Application of modified ZIF-L, pervaporation membrane and application of pervaporation membrane

By combining ZIF-L with CS-PVA polymer matrix, a high permeability and thermally stable permeability vaporization membrane was prepared, which solved the contradiction between water flux and intercept rate in the prior art and achieved efficient seawater Desalination and sewage regeneration.

CN118987979APending Publication Date: 2024-11-22SHANGHAI UNIV OF ENG SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411041402.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing permeable vaporization membrane reduces the retention rate when increasing the water flux. Conversely, the phenomenon of "seesaw" in which the water flux decreases when the interception rate increases, making it difficult to achieve efficient desalination in water treatment fields such as seawater desalination.

Method used

Using modified ZIF-L material combined with CS-PVA polymer matrix, the ZIF-L nanocomposite was grafted by PFSA solution to prepare a permeable vaporization membrane with high permeability, excellent hydrophilicity and thermal stability. The cast film liquid was repeatedly scraped on the porous support layer and dried to obtain a film having a thickness of 1-3 μm.

Benefits of technology

The water flux was increased to 9-40kg·m-2·h-1 and the salt retention rate reached 99.98-99.99%, while the thermal stability and hydrophilicity of the membrane were improved, and the water flux and retention rate were solved. The 'seesaw' phenomenon between the two is suitable for seawater desalination and sewage regeneration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118987979A_ABST
    Figure CN118987979A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of pervaporation membrane preparation, and particularly relates to application of modified ZIF-L, a pervaporation membrane and application of the pervaporation membrane, and the pervaporation membrane is prepared by coating an activated porous supporting layer with a membrane casting solution containing a modified ZIF-L material and drying after membrane forming. The PFSA-g-ZIF-L / CS-PVA pervaporation membrane is prepared by a solution coating method, that is, a thin pervaporation layer is coated on a porous support layer by a scraper, the porous support layer is coated with a membrane casting solution with a main component of a modified ZIF-L material, and then the PFSA-g-ZIF-L / CS-PVA pervaporation membrane is obtained by solvent evaporation. Meanwhile, the water flux of the pervaporation membrane can be increased to 9-40 kg.m <-2 >. H <-1 >, and the salt rejection rate can be increased to 99.98-99.99%; the invention aims to overcome the defects in the prior art, namely a'seesaw 'phenomenon that the retention rate is reduced when the water flux of a membrane is increased and the water flux is reduced when the retention rate is increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an application of modified ZIF-L, a pervaporation membrane and the application thereof, and belongs to the technical field of pervaporation membrane preparation. Background Art

[0002] With the development of industry and the increase in population, the problem of water shortage has rapidly become serious. Therefore, it is crucial to develop wastewater recycling and seawater desalination technologies. Viable methods include reverse osmosis (RO), membrane distillation (MD) and pervaporation. Pervaporation seawater desalination can separate brine at a lower heating temperature (50-90°C) by driving the chemical potential gradient. The heat used in the pervaporation process can come from low-grade (waste heat from industrial processes) or renewable (from solar or geothermal energy), which has great development prospects in terms of energy consumption. However, their performance is often limited by inherent characteristics such as low permeability and low selectivity. For example, in literature 1 (Ultrathin two-dimensional MXene membrane for pervaporation desalination [J]. Journal of membrane science, 2018, 548: 548-558.), an ultrathin MXene membrane with a thickness as low as tens of nanometers was prepared by stacking on a PAN substrate and used for pervaporation desalination. The water flux of the membrane is significantly improved, but the desalination rate is not high (only 99.5%); Reference 2 (Fabrication of La / Y-codoped microporous organosilica membranes for high-performance pervaporation desalination [J]. Journal of membrane science, 2019, 584: 353-363.) successfully prepared La / Y co-doped microporous organosilica membranes by sol-gel method. The desalination rate of the membrane can reach more than 99.9, but its maximum flux is only 10.3 kg·m -2 ·h -1; Literature 3 (Preparation and characterization of PVA-g-GO / PVA / PAN composite membrane for pervaporation desalination [J]. The Canadian Journal of Chemical Engineering, 2023, 101: 2199-2211.) prepared a PVA-g-GO / PVA / PAN pervaporation membrane, and obtained a high rejection rate of 99.99% and a pervaporation rate of 4.46 kg·m -2 ·h -1 The low flux, that is, the "seesaw" phenomenon in which the rejection rate decreases when the membrane water flux increases, and the water flux decreases when the rejection rate increases.

[0003] Therefore, selecting a suitable material and preparing a mixed matrix membrane that can overcome the "seesaw" phenomenon in which the rejection rate decreases when the water flux increases and the water flux decreases when the rejection rate increases is of great significance for water treatment fields such as seawater desalination. Summary of the invention

[0004] The present invention provides an application of modified ZIF-L, a pervaporation membrane and the application thereof. In the pervaporation membrane, the modified ZIF-L (abbreviated as PFSA-g-ZIF-L) has good compatibility with a CS-PVA polymer matrix and is mixed into the CS-PVA polymer matrix, so that the pervaporation membrane has high permeability, high salt rejection rate, excellent hydrophilicity and good thermal stability.

[0005] The technical problem to be solved by the present invention is achieved by adopting the following technical solutions:

[0006] The modified ZIF-L material can be used for preparing casting liquid, pervaporation membrane, treating chemical wastewater, pharmaceutical wastewater, seawater desalination and sewage regeneration materials. The modified ZIF-L material is prepared by grafting PFSA solution onto the surface of amino-containing ZIF-L material.

[0007] A pervaporation membrane is obtained by coating a casting liquid containing a modified ZIF-L material on an activated porous support layer, forming a membrane and then drying it. The thickness of the casting liquid after film formation and drying is 1 to 3 μm.

[0008] Preferably, the casting solution is repeatedly scraped twice on the dried porous support layer to form a membrane, and then placed in a 45-55° C. oven for drying for 24-36 hours to obtain a high-performance PFSA-g-ZIF-L / CS-PVA pervaporation membrane.

[0009] It should be noted that in the above coating method, the casting solution is repeatedly scraped twice on the activated porous support layer using a scraper, and the second scraping can be performed only after the solution on the membrane is completely dry.

[0010] Furthermore, the film has a thickness of 1.5 to 2.5 μm and is dried at 45 to 50° C. for 24 to 30 hours.

[0011] Furthermore, the film thickness was 2 μm and dried at 50° C. for 24 h.

[0012] Preferably, the modified ZIF-L material is prepared by grafting a PFSA solution onto the surface of an amino-containing ZIF-L material (abbreviated as NH2-ZIF-L).

[0013] Furthermore, the modified ZIF-L material is modified from an amino-containing ZIF-L material as a raw material in the following manner: NH2-ZIF-L nanoparticles are dissolved in an alcohol aqueous solution containing 0.3-3wt% PFSA, the mass ratio of the PFSA solution to the amino-containing ZIF-L material is 1-10:1, and the reaction is carried out at 25-45°C for 24-35h to obtain a PFSA-g-ZIF-L nanocomposite, which is then post-treated to obtain a PFSA-g-ZIF-L nanocomposite, i.e., the modified ZIF-L material.

[0014] It should be noted that the temperature is set at 25-45°C, which is conducive to accelerating the reaction, and the time is set at 24-35h, which is conducive to the full reaction of PFSA and ZIF-L; through the electrophilic substitution reaction between the amino group of NH2-ZIF-L and the sulfonic acid group of the PFSA solution, the PFSA-g-ZIF-L nanocomposite, that is, the modified ZIF-L material, is obtained.

[0015] Preferably, the mass ratio of the PFSA solution to the amino-containing ZIF-L material is 1-10:1, and the grafting conditions are: mixing at 25-30° C. for 24-30 hours.

[0016] Preferably, the amino-containing ZIF-L material is NH2-Co / Zn-ZIF-L nanoparticles, and the PFSA solution is a PFSA alcohol aqueous solution, and its concentration is 0.01-0.1 g·mL -1 ; The volume ratio of alcohol to water is 1:0.5-2. In a preferred embodiment of the present invention, the volume ratio of alcohol to water is 1:1.

[0017] Preferably, the casting solution is obtained by mixing modified ZIF-L material, CS-PVA, a solvent and a cross-linking agent.

[0018] Preferably, the mixing conditions of the casting solution are: stirring at 20-25° C. for 24-30 hours; the mass ratio of the total amount of CS and PVA, modified ZIF-L material, cross-linking agent, and solvent is 1: 0.02-0.1: 0.02-0.05: 25-35, and the mass ratio of CS to PVA is 3.5-4.5: 1.

[0019] It should be noted that the total mass of the substances in the casting solution formula is a constant. When the addition amounts of CS, PVA, and MA are fixed, changing the addition amount of PFSA-g-ZIF-L nanocomposite will change the corresponding amount of solvent. Increasing the content of PFSA-g-ZIF-L nanocomposite will affect the structure, water flux, retention rate, and surface roughness of the membrane.

[0020] Preferably, the activated porous support layer is activated by the porous support layer in the following manner:

[0021] The porous support layer is immersed in a NaOH aqueous solution for hydrolysis treatment; after the hydrolysis is completed, the porous support layer is taken out, and repeatedly rinsed with deionized water until the pH is neutral, and dried at room temperature.

[0022] Furthermore, the concentration of the NaOH aqueous solution is 0.8-1.2 mol / L, the soaking time is 1-2 hours, and the flushing time is 5-8 minutes.

[0023] Preferably, the solvent is water and acetic acid, and the mass ratio of water to acetic acid is 40-50:1, and the cross-linking agent is maleic anhydride.

[0024] Preferably, the activated porous supporting layer is an activated PAN base membrane.

[0025] Preferably, the coating thickness is 1-3 μm, and the coating is dried at 45-55° C. for 24-36 hours.

[0026] The above-mentioned pervaporation membrane is used in the preparation and treatment of chemical wastewater, pharmaceutical wastewater, seawater desalination and sewage regeneration materials.

[0027] The beneficial effects of the present invention are:

[0028] (1) In the present invention, the PFSA-g-ZIF-L / CS-PVA pervaporation membrane is prepared by a solution coating method, that is, a thin pervaporation layer is coated on a porous support layer with a doctor blade, and then the solvent is evaporated to obtain the pervaporation membrane. When the PFSA-g-ZIF-L nanocomposite is added to the polymer matrix, the water flux of the pervaporation membrane can be increased to 9-40 kg·m -2 ·h -1) and salt rejection rate to 99.98-99.99%, which solves the shortcomings of the prior art, that is, the "seesaw" phenomenon that the rejection rate decreases when the membrane water flux increases, and conversely, the water flux decreases when the rejection rate increases.

[0029] (2) The present invention effectively improves the hydrophilicity and swelling degree of the pervaporation membrane, and improves the thermal stability of the pervaporation membrane, which is conducive to performing pervaporation experiments at a high temperature of about 65°C;

[0030] (3) The pervaporation membrane of the present invention is easy to prepare, low in cost, has a wide range of applications, and has good application prospects;

[0031] (4) During the preparation of the pervaporation membrane of the present invention, due to the grafting modification of ZIF-L by PFSA, the PFSA-g-ZIF-L nanocomposite can stably exist in the pervaporation membrane, thereby improving the stability and long-term performance of the pervaporation membrane;

[0032] (5) The reason why adding PFSA-g-ZIF-L nanocomposite to modify CS-PVA pervaporation membrane can improve the water flux and salt retention rate of the pervaporation membrane is as follows:

[0033] (A) The addition of the PFSA-g-ZIF-L nanocomposite of the present invention increases the transport path of water molecules in the pervaporation membrane and reduces the mass transfer resistance during the permeation of components;

[0034] (B) Amino groups and -SO3 in the PFSA-g-ZIF-L nanocomposite of the present invention - The hydrophilic groups enhance the hydrophilicity of the pervaporation membrane, and at the same time increase the membrane's ability to bind salt ions and the steric hindrance within the membrane, thereby increasing the membrane's selectivity for salt ions.

[0035] (C) PFSA grafting provides additional cross-linking sites, thus forming a denser network that can inhibit the diffusion of salt ions and improve the retention rate of the pervaporation membrane;

[0036] (D) The pore size (0.663 nm) of the PFSA-g-ZIF-L nanocomposite of the present invention determined by nitrogen adsorption measurement is located between water molecules (~0.27 nm) and hydrated sodium (~0.72 nm), allowing the pervaporation membrane to intercept salt ions with a high retention rate.

[0037] In summary, the excellent performance of the PFSA-g-ZIF-L nanocomposite can be used to effectively improve the hydrophilicity of the membrane, while having a higher water flux and salt retention rate. At the same time, compared with pure CS-PVA pervaporation membrane, the PFSA-g-ZIF-L / CS-PVA membrane has higher thermal stability. Moreover, due to the grafting modification of ZIF-L by PFSA, the PFSA-g-ZIF-L nanocomposite can stably exist in the membrane, thereby improving the long-term performance of the membrane. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 The infrared spectra of PFSA, Co / Zn-ZIF-L, NH2-ZIF-L and PFSA-g-ZIF-L nanomaterials in the embodiments of the present invention;

[0039] Figure 2 XRD spectra of PFSA, Co / Zn-ZIF-L, NH2-ZIF-L and PFSA-g-ZIF-L nanomaterials in the embodiments of the present invention;

[0040] Figure 3 This is a pore structure analysis diagram of the PFSA-g-ZIF-L nanomaterial in an embodiment of the present invention;

[0041] Figure 4 The scanning electron microscope (SEM) images of PFSA, Co / Zn-ZIF-L, NH2-ZIF-L and PFSA-g-ZIF-L nanomaterials in the embodiments of the present invention are shown;

[0042] Figure 5 1 is a scanning electron microscope (SEM) image of the upper surface and cross section of the pervaporation membrane in an embodiment of the present invention;

[0043] Figure 6 This is a graph showing the water flux and retention rate of the membrane for desalination of a 3.5 wt. % NaCl aqueous solution at 35° C. in an example of the present invention. DETAILED DESCRIPTION

[0044] In order to make the technical means, creative features, objectives and effects of the present invention easier to understand, the present invention is further described below with reference to specific illustrations.

[0045] In the present invention, the post-treatment process used is the basic knowledge known in the art, including centrifugation, deionized washing, ethanol washing and freeze drying. The specific process parameters depend on the actual situation and are not elaborated in detail in this article.

[0046] The present invention adds modified ZIF-L material to the polymer separation layer of the pervaporation membrane for the first time. Different from the PFSA-g-GO nanomaterial in the prior art, which desalinates through the interlayer spaces stacked between GO nanosheets, the two-dimensional ZIF-L has abundant micropores, providing more water channels for the pervaporation membrane.

[0047] The following terms of the present invention are explained:

[0048] English abbreviation Chinese name PFSA Perfluorosulfonic acid PVA Polyvinyl alcohol ZIF-L Zeolite imidazolate framework materials CS Chitosan 2-MeIm 2-Methylimidazole CS-PVA Polymer Matrix Molecular chain formed by PFSA, CS and PVA Polymer chain PAN Polyacrylonitrile GO Graphene oxide g graft PFSA-g-ZIF-L Modified ZIF-L after PFSA grafting

[0049] Example 1

[0050] The preparation method of PFSA-g-ZIF-L nanomaterials has the following specific steps:

[0051] (1) Co / Zn-ZIF-L nanoparticles were synthesized at room temperature. First, 0.723 g Zn(NO3)2·6H2O powder and 0.707 g Co(NO3)2·6H2O powder were added to 100 mL deionized water, named solution A. Another 100 mL deionized water was added with 2.384 g 2-MeIm powder, named solution B. Solution B was poured into solution A to obtain a mixture, and then the mixture was reacted at 25°C for 95 min. After post-treatment, Co / Zn-ZIF-L nanoparticles were obtained. The infrared spectrum of the prepared Co / Zn-ZIF-L nanoparticles (see Figure 2) Figure 1 Co / Zn-ZIF-L nanoparticles in) and SEM images (such as Figure 4 shown).

[0052] (2) The preparation process of NH2-ZIF-L nanomaterials is as follows: first, 3 g of 2-aminoimidazole is dissolved in 50 mL of deionized water and stirred to obtain a mixed solution. 1 g of Co / Zn-ZIF-L nanoparticles is added to the mixed solution to obtain a mixture. The mixture is reacted at 25°C for 12 h. After post-treatment (centrifugation, deionized water washing, ethanol washing, and freeze drying), NH2-ZIF-L nanoparticles are obtained. The infrared spectrum of the prepared NH2-ZIF-L nanoparticles (see Figure 1 NH2-ZIF-L), XRD spectrum and SEM diagram, such as Figure 1 , 2 , as shown in 4;

[0053] (3) Preparation of PFSA-g-ZIF-L nanocomposite (modified ZIF-L material): First, 9 g PFSA was dissolved in 30 mL of alcohol aqueous solution (15 mL ethanol and 15 mL pure water) to obtain a concentration (c1) of 0.3 g mL -1The solution was clarified, and then 9 g of NH2-ZIF-L nanoparticles were added to the solution to obtain a mixture. The mixture was then reacted at a temperature of (T1) 25°C for 24 h (t1). Finally, the mixture was centrifuged, washed with deionized water, washed with ethanol, and dried to obtain a PFSA-g-ZIF-L nanocomposite. The infrared spectrum of the prepared PFSA-g-ZIF-L nanocomposite (as shown in FIG. Figure 1 PFSA-g-ZIF-L).

[0054] Depend on Figure 1 As can be seen from the ATR-FTIR spectra of PFSA, ZIF-L, NH2-ZIF-L and PFSA-g-ZIF-L nanomaterials, the absorption peak of PFSA is at 1041 cm -1 Corresponding to -SO3 2- Tensile vibration; 963cm -1 The peaks at 1200 and 1126 cm are related to the symmetric stretching vibration of COC; -1 The peak at 3273 cm corresponds to the CF stretching vibration. -1 Corresponds to the hydroxyl bond. For NH2-ZIF-L, 3432 cm -1 A new peak (NH bond stretching) appears near 1610 cm -1 (bending of the NH bond), which indicates that -NH2 was successfully synthesized on ZIF-L.

[0055] For PFSA-g-ZIF-L, 3432, 1636, and 1425 cm -1 The characteristic peaks of NH2-ZIF-L are retained at 1237 and 1147, 1053 and 971 cm -1 The peaks at correspond to CF and SO3 in PFSA. 2- stretching vibration and COC symmetric stretching vibration; it shows that during the preparation of the modified ZIF-L material, a bonding interaction occurred between PFSA and ZIF-L crystals, and the PFSA-g-ZIF-L nanomaterial was successfully synthesized.

[0056] Figure 2 It can be seen from the XRD spectra of NH2-ZIF-L and PFSA-g-ZIF-L that the peak at 16.38° only shows the diffuse reflection peak of the amorphous polymer PFSA, but does not show the typical characteristic peak of NH2-ZIF-L. The reason is that the signal of NH2-ZIF-L as a substrate is masked by the molecular chain of PFSA. The small and sharp peaks at 28.14° and 31.45° should be the characteristic peaks of ZIF-L, which also indicates the successful grafting of PFSA on NH2-ZIF-L. The synthesized PFSA-g-ZIF-L is a cross-shaped multi-petal material, which can be seen from Figure 4Learn.

[0057] Embodiments 2 to 5

[0058] The preparation method of PFSA-g-ZIF-L nanocomposite, the specific steps of which are basically the same as those of Example 1, except for the reaction parameters, which are specifically shown in Table 1;

[0059] Table 1

[0060] Preparation parameters <![CDATA[T1]]> <![CDATA[t1]]> <![CDATA[c1]]> <![CDATA[W1]]> unit ℃ h wt% Example 2 25 24 0.6 2.5:1 Example 3 28 24 1.6 5:1 Example 4 25 28 3 10:1 Example 5 30 30 0.3 1:1

[0061] Among them, the infrared spectrum of Example 3 is shown in Figure 1 PFSA-g-ZIF-L in; XRD pattern of Example 3 is shown in Figure 2 ; BET and pore size analysis of Example 3 are shown in Figure 3 ; Examples 2 to 5 were subjected to scanning electron microscope (SEM) tests, and the test results were as follows Figure 4 shown.

[0062] from Figure 3 It can be seen that the pore size of ZIF-L and PFSA-g-ZIF-L measured by nitrogen adsorption is 0.663nm, which is between water molecules (~0.27nm) and hydrated sodium molecules (~0.72nm), allowing water molecules to pass through the membrane while hydrated sodium ions are excluded. Therefore, the pervaporation membrane has a high rejection rate.

[0063] Example 6

[0064] A method for preparing a pervaporation membrane, the specific steps are as follows:

[0065] (1) After mixing the PFSA-g-ZIF-L prepared in Example 1, the CS-PVA solution and maleic anhydride, the mixture was stirred at 23° C. for 24 h to obtain a casting solution, wherein the mass of the CS-PVA solution was 90 g, including 2.4 g of CS, 0.6 g of PVA, 85 g of water, 2 g of acetic acid, 0.06 g of the PFSA-g-ZIF-L nanocomposite, and 0.09 g of the crosslinking agent MA;

[0066] (2) Prepare a 1 mol / L NaOH aqueous solution (add 40 g of NaOH particles to 1 L of pure water), and immerse the PAN base film in the solution for 1 hour for hydrolysis. Then take out the PAN base film, rinse it repeatedly with deionized water for 8 minutes, and then dry it at room temperature;

[0067] (3) The casting solution was repeatedly scraped on the dried PAN base film twice to form a film, and then placed in a 50°C oven for drying for 24 hours to obtain a high-performance PFSA-g-ZIF-L / CS-PVA pervaporation membrane with a thickness of 2 μm;

[0068] In addition, Example 6 was selected for TG test. The test method is detailed in Reference 3. The test results are shown in Table 3.

[0069] Example 6 was selected to perform water contact angle test. The test method is detailed in Reference 3. The test results are shown in Table 3.

[0070] Embodiments 7 to 12

[0071] A method for preparing a pervaporation membrane, the specific steps are as follows:

[0072] (1) After mixing the PFSA-g-ZIF-L, CS-PVA, solvent and cross-linking agent prepared in Examples 2 to 4, the mixture was stirred at a temperature (T2) of 20 to 25°C for 24 to 30 hours (t2) to obtain a casting solution, wherein the mass ratio (W2) of the solvent to the PFSA-g-ZIF-L nanocomposite was 290 to 5772:1, the mass ratio (W3) of the solvent to the CS-PVA was 28 to 30:1, and the mass ratio (W4) of the cross-linking agent MA to the CS-PVA was 3% to 5%; the solvent was a mixture of acetic acid and water in a mass ratio of 1:40.

[0073] (2) The casting solution was repeatedly scraped on the dried PAN substrate twice to form a film, and the film thickness was controlled to be 2 μm. The film was placed in a 50° C. oven and dried for 24 h to obtain a high-performance PFSA-g-ZIF-L / CS-PVA pervaporation membrane;

[0074] The specific preparation parameters of Examples 7 to 12 are shown in Table 2, wherein MA is maleic anhydride;

[0075] Table 2

[0076] Preparation parameters X Crosslinking agent <![CDATA[T2]]> <![CDATA[t2]]> <![CDATA[W2]]> <![CDATA[W3]]> <![CDATA[W4]]> unit ℃ h % Example 7 2 MA 22 24 1441 29 3 Example 8 3 MA 25 30 1441 29 3 Example 9 4 MA 23 23 1441 29 3 Example 10 3 MA 24 26 5772 28 3 Embodiment 11 3 MA 24 24 580 28 3 Example 12 3 MA 21 28 290 30 3

[0077] In addition, Examples 7 to 12 were selected for TG testing. The testing method is detailed in Reference 3, and the test results are shown in Table 3.

[0078] Examples 7 to 12 were selected for water contact angle test. The test method is detailed in Reference 3. The test results are shown in Table 3.

[0079] The upper surface and cross section of M9 were selected for scanning electron microscope (SEM) testing. The test results are as follows: Figure 5 shown.

[0080] Comparative Example 1

[0081] A method for preparing a CS-PVA pervaporation membrane, wherein the steps are substantially the same as those of Example 6, except that the PFSA-g-ZIF-L nanocomposite is not added.

[0082] Comparative Example 2

[0083] A method for preparing a ZIF-L / CS-PVA pervaporation membrane, wherein the steps are substantially the same as those of Example 6, except that the added PFSA-g-ZIF-L nanocomposite is replaced by ZIF-L nanoparticles.

[0084] Comparing Example 11 with Comparative Example 2, the water flux and retention rate of Comparative Example 2 are lower than those of Example 11.

[0085] Comparative Example 3

[0086] A method for preparing a PFSA / CS-PVA pervaporation membrane, wherein the steps are substantially the same as those of Example 6, except that the added PFSA-g-ZIF-L nanocomposite is replaced with PFSA. The infrared spectrum of PFSA is as follows: Figure 1 shown.

[0087] test:

[0088] M1~M3 were selected for TG test. The test method is detailed in Reference 3 and the test results are shown in Table 3.

[0089] M1~M3 were selected for water contact angle test. The test method is detailed in Reference 3. The test results are shown in Table 3.

[0090] The upper surface and cross section of M1 were selected for scanning electron microscope (SEM) testing. The test results are as follows: Figure 5 As shown;

[0091] Select M1-M3 for water flux and interception rate test. The test results are as follows: Figure 6 shown.

[0092] like Figure 5 As shown, the modified ZIF-L material on the pervaporation membrane is evenly distributed, and by comparing Example 11 with Comparative Example 1, it is found that Example 11 has a flatter surface. The reason is that the grafting of the polymer (i.e., PFSA solution) in the modified ZIF-L material provides additional cross-linking sites, and PFSA interacts with CS-PVA to form a denser network, which can inhibit the diffusion of salt ions.

[0093] from Figure 6 It can be found that the pervaporation desalination performance of Example 11 and Example 12 is almost the same, and the amount of modified ZIF-L material added in Example 11 is only half of that in Example 12. Therefore, Example 11 is more economical and is conducive to industrial production and application.

[0094] The performance indicators of the pervaporation membranes prepared in Comparative Examples 1 to 3 are shown in Table 3, wherein the rejection rate is the rejection rate for salt ions, and the residual weight is the residual weight at 800°C after TG test; the pervaporation membranes are numbered M1-M3, and the specific corresponding relationship is shown in Table 3;

[0095] The performance indicators of the PFSA-g-ZIF-L / CS-PVA pervaporation membranes prepared in Examples 6 to 12 are shown in Table 3, where the retention rate is the retention rate for salt ions, and the residual weight is the residual weight at 800°C after TG test; the pervaporation membrane numbers are M4-M 10 , the specific corresponding relationship is shown in Table 3.

[0096] Table 3

[0097] Serial number Film serial number Water flux Retention rate Film thickness Residual weight Water contact angle unit <![CDATA[kg·m -2 ·h -1 ]]> % μm % ° Comparative Example 1 M1 6.7 99.95 1.664 32.35 59.01 Comparative Example 2 M2 8.9 99.97 1.920 28.50 65.18 Comparative Example 3 M3 9.4 99.98 1.584 30.87 60.54 Example 6 M4 11.6 99.99 1.754 33.65 56.05 Example 7 M5 12.4 99.99 1.826 34.02 55.66 Example 8 M6 13.1 99.99 1.846 34.11 55.23 Example 9 M7 9.5 99.98 1.569 35.42 56.45 Example 10 M8 11.5 99.99 1.746 37.66 55.65 Embodiment 11 M9 15.6 99.99 1.668 39.02 53.60 Example 12 M10 15.8 99.99 1.775 40.12 52.23

[0098] As shown in Table 3, the water contact angles of Examples 11 and 12 are smaller than those of Comparative Example 1, indicating that the pervaporation membranes in Examples 11 and 12 are hydrophilic. The reason is that: with the addition of PFSA-g-ZIF-L nanocomposites in Examples 11 and 12, the hydrophilic PFSA-g-ZIF-L contains abundant hydrophilic functional groups and long polymer chains, which enhances the hydrophilicity of the membrane. In addition, the sulfonic acid groups can bind water molecules and form a hydration layer, which can tightly capture water molecules, increase the ability to absorb water molecules, and indirectly reduce hydrophobicity. The abundant hydrophilic groups also increase the water volume fraction, making the pervaporation membrane surface more hydrophilic.

[0099] As can be seen from Table 3, the residual weight of the pervaporation membranes in Examples 11 and 12 is greater than that in other Examples and Comparative Examples, indicating that the addition of PFSA-g-ZIF-L improves the thermal stability of the pervaporation membrane. Since PFSA has excellent thermal stability and the polymer chain has good compatibility with PFSA-g-ZIF-L, the amino and sulfonic acid groups in PFSA-g-ZIF-L are cross-linked with the hydrophilic groups in CS-PVA, resulting in uniform dispersion of PFSA-g-ZIF in the polymer matrix, forming a more stable intramolecular structure, reducing the mobility of the polymer chain, and improving the thermal stability of the membrane.

[0100] In addition, other groups present in the polymer, such as sulfonate groups, increase the membrane's ability to bind to salt ions and increase the membrane's steric hindrance, thereby increasing the membrane's selectivity for salt ions. In addition, amino modification and PFSA grafting make PFSA-g-ZIF-L rich in hydrophilic groups (such as amino groups and sulfonic acid groups), making it easier for water molecules to adsorb on the membrane, so the water flux increases with the increase in the amount of PFSA grafting. Moreover, the addition of porous modified ZIF-L materials increases the transport path of water molecules in the pervaporation membrane and reduces the mass transfer resistance during the component permeation process, which is one of the reasons for the increase in water flux.

[0101] Application Example 1

[0102] At 35°C, a 3.5 wt% salt solution (35 g of sodium chloride granules added to 965 g of pure water) was subjected to a pervaporation test, specifically:

[0103] The pervaporation membrane of the present invention is sealed in a stainless steel module with an effective area of ​​12.56 cm 2 The feed tank was placed in a constant temperature water bath to maintain a stable temperature of 35°C. The raw material solution was pumped through a peristaltic pump at a rate of 100 L·h -1 The liquid is then sucked into the membrane assembly at a rate of , and then the feed liquid returns to the feed tank. The steam on the permeation side of the membrane assembly is collected by a liquid nitrogen cold trap, and the membrane evaporation side is evacuated at 2.0 kPa by a vacuum pump, and the permeation steam is collected by a liquid nitrogen cold trap for pervaporation testing.

[0104] In addition, the pervaporation test of M9 at 35℃~65℃ was selected, and the test conditions were consistent with those of Application Example 1. The test results are shown in Table 4;

[0105] Table 4

[0106]

[0107] In Table 4, the pervaporation membrane has a rejection rate of up to 99.99% for 3.5 wt.% NaCl aqueous solution at 35°C, and a water flux of 15.6 kg·m -2 ·h -1 , see Table 4.

[0108] It can still maintain excellent water flux (37.5kg·m -2 ·h -1 ) and retention rate (99.99%), effectively improving the pervaporation performance of the membrane and enhancing the hydrophilicity and thermal stability of the membrane.

[0109] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. Application of modified ZIF-L materials in the preparation of casting solution, pervaporation membrane, treatment of chemical wastewater, pharmaceutical wastewater, seawater desalination and sewage regeneration materials. The modified ZIF-L materials are prepared by grafting PFSA solution onto the surface of amino-containing ZIF-L materials.

2. A pervaporation membrane, characterized in that: The casting solution containing the modified ZIF-L material is coated on the activated porous support layer, and the film is formed and then dried to obtain the film.

3. A pervaporation membrane according to claim 2, characterized in that: The modified ZIF-L material is prepared by grafting a PFSA solution onto the surface of a ZIF-L material containing amino groups.

4. A pervaporation membrane according to claim 3, characterized in that: The amino-containing ZIF-L material is NH2-Co / Zn-ZIF-L nanoparticles, and the PFSA solution is a PFSA alcohol aqueous solution.

5. A pervaporation membrane according to claim 2, characterized in that: The casting solution is obtained by mixing modified ZIF-L material, CS-PVA, solvent and cross-linking agent.

6. A pervaporation membrane according to claim 5, characterized in that: The mass ratio of the total amount of CS-PVA, the modified ZIF-L material, the cross-linking agent and the solvent is 1:0.02-0.1:0.001-0.05:25-35, and the mass ratio of CS to PVA is 3.5-4.5:

1.

7. A pervaporation membrane according to claim 5 or 6, characterized in that: The solvent is water and acetic acid, and the mass ratio of water to acetic acid is 45-50:

1. The cross-linking agent is maleic anhydride.

8. A pervaporation membrane according to claim 2, characterized in that: The activated porous supporting layer is an activated PAN base membrane.

9. A pervaporation membrane according to claim 2, characterized in that: The thickness of the film formed by the casting liquid after drying is 1-3 μm, and it is dried at 45-55° C. for 24-36 hours.

10. Use of the pervaporation membrane according to any one of claims 2 to 9 in the preparation of materials for treating chemical wastewater, pharmaceutical wastewater, seawater desalination and sewage regeneration.