Negative current collector for negative-electrode-free battery and negative-electrode-free battery comprising same
By using a conductive layer of an ionic conductive polymer composed of vinylidene fluoride, hexafluoropropylene or chloroethylene trifluoroethylene in a negative electrode-free battery, lithium dendrites are formed into a solid electrolyte interface layer in combination with lithium salt, and lithium dendrites are solved. The formation of lithium dendrites and electrolytes are solved. The problem of side reactions has achieved efficient improvements in lithium ion conductivity and charge and discharge performance.
Patent Information
- Application Number
- CN202380033272.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-06-15
- Filing Date
- 2023-06-15
- Publication Date
- 2024-11-19
AI Technical Summary
The formation of lithium dendrites during the charging process of the negative electrode battery leads to a reduction in charge and discharge efficiency and deterioration in life performance. Due to the lack of the negative electrode material layer, there are problems with electrolyte side reactions and low electroplating density of the lithium metal layer.
Using a conductive layer containing an ion-conducting polymer, the conductive layer consists of a monomer derived from vinylidene fluoride, hexafluoropropylene or chlorotrifluoroethylene, and the crystallization is adjusted by X-ray diffraction analysis to inhibit lithium dendrites. and a solid electrolyte interface layer is formed by a lithium salt to improve ion conductivity and flexibility.
Effectively inhibit the formation of lithium dendrites, improve lithium ion conductivity and charge and discharge efficiency, extend battery life, ensure safety and improve energy density.
Smart Images

Figure CN118985054A_ABST
Abstract
Description
Technical Field
[0001] [CROSS-REFERENCE TO RELATED APPLICATIONS]
[0002] This application claims priority to Korean Patent Application No. 10-2022-0073087, filed on June 15, 2022, the disclosure of which is incorporated herein by reference. Technical Field
[0003] The invention relates to a negative electrode current collector for a negative electrode-free battery and a negative electrode-free battery comprising the negative electrode current collector. Background Art
[0004] With the recent development of the information society, personal IT devices and computer networks have been developed, and the dependence of the entire society on electric energy has increased, requiring the development of battery technology that efficiently stores and utilizes electric energy.
[0005] In particular, as concerns arise about solving environmental problems and realizing a sustainable recycling society, energy storage devices such as electric double layer capacitors and lithium ion batteries have been extensively studied. Among them, lithium secondary batteries have attracted much attention as the battery system with the highest theoretical energy density in battery technology.
[0006] A lithium secondary battery generally has a structure in which an electrolyte is impregnated in an electrode assembly consisting of a positive electrode, a negative electrode, and a separator. In addition, generally, the positive electrode is generally prepared by coating an aluminum foil with a positive electrode material mixture containing a positive electrode active material, and the negative electrode is prepared by coating a copper foil with a negative electrode material mixture containing a negative electrode active material. In this case, a lithium transition metal oxide is generally used as the positive electrode active material, and a carbon-based active material or a silicon-based active material is used as the negative electrode active material.
[0007] Recently, lithium metal batteries using lithium metal itself as a negative electrode active material have been commercialized, and research is being conducted on negative electrode-free batteries or anode-free batteries, in which only a negative electrode current collector is used as a negative electrode when preparing an electrode, but lithium is provided from a positive electrode by charging, thereby using lithium metal as a negative electrode active material. Since a negative electrode-free battery does not include a negative electrode material mixture layer, it can include more positive electrode material mixture layers, and thus it is desirable in terms of high energy density.
[0008] However, during the charging of the negative electrode-free battery, there is a risk that the lithium transferred from the positive electrode is plated on the negative electrode collector and then forms lithium dendrites. The negative electrode-free battery may have a problem of increasing irreversible capacity due to the growth of these lithium dendrites, thereby reducing the charge and discharge efficiency. In addition, because the lithium metal layer formed on the negative electrode collector during the charging of the negative electrode-free battery has a low plating density, it may cause electrolyte side reactions, so that rapid degradation of life performance may occur.
[0009] Korean Patent Application Publication No. 10-2019-0083878 discloses a negative electrode-free lithium metal battery, but does not propose an alternative solution to the above-mentioned problems.
[0010] Prior art literature
[0011] [Patent Document]
[0012] Korean Patent Application Publication No. 10-2019-0083878 Summary of the invention
[0013] Technical issues
[0014] One aspect of the present invention provides a negative electrode collector for a negative electrode-free battery, wherein the charge and discharge efficiency and life performance are improved by suppressing the formation of lithium dendrites and improving electrolyte impregnation and ion conductivity during charging and discharging of the negative electrode-free battery including the negative electrode collector.
[0015] Another aspect of the present invention provides a negative electrode-free battery including the negative electrode current collector for a negative electrode-free battery.
[0016] Technical Solution
[0017] According to one aspect of the present invention, there is provided a negative electrode collector for a negative electrode-free battery, the negative electrode collector comprising: a metal collector substrate; and a conductive layer disposed on the metal collector substrate, wherein the conductive layer comprises an ion conductive polymer, and the ion conductive polymer comprises a unit derived from vinylidene fluoride and a unit derived from at least one monomer selected from the group consisting of hexafluoropropylene and chlorotrifluoroethylene, wherein during X-ray diffraction analysis of the conductive layer, a main peak exists in the 2θ range of 20.5° to 20.9°.
[0018] According to another aspect of the present invention, there is provided a negative electrode-free battery, comprising: the negative electrode collector for the negative electrode-free battery described above; a positive electrode facing the negative electrode collector for the negative electrode-free battery; a separator arranged between the negative electrode collector for the negative electrode-free battery and the positive electrode; and an electrolyte, wherein the conductive layer is arranged to face the separator.
[0019] Beneficial Effects
[0020] The negative electrode current collector for a negative electrode-free battery according to the present invention is characterized in that it contains a conductive layer containing an ion-conductive polymer, the ion-conductive polymer containing a unit derived from vinylidene fluoride and a unit derived from at least one monomer selected from the group consisting of hexafluoropropylene and chlorotrifluoroethylene, wherein during the X-ray diffraction analysis of the conductive layer, a main peak exists in the 2θ range of 20.5° to 20.9°. By adjusting the crystallization to a desired level in the 2θ range during the X-ray diffraction analysis of the conductive layer, the piezoelectric property can be improved, and therefore, the formation of lithium dendrites can be effectively suppressed during lithium plating according to the piezoelectric property of the conductive layer. The ion-conductive polymer contained in the conductive layer contains a unit derived from vinylidene fluoride and a unit derived from at least one monomer selected from the group consisting of hexafluoropropylene and chlorotrifluoroethylene in the polymer, and in particular, the unit derived from hexafluoropropylene and / or chlorotrifluoroethylene improves lithium ion conductivity by improving the electrolyte impregnation of the conductive layer, and can effectively accommodate the volume change during lithium plating and detachment by improving the flexibility of the conductive layer.
[0021] Therefore, the negative electrode-free battery including the above-mentioned negative electrode collector for the negative electrode-free battery can have a high energy density as a whole because a separate negative electrode active material layer is not formed, and can ensure safety by suppressing the formation of lithium dendrites which is a problem of the negative electrode-free battery, and can improve lithium ion conductivity. As a result, lithium from the positive electrode can be effectively plated and detached on the negative electrode, and thus can exhibit excellent charge and discharge efficiency and life performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The graph shows the results of X-ray diffraction analysis of the conductive layer included in the negative electrode current collector for a negative electrode-free battery of Example 1.
[0023] Figure 2 The graph shows the results of X-ray diffraction analysis of the conductive layer included in the negative electrode current collector for a negative electrode-free battery of Comparative Example 1.
[0024] Figure 3 3 is a graph showing the life performance evaluation of the negative electrode-free batteries of Examples 1 to 5 and Comparative Examples 1 and 2. DETAILED DESCRIPTION
[0025] It will be understood that the words or terms used in the specification and claims should not be interpreted as the meanings defined in commonly used dictionaries. It will be further understood that the words or terms should be interpreted as having meanings consistent with their meanings in the relevant art background and technical concepts of the present invention, on the basis that the inventor can appropriately define the meanings of the words or terms to best explain the principles of the invention.
[0026] In addition, it will be further understood that the terms "include", "comprises" or "has" in this specification indicate the presence of the features, numbers, steps, elements or a combination thereof, but do not exclude the presence or addition of one or more other features, numbers, steps, elements or a combination thereof.
[0027] In this specification, the average particle size (D 50 ) can be defined as the particle size at which the cumulative volume in the particle size distribution curve is 50%. For example, the average particle size (D 50 ) can be measured by using laser diffraction. Laser diffraction can generally measure particle sizes ranging from submicron to several millimeters, and can obtain highly reproducible and high-resolution results.
[0028] Negative electrode collector for negative electrode-free battery
[0029] The present invention provides a negative electrode current collector for a negative electrode-free battery. Specifically, the negative electrode current collector for a negative electrode-free battery can be a negative electrode current collector for a negative electrode-free lithium secondary battery.
[0030] Specifically, as a negative electrode collector for a negative electrode-free battery, the negative electrode collector is characterized in that it comprises: a metal collector substrate; and a conductive layer arranged on the metal collector substrate, wherein the conductive layer comprises an ion conductive polymer, and the ion conductive polymer comprises a unit derived from vinylidene fluoride and a unit derived from at least one monomer selected from the group consisting of hexafluoropropylene and chlorotrifluoroethylene, wherein during X-ray diffraction analysis of the conductive layer, a main peak exists in the 2θ range of 20.5° to 20.9°.
[0031] The metal current collecting substrate is not particularly limited as long as it has high conductivity and does not cause adverse chemical changes in the battery. Specifically, the metal current collecting substrate may include at least one selected from the group consisting of copper, stainless steel, aluminum, nickel, titanium and aluminum-cadmium alloy, and specifically may include copper.
[0032] The metal current collector substrate may have a thickness of 3 μm to 500 μm, and may specifically have a thickness of 3 μm to 20 μm in consideration of high energy density and mechanical strength.
[0033] The metal current collecting substrate may be used in various shapes such as a film, a sheet, a foil, a mesh, a porous body, a foam body, a nonwoven fabric body, and the like.
[0034] A concavo-convex structure may be formed on the surface of the metal current collector substrate, and the concavo-convex structure may allow a negative electrode-free battery including the negative electrode current collector for a negative electrode-free battery to be plated with lithium more smoothly during charge and discharge.
[0035] The conductive layer is disposed on the metal current collector substrate. Specifically, the conductive layer may be disposed on at least one surface of the metal current collector substrate, specifically, on one surface or both surfaces of the metal current collector substrate.
[0036] The conductive layer includes an ion conductive polymer. The ion conductive polymer includes a unit derived from vinylidene fluoride (VdF) and a unit derived from at least one monomer selected from the group consisting of hexafluoropropylene (HFP) and chlorotrifluoroethylene (CTFE).
[0037] Generally, for polymers containing only units derived from vinylidene fluoride (specifically PVdF), because they have piezoelectric properties, they have ion conductivity higher than a certain level, but there are problems in terms of poor performance in terms of electrolyte impregnation and poor performance in terms of flexibility. In particular, in the negative electrode for a negative electrode-free battery, in the case where the electrolyte is not fully impregnated, because the mobility of lithium ions cannot be fully ensured, the formation of lithium dendrites is promoted, and there is a risk of significant deterioration in life performance. In addition, in the case where the flexibility of the conductive layer is reduced, because the volume change during the electroplating of lithium from the positive electrode cannot be easily accommodated, there is a problem that a stable charge and discharge efficiency cannot be exerted.
[0038] In order to solve these problems, the conductive layer according to the present invention includes an ion conductive polymer, the ion conductive polymer including a unit derived from vinylidene fluoride and a unit derived from at least one monomer selected from the group consisting of hexafluoropropylene and chlorotrifluoroethylene. In the case where the ion conductive polymer includes a unit derived from at least one monomer selected from the group consisting of hexafluoropropylene and chlorotrifluoroethylene, the conductive layer improves the mobility of lithium ions by increasing the impregnation of the electrolyte without impairing the ion conductivity brought about by the piezoelectric properties of the unit derived from vinylidene fluoride, prevents the formation of lithium dendrites at a significant level, and easily accommodates the volume change caused by lithium plating, so that a negative electrode for a negative electrode-free battery with high charge and discharge performance and life performance can be realized.
[0039] Specifically, the ion conductive polymer may be a vinylidene fluoride-hexafluoropropylene copolymer, a vinylidene fluoride-chlorotrifluoroethylene copolymer, or a vinylidene fluoride-hexafluoropropylene-chlorotrifluoroethylene copolymer.
[0040] In addition, the ion conductive polymer may contain the unit derived from at least one monomer selected from the group consisting of hexafluoropropylene and chlorotrifluoroethylene in an amount of 1 wt % to 30 wt %, particularly 3 wt % to 25 wt %, more particularly 5 wt % to 20 wt %, and still more particularly 12 wt % to 18 wt %. When the amount of the unit is within the above range, high electrolyte impregnation property can be exhibited without impairing the piezoelectric properties and ion conductivity resulting from the unit derived from vinylidene fluoride, and thus, it is preferred.
[0041] In addition, during the X-ray diffraction analysis of the conductive layer, there is a main peak in the 2θ (2-theta) range of 20.5° to 20.9°. Generally, PVdF has a crystal structure and is known to be a material with piezoelectric properties. In this case, piezoelectric properties are defined as the mutual conversion effect in which mechanical vibration energy and electrical energy can be mutually converted, and accordingly, materials with piezoelectric properties can generate voltage when pressure is applied and can generate mechanical deformation when an electric field is applied. The piezoelectric properties of PVdF are caused by the polarity of the cross-polymerized CH2 groups and CF2 groups in PVdF. In PVdF, there are α phase, β phase, γ phase or δ phase according to the spatial structure. The CF bond in PVdF has a strong polarity due to the high electronegativity of fluorine (F), wherein for the α phase, because the VdF monomers in PVdF are aligned in opposite directions to offset the dipole moment, the piezoelectric properties do not exist or are not large, and for the β phase, because the VdF monomers in PVdF can be aligned in the same direction to maximize the dipole moment, it can be understood that the piezoelectric properties are relatively excellent.
[0042] In this case, the presence of a main peak in the 2θ (2-theta) range of 20.5° to 20.9° during the X-ray diffraction analysis of the conductive layer may mean that, in the unit derived from vinylidene fluoride contained in the ion conductive polymer or in the polymer containing it, the β phase of the unit derived from vinylidene fluoride exists as a dominant phase compared with other phases. Regarding the conductive layer according to the present invention containing the unit derived from vinylidene fluoride containing the β phase as a main component and embodied as having low crystallinity, it can be understood that it has a relatively stronger dipole moment and better piezoelectric properties than the conductive layer containing the unit derived from vinylidene fluoride containing the α phase as a main component. On the contrary, in the case where the α phase of PVdF exists as a dominant phase compared with other phases, the main peak exists in the 2θ (2-theta) range of about 20.0° during the X-ray diffraction analysis. In the case where PVdF contained in the conductive layer contains an α phase as a main component, not only electrolyte impregnation and ion conductivity are reduced but also piezoelectric properties are reduced because of high crystallinity, whereby precipitation of lithium dendrites may not be sufficiently prevented.
[0043] Thus, since the conductive layer included in the negative electrode current collector for a negative electrode battery without the present invention includes an ion conductive polymer, the ion conductive polymer includes a unit derived from at least one monomer selected from the group consisting of hexafluoropropylene and chlorotrifluoroethylene and a unit derived from vinylidene fluoride, and there is a main peak in the 2θ (2-theta) range of 20.5° to 20.9° during X-ray diffraction analysis, the mobility of lithium ions can be improved, the formation of lithium dendrites can be prevented at a significant level, and a negative electrode for a negative electrode battery without the negative electrode having high life performance can be realized. The 2θ range during the X-ray diffraction analysis of the conductive layer is controlled by the arrangement structure of the vinylidene fluoride unit, but since the conductive layer only including PVdF containing only the vinylidene fluoride unit therein not only exhibits piezoelectric properties but also has very low flexibility, it may not be able to accommodate the volume change caused by the electroplating of lithium, and as a result, there is a concern that the formation of lithium dendrites is promoted. In this regard, the conductive layer according to the present invention includes a unit derived from hexafluoropropylene and / or chlorotrifluoroethylene in the ion conductive polymer while adjusting the 2θ (2-theta) range during X-ray diffraction analysis to a specific range, thereby even exhibiting the effect of improving the flexibility of the conductive layer.
[0044] The 2θ value at the main peak appearing during the X-ray diffraction analysis of the conductive layer comes from the arrangement structure of the units derived from vinylidene fluoride, but even if hexafluoropropylene or chlorotrifluoroethylene is copolymerized with vinylidene fluoride, the 2θ value at the main peak appearing during the X-ray diffraction analysis of the conductive layer does not change because the main chain structure of vinylidene fluoride and the arrangement structure of the units derived from vinylidene fluoride in the copolymer are maintained.
[0045] In the present specification, the expression "main peak" refers to a peak at which the intensity is highest when a graph of 2θ and intensity is plotted using X-ray diffraction analysis.
[0046] The conductive layer may further include a lithium salt and an ion conductive polymer. The lithium salt may help to form a solid electrolyte interface layer (SEI layer) on the surface of the negative electrode current collector during initial charge, thereby further improving the ion conductivity of the conductive layer and helping to improve life performance.
[0047] The lithium salt may include at least one selected from the group consisting of LiCl, LiBr, LiI, LiNO3, LiClO4, LiBF4, LiB 10 Cl 10, LiPF6, LiCF3SO3, LiCF3CO2, LiAsF6, LiSbF6, LiAlCl4, CH3SO3Li, CF3SO3Li, LiSCN, LiC(CF3SO2)3, (CF3SO2)2NLi, (FSO2)2NLi, lithium chloroborane, lithium lower aliphatic carboxylate, lithium 4-phenylborate and lithium imide, and specifically may include LiNO3 in terms of suppressing the formation of lithium dendrites by promoting the formation of a stable SEI layer having a larger amount of inorganic materials such as Li3N and Li2O on the surface of the negative electrode collector and inducing the surface shape of the plated lithium metal to form a spherical shape during charging.
[0048] In the case where a lithium salt is included in the conductive layer, the content of the lithium salt in the conductive layer may be 0.1 wt % to 20 wt %, more specifically 2 wt % to 10 wt %. When the amount of the lithium salt is within the above range, a stable SEI layer is formed, the effect of preventing the formation of lithium dendrites is achieved, and the concentration gradient caused by the consumption of lithium ions on the surface of the negative electrode collector during charge and discharge is effectively compensated, while preventing the increase in resistance when an excessive amount of lithium salt is added, so it is preferred.
[0049] The conductive layer may further contain at least one other polymer selected from the group consisting of acrylic polymer, polyurethane, polyurea, styrene-butadiene rubber, polyimide and polystyrene in addition to the ion conductive polymer. The other polymer may be contained in the conductive layer in terms of improving the electrolyte impregnation property by increasing the swelling degree of the conductive layer. Even if the other polymer is contained in the conductive layer, it has no significant effect on the crystal formation of the polymer containing vinylidene fluoride units because micro separation occurs during drying in the preparation of the conductive layer, and thus the 2θ value at the main peak during the X-ray diffraction analysis of the conductive layer does not change depending on whether the other polymer is added.
[0050] The acrylic polymer may be a polymer obtained by polymerizing at least one monomer selected from the group consisting of butyl acrylate, acrylic acid, and acrylonitrile.
[0051] In the case where the conductive layer further contains the other polymer, the weight ratio of the ion conductive polymer to the other polymer contained in the conductive layer may be in the range of 10:90 to 99.9:0.1, specifically 50:50 to 99.5:0.5. When the weight ratio is within the above range, it is desirable in terms of maintaining the shape of the conductive layer and increasing electrolyte impregnation.
[0052] The conductive layer can have a thickness of 1 μm to 50 μm, particularly 2 μm to 10 μm, more particularly 2 μm to 3 μm, and when the thickness is within the above range, the energy density of the secondary battery can be improved because the effects of suppressing the formation of lithium dendrites and improving electrolyte impregnation brought about by the use of the conductive layer can be achieved, and at the same time the volume of the negative electrode collector including the conductive layer can be reduced.
[0053] The conductive layer can be prepared by applying a conductive layer-forming composition containing an ion conductive polymer to a metal current collecting substrate and drying the composition. In this case, it is important to appropriately control the drying temperature so that the β phase in PVdF can become the dominant phase. If the drying temperature is too high, it is difficult to achieve the conductive layer desired by the present invention because crystallization proceeds excessively and the amount of the α phase of PVdF increases.
[0054] Specifically, the method of preparing the conductive layer may include the following steps.
[0055] (a) applying a conductive layer-forming composition comprising an ion-conductive polymer onto a metal current collecting substrate; and
[0056] (b) Drying the applied conductive layer-forming composition.
[0057] The conductive layer-forming composition may further contain a solvent in addition to the ion-conductive polymer. For example, the solvent may be N-methylpyrrolidone (NMP).
[0058] The drying temperature during drying may be appropriately adjusted according to the type of polymer, for example, the drying temperature may be in the range of 95° C. or less, specifically 30° C. to 75° C., and more specifically 40° C. to 65° C. In this case, the drying time may be in the range of 1 hour to 5 hours.
[0059] The drying can be performed, for example, under vacuum conditions.
[0060] After the drying, additional drying may be further performed after lowering the temperature to room temperature (specifically, 20° C. to 25° C.). For example, the additional drying may be performed for 1 hour to 100 hours, specifically, 24 hours to 80 hours.
[0061] No negative electrode battery
[0062] In addition, the present invention provides a negative electrode-free battery comprising the negative electrode current collector for the negative electrode-free battery. The negative electrode-free battery may be a negative electrode-free lithium secondary battery.
[0063] Specifically, the negative electrode-free battery comprises: the negative electrode current collector for the negative electrode-free battery; a positive electrode facing the negative electrode current collector for the negative electrode-free battery; a separator disposed between the negative electrode current collector for the negative electrode-free battery and the positive electrode; and an electrolyte. In this case, the conductive layer may be disposed to face the separator.
[0064] The characteristics of the negative electrode current collector for the negative electrode-free battery are as described above.
[0065] The negative electrode current collector for a negative electrode-free battery can itself be used as a negative electrode for a negative electrode-free battery.
[0066] The negative electrode for a non-negative electrode battery or the negative electrode current collector for a non-negative electrode battery does not contain a separate lithium intercalation material or lithium metal, and can be assembled into an electrode assembly and a non-negative electrode battery together with a positive electrode and a separator. As described below, in a non-negative electrode battery including the negative electrode for a non-negative electrode battery or the negative electrode current collector for a non-negative electrode battery, lithium ions from the positive electrode can move to the negative electrode for a non-negative electrode battery or the negative electrode current collector for a non-negative electrode battery during charging to form a lithium metal layer. The non-negative electrode battery can be charged and discharged by forming or removing the lithium metal layer.
[0067] The positive electrode is arranged to face the negative electrode current collector for a battery without a negative electrode.
[0068] The positive electrode may include a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector.
[0069] The positive electrode current collector is not particularly limited as long as it has high conductivity and does not cause adverse chemical changes in the battery. For example, stainless steel, aluminum, nickel, titanium, sintered carbon, or aluminum or stainless steel surface-treated with one of carbon, nickel, titanium, silver, etc. can be used.
[0070] The thickness of the positive electrode current collector may generally be 3 μm to 500 μm.
[0071] The positive electrode active material layer is formed on the positive electrode current collector and includes a positive electrode active material.
[0072] The positive electrode active material is a compound capable of reversibly inserting and deinserting lithium, wherein the positive electrode active material may specifically contain a lithium composite metal oxide containing lithium and at least one metal such as cobalt, manganese, nickel or aluminum. More specifically, the lithium composite metal oxide may include: lithium-manganese oxides (such as LiMnO2, LiMn2O4, etc.), lithium-cobalt oxides (such as LiCoO2, etc.), lithium-nickel oxides (such as LiNiO2, etc.), lithium-nickel-manganese oxides (such as LiNi 1-Y Mn Y O2 (where 0 <Y<1)、LiMn 2-Z Ni ZO4 (where 0 < Z < 2, etc.), lithium-nickel-cobalt oxides (such as LiNi 1-Y1 Co Y1 O2 (where 0 < Y1 < 1)), lithium-manganese-cobalt oxides (such as LiCo 1-Y2 Mn Y2 O2 (where 0 < Y2 < 1), LiMn 2-Z1 Co Z1 O4 (where 0 < Z1 < 2, etc.), lithium-nickel-manganese-cobalt oxides (such as Li(Ni p Co q Mn r1 )O2 (where 0 < p < 1, 0 < q < 1, 0 < r1 < 1 and p + q + r1 = 1) or Li(Ni p1 Co q1 Mn r2 )O4 (where 0 < p1 < 2, 0 < q1 < 2, 0 < r2 < 2 and p1 + q1 + r2 = 2) etc.) or lithium-nickel-cobalt-transition metal (M) oxides (such as Li(Ni p2 Co q2 Mn r3 M s2 )O2 (where M is selected from the group consisting of aluminum (Al), iron (Fe), vanadium (V), chromium (Cr), titanium (Ti), tantalum (Ta), magnesium (Mg) and molybdenum (Mo), and p2, q2, r3 and s2 are atomic fractions of respective independent elements, where 0 < p2 < 1, 0 < q2 < 1, 0 < r3 < 1, 0 < s2 < 1 and p2 + q2 + r3 + s2 = 1) etc.), and may include any one of them or a mixture of two or more thereof. Among these materials, in terms of improving the capacity characteristics and stability of the battery, the lithium composite metal oxide may be LiCoO2, LiMnO2, LiNiO2, lithium nickel manganese cobalt oxide (such as Li(Ni 0.6 Mn 0.2 Co 0.2 )O2, Li(Ni 0.5 Mn 0.3 Co 0.2 )O2 or Li(Ni 0.8 Mn 0.1 Co 0.1 )O2 etc.) or lithium nickel cobalt aluminum oxide (such as Li(Ni 0.8 Co 0.15 Al 0.05 )O2 etc.).
[0073] Based on the total weight of the positive electrode active material layer, the content of the positive electrode active material may be 80% by weight to 99% by weight.
[0074] The positive electrode active material layer may optionally further include at least one additive selected from the group consisting of a binder and a conductive material in addition to the positive electrode active material.
[0075] The binder is a component that helps the bonding between the conductive material and the active material and the bonding with the current collector, wherein the addition amount of the binder is generally 1 wt % to 30 wt % based on the total weight of the positive electrode active material layer. Examples of the binder may be polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene propylene diene monomer rubber (EPDM), sulfonated EPDM, styrene butadiene rubber, fluororubber and various copolymers.
[0076] Any conductive material can be used without particular limitation, as long as it has conductivity and does not cause adverse chemical changes in the battery, for example, conductive materials such as graphite, carbon materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, and thermal black, conductive fibers such as carbon fibers or metal fibers, fluorocarbon powders, metal powders such as aluminum powder and nickel powder, conductive whiskers such as zinc oxide whiskers and potassium titanate whiskers, conductive metal oxides such as titanium oxide, or polyphenylene derivatives. Specific examples of commercially available conductive materials can be: acetylene black products (Chevron Chemical Company; Denka Black (Denka Singapore Private Limited); or Gulf Oil Company); Ketjen black; EC products (Armak Company); Vulcan XC-72 (Cabot Company); and Super P (Timcal Graphite & Carbon).
[0077] The conductive material may be included in an amount of 1 wt % to 30 wt % based on the total weight of the positive electrode active material layer.
[0078] The positive electrode active material layer may be prepared by adding a positive electrode active material and optionally an additive including a binder and / or a conductive material to a solvent to prepare a positive electrode slurry, coating the positive electrode slurry on a positive electrode collector, and rolling and drying the coated positive electrode collector.
[0079] The solvent may include an organic solvent such as N-methyl-2-pyrrolidone (NMP), and may be used in an amount such that a desired viscosity is obtained when the positive electrode active material and optional binder and conductive material are included. For example, the content of the solvent may be such that the concentration of the solid component containing the positive electrode active material and optional binder and conductive material is in the range of 50 wt % to 95 wt %, preferably 70 wt % to 90 wt %.
[0080] The separator separates the negative electrode and the positive electrode and provides a path for the movement of lithium ions, wherein any separator can be used without particular limitation, as long as it is commonly used as a separator in a lithium secondary battery, in particular, a separator having high moisture retention capacity for the electrolyte and low resistance to electrolyte ion transfer can be used. Specifically, a porous polymer film, for example, a porous polymer film prepared from a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer; or a laminated structure having two or more layers thereof can be used. In addition, a typical porous non-woven fabric can be used, such as a non-woven fabric formed of a high melting point glass fiber or a polyethylene terephthalate fiber. In addition, a coated separator comprising a ceramic component or a polymer material can be used to ensure heat resistance or mechanical strength, and a separator having a single-layer or multilayer structure can be optionally used.
[0081] In addition, the electrolyte used in the present invention may include an organic liquid electrolyte, an inorganic liquid electrolyte, a solid polymer electrolyte, a gel-type polymer electrolyte, a solid inorganic electrolyte or a molten inorganic electrolyte that can be used in the preparation of a lithium secondary battery, but the present invention is not limited thereto.
[0082] Specifically, the electrolyte may include an organic solvent and a lithium salt.
[0083] As the organic solvent, any organic solvent can be used without particular limitation, as long as it can be used as a medium through which ions participating in the electrochemical reaction of the battery can move. Specifically, the following substances can be used as the organic solvent: ester solvents such as methyl acetate, ethyl acetate, γ-butyrolactone and ε-caprolactone; ether solvents such as dibutyl ether or tetrahydrofuran; ketone solvents such as cyclohexanone; aromatic hydrocarbon solvents such as benzene and fluorobenzene; carbonate solvents such as dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC) and propylene carbonate (PC); alcohol solvents such as ethanol and isopropanol; nitrile such as R-CN (wherein R is a linear, branched or cyclic C2-C20 hydrocarbon group and may contain a double bond aromatic ring or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolanes; or cyclopentane sulfone. In these solvents, carbonate solvents are preferred, more preferably a mixture of cyclic carbonate (such as ethylene carbonate or propylene carbonate) with high ion conductivity and high dielectric constant and low viscosity linear carbonate compound (such as ethyl methyl carbonate, dimethyl carbonate or diethyl carbonate) that can improve the charge and discharge performance of the battery. In this case, when cyclic carbonate and chain carbonate are mixed with a volume ratio of about 1:1 to about 1:9, the performance of the electrolyte can be excellent.
[0084] The lithium salt can be used without particular limitation, as long as it is a compound that can provide lithium ions used in lithium secondary batteries. Specifically, the following substances can be used as lithium salts: LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI or LiB(C2O4)2. The lithium salt can be used in a concentration range of 0.1 M to 2.0 M. If the concentration of the lithium salt is included in the above range, since the electrolyte can have appropriate conductivity and viscosity, excellent electrolyte performance can be obtained, and lithium ions can be effectively moved.
[0085] The negative electrode-free battery may further include a lithium metal layer formed on the negative electrode current collector for the negative electrode-free battery, wherein the lithium metal layer may be formed by charging the negative electrode-free battery to allow lithium ions to move from the positive electrode. The lithium metal layer may be specifically formed or disposed between the metal current collector substrate and the conductive layer.
[0086] As described above, the negative electrode-free battery according to the present invention is suitable for: portable devices such as mobile phones, notebook computers and digital cameras; and electric vehicles such as hybrid electric vehicles (HEVs), and in particular, can be preferably used as a constituent battery of a medium-to-large battery module. Therefore, the present invention also provides a medium-to-large battery module comprising the above-mentioned negative electrode-free battery as a unit cell.
[0087] The middle and large-sized battery module may be preferably used in power sources for devices requiring high output and large capacity, such as electric vehicles, hybrid electric vehicles, and power storage systems.
[0088] Hereinafter, embodiments of the present invention will be described in detail in a manner that can be easily implemented by those skilled in the art. However, the present invention can be embodied in many different forms and should not be construed as being limited to the embodiments set forth herein.
[0089] Examples and Comparative Examples
[0090] Example 1: Preparation of negative electrode current collector for negative electrode-free battery
[0091] A copper foil was prepared as a metal current collecting substrate (thickness: 15 μm).
[0092] A conductive layer-forming composition (solid content: 10 wt %) in which a vinylidene fluoride-hexafluoropropylene copolymer (VdF-HFP copolymer) containing 15 wt % of units derived from hexafluoropropylene (HFP) as an ion conductive polymer was dispersed in an N-methylpyrrolidone (NMP) solvent was prepared, applied to a metal current collector substrate, dried at 60° C. for 2 hours under vacuum conditions (about −0.1 MPa), then slowly lowered to room temperature and dried for an additional 70 hours to form a conductive layer (thickness: 2.5 μm). The metal current collector substrate having the conductive layer formed thereon was used as a negative electrode current collector for a negative electrode-free battery.
[0093] Example 2: Preparation of negative electrode current collector for negative electrode-free battery
[0094] A negative electrode current collector for a negative electrode-free battery was prepared in the same manner as in Example 1 except that LiNO 3 as a lithium salt was further contained in the conductive layer-forming composition in an amount of 5 wt % based on the weight of the solid content of the conductive layer-forming composition.
[0095] The thickness of the conductive layer included in the negative electrode current collector for a negative electrode-free battery of Example 2 was 2.5 μm.
[0096] Example 3: Preparation of negative electrode current collector for negative electrode-free battery
[0097] A negative electrode current collector for a negative electrode-free battery was prepared in the same manner as in Example 1, except that a VdF-HFP copolymer containing 5 wt % of units derived from HFP was used instead of a VdF-HFP copolymer containing 15 wt % of units derived from HFP.
[0098] The thickness of the conductive layer included in the negative electrode current collector for a negative electrode-free battery of Example 3 was 2.5 μm.
[0099] Example 4: Preparation of negative electrode current collector for negative electrode-free battery
[0100] A negative electrode current collector for a negative electrode-free battery was prepared in the same manner as in Example 1, except that a VdF-HFP copolymer containing 20 wt % of units derived from HFP was used instead of a VdF-HFP copolymer containing 15 wt % of units derived from HFP.
[0101] The thickness of the conductive layer included in the negative electrode current collector for a negative electrode-free battery of Example 4 was 2.5 μm.
[0102] Example 5: Preparation of negative electrode collector for negative electrode-free battery
[0103] A negative electrode current collector for a negative electrode-free battery was prepared in the same manner as in Example 1, except that a VdF-CTFE copolymer containing 20 wt % of units derived from chlorotrifluoroethylene (CTFE) was used instead of a VdF-HFP copolymer containing 15 wt % of units derived from HFP.
[0104] The thickness of the conductive layer included in the negative electrode current collector for a negative electrode-free battery of Example 5 was 2.5 μm.
[0105] Comparative Example 1: Preparation of negative electrode current collector for negative electrode-free battery
[0106] A negative electrode current collector for a negative electrode-free battery was prepared in the same manner as in Example 1, except that when drying the conductive layer-forming composition, drying was performed at 100° C. for 10 hours under a vacuum condition (about −0.1 MPa) and no additional drying was performed.
[0107] The thickness of the conductive layer included in the negative electrode current collector for a negative electrode-free battery of Comparative Example 1 was 2.5 μm.
[0108] Comparative Example 2: Preparation of negative electrode current collector for negative electrode-free battery
[0109] A negative electrode current collector for a negative electrode-free battery was prepared in the same manner as in Example 1, except that polyvinylidene fluoride (PVdF) was used instead of the VdF-HFP copolymer containing 15 wt % of units derived from HFP.
[0110] The thickness of the conductive layer included in the negative electrode current collector for a negative electrode-free battery of Comparative Example 2 was 2.5 μm.
[0111] Experimental Example 1: X-ray diffraction analysis
[0112] The negative electrode current collectors for negative electrode-free batteries prepared in Example 1 and Comparative Example 1 were subjected to X-ray diffraction analysis of the conductive layer. Figure 1 and Figure 2 The results of X-ray diffraction analysis of the conductive layers of Example 1 and Comparative Example 1 are shown respectively.
[0113] The XRD analysis conditions are as follows.
[0114] 1) Type and wavelength of light source: An X-ray wavelength generated by Cu Kα was used, and the wavelength (λ) of the light source was 0.15406 nm.
[0115] 2) Sample preparation method: After cutting the conductive layer into the size of a cover glass, prepare the sample by bonding the conductive layer to the cover glass with a double-sided tape. After attaching the prepared sample to the groove of the holder, perform a flattening operation using a slide glass so that the height of the sample is constant.
[0116] 3) XRD analysis equipment setting conditions: The fixed divergence slit (FDS) was set to 0.5 and an energy dispersive 1D detector was used as a detector. The measurement mode was set to the linear mode, the measurement range was set to a 2θ range of 10° to 30°, and the measurement conditions were set to perform a 2θ scan at 0.016° in 4 seconds.
[0117] refer to Figure 1 In the conductive layer of Example 1, a main peak was observed at about 20.7°. Therefore, it was confirmed that the β phase was the dominant phase in the PVdF contained in the conductive layer of Example 1.
[0118] In contrast, in the conductive layer of Comparative Example 1, a main peak was observed at about 20.0°. Therefore, it was confirmed that the α phase was the dominant phase in the PVdF contained in the conductive layer of Comparative Example 1.
[0119] When the general Figure 1 and Figure 2 When compared with each other, it can be understood that the main peak intensity in the X-ray diffraction analysis result of Comparative Example 1 is higher than that of Example 1. This means that the crystallinity of the conductive layer of Comparative Example 1 is higher than that of the conductive layer of Example 1.
[0120] Taking these points into consideration, it can be understood that the conductive layer of Example 1 and the negative electrode current collector for a negative electrode-free battery including the same include PVdF having a relatively low crystallinity and having the β phase as a dominant phase.
[0121] Experimental Example 2: Evaluation of charge and discharge efficiency
[0122] <Preparation of negative electrode-free battery>
[0123] LiCoO2 as a positive electrode active material, carbon black as a conductive material, and PVDF as a binder were mixed in an N-methylpyrrolidone solvent in a weight ratio of 96:2:2 to prepare a positive electrode slurry, and the positive electrode slurry was coated on an aluminum current collector (thickness: 20 μm), and then dried and rolled to form a positive electrode active material layer (thickness: 130 μm), which was used as a positive electrode.
[0124] An electrode assembly is prepared, the electrode assembly comprising a negative electrode collector for a negative electrode-free battery according to Example 1, a positive electrode facing the negative electrode collector, and a polyethylene separator disposed between the positive electrode and the negative electrode, and after the electrode assembly is housed in a battery case, an electrolyte is injected and the battery case is sealed to prepare a negative electrode-free battery.
[0125] In this case, as the electrolyte, an electrolyte was used in which ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were mixed in a volume ratio of 2:8 as an organic solvent, 0.5 wt % of vinylene carbonate (VC) was added as an additive based on the total weight of the electrolyte, and LiPF6 was added as a lithium salt at a concentration of 1.2 mol / L.
[0126] Negative electrode-free batteries of Examples 2 to 5 and Comparative Examples 1 and 2 were prepared in the same manner as in Example 1, except that the negative electrode current collectors for negative electrode-free batteries of Examples 2 to 5 and Comparative Examples 1 and 2 were used.
[0127] <Evaluation of Capacity Retention Rate>
[0128] The negative electrode-free batteries of the above-prepared examples and comparative examples were cyclically charged and discharged at 25°C under the following conditions to evaluate the capacity retention rate. The graph of the capacity retention rate as a function of the cycle is shown in Figure 3 The capacity retention rate at the 5th cycle is shown in the following Table 1.
[0129] The capacity retention rate was evaluated by the following formula.
[0130] Capacity retention rate (%) = {(discharge capacity of the battery without negative electrode at the Nth cycle) / (discharge capacity of the battery without negative electrode at the first cycle)}×100
[0131] (In the above formula, N is an integer greater than 1)
[0132] * Charge and discharge conditions
[0133] Charging: CC / CV (constant current / constant voltage) mode; 0.1 C; 4.45 V, 1 / 20 C cutoff
[0134] Discharge: CC mode; 0.1 C; 3.0 V cutoff
[0135]
[0136] Refer to Table 1 and Figure 3 It can be understood that the negative electrode-free battery according to the embodiment has better charge and discharge efficiency than the negative electrode-free battery according to the comparative example.
Claims
1. A negative electrode current collector for a negative electrode-free battery, the negative electrode current collector comprising: a metal current collecting substrate; and A conductive layer disposed on the metal current collecting substrate, wherein the conductive layer comprises an ion-conducting polymer, and The ion-conducting polymer comprises: units derived from vinylidene fluoride, and units derived from at least one monomer selected from the group consisting of hexafluoropropylene and chlorotrifluoroethylene, During X-ray diffraction analysis of the conductive layer, a main peak exists within a 2θ range of 20.5° to 20.9°. 2 . The negative electrode current collector for a negative electrode-free battery according to claim 1 , wherein the content of the unit derived from at least one monomer selected from the group consisting of hexafluoropropylene and chlorotrifluoroethylene in the ion conductive polymer is 1% by weight to 30% by weight. 3 . The negative electrode current collector for a negative electrode-free battery according to claim 1 , wherein the conductive layer further comprises a lithium salt.
4. The negative electrode current collector for a negative electrode-free battery according to claim 3, wherein the lithium salt comprises at least one selected from the group consisting of LiCl, LiBr, LiI, LiNO3, LiClO4, LiBF4, LiB 10 Cl 10 , LiPF6, LiCF3SO3, LiCF3CO2, LiAsF6, LiSbF6, LiAlCl4, CH3SO3Li, CF3SO3Li, LiSCN, LiC(CF3SO2)3, (CF3SO2)2NLi, (FSO2)2NLi, lithium chloroborane, lithium lower aliphatic carboxylate, lithium 4-phenylborate and lithium imide. 5 . The negative electrode current collector for a negative electrode-free battery according to claim 3 , wherein the lithium salt comprises LiNO 3 . 6 . The negative electrode current collector for a negative electrode-free battery according to claim 3 , wherein the content of the lithium salt in the conductive layer is 0.1 wt % to 20 wt %. 7 . The negative electrode current collector for a negative electrode-free battery according to claim 1 , wherein the conductive layer has a thickness of 1 μm to 50 μm. 8 . The negative electrode current collector for a negative electrode-free battery according to claim 1 , wherein the metal current collector substrate comprises at least one selected from the group consisting of copper, stainless steel, aluminum, nickel, titanium, and aluminum-cadmium alloy. 9 . The negative electrode current collector for a negative electrode-free battery according to claim 1 , wherein the metal current collector substrate comprises copper.
10. A negative electrode-free battery, comprising: A negative electrode current collector for a negative electrode-free battery according to claim 1; A positive electrode facing the negative electrode current collector for the negative electrode-free battery; A separator disposed between the negative electrode current collector for the negative electrode-free battery and the positive electrode; and Electrolytes, The conductive layer is arranged to face the diaphragm.
11. The negative electrode-free battery according to claim 10, further comprising a lithium metal layer, wherein the lithium metal layer is formed on the negative electrode current collector for the negative electrode-free battery. The lithium metal layer is formed by charging the negative electrode-free battery to move lithium ions from the positive electrode.