers, alternating copolymers, block copolymers, graft copolymers, and the like.
[0119] In the block copolymer or random copolymer of EO and PO, from the viewpoint of solubility in water, washability, etc., the molar ratio of EO to PO constituting the copolymer (EO / PO) is preferably greater than 1, more preferably 2 or more, and further preferably 3 or more (e.g. 5 or more).
[0120] In the embodiment where the polishing composition contains an optional water-soluble polymer, the content ratio of the optional water-soluble polymer in the total water-soluble polymer contained in the polishing composition is not particularly limited. From the viewpoint of effectively exerting the effects of the first, second and third water-soluble polymers, it is appropriate to set it to about 50% by weight or less (for example, less than 50% by weight), and it can be 30% by weight or less, less than 10% by weight, less than 3% by weight, or less than 1% by weight. The technology disclosed herein can be preferably implemented in an embodiment where the polishing composition does not substantially contain an optional water-soluble polymer.
[0121] <Surfactant>
[0122] In some embodiments, the grinding composition preferably includes at least one surfactant. By making the grinding composition contain a surfactant, the haze of the ground surface can be reduced more effectively. According to the technology disclosed herein, by comprising the combination of the above-mentioned water-soluble polymer and the composition of the surfactant, the quality of the ground surface (specifically haze) can be maintained and the grinding rate can be improved. As a surfactant, anionic, cationic, nonionic, amphoteric surfactants can be used. Anionic or nonionic surfactants can usually be preferably used. From the viewpoint of low foaming and the ease of pH adjustment, nonionic surfactants are more preferably used. Examples include oxyalkylene polymers such as polyethylene glycol, polypropylene glycol, and polytetramethylene glycol; polyoxyalkylene derivatives (e.g., polyoxyalkylene adducts) such as polyoxyethylene alkyl ethers, polyoxyethylene alkylphenyl ethers, polyoxyethylene alkylamines, polyoxyethylene fatty acid esters, polyoxyethylene glycerol ether fatty acid esters, and polyoxyethylene sorbitan fatty acid esters; and nonionic surfactants such as copolymers of multiple oxyalkylene groups (e.g., diblock copolymers, triblock copolymers, random copolymers, and alternating copolymers). The surfactant may be used alone or in combination of two or more.
[0123] Specific examples of the nonionic surfactant include block copolymers of ethylene oxide (EO) and propylene oxide (PO) (diblock copolymers, PEO (polyethylene oxide) -PPO (polypropylene oxide) -PEO type triblocks, PPO-PEO-PPO type triblock copolymers, etc.), random copolymers of EO and PO, polyoxyethylene glycol, polyoxyethylene propyl ether, polyoxyethylene butyl ether, polyoxyethylene pentyl ether, polyoxyethylene hexyl ether, polyoxyethylene octyl ether, polyoxyethylene-2-ethylhexyl ether, polyoxyethylene nonyl ether, polyoxyethylene decyl ether, polyoxyethylene isodecyl ether, polyoxyethylene tridecyl ether, polyoxyethylene lauryl ether, polyoxyethylene cetyl ether, polyoxyethylene stearyl ether, polyoxyethylene isostearyl ether, polyoxyethylene Ethyl oleyl ether, polyoxyethylene phenyl ether, polyoxyethylene octyl phenyl ether, polyoxyethylene nonyl phenyl ether, polyoxyethylene dodecyl phenyl ether, polyoxyethylene styrenated phenyl ether, polyoxyethylene laurylamine, polyoxyethylene stearylamine, polyoxyethylene oleylamine, polyoxyethylene monolaurate, polyoxyethylene monostearate, polyoxyethylene distearate, polyoxyethylene monooleate, polyoxyethylene dioleate, polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monopalmitate, polyoxyethylene sorbitan monostearate, polyoxyethylene sorbitan monooleate, polyoxyethylene sorbitan trioleate, polyoxyethylene sorbitan tetraoleate, polyoxyethylene castor oil, polyoxyethylene hydrogenated castor oil, etc. Particularly preferred surfactants include block copolymers of EO and PO (particularly PEO-PPO-PEO triblock copolymers), random copolymers of EO and PO, and polyoxyethylene alkyl ethers (e.g., polyoxyethylene decane ether). As polyoxyethylene alkyl ethers, those having an EO addition molar number of about 1 to 10 (e.g., about 3 to 8) are preferably used.
[0124] In some embodiments, it is preferred to use a nonionic surfactant. By using a nonionic surfactant, the haze reduction performance tends to be further improved.
[0125] The molecular weight of the surfactant is, for example, less than 1×10 4, from the viewpoints of filterability and cleaning properties, it is preferably 9500 or less, for example, it can be less than 9000. In addition, from the viewpoints of surface activity, etc., it is appropriate that the molecular weight of the surfactant is usually 200 or more, and from the viewpoint of haze reduction effect, etc., it is preferably 250 or more (for example, 300 or more). The more preferred range of the molecular weight of the surfactant may also vary depending on the type of the surfactant. For example, when polyoxyethylene alkyl ether is used as a surfactant, its molecular weight is, for example, preferably less than 2000, more preferably less than 1900 (for example, less than 1800), further preferably less than 1500, and can also be less than 1000 (for example, less than 500). In addition, for example, when a block copolymer of EO and PO is used as a surfactant, its weight average molecular weight can be, for example, more than 500, more than 1000, more than 1500, more than 2000, or more than 2500. The upper limit of the above-mentioned weight average molecular weight is, for example, less than 1×10 4 , preferably less than 9500, for example, less than 9000, less than 7000, and even less than 5000.
[0126] As the molecular weight of the surfactant, the molecular weight calculated by the chemical formula can be used, or the value of the weight average molecular weight obtained by GPC can be used (water system, polyethylene glycol conversion). For example, in the case of polyoxyethylene alkyl ether, it is preferred to use the molecular weight calculated by the chemical formula, and in the case of the block copolymer of EO and PO, it is preferred to use the weight average molecular weight obtained by the above-mentioned GPC.
[0127] Although not particularly limited, in the embodiment where the polishing composition includes a surfactant, from the viewpoint of cleaning properties, etc., it is appropriate that the content of the surfactant is usually set to 20 parts by weight or less, preferably 10 parts by weight or less, and more preferably 6 parts by weight or less (e.g., 3 parts by weight or less) relative to 100 parts by weight of abrasive grains (typically silica grains). From the viewpoint of better exerting the effect of the use of the surfactant, it is appropriate that the content of the surfactant is 0.001 parts by weight or more, preferably 0.01 parts by weight or more, more preferably 0.1 parts by weight or more, and may be 0.5 parts by weight or more relative to 100 parts by weight of abrasive grains.
[0128] <Water>
[0129] As the water contained in the polishing composition disclosed herein, ion exchange water (deionized water), pure water, ultrapure water, distilled water, etc. can be preferably used. In order to avoid the effects of other components contained in the polishing composition being hindered as much as possible, the water used, for example, preferably has a total content of transition metal ions below 100 ppb. The purity of water can be improved by, for example, removing impurity ions using ion exchange resins, removing foreign matter using filters, distillation, and other operations. It should be noted that the polishing composition disclosed herein may also further contain an organic solvent (lower alcohol, lower ketone, etc.) that can be uniformly mixed with water as needed. Preferably, 90% or more of the solvent contained in the polishing composition is water, and more preferably 95% or more (for example, 99 to 100% by volume) is water.
[0130] <Other ingredients>
[0131] The polishing composition disclosed herein may further contain known additives such as organic acids, organic acid salts, inorganic acids, inorganic acid salts, chelating agents, preservatives, and mildew inhibitors that can be used in polishing compositions (e.g., polishing compositions used in the fine polishing process of silicon wafers) as needed, within the range that does not significantly hinder the effects of the present invention.
[0132] Organic acids and salts thereof, and inorganic acids and salts thereof can be used alone or in combination of two or more. Examples of organic acids include fatty acids such as formic acid, acetic acid, propionic acid, aromatic carboxylic acids such as benzoic acid and phthalic acid, itaconic acid, citric acid, oxalic acid, tartaric acid, malic acid, maleic acid, fumaric acid, succinic acid, glycolic acid, malonic acid, gluconic acid, alanine, glycine, lactic acid, hydroxyethylidene diphosphoric acid (HEDP), organic sulfonic acids such as methanesulfonic acid, organic phosphonic acids such as nitrilotris(methylenephosphoric acid) (NTMP), and phosphonobutanetricarboxylic acid (PBTC). Examples of organic acid salts include alkali metal salts (sodium salts, potassium salts, etc.) and ammonium salts of organic acids. Examples of inorganic acids include hydrochloric acid, phosphoric acid, sulfuric acid, phosphonic acid, nitric acid, phosphinic acid, boric acid, and carbonic acid. Examples of inorganic acid salts include alkali metal salts (sodium salts, potassium salts, etc.) and ammonium salts of inorganic acids.
[0133] The above-mentioned chelating agent can be used alone or in combination of two or more. Examples of the above-mentioned chelating agent include aminocarboxylic acid chelating agents and organic phosphonic acid chelating agents. Suitable examples of the chelating agent include ethylenediaminetetrakis (methylenephosphonic acid), diethylenetriaminepenta (methylenephosphonic acid) and diethylenetriaminepentaacetic acid. Examples of the above-mentioned preservatives and mildewproofing agents include isothiazolin compounds, parabens, phenoxyethanol, etc.
[0134] The grinding composition disclosed herein is preferably substantially free of oxidant. This is because, when the grinding composition includes an oxidant, the grinding composition is supplied to a substrate (such as a silicon wafer), so that the surface of the substrate is oxidized to produce an oxide film, and the grinding rate may be reduced. As a specific example of the so-called oxidant here, hydrogen peroxide (H2O2), sodium persulfate, ammonium persulfate, sodium dichloroisocyanurate, etc. can be listed. It should be noted that the grinding composition substantially does not contain an oxidant, which means that at least it does not intentionally contain an oxidant. Therefore, the grinding composition that inevitably contains a trace amount of oxidant (for example, the molar concentration of the oxidant in the grinding composition is less than 0.0005 mol / L, preferably less than 0.0001 mol / L, more preferably less than 0.00005 mol / L, particularly preferably less than 0.00001 mol / L) due to raw materials, preparation methods, etc. can be included in the concept of the so-called grinding composition substantially free of oxidant here.
[0135] <ph>
[0136] The pH of the polishing composition disclosed herein is not particularly limited, and an appropriate pH can be adopted according to the substrate, etc. In some embodiments, the pH of the polishing composition is appropriately 8.0 or more, preferably 8.5 or more, and more preferably 9.0 or more. If the pH of the polishing composition becomes higher, there is a tendency for the polishing rate to increase. On the other hand, from the viewpoint of preventing the silicon dioxide particles from dissolving and suppressing the reduction of the mechanical polishing effect, the pH of the polishing composition is usually appropriately 12.0 or less, preferably 11.0 or less, more preferably 10.8 or less, and further preferably 10.5 or less.
[0137] It should be noted that in the technology disclosed herein, the pH of the polishing composition can be determined as follows: using a pH meter (e.g., a glass electrode hydrogen ion concentration indicator (model F-72) manufactured by Horiba, Ltd.), after performing a three-point calibration using a standard buffer solution (phthalate pH buffer solution pH: 4.01 (25°C), neutral phosphate pH buffer solution pH: 6.86 (25°C), carbonate pH buffer solution pH: 10.01 (25°C)), the glass electrode is inserted into the composition to be measured, and the value after stabilization for more than 2 minutes is measured.
[0138] <Polishing fluid>
[0139] The grinding composition disclosed herein is typically supplied to the surface of the substrate in the form of a grinding liquid containing the grinding composition, and is used for grinding the substrate. The above-mentioned grinding liquid can be, for example, a grinding liquid prepared by diluting any type of grinding composition disclosed herein (typically by diluting with water). Alternatively, the grinding composition can also be used directly as a grinding liquid. As other examples of grinding liquids containing the grinding composition disclosed herein, a grinding liquid formed by adjusting the pH of the composition can be listed.
[0140] The content of abrasive grains (typically silica particles) in the polishing liquid is not particularly limited, for example, 0.01% by weight or more, preferably 0.05% by weight or more, more preferably 0.10% by weight or more, and further preferably 0.15% by weight or more. With the increase of the content of abrasive grains, a higher polishing rate can be achieved. It is appropriate that the above content is 10% by weight or less, preferably 7% by weight or less, more preferably 5% by weight or less, and further preferably 2% by weight or less, for example, 1% by weight or less, 0.5% by weight or less, and 0.4% by weight or less. Thus, it is easy to maintain the surface quality.
[0141] The content of the alkaline compound in the polishing liquid is not particularly limited. From the viewpoint of improving the polishing rate, it is usually appropriate to set the above content to more than 0.0005 weight %, preferably to more than 0.001 weight %, and further preferably to more than 0.003 weight %. In addition, from the viewpoint of improving the surface quality (for example, reducing the haze), it is appropriate to set the above content to less than 0.1 weight %, preferably to less than 0.05 weight %, and more preferably to less than 0.03 weight % (for example, less than 0.025 weight %, further less than 0.01 weight %).
[0142] Although there is no particular limitation, in some embodiments, from the viewpoint of improving the surface quality, the content C1 of the first water-soluble polymer (specifically, a cellulose derivative) in the polishing liquid can be, for example, 0.0001% by weight or more, and it is usually appropriate to set it to 0.0005% by weight or more, preferably 0.001% by weight or more, for example, it can be 0.002% by weight or more. The upper limit of the content C1 of the above-mentioned first water-soluble polymer is not particularly limited, for example, it can be set to 0.05% by weight or less. From the viewpoint of stability, polishing rate, cleaning properties, etc. in the concentrated liquid stage, in some embodiments, the content C1 of the first water-soluble polymer is preferably 0.03% by weight or less, more preferably 0.015% by weight or less, and further preferably 0.01% by weight or less. The polishing liquid disclosed herein can also be preferably implemented in an embodiment in which, for example, the content C1 of the first water-soluble polymer is 0.008% by weight or less, 0.006% by weight or less, or 0.004% by weight or less.
[0143] Although there is no particular limitation, in some embodiments, from the viewpoint of improving the surface quality, the content C2 of the second water-soluble polymer (specifically, a polyvinyl alcohol-based polymer) in the polishing liquid can be, for example, 0.0001% by weight or more, and it is usually appropriate to set it to 0.0005% by weight or more, preferably 0.001% by weight or more, for example, 0.002% by weight or more, or 0.003% by weight or more. The upper limit of the content C2 of the second water-soluble polymer is not particularly limited, for example, it can be set to 0.05% by weight or less. From the viewpoint of stability, polishing rate, cleaning properties, etc. in the concentrated liquid stage, in some embodiments, the content C2 of the second water-soluble polymer is preferably 0.03% by weight or less, more preferably 0.015% by weight or less, and further preferably 0.01% by weight or less. The polishing liquid disclosed herein can also be implemented in an embodiment in which, for example, the content C2 of the second water-soluble polymer is 0.008% by weight or less, 0.006% by weight or less, or 0.004% by weight or less.
[0144] Although not particularly limited, in some embodiments, from the viewpoint of improving surface quality, the content C3 of the third water-soluble polymer (specifically, a polymer containing nitrogen atoms) in the polishing liquid can be, for example, 0.0001% by weight or more, and it is usually appropriate to set it to 0.0005% by weight or more, preferably 0.001% by weight or more, more preferably 0.002% by weight or more, and can be 0.003% by weight or more, or 0.005% by weight or more. The upper limit of the content C3 of the third water-soluble polymer is not particularly limited, and can be, for example, 0.1% by weight or less. From the viewpoint of stability, polishing rate, cleaning properties, etc. in the concentrated liquid stage, in some embodiments, the content C3 of the third water-soluble polymer is preferably 0.05% by weight or less, more preferably 0.02% by weight or less, and further preferably 0.01% by weight or less.
[0145] The total content (C1+C2+C3) of the first water-soluble polymer, the second water-soluble polymer and the third water-soluble polymer in the polishing liquid is not particularly limited, and in some embodiments, for example, can be set to more than 0.0001% by weight. From the viewpoint of reducing haze, the above-mentioned total content is preferably more than 0.0005% by weight, more preferably more than 0.001% by weight, and further preferably more than 0.002% by weight, for example, can be more than 0.005% by weight. In addition, the upper limit of the above-mentioned total content is, for example, less than 0.5% by weight, and from the viewpoint of polishing rate, it is preferably set to less than 0.2% by weight, more preferably set to less than 0.1% by weight, and further preferably set to less than 0.05% by weight (for example, less than 0.02% by weight, further less than 0.015% by weight).
[0146] In the case of comprising a surfactant, the content of the surfactant in the polishing liquid (its total content in the case of comprising two or more surfactants) is not particularly limited as long as it is in the scope that does not significantly hinder the effect of the present invention. Usually, from the viewpoint of cleanability, the content of the above-mentioned surfactant can be, for example, set as more than 0.00001 weight %. From the viewpoint of reducing haze, the preferred content is more than 0.0001 weight %, more preferably more than 0.0005 weight %, and more preferably more than 0.001 weight %. In addition, from the viewpoint of polishing rate, it is preferred that the above-mentioned content is set to less than 0.1 weight %, more preferably less than 0.01 weight %, and more preferably less than 0.005 weight % (for example less than 0.002 weight %).
[0147] <Concentrate>
[0148] The grinding composition disclosed herein may be in a concentrated form (i.e., in the form of a concentrated solution of the grinding liquid) before being supplied to the substrate. The grinding composition in this concentrated form is advantageous from the viewpoints of convenience, cost reduction, etc. during manufacture, circulation, storage, etc. The concentration ratio is not particularly limited, and for example, it may be set to be about 2 to 100 times in volume conversion, and generally about 5 to 50 times (e.g., about 10 to 40 times) is appropriate. Such a concentrated solution can be diluted at a desired time to prepare a grinding liquid (working slurry), and the grinding liquid is supplied to an embodiment of the substrate for use. The above-mentioned dilution can be performed by, for example, adding water to the above-mentioned concentrated solution and mixing.
[0149] When the polishing composition (i.e., concentrated solution) is diluted and used for polishing, the content of abrasive grains in the concentrated solution can be set to, for example, 25% by weight or less. From the viewpoints of dispersion stability and filterability of the polishing composition, the above content is usually preferably 20% by weight or less, and more preferably 15% by weight or less. In some preferred embodiments, the content of abrasive grains can be set to 10% by weight or less, and can also be set to 5% by weight or less. In addition, from the viewpoints of convenience during manufacture, circulation, storage, etc., cost reduction, etc., the content of abrasive grains in the concentrated solution can be set to, for example, 0.1% by weight or more, preferably 0.5% by weight or more, more preferably 0.7% by weight or more, and further preferably 1% by weight or more.
[0150] In some embodiments, the content of the alkaline compound in the above-mentioned concentrated solution can be set to, for example, less than 2% by weight. From the viewpoint of storage stability, etc., the above-mentioned content is usually preferably 1% by weight or less, more preferably 0.5% by weight or less, and further preferably 0.1% by weight or less. In addition, from the viewpoint of convenience during manufacture, circulation, storage, etc., cost reduction, etc., the content of the alkaline compound in the concentrated solution can be set to, for example, 0.005% by weight or more, preferably 0.01% by weight or more, more preferably 0.05% by weight or more, and further preferably 0.1% by weight or more.
[0151] In some embodiments, the total content of the first water-soluble polymer, the second water-soluble polymer and the third water-soluble polymer in the above-mentioned concentrated solution can be set to, for example, less than 3% by weight. From the viewpoints of filterability, cleanability, etc. of the grinding composition, usually, the above-mentioned content is preferably less than 1% by weight, more preferably less than 0.5% by weight. In addition, from the viewpoints of convenience, cost reduction, etc. during manufacture, circulation, preservation, etc., it is appropriate that the above-mentioned content is usually more than 0.001% by weight, preferably more than 0.005% by weight, more preferably more than 0.01% by weight. It should be noted that in the embodiment in which the above-mentioned concentrated solution also includes an optional water-soluble polymer in addition to the first, second and third water-soluble polymers, the total content of the water-soluble polymers contained in the concentrated solution can also be set by the above-mentioned range.
[0152] In the embodiment where the polishing composition contains a surfactant, the content of the surfactant in the concentrated solution can be, for example, 0.25 wt% or less, preferably 0.15 wt% or less, more preferably 0.1 wt% or less, 0.05 wt% or less, or 0.025 wt% or less. In addition, the content of the surfactant in the concentrated solution can be, for example, 0.0001 wt% or more, preferably 0.001 wt% or more, more preferably 0.005 wt% or more, and even more preferably 0.01 wt% or more.
[0153] <Preparation of Polishing Composition>
[0154] The polishing composition used in the technology disclosed herein may be a single-component type or a multi-component type including a two-component type. For example, the polishing composition may be composed as follows: a part A containing at least abrasive grains among the constituent components of the polishing composition is mixed with a part B containing at least a part of the remaining components, and the two are mixed and diluted at an appropriate time as needed to prepare a polishing liquid.
[0155] The preparation method of the grinding composition is not particularly limited. For example, known mixing devices such as a blade stirrer, an ultrasonic disperser, and a homogenizer can be used to mix the components constituting the grinding composition. The embodiment of mixing these components is not particularly limited, and for example, all the components can be mixed at once or in a properly set order.
[0156] <Purpose>
[0157] The polishing composition disclosed herein can be applied to the polishing of substrates having various materials and shapes. The material of the substrate can be, for example, metals or semi-metals such as silicon materials, aluminum, nickel, tungsten, copper, tantalum, titanium, stainless steel, or their alloys; glassy substances such as quartz glass, aluminosilicate glass, and glassy carbon; ceramic materials such as aluminum oxide, silicon dioxide, sapphire, silicon nitride, tantalum nitride, and titanium carbide; compound semiconductor substrate materials such as silicon carbide, gallium nitride, and gallium arsenide; resin materials such as polyimide resin, etc. It can also be a substrate composed of multiple materials among them. The shape of the substrate is not particularly limited. The polishing composition disclosed herein can be applied to the polishing of substrates having a flat surface, such as a plate-shaped or polyhedral shape, or the polishing of the end of a substrate (such as the polishing of a wafer edge).
[0158] The polishing composition disclosed herein is preferably used for polishing of a surface formed by a silicon material. As specific examples of silicon materials, single crystal silicon, amorphous silicon and polycrystalline silicon etc. can be listed. The polishing composition disclosed herein can be particularly preferably used for polishing of a surface formed by single crystal silicon (e.g., polishing of a silicon wafer).
[0159] The grinding composition disclosed herein can be preferably applied to the polishing process of a substrate (e.g., silicon wafer). For the substrate, before the polishing process performed using the grinding composition disclosed herein, general processing such as grinding and etching that can be applied to the substrate in a process further upstream of the polishing process can be implemented.
[0160] The grinding composition disclosed herein is effective for the finishing process of a substrate (e.g., a silicon wafer) or the polishing process immediately before it, and is particularly preferably used in the fine polishing process. Here, the fine polishing process refers to the last polishing process in the manufacturing process of the target object (i.e., a process in which no further polishing is performed after this process). In addition, the grinding composition disclosed herein can also be used in a polishing process upstream of the fine polishing (referring to a pre-polishing process between a rough grinding process and a final grinding process. Typically, it includes at least one polishing process, and can further include 2, 3, etc. polishing processes), such as a polishing process performed immediately before the fine polishing.
[0161] The polishing composition disclosed herein is effective in polishing (typically fine polishing or polishing before) a silicon wafer whose surface state is adjusted to a surface roughness of 0.01 nm to 100 nm by an upstream process. It is particularly preferably applied to fine polishing. The surface roughness Ra of the substrate can be measured using, for example, a laser scanning surface roughness meter "TMS-3000WRC" manufactured by Schmitt Measurement System Inc.
[0162] <Grinding>
[0163] The polishing composition disclosed herein can be used for polishing a substrate in an embodiment including, for example, the following operations. A preferred embodiment of a method for polishing a silicon wafer as a substrate using the polishing composition disclosed herein will be described below.
[0164] That is, a polishing liquid containing any of the polishing compositions disclosed herein is prepared. When preparing the above-mentioned polishing liquid, the polishing liquid may be prepared by operations such as concentration adjustment (e.g., dilution) and pH adjustment of the polishing composition. Alternatively, the polishing composition may be directly used as the polishing liquid.
[0165] Next, the polishing liquid is supplied to the substrate and polished by a conventional method. For example, in the case of fine polishing of a silicon wafer, typically, the silicon wafer that has undergone a grinding process is placed in a general polishing device, and the polishing liquid is supplied to the polishing target surface of the above-mentioned silicon wafer through the polishing pad of the polishing device. Typically, while continuously supplying the above-mentioned polishing liquid, the polishing pad is pressed against the polishing target surface of the silicon wafer, and the two are moved relative to each other (for example, rotationally moved). After this polishing process, the polishing of the substrate is completed.
[0166] The grinding pad used in the above-mentioned grinding process is not particularly limited. For example, a grinding pad of a foamed polyurethane type, a nonwoven type, a suede type, etc. can be used. Each grinding pad can contain abrasive particles or can contain no abrasive particles. It is usually preferred to use a grinding pad that does not contain abrasive particles.
[0167] The substrate polished using the polishing composition disclosed herein is typically cleaned. Cleaning can be performed using an appropriate cleaning solution. The cleaning solution used is not particularly limited. For example, in the field of semiconductors, general SC-1 cleaning solution (a mixture of ammonium hydroxide (NH4OH), hydrogen peroxide (H2O2) and water (H2O)), SC-2 cleaning solution (a mixture of HCl, H2O2 and H2O), etc. can be used. The temperature of the cleaning solution can be set, for example, to a range of above room temperature (typically about 15°C to 25°C) to about 90°C. From the viewpoint of improving the cleaning effect, a cleaning solution of about 50°C to 85°C can be preferably used.
[0168] As described above, the technology disclosed herein may include: providing a method for manufacturing a polished product (eg, a method for manufacturing a silicon wafer) including a polishing step (preferably fine polishing) using any of the above-mentioned polishing methods, and a polished product (eg, a silicon wafer) manufactured by the method.
[0169] Example
[0170] The following description is about several embodiments of the present invention, but is not intended to limit the present invention to the contents disclosed in the embodiments. In addition, in the following description, "parts" and "%" are weight references unless otherwise specified.
[0171] <Preparation of Polishing Composition>
[0172] (Examples 1 to 7)
[0173] Abrasive grains, alkaline compounds, water-soluble polymers, surfactants, and deionized water were mixed to prepare concentrated solutions of polishing compositions of various examples. Colloidal silica (average primary particle size: 27 nm, average aspect ratio: 1.3) was used as abrasive grains. Ammonia was used as an alkaline compound. As a water-soluble polymer, a 2.8×10- 5 Hydroxyethyl cellulose (HEC; the first water-soluble polymer), Mw is about 1.0×10 4 Acetalized polyvinyl alcohol (ac-PVA; the second water-soluble polymer) and Mw of about 4.7×10 5 Polyacryloylmorpholine (PACMO; the third water-soluble polymer) of 3000 Mw was used as a surfactant. A PEO-PPO-PEO block copolymer (PEO-PPO-PEO) having a Mw of about 3000 was used. The obtained concentrated solution of the polishing composition was diluted with deionized water to a volume ratio of 20 times, thereby obtaining polishing compositions of each example in which the concentration of the abrasive was set to 0.175%, the concentration of the alkaline compound was set to 0.005%, the concentrations of HEC, ac-PVA and PACMO were set to the concentrations shown in Table 1, and the concentration of PEO-PPO-PEO was set to 0.0016%.
[0174] (Example 8)
[0175] As the second water-soluble polymer, a polyvinyl alcohol (PVA) with a saponification degree of 98.5% or more and a Mw of 4.0×10 4 The graft copolymer (hereinafter referred to as "PVA-g-PEO") was prepared. In addition, the concentration of HEC was set to 0.00850%. The polishing composition of this example was prepared in the same manner as in Example 1.
[0176] (Example 9)
[0177] As the second water-soluble polymer, a polymer having a 1,2-diol structure in the side chain and a Mw of 1.0×10 4 The butene glycol-vinyl alcohol copolymer (BVOH) was prepared. In addition, the concentration of HEC was set to 0.00850%. The polishing composition of this example was prepared in the same manner as in Example 1. The saponification degree of the butene glycol-vinyl alcohol copolymer was 98% or more.
[0178] (Example 10)
[0179] As the second water-soluble polymer, a polymer having a Mw of 7.0×10 4 The polishing composition of this example was prepared in the same manner as in Example 1 using completely saponified (saponification degree 98% or more) PVA.
[0180] (Comparative Example 1)
[0181] The concentration of HEC was set to 0.00850%, and ac-PVA as the second water-soluble polymer and PACMO as the third water-soluble polymer were not added. The polishing composition of this example was prepared in the same manner as in Example 1.
[0182] (Comparative Examples 2 to 7)
[0183] The concentrations of HEC and ac-PVA were changed as shown in Table 1, and PACMO was not added as the third water-soluble polymer. Otherwise, the polishing composition of this example was prepared in the same manner as in Example 1.
[0184] (Comparative Example 8)
[0185] The concentrations of ac-PVA and PACMO were changed as shown in Table 1, and HEC was not added as the first water-soluble polymer. Otherwise, the polishing composition of this example was prepared in the same manner as in Example 1.
[0186] <Silicon Wafer Grinding>
[0187] Prepare a commercially available single crystal silicon wafer (conductivity type: P type, crystal orientation: <100> A silicon wafer having no COP (Crystal Originated Particle) was used as the substrate and pre-polished according to the following polishing condition 1. The pre-polishing was performed using a polishing liquid containing 1.0% abrasive grains (colloidal silica with an average primary particle size of 35 nm) and 0.068% potassium hydroxide in deionized water.
[0188] [Grinding Condition 1]
[0189] Grinding device: Single-wafer grinding device model "PNX-332B" manufactured by Okamoto Machine Tool Co., Ltd.
[0190] Grinding load: 20kPa
[0191] Plate speed: 20rpm
[0192] Grinding head (carrier) speed: 20rpm
[0193] Polishing pad: Made by NITTA DuPont, product name "SUBA400"
[0194] Grinding liquid supply rate: 1.0L / min
[0195] Grinding fluid temperature: 20°C
[0196] Plate cooling water temperature: 20℃
[0197] Grinding time: 2min
[0198] The pre-polished silicon wafer was polished under the following polishing conditions 2 using the polishing composition of each example prepared above as a polishing liquid.
[0199] [Grinding Condition 2]
[0200] Grinding device: Single-wafer grinding device model "PNX-332B" manufactured by Okamoto Machine Tool Co., Ltd.
[0201] Grinding load: 20kPa
[0202] Plate speed: 50rpm
[0203] Grinding head (carrier) speed: 50rpm
[0204] Polishing pad: FUJIBO Ehime Co., Ltd., product name "POLYPAS27NX"
[0205] Grinding liquid supply rate: 1.5L / min
[0206] Grinding fluid temperature: 20°C
[0207] Plate cooling water temperature: 20℃
[0208] Grinding time: 4min
[0209] The ground silicon wafer is removed from the grinding device and cleaned using a cleaning solution of NH4OH (29%): H2O2 (31%): deionized water (DIW) = 2: 5.3: 48 (volume ratio) (SC-1 cleaning). More specifically, a first cleaning tank equipped with an ultrasonic oscillator is prepared, the above-mentioned cleaning solution is stored in the first cleaning tank, maintained at 70°C, and the ground silicon wafer is immersed in the cleaning tank for 6 minutes. Then, after being immersed in a second cleaning tank filled with 25°C ultrapure water for 15 minutes, it is immersed in the first cleaning tank again for 6 minutes and in the second cleaning tank for 16 minutes, and then the silicon wafer is dried.
[0210] <Haze measurement>
[0211] The haze (ppm) of the cleaned silicon wafer surface was measured using a wafer inspection device manufactured by KLA-Tencor, trade name "Surfscan SP5" in DWO mode. The obtained result was converted into a relative value (haze) with the haze value of Comparative Example 1 as 100%. The smaller the haze value, the higher the haze improvement effect.
[0212] <Grinding Rate>
[0213] Prepare a 200mm diameter silicon wafer (conductivity type: P type, crystal orientation: <100> , without COP) as the polishing object, immersed in an HF aqueous solution (HF concentration: 2%) for 60 seconds to remove the oxide film, and polished according to the following polishing condition 3 using the polishing composition of each example as the polishing liquid.
[0214] [Grinding Condition 3]
[0215] Grinding device: Single-wafer grinding device model "PNX-322" manufactured by Okamoto Machine Tool Co., Ltd.
[0216] Grinding load: 15kPa
[0217] Plate speed: 30rpm
[0218] Grinding head (carrier) speed: 30rpm
[0219] Polishing pad: FUJIBO Ehime Co., Ltd., product name "POLYPAS275NX"
[0220] Grinding liquid supply rate: 0.4L / min
[0221] Grinding fluid temperature: 20°C
[0222] Plate cooling water temperature: 20℃
[0223] Grinding time: 10min
[0224] The ground silicon wafer was removed from the grinding device and immersed in a cleaning solution of NH4OH (29%): H2O2 (31%): deionized water = 1:1:12 (volume ratio) for 5 minutes for cleaning (SC-1 cleaning). Then, it was immersed in deionized water with an ultrasonic oscillator operating and dried using a centrifugal dryer.
[0225] (evaluate)
[0226] The weight of the silicon wafer before and after grinding was measured, and the grinding rate [nm / min] was calculated from the weight difference and the specific gravity of silicon. The obtained result was converted into a relative value with the grinding rate of Comparative Example 1 as 100%. The larger the value, the higher the grinding rate. If the grinding rate exceeds 100%, it can be evaluated as an improvement in the grinding rate.
[0227] The summary and evaluation results of each example are shown in Table 1. In addition, in the table, "-" represents that it does not contain.
[0228] [Table 1]
[0229]
[0230] As shown in Table 1, in Examples 1 to 10 using a polishing composition containing silica particles, a basic compound and water, which contains a cellulose derivative, a polyvinyl alcohol polymer and a nitrogen atom-containing polymer, and in which the ratio of the content C1 of the first water-soluble polymer to the total content of the content C2 of the second water-soluble polymer and the content C3 of the third water-soluble polymer (C1 / (C2+C3)) is 0.1 or more, the polishing rate is improved while maintaining the same haze as that of Comparative Example 1 using a polishing composition containing only a cellulose derivative (specifically, HEC) as the water-soluble polymer. On the other hand, in Comparative Examples 2 to 7 using only two water-soluble polymers, a cellulose derivative (specifically, HEC) and a polyvinyl alcohol polymer (specifically, ac-PVA), as the water-soluble polymer, the haze becomes higher than that of Comparative Example 1, and it is impossible to achieve both surface quality and polishing rate. More specifically, by using the above-mentioned cellulose derivative and polyvinyl alcohol polymer in combination, although the polishing rate is improved, the haze becomes high (Comparative Example 2), and the haze cannot be reduced even if the amount of polyvinyl alcohol polymer used is increased. In addition, for Comparative Example 8, which uses only two water-soluble polymers, polyvinyl alcohol polymer (specifically ac-PVA) and polymer containing nitrogen atoms (specifically PACMO), as water-soluble polymers, the polishing rate is lower than that of Comparative Example 1, which uses a cellulose derivative alone, and it is impossible to achieve both surface quality and polishing rate.
[0231] The above results show that by selecting three specific water-soluble polymers (cellulose derivatives, polyvinyl alcohol polymers and nitrogen-containing polymers) from a composition including silica particles, alkaline compounds and water and using them at a specified ratio, it is possible to maintain high surface quality and increase the polishing rate.
[0232] Although specific examples of the present invention have been described in detail above, these are merely examples and do not limit the claims. The technology described in the claims includes various modifications and changes to the specific examples described above.< / ph>
Claims
1. A polishing composition comprising: Silica particles as abrasive particles, a basic compound, water, a cellulose derivative as a first water-soluble polymer, a polyvinyl alcohol-based polymer as a second water-soluble polymer, and a nitrogen atom-containing polymer as a third water-soluble polymer, The ratio of the first water-soluble polymer content C1 to the total content of the second water-soluble polymer content C2 and the third water-soluble polymer content C3, i.e., C1 / (C2+C3), is 0.1 or more on a weight basis.
2. The polishing composition according to claim 1, wherein The ratio of the content C3 of the third water-soluble polymer to the content C2 of the second water-soluble polymer, namely C3 / C2, is 0.05 or more and less than 5 on a weight basis.
3. The polishing composition according to claim 1 or 2, wherein The ratio of the third water-soluble polymer content C3 to the total content of the first water-soluble polymer content C1 and the second water-soluble polymer content C2, i.e., C3 / (C1+C2), is 0.18 or more and less than 10 on a weight basis.
4. The polishing composition according to any one of claims 1 to 3, wherein The silica particles have an average aspect ratio of 1.0 to 3.
0.
5. The polishing composition according to any one of claims 1 to 4, wherein The weight average molecular weight of the third water-soluble polymer is 50,000 or more.
6. The polishing composition according to any one of claims 1 to 5, wherein The third water-soluble polymer is an acryloylmorpholine polymer.
7. The polishing composition according to any one of claims 1 to 6, wherein On a weight basis, the content C1 of the first water-soluble polymer, the content C2 of the second water-soluble polymer, and the content C3 of the third water-soluble polymer satisfy the following relationship: C1<(C2+C3). 8 . The polishing composition according to claim 1 , which is used for polishing a surface formed of a silicon material.
9. A concentrated solution of the polishing composition according to any one of claims 1 to 8.