Preparation method and application of adsorbent for removing cationic dye in wastewater

By introducing active functional groups on the Mg/Al-LDH surface to prepare ionic liquid modified magnesium-aluminum layered bimetallic hydroxide, the problem of insufficient adsorption capacity of existing adsorbents on cationic dyes is solved, and high-efficiency and low-cost cationic dyes are achieved Removes effects and supports multiple use of materials.

CN118988240APending Publication Date: 2024-11-22LUOYANG INST OF SCI & TECH

Patent Information

Application Number
CN202411251861.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing adsorbents have problems such as poor selectivity, high cost and difficulty in reusing cationic dye wastewater, especially the lack of adsorption capacity of magnesium-aluminum layered bimetallic hydroxides on cationic dyes.

Method used

By introducing active functional groups on the surface of Mg/Al-LDH, an ionic liquid modified magnesium-aluminum layered bimetallic hydroxide was prepared by in-situ coprecipitation method, and its surface properties were regulated to improve the selective adsorption effect of cationic dyes, and to achieve the Multiple reuse of materials.

Benefits of technology

It realizes efficient selective adsorption of cationic dyes in wastewater, with a removal rate of 98%, an adsorption amount of 1225mg/g, and the materials can be reused, reducing the cost of wastewater treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118988240A_ABST
    Figure CN118988240A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method and application of an adsorbent for removing cationic dye in wastewater, the preparation method comprises the following steps: adding Mg (NO3) 2.6 H2O and Al (NO3) 3.9 H2O into a beaker, adding deionized water, fully stirring to dissolve the Mg (NO3) 2.6 H2O and the Al (NO3) 3.9 H2O, then adding 1-propyl sulfonic acid-3-methylimidazole chloride ionic liquid into the beaker, continuously stirring, slowly dropwise adding a saturated NaOH solution, adjusting the pH value of the mixed solution to 10.5 + / -0.5, and reacting for 2-4 hours at the temperature of 30-60 DEG C; and then, putting the beaker into a constant-temperature water bath kettle, carrying out constant-temperature reaction for 24-48 hours at 65 DEG C, carrying out centrifugal separation on the obtained colloidal precipitate, washing the precipitate with deionized water until the precipitate is neutral, and carrying out vacuum drying, so that the modified magnesium-aluminum layered double-metal hydroxide adsorbent is obtained. The ionic liquid modified magnesium-aluminum layered double-metal hydroxide is prepared by utilizing an in-situ coprecipitation method, the preparation method is simple and convenient, the condition is mild, and the obtained product has a relatively large specific surface area, has excellent removal efficiency on cationic dyes in wastewater and can be repeatedly used.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of dye wastewater adsorption treatment, and more specifically to a preparation method and application of an adsorbent for removing cationic dyes from wastewater. Background Art

[0002] Cationic dyes are a type of textile dye that can generate positively charged colored ions when dissolved in water. The cations of the dye can combine with the acidic groups of the third monomer in the fabric to dye the fiber. It is a special dye for dyeing acrylic fibers, with the advantages of high strength, bright color, and good light fastness. However, due to the complex aromatic groups that make it difficult to biodegrade and decolorize, cationic dye wastewater has become one of the main harmful industrial wastewaters, posing a serious threat to the water environment and ecosystem. Therefore, the development of efficient and environmentally friendly wastewater treatment technology, especially the selective removal technology for cationic dyes, has become an urgent need in the current field of environmental protection.

[0003] As a commonly used wastewater treatment technology, adsorption has the advantages of simple operation and significant effect. Although traditional adsorbents (such as activated carbon, etc.) have certain adsorption capacity, they often have problems such as poor selectivity and difficulty in regeneration. In recent years, the research and development of new adsorbents has made significant progress. Layered double hydroxides (LDHs) are a typical representative of them. Their composition can be expressed as: [M 1-x 2+ M x 3+ (OH)2(A n- ) x / n ] x+ .mH2O, where M 2+ and M 3+ For divalent and trivalent metal cations, A n- Due to the unique layered structure, interlayer anion exchangeability, high anion exchange capacity, simple synthesis and low cost of LDHs, their application in the adsorption field has attracted increasing attention.

[0004] In recent years, magnesium aluminum layered double hydroxides (Mg / Al-LDH) have gradually attracted people's attention in the adsorption of environmental pollutants, but they are mostly used for inorganic anion adsorption (CN 117563550 A, CN 115845792A, CN105032342A), and are less used in the adsorption of anionic dyes (RSC Advances., 2024, 14: 15281, Journal of Water Process Engineering, 2024, 63: 105418, Process Safety and Environmental Protection, 2024, 186: 1387-1396), but have almost no adsorption capacity for cationic dyes. At present, commercial adsorbents (such as activated carbon) in the field of dye wastewater adsorption treatment have high cost, lack of selectivity and are difficult to reuse. Therefore, it is necessary to develop an adsorbent with simple preparation, low cost and excellent adsorption performance to achieve efficient adsorption and removal of cationic dyes in wastewater. Summary of the invention

[0005] The purpose of the present invention is to provide a preparation method and application of an adsorbent for removing cationic dyes in wastewater. Active functional groups are introduced into the surface of Mg / Al-LDH through surface modification, and its surface properties are regulated. An ionic liquid-modified magnesium aluminum layered double hydroxide is prepared by an in-situ coprecipitation method. The magnesium aluminum layered double hydroxide has a highly efficient selective adsorption effect on cationic dyes in wastewater and can be reused.

[0006] A preparation method of an adsorbent for removing cationic dyes from wastewater provided by the present invention comprises the following steps: adding Mg(NO3)2·6H2O and Al(NO3)3·9H2O into a beaker, adding deionized water and stirring thoroughly to dissolve Mg(NO3)2·6H2O and Al(NO3)3·9H2O, then adding 1-propylsulfonic acid-3-methylimidazolium chloride ion liquid into the beaker, continuing stirring, slowly dropping saturated NaOH solution into the obtained mixed solution, adjusting the pH value of the mixed solution to 10.5±0.5, continuing stirring for 2-6 hours, then placing the beaker in a constant temperature water bath, reacting at a constant temperature of 65°C for 24-48 hours, centrifuging the obtained colloidal precipitate, washing the centrifuged precipitate with deionized water until it is neutral, and then vacuum drying to obtain a modified magnesium-aluminum layered double metal hydroxide adsorbent.

[0007] The molecular formula of the 1-propylsulfonic acid-3-methylimidazolium chloride ion liquid is C7H 13 ClN2O3S, molecular weight is 240.71, purity is 99%, and its molecular structure is as follows:

[0008]

[0009] Preferably, the molar ratio of Mg(NO3)2·6H2O to Al(NO3)3·9H2O is (1-3):(1-3).

[0010] Preferably, the ratio of the mass (g) of 1-propylsulfonic acid-3-methylimidazolium chloride ion liquid to the sum of the moles (mol) of Mg(NO3)2·6H2O and Al(NO3)3·9H2O is (1-3)g:0.2mol.

[0011] Preferably, during centrifugal separation, the centrifuge speed is 8000 r / min and the centrifugation time is 5 min.

[0012] Preferably, the vacuum drying temperature is 60-80° C. and the time is 10-20 h.

[0013] The modified magnesium-aluminum layered double hydroxide adsorbent prepared according to the above method has a lamellar structure with a lateral size of about 500 nm, an average thickness of about 0.7 nm, and a specific surface area of ​​254 m 2 / g, and the pore size is 48.79nm.

[0014] The present invention also provides a modified magnesium aluminum layered double metal hydroxide obtained according to the aforementioned preparation method for use as an adsorbent in removing cationic dyes from wastewater. The adsorbent has an excellent selective removal effect on cationic dyes in wastewater, and its removal rate for cationic dyes can reach 98%, and the adsorption amount can reach 1225 mg / g. It is a cationic dye adsorbent with excellent performance.

[0015] Compared with the prior art, the present invention has obvious advantages and beneficial effects. By means of the above technical solution, the present invention can achieve considerable technical progress and practicality, and has a wide range of utilization value, and has at least the following advantages:

[0016] 1) The preparation method of the ionic liquid modified magnesium aluminum layered double hydroxide adsorbent for removing cationic dyes from wastewater described in the present invention solves the defects of traditional layered double hydroxides that are easy to agglomerate, small specific surface area, and few surface adsorption sites. After ionic liquid modification, the adsorbent surface contains hydrophilic ionic liquid functional groups, which makes the adsorbent more dispersible in water, showing the advantages of not easy to agglomerate, large specific surface area, many surface adsorption sites, and high adsorption performance.

[0017] 2) The present invention adopts sulfonic acid functionalized ionic liquid as a modifier. The hydrophilic sulfonic acid functionalized ionic liquid is chemically bonded to the surface of the magnesium aluminum layered double hydroxide. The ionic liquid is not easy to be lost. The adsorption performance of the modified material for cationic dyes is significantly improved. The modified material can be regenerated after use and can be reused many times, which can effectively reduce the cost of wastewater treatment.

[0018] 3) The ionic liquid modified magnesium aluminum layered double metal hydroxide adsorbent obtained by the preparation method of the present invention has selective adsorption performance for cationic dyes in wastewater, and its adsorption efficiency for cationic dyes is significantly better than that for anionic dyes. In addition, the preparation method of the present invention is simple to operate, mild in conditions, easy to prepare, and easy to use in mass production. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 These are electron photographs of the methylene blue solution before and after being adsorbed by the adsorbent X-1 of Example 1.

[0020] Figure 2 These are electron photographs of the malachite green solution before and after adsorption by the adsorbent X-3 of Example 3.

[0021] Figure 3 These are electronic photographs of the methyl orange solution before and after being adsorbed by the adsorbent X-4 of Example 4.

[0022] Figure 4 This is a SEM image of the modified magnesium aluminum layered double hydroxide prepared in Example 1.

[0023] Figure 5 It is the N2 adsorption-desorption curve diagram (a) and particle size distribution diagram (b) of the modified magnesium aluminum layered double hydroxide prepared in Example 1.

[0024] Figure 6 It is the thermogravimetric analysis diagram of magnesium aluminum layered double hydroxide before (comparative example) and after (example 2) modification by ionic liquid.

[0025] Figure 7 This is the infrared spectrum of the modified magnesium aluminum layered double hydroxide prepared in Example 1.

[0026] Figure 8 This is a diagram showing the removal effect of the adsorbent X-2 prepared in Example 2 after being recycled 5 times. DETAILED DESCRIPTION

[0027] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with specific embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] In the following examples, if no specific conditions are specified, all the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. The raw materials and reagents used, if no manufacturer is specified, are all conventional products that can be purchased from the market.

[0029] Example 1

[0030] 0.005 mol of Mg(NO3)2·6H2O and 0.015 mol of Al(NO3)3·9H2O were added to a beaker, and then 50 mL of deionized water was added. The mixture was stirred thoroughly to dissolve Mg(NO3)2·6H2O and Al(NO3)3·9H2O. Then 0.1 g of 1-propylsulfonic acid-3-methylimidazolium chloride ion liquid was added to the beaker and the stirring was continued. Saturated NaOH solution was slowly added dropwise to the obtained mixed solution to adjust the pH value of the mixed solution to 10.5±0.5. The stirring was continued for 2 h. The beaker was then placed in a constant temperature water bath and reacted at 65°C for 24 h. The obtained colloidal precipitate was centrifuged at a centrifuge speed of 8000 r / min and a centrifugation time of 5 min. The precipitate obtained by centrifugation was washed with deionized water until it was neutral. Then, the precipitate was vacuum dried at 60°C for 12 h to obtain a modified magnesium-aluminum layered double hydroxide, which was recorded as adsorbent X-1.

[0031] A 0.5 mg / mL methyl blue solution was prepared as simulated wastewater. 25 mL of the simulated wastewater was taken, 10 mg of the adsorbent X-1 prepared in this example was added thereto, and the mixture was oscillated in a constant temperature oscillator at room temperature for 30 min and then centrifuged. The absorbance of methyl blue in the supernatant was measured at 664 nm and recorded as A1. The removal rate of methyl blue by the adsorbent X-1 was calculated to be 89% according to formula (1). The adsorption amount of methyl blue by the adsorbent X-1 was calculated to be 1113 mg / g according to formula (2).

[0032] Removal rate = [(C0-C1) / C0] × 100% (1)

[0033] Adsorption amount = [V × (C0-C1)] / m (2)

[0034] In formula (1) and formula (2), C0 is the initial concentration of the cationic dye in the simulated wastewater, unit: mg / mL, which is 0.5 mg / mL in this example; C1 is the residual concentration of the cationic dye in the supernatant after adsorption is completed, unit: mg / mL; V is the volume of the simulated wastewater in the adsorption test, unit: mL, which is 25 mL in this example; m is the amount of adsorbent used, unit: g, which is 0.01 g in this example. Among them, the calculation of C1 can be obtained by substituting A1 into the methylene blue standard curve equation. The method for obtaining the methylene blue standard curve equation is as follows: prepare a methylene blue standard solution of a certain concentration, take a certain volume of the methylene blue standard solution and dilute it by different multiples to obtain a series of methylene blue test solutions of different concentrations, use spectrophotometry to measure the absorbance of a series of methylene blue test solutions of different concentrations at 664nm, and draw a standard curve with the concentration of the methylene blue test solution as the horizontal coordinate and the corresponding absorbance as the vertical coordinate to obtain the methylene blue standard curve equation, and then substitute A1 into the methylene blue standard curve equation to obtain the residual concentration C1 of the cationic dye in the supernatant after the adsorption is completed.

[0035] The electron photos of methyl blue solution before and after adsorption by adsorbent X-1 are as follows Figure 1 As shown, Figure 1 The left side is the electron photograph before adsorption, and the right side is the electron photograph after adsorption. It can be seen that the methylene blue solution is basically colorless after being adsorbed by adsorbent X-1.

[0036] Example 2

[0037] 0.015 mol of Mg(NO3)2·6H2O and 0.005 mol of Al(NO3)3·9H2O were added to a beaker, and then 50 mL of deionized water was added. The mixture was stirred thoroughly to dissolve Mg(NO3)2·6H2O and Al(NO3)3·9H2O. Then 0.3 g of 1-propylsulfonic acid-3-methylimidazolium chloride ion liquid was added to the beaker and the stirring was continued. Saturated NaOH solution was slowly added dropwise to the obtained mixed solution to adjust the pH value of the mixed solution to 10.5±0.5. The stirring was continued for 2 h. The beaker was then placed in a constant temperature water bath and reacted at 65°C for 24 h. The obtained colloidal precipitate was centrifuged at a centrifuge speed of 8000 r / min and a centrifugation time of 5 min. The precipitate obtained by centrifugation was washed with deionized water until it was neutral. Then, it was vacuum dried at 60°C for 12 h to obtain a modified magnesium-aluminum layered double metal hydroxide, which was recorded as adsorbent X-2.

[0038] The removal rate of methyl blue by adsorbent X-2 was tested according to the method of Example 1 and the result was 98%. The adsorption amount of methyl blue by adsorbent X-2 was 1225 mg / g.

[0039] Example 3

[0040] 0.015 mol of Mg(NO3)2·6H2O and 0.005 mol of Al(NO3)3·9H2O were added to a beaker, and then 50 mL of deionized water was added. The mixture was stirred thoroughly to dissolve Mg(NO3)2·6H2O and Al(NO3)3·9H2O. Then 0.2 g of 1-propylsulfonic acid-3-methylimidazolium chloride ion liquid was added to the beaker and the stirring was continued. Saturated NaOH solution was slowly added dropwise to the obtained mixed solution to adjust the pH value of the mixed solution to 10.5±0.5. The stirring was continued for 2 h. The beaker was then placed in a constant temperature water bath and reacted at 65°C for 24 h. The obtained colloidal precipitate was centrifuged at a centrifuge speed of 8000 r / min and a centrifugation time of 5 min. The precipitate obtained by centrifugation was washed with deionized water until it was neutral, and then vacuum dried at 60°C for 12 h to obtain a modified magnesium-aluminum layered double metal hydroxide, which was recorded as adsorbent X-3.

[0041] A malachite green solution with a concentration of 0.5 mg / mL was prepared as simulated wastewater. 25 mL of simulated wastewater was taken, and 10 mg of the adsorbent X-3 prepared in this example was added thereto. The solution was oscillated in a thermostatic oscillator at room temperature for 30 min and then centrifuged. The absorbance of malachite green in the supernatant was measured at 617 nm and recorded as A1. A standard curve of malachite green absorbance versus concentration was drawn according to the method of Example 1 to obtain a linear equation of malachite green absorbance versus concentration. The absorbance A1 in this example was substituted into the linear equation of malachite green absorbance versus concentration to obtain the residual concentration C1 of the cationic dye malachite green in the supernatant after adsorption. The removal rate of malachite green by the adsorbent X-3 was calculated by formula (1) and formula (2) according to the method of Example 1, and the adsorption amount of malachite green by the adsorbent X-3 was 97%, and the adsorption amount of malachite green by the adsorbent X-3 was 1213 mg / g.

[0042] The electron photos of malachite green solution before and after adsorption by adsorbent X-3 are as follows Figure 2 As shown, Figure 2 The left side is the electron photograph before adsorption, and the right side is the electron photograph after adsorption. It can be seen that the malachite green solution is basically colorless after being adsorbed by adsorbent X-3.

[0043] Example 4

[0044] 0.010 mol of Mg(NO3)2·6H2O and 0.010 mol of Al(NO3)3·9H2O were added to a beaker, and then 50 mL of deionized water was added. The mixture was stirred thoroughly to dissolve Mg(NO3)2·6H2O and Al(NO3)3·9H2O. Then 0.1 g of 1-propylsulfonic acid-3-methylimidazolium chloride ion liquid was added to the beaker and the stirring was continued. Saturated NaOH solution was slowly added dropwise to the obtained mixed solution to adjust the pH value of the mixed solution to 10.5±0.5. The stirring was continued for 2 h. The beaker was then placed in a constant temperature water bath and reacted at 65°C for 24 h. The obtained colloidal precipitate was centrifuged at a centrifuge speed of 8000 r / min and a centrifugation time of 5 min. The precipitate obtained by centrifugation was washed with deionized water until it was neutral. Then, it was vacuum dried at 60°C for 12 h to obtain a modified magnesium-aluminum layered double metal hydroxide, which was recorded as adsorbent X-4.

[0045] A methyl orange solution with a concentration of 0.5 mg / mL was prepared as simulated wastewater. 25 mL of the simulated wastewater was taken, and 10 mg of the adsorbent X-4 prepared in this example was added thereto. The solution was oscillated in a thermostatic oscillator at room temperature for 30 min and then centrifuged. The absorbance of methyl orange in the supernatant was measured at 464 nm and recorded as A1. A standard curve of the absorbance of methyl orange versus concentration was drawn according to the method of Example 1 to obtain a linear equation of the absorbance of methyl orange versus concentration. The absorbance A1 in this example was substituted into the linear equation of the absorbance of methyl orange versus concentration to obtain the residual concentration C1 of methyl orange in the supernatant after adsorption. The removal rate of methyl orange by the adsorbent X-4 was calculated to be 18% by formula (1) and formula (2) according to the method of Example 1, and the adsorption amount of methyl orange by the adsorbent X-4 was 200 mg / g.

[0046] The electron photos of methyl orange solution before and after adsorption by adsorbent X-4 are shown in the figure below. Figure 3 As shown, Figure 3 The left side is the electron photograph before adsorption, and the right side is the electron photograph after adsorption. It can be seen that the color of the methyl orange solution becomes lighter after being adsorbed by adsorbent X-4.

[0047] Comparative Example

[0048] Add 0.015 mol of Mg(NO3)2·6H2O and 0.005 mol of Al(NO3)3·9H2O into a beaker, then add 50 mL of deionized water, stir thoroughly to dissolve Mg(NO3)2·6H2O and Al(NO3)3·9H2O, slowly drop saturated NaOH solution into the obtained mixed solution, adjust the pH value of the mixed solution to 10.5±0.5, continue stirring for 2 h, then place the beaker in a constant temperature water bath, react at 65°C for 24 h, centrifuge the obtained product, the centrifuge speed is 8000 r / min, the centrifugation time is 5 min, wash the precipitate obtained by centrifugation to neutrality with deionized water, and then vacuum dry at 60°C for 12 h to obtain unmodified magnesium-aluminum layered double hydroxide.

[0049] Figure 4 This is a SEM image of the modified magnesium aluminum layered double metal hydroxide prepared in Example 1. It can be seen that the modified magnesium aluminum layered double metal hydroxide has a lamellar structure with a lateral dimension of about 500 nm and an average thickness of about 0.7 nm.

[0050] Figure 5 The N2 adsorption-desorption curve (a) and particle size distribution diagram (b) of the modified magnesium-aluminum layered double hydroxide prepared in Example 1 show that the specific surface area of ​​the modified magnesium-aluminum layered double hydroxide is 254 m 2 / g, pore diameter is 48.79nm, pore volume is 0.003725cm 3 / g.

[0051] Figure 6 This is the thermogravimetric analysis diagram of magnesium aluminum layered double hydroxide before (comparative example) and after modification (Example 2) by ionic liquid. It can be concluded that the material before modification loses about 15% of its weight, while the material after modification loses about 25% of its weight, indicating that the ionic liquid after modification is successfully connected to the surface of magnesium aluminum layered double hydroxide.

[0052] Figure 7 This is the infrared spectrum of the modified magnesium-aluminum layered double hydroxide prepared in Example 1. It can be seen that 3487 cm -1 The stretching vibration absorption peak of -OH on the laminate is 1649 cm -1 The absorption peak of imidazole ring is 1384cm -1 The stretching vibration absorption peak of -SO3H in ionic liquid is 671cm -1 and 449cm -1 The locations are the vibration absorption peaks of Mg-O and Al-O in the layer plates. Therefore, the surface of the modified material has the functional groups of ionic liquids.

[0053] A 0.5 mg / mL methyl blue solution was prepared as simulated wastewater, 25 mL of the simulated wastewater was taken, 10 mg of the adsorbent X-2 prepared in Example 2 was added thereto, the mixture was oscillated in a thermostatic oscillator at room temperature for 30 min, and then centrifuged. The absorbance of methyl blue in the supernatant was measured at 664 nm, which was recorded as A1. The removal rate of methyl blue by the adsorbent X-2 was calculated according to the method of Example 1 according to formula (1). The adsorbent after use and centrifugation was dried, and then put into 25 mL of 0.5 mg / mL simulated wastewater again, oscillated in a thermostatic oscillator at room temperature for 30 min, and then centrifuged. The absorbance of methyl blue in the supernatant was measured at 664 nm, which was recorded as A2. The removal rate of methyl blue by the adsorbent X-2 after two cycles of use was calculated according to formula (1) according to the method of Example 1. According to this method, the adsorbent X-2 was recycled for 5 times, and the removal rate of methyl blue by the adsorbent X-2 after each use was calculated. The number of recycled uses was used as the horizontal axis, and the removal rate of methyl blue by the adsorbent X-2 after each use was used as the vertical axis. The results are shown in the figure. Figure 8 As shown, it can be seen that when the adsorbent X-2 prepared in Example 2 was used for adsorption treatment of methyl blue simulated wastewater, it was recycled for 5 times and the removal rate did not change much, which fully demonstrated that the modified magnesium-aluminum layered double metal hydroxide adsorbent prepared by the present invention has good recycling stability for the adsorption treatment of cationic dyes.

[0054] The above is only an embodiment of the present invention, and does not limit the present invention in any form. The present invention can also have other forms of embodiments according to the above structures and functions, which are not listed one by one. Therefore, any simple modification, equivalent change and modification made by any technician familiar with the profession to the above embodiment according to the technical essence of the present invention without departing from the scope of the technical solution of the present invention still falls within the scope of the technical solution of the present invention.

Claims

1. A method for preparing an adsorbent for removing cationic dyes from wastewater, characterized in that The method comprises the following steps: adding Mg(NO3)2·6H2O and Al(NO3)3·9H2O into a beaker, adding deionized water and stirring thoroughly to dissolve Mg(NO3)2·6H2O and Al(NO3)3·9H2O, then adding 1-propylsulfonic acid-3-methylimidazolium chloride ion liquid into the beaker, continuing stirring, slowly dropping a saturated NaOH solution into the obtained mixed solution, adjusting the pH value of the mixed solution to 10.5±0.5, continuing stirring for 2-6 hours, then placing the beaker in a constant temperature water bath, reacting at a constant temperature of 65°C for 24-48 hours, centrifuging the obtained colloidal precipitate, washing the centrifuged precipitate with deionized water until it is neutral, and then vacuum drying to obtain a modified magnesium-aluminum layered double metal hydroxide adsorbent.

2. The method for preparing an adsorbent for removing cationic dyes from wastewater as claimed in claim 1, characterized in that The molar ratio of Mg(NO3)2·6H2O to Al(NO3)3·9H2O is (1~3):(1~3).

3. The method for preparing an adsorbent for removing cationic dyes from wastewater as claimed in claim 1, characterized in that The ratio of the mass of 1-propylsulfonic acid-3-methylimidazolium chloride ion liquid to the sum of the molar numbers of Mg(NO3)2·6H2O and Al(NO3)3·9H2O is (1-3) g:0.2 mol.

4. The method for preparing an adsorbent for removing cationic dyes from wastewater as claimed in claim 1, characterized in that During centrifugal separation, the centrifuge speed is 8000r / min and the centrifugal time is 5min.

5. The method for preparing an adsorbent for removing cationic dyes from wastewater as claimed in claim 1, characterized in that The vacuum drying temperature is 60-80°C and the time is 10-20 hours.

6. The method for preparing an adsorbent for removing cationic dyes from wastewater as claimed in claim 1, characterized in that The prepared modified magnesium-aluminum layered double hydroxide adsorbent has a lamellar structure with an average thickness of 0.7 nm and a specific surface area of ​​254 m 2 / g, and the pore size is 48.79nm.

7. Use of the modified magnesium aluminum layered double metal hydroxide obtained by the preparation method as claimed in claim 1 as an adsorbent in removing cationic dyes from wastewater.

Citation Information

Patent Citations

  • Preparation method of stratiform bimetallic oxide sorbent capable of effectively removing low-concentrated phosphate radical

    CN105032342A

  • Preparation method and application of transition metal doped magnesium-aluminum layered double-metal hydroxide material

    CN115845792A

  • Layered double-metal hydroxide composite material as well as preparation method and application thereof

    CN117563550A

  • Modified composite adsorbent as well as preparation method and application thereof

    CN110665469A

  • Preparation method and application of Co / Fe layered double-metal hydroxide nanosheet

    CN113493225A

Cited By

  • Cobalt-doped MgAl-LDH adsorbent and preparation method and application thereof

    CN120079343A