Preparation method of anion exchange chromatography medium for enhancing hydrogen-bond interaction

By bonding primary amine groups and hydroxyl compounds to the surface of porous microspheres to enhance hydrogen bonding in anion exchange chromatography medium, the problem of insufficient protein adsorption capacity under high salt conditions is solved, achieving simple and efficient preparation and high protein adsorption effect under high salt conditions.

CN118988269APending Publication Date: 2024-11-22BEIJING INSTITUTE OF PETROCHEMICAL TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411318455.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-20
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In existing technologies, anion exchange chromatography media have insufficient protein adsorption capacity under high salt conditions, and the preparation process is complex, increasing the cost and time of separation and purification.

Method used

Polymers with primary amine groups are chemically bonded to the surface of porous microspheres, and the amine groups are coupled with hydroxyl compounds to form an anion exchange chromatography medium that enhances hydrogen bonding and expands its ionic strength tolerance range.

Benefits of technology

The preparation process is simple, and the resulting medium maintains a high protein adsorption capacity at high salt concentrations, reducing operational complexity and cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118988269A_ABST
    Figure CN118988269A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of an anion exchange chromatography medium for enhancing hydrogen-bond interaction. The preparation method comprises the following steps: chemically bonding a polymer with a primary amine group to the surface of a porous microsphere with an epoxy group; and coupling a compound with a hydroxyl group to the surface of the obtained porous microsphere through a reaction of an amino group and epoxy to prepare the enhanced hydrogen bond type anion exchange chromatography medium. According to the method, the preparation process is simple and easy to operate, the ligand selection range is wide, and the prepared hydrogen bond enhanced anion exchange chromatography medium has a wide ionic strength tolerance range and can keep high protein adsorption capacity under high salt concentration.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ion exchange chromatography medium preparation and application, and in particular to a method for preparing anion exchange chromatography medium capable of enhancing hydrogen bonding. Background Art

[0002] Ion exchange chromatography is a widely used chromatographic mode in chromatographic separation technology. In the separation and purification of many biological products, anion exchange chromatography is often used in the first capture and purification step. It is well known that in this chromatographic mode, the protein molecules and the chromatographic fillers are mainly adsorbed through electrostatic interactions. The ionic strength in the feed liquid has a significant effect on the protein adsorption capacity (there is almost no adsorption effect on the protein when the conductivity is greater than 18s / cm). Therefore, the ionic strength of the feed liquid needs to be reduced before loading, such as ultrafiltration desalination or dilution treatment. This operation increases the operating steps and equipment, and invests in manpower, material resources, and time costs, which correspondingly increases the separation and purification costs and reduces production efficiency. In order to solve the above problems, developing salt-resistant anion exchange chromatography media is one of the better solutions.

[0003] The preparation methods of the prior art mostly bond the polymer with primary amine to the surface of the material, and use the proton sponge effect of the primary amine group to shield a part of the ions, so that a certain amount of protein adsorption capacity can still be maintained under a certain ionic strength. The range of its tolerance to ionic strength mainly depends on the molecular weight of the bonded polymer. The larger the molecular weight, the higher the ionic strength it tolerates. The larger the molecular weight of the polymer, the stronger the steric effect in the bonding process. At the same time, it is easy to block the pore size of the porous material, causing the mass transfer performance of the final chromatographic medium to decrease, so the degree of improvement of its tolerance to salt concentration is limited; at the same time, the pH value of the primary amine group is usually within the range of 7-9, and in most protein molecule purification processes, protein is adsorbed within the pH range of 6-8 close to neutral. At this time, the primary amine group exists in a non-protonated form (-NH2), which is not conducive to protein adsorption, so its load is difficult to increase, and this non-protonated form is also not conducive to hydrogen bond formation, and its shielding ionic strength range is small, that is, the salt tolerance concentration is low. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing an anion exchange chromatography medium with enhanced hydrogen bonding. The preparation process of the method is simple and easy to operate, and the range of ligands that can be selected is wide. The prepared hydrogen bond enhanced anion exchange chromatography medium has a wide ionic strength tolerance range and can maintain a high protein adsorption capacity at a high salt concentration.

[0005] The objective of the present invention is achieved through the following technical solutions:

[0006] A method for preparing an anion exchange chromatography medium for enhancing hydrogen bonding, the method comprising:

[0007] Step 1, chemically bonding a polymer with a primary amine group to the surface of a porous microsphere with an epoxy group;

[0008] Step 2: coupling the compound with hydroxyl groups to the surface of the porous microspheres obtained in step 1 through an amine-epoxy reaction to prepare an enhanced hydrogen-bond anion exchange chromatography medium.

[0009] In step 1, the porous microspheres are polyacrylate microspheres having epoxy groups on their surfaces.

[0010] In step 1, the polymer having a primary amine group is specifically a water-soluble polymer having a primary amine group in its side chain.

[0011] The polymer having primary amine groups includes polyethyleneimine, polyvinylamine or polyallylamine.

[0012] In step 2, the compound with hydroxyl group includes a group having an epoxy group, an aldehyde group, a carboxyl group or an acyl chloride group at one end which can react with a primary amine group, and a compound having a hydroxyl group or a compound which can be converted into a hydroxyl group at the other end.

[0013] In step 2, the compound having a hydroxyl group includes glycidol, 3-hydroxypropanal, hydroxyacetaldehyde, hydroxybutyraldehyde, 4,4-dihydroxybutyraldehyde or glycolic acid.

[0014] In step 2, the obtained enhanced hydrogen-bonding anion exchange chromatography medium has a tolerance ionic strength range of 0.1 to 0.7 mol / L NaCl solution;

[0015] The protein loading range was 25-150 mg bovine serum albumin (BSA) / mL wet medium.

[0016] It can be seen from the technical solution provided by the present invention that the preparation process of the above method is simple and easy to operate, the range of ligands available is wide, and the prepared hydrogen bond enhanced anion exchange chromatography medium has a wide ionic strength tolerance range and can maintain a high protein adsorption capacity at a higher salt concentration. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0018] Figure 1 A schematic flow chart of a method for preparing an anion exchange chromatography medium with enhanced hydrogen bonding provided in an embodiment of the present invention;

[0019] Figure 2 This is a schematic diagram of the reaction process for preparing an anion exchange chromatography medium for enhancing hydrogen bonding according to an embodiment of the present invention. DETAILED DESCRIPTION

[0020] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in conjunction with the accompanying drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments, which does not constitute a limitation of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] like Figure 1 The figure shows a schematic flow chart of a method for preparing an anion exchange chromatography medium with enhanced hydrogen bonding provided by an embodiment of the present invention, wherein the method comprises:

[0022] Step 1, chemically bonding a polymer with a primary amine group to the surface of a porous microsphere with an epoxy group;

[0023] In this step, the porous microspheres may be polyacrylate microspheres having epoxy groups on their surfaces.

[0024] The polymer having a primary amine group is specifically a water-soluble polymer having a primary amine group in a side chain.

[0025] Specifically, the polymer having a primary amine group may include polyethyleneimine, polyvinylamine or polyallylamine.

[0026] Step 2: coupling the compound with hydroxyl groups to the surface of the porous microspheres obtained in step 1 through an amine-epoxy reaction to prepare an enhanced hydrogen-bond anion exchange chromatography medium.

[0027] In this step, the compound with hydroxyl group includes a group having an epoxy group, an aldehyde group, a carboxyl group or an acyl chloride group at one end which can react with a primary amine group, and a compound having a hydroxyl group or being convertible into a hydroxyl group at the other end.

[0028] Specifically, the compound having a hydroxyl group may include glycidol, 3-hydroxypropionaldehyde, hydroxyacetaldehyde, hydroxybutyraldehyde, 4,4-dihydroxybutyraldehyde or glycolic acid, etc.

[0029] like Figure 2 The figure shows a schematic diagram of the reaction process for preparing the anion exchange chromatography medium with enhanced hydrogen bonding as described in an embodiment of the present invention. The tolerance ionic strength range of the finally obtained enhanced hydrogen bonding anion exchange chromatography medium is 0.1 to 0.7 mol / L NaCl solution; the protein loading range is 25 to 150 mg bovine serum albumin (BSA) / mL wet medium.

[0030] The preparation process and performance of the method described in the embodiment of the present invention are illustrated by using specific examples below:

[0031] Example 1, step 1: high molecular weight polyvinyl amine and polyacrylate microspheres with epoxy groups on the surface are mixed in an aqueous solution at a mass ratio of 2:1, stirred and mixed, the reaction temperature is controlled to be 50°C, the reaction time is 12h, after the reaction is completed, deionized and washed to neutrality, and the obtained microspheres are drained for use;

[0032] Step 2: Mix the microspheres prepared in step 1 with propylene oxide in a volume-to-mass ratio of 10 (mL): 5 (g), then add 20 mL of deionized water, stir and react at 50° C. for 12 h, and wash with deionized water after the reaction to prepare a hydrogen bond enhanced anion exchange chromatography medium.

[0033] The ligand density of the hydrogen bond enhanced anion exchange chromatography medium is 0.15 mmol / mL, the salt tolerance range is 0.1-0.7 M NaCl aqueous solution, and the protein adsorption capacity range is shown in Table 1. In the range of 0.1-0.7 M NaCl solution, the protein adsorption capacity ranges from 150 to 30 mg / mL, and the protein adsorption capacity decreases with increasing salt concentration.

[0034] Table 1 Tolerance salt concentration range of the hydrogen bond enhanced anion exchange chromatography medium obtained in Example 1 and its corresponding protein adsorption capacity

[0035]

[0036] Example 2, step 1: high molecular weight polyallylamine and agarose microspheres with epoxy groups on the surface are mixed in an aqueous solution at a mass ratio of 1:1, stirred and mixed, the reaction temperature is controlled to be 60°C, the reaction time is 24h, after the reaction is completed, deionized and washed to neutrality, and the obtained microspheres are drained for use;

[0037] Step 2: The microspheres prepared in step 1 were mixed with hydroxybutyraldehyde in a volume to mass ratio of 10 (mL): 5 (g), and then 20 mL of deionized water was added, and the mixture was stirred at 30°C for 12 hours. The pH of the solution was then adjusted to 8.0, and 2.0 g of sodium cyanoborohydride was added, and the mixture was stirred at 30°C for 5 hours. After the reaction was completed, the mixture was washed with deionized water to prepare a hydrogen bond enhanced anion exchange chromatography medium.

[0038] The ligand density of the hydrogen bond enhanced anion exchange chromatography medium is 0.22 mmol / mL, and the salt tolerance range is 0.1-0.7 M NaCl aqueous solution. The protein adsorption capacity range is shown in Table 2. In the range of 0.1-0.7 M NaCl solution, the protein adsorption capacity ranges from 120 to 25 mg / mL, and the protein adsorption capacity decreases with increasing salt concentration.

[0039] Table 2 Tolerance salt concentration range of the hydrogen bond enhanced anion exchange chromatography medium obtained in Example 2 and its corresponding protein adsorption capacity

[0040]

[0041] Example 3, step 1: high molecular weight polyethyleneimine and polystyrene microspheres with epoxy groups on the surface are mixed in an aqueous solution at a mass ratio of 1:1, stirred and mixed, the reaction temperature is controlled to be 55°C, the reaction time is 12h, after the reaction is completed, deionized and washed to neutrality, and the obtained microspheres are drained for use;

[0042] Step 2: The microspheres prepared in step 1 were mixed with glycolic acid in a volume to mass ratio of 10 (mL): 10 (g), and then 2.0 g of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide was added as a shrinking agent, and then 20 mL of deionized water was added. The reaction was stirred at 50° C. for 12 h. After the reaction was completed, it was washed with deionized water to prepare a hydrogen bond enhanced anion exchange chromatography medium.

[0043] The ligand density of the hydrogen bond enhanced anion exchange chromatography medium is 0.25 mmol / mL, and the salt tolerance range is 0.1-0.7 M NaCl aqueous solution. The protein adsorption capacity range is shown in Table 3. In the range of 0.1-0.7 M NaCl solution, the protein adsorption capacity ranges from 140 to 32 mg / mL, and the protein adsorption capacity decreases with increasing salt concentration.

[0044] Table 3 Tolerance salt concentration range of the hydrogen bond enhanced anion exchange chromatography medium obtained in Example 3 and its corresponding protein adsorption capacity

[0045]

[0046] The surface grafted ligand density and protein adsorption capacity of the obtained hydrogen bond enhanced anion exchange chromatography medium were measured as follows:

[0047] 1. Determination of density of grafted ligands on the surface of the medium

[0048] Step 1: Hydroxyl transformation

[0049] The medium was transferred to the exchange column and slowly settled until the volume reached 20 mL. 60 mL of 1 mol / L sodium hydroxide solution was passed through the column and the solution was completely drained within 1 h. The solution was then washed with deionized water until the outflowing liquid did not change color when exposed to phenolphthalein indicator.

[0050] Step 2: Acid-base neutralization

[0051] 1) Use an acid burette to accurately measure 50 mL of standard hydrochloric acid solution, add it to the above exchange column, let it drip slowly, and collect it in a conical flask;

[0052] 2) Then add 30 mL of 1 mol / L sodium chloride solution dropwise through the column and collect it in the above-mentioned conical flask.

[0053] Step 3: Back-drip collected hydrochloric acid

[0054] 1) Add 2-3 drops of phenolphthalein indicator to the liquid collected in the second step, and titrate with 0.1 mol / L sodium hydroxide standard solution until it turns pink and remains unchanged for 15 seconds as the end point, and record the volume of sodium hydroxide consumed;

[0055] 2) The ligand density of the medium sample is calculated according to the following formula.

[0056] E=(C1 V1-C2 V2) / V(mmol / mL)

[0057] Wherein, C1 is the concentration of hydrochloric acid standard solution (mol / L); V1 is the volume of hydrochloric acid standard solution (mL); C2 is the concentration of sodium hydroxide standard solution (mol / L); V2 is the volume of sodium hydroxide standard solution consumed during titration (mL); V is the volume of the medium in the column (mL).

[0058] The grafted ligand density of the salt-tolerant cation exchange chromatography media prepared in Examples 1 to 2 above was determined by this method.

[0059] 2. Protein adsorption capacity determination

[0060] Using pH=7.0, 20mM phosphate buffer as solvent, prepare NaCl solutions of different concentrations, the concentration range of which is 0.1-0.7M, and use 3mg / mL bovine serum albumin solution (BSA for short) as the adsorption model protein. Mix a certain volume of chromatography medium with the protein solution, adsorb for 5h at room temperature, and centrifuge at 5000rpm for 10 minutes. Take the supernatant and measure the ultraviolet absorption value at 280nm to calculate the protein adsorption capacity per unit volume of medium.

[0061] The protein adsorption capacity of the hydrogen bond enhanced anion exchange medium prepared in the above examples at different salt concentrations was determined using this method.

[0062] The ligand density, protein loading capacity and salt tolerance range of the prepared hydrogen bond enhanced anion exchange chromatography medium were measured. The results showed that the ligand density of this type of medium was 0.15-0.55 mmol / mL wet medium. Bovine serum albumin (BSA) was used as the test object. The protein loading range of this type of medium was 25-150 mg / mL, and the protein recovery rate was above 90%. The loading capacity increased with the ligand density of the microspheres, and the salt tolerance also increased with the ligand density. The salt tolerance range was 0.1-0.7 mol / L NaCl solution.

[0063] It is worth noting that the contents not described in detail in the embodiments of the present invention belong to the prior art known to professional and technical personnel in the field.

[0064] In summary, the method described in the embodiment of the present invention bonds a polymer that can form a large number of hydrogen bonds on the surface of the porous microsphere material. The polymer has amine groups and hydroxyl groups, and is easy to form weak interactions such as hydrogen bonds with biological macromolecules such as proteins, and can maintain a certain protein adsorption capacity in high salt solutions. The amine groups are mostly tertiary amine groups after coupling modification, and their application pH range is wider than that of primary amines. At the same time, the large number of hydroxyl groups that exist are easy to form hydrogen bonds and are less affected by changes in pH and salt concentration. Therefore, the obtained anion exchange chromatography medium has a higher protein adsorption capacity in high salt solutions.

[0065] The above is only a preferred specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by any technician familiar with the technical field within the technical scope disclosed in the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims. The information disclosed in the background technology section of this article is only intended to deepen the understanding of the overall background technology of the present invention, and should not be regarded as an admission or in any form that the information constitutes prior art known to those skilled in the art.

Claims

1. A method for preparing an anion exchange chromatography medium with enhanced hydrogen bonding, characterized in that: The method comprises: Step 1, chemically bonding a polymer with a primary amine group to the surface of a porous microsphere with an epoxy group; Step 2: coupling the compound with hydroxyl groups to the surface of the porous microspheres obtained in step 1 through an amine-epoxy reaction to prepare an enhanced hydrogen-bond anion exchange chromatography medium.

2. The method for preparing an anion exchange chromatography medium with enhanced hydrogen bonding according to claim 1, characterized in that: In step 1, the porous microspheres are polyacrylate microspheres having epoxy groups on their surfaces.

3. The method for preparing an anion exchange chromatography medium with enhanced hydrogen bonding according to claim 1, characterized in that: In step 1, the polymer having a primary amine group is specifically a water-soluble polymer having a primary amine group in its side chain.

4. The method for preparing an anion exchange chromatography medium with enhanced hydrogen bonding according to claim 3, characterized in that: The polymer having primary amine groups includes polyethyleneimine, polyvinylamine or polyallylamine.

5. The method for preparing an anion exchange chromatography medium with enhanced hydrogen bonding according to claim 1, characterized in that: In step 2, the compound with hydroxyl group includes a group having an epoxy group, an aldehyde group, a carboxyl group or an acyl chloride group at one end which can react with a primary amine group, and a compound having a hydroxyl group or a compound which can be converted into a hydroxyl group at the other end.

6. The method for preparing an anion exchange chromatography medium with enhanced hydrogen bonding according to claim 5, characterized in that: In step 2, the compound having a hydroxyl group includes glycidol, 3-hydroxypropanal, hydroxyacetaldehyde, hydroxybutyraldehyde, 4,4-dihydroxybutyraldehyde or glycolic acid.

7. The method for preparing an anion exchange chromatography medium with enhanced hydrogen bonding according to claim 1, characterized in that: In step 2, the obtained enhanced hydrogen-bonding anion exchange chromatography medium has a tolerance ionic strength range of 0.1 to 0.7 mol / L NaCl solution; The protein loading range was 25-150 mg bovine serum albumin (BSA) / mL wet medium.