Catalytic material for triboelectric / piezoelectric catalytic oxidation of CO and preparation method of catalytic material

By growing ZnO nanorod arrays on mesh substrates coated with textile cotton thread and PDMS in the catalyst, combined with triboelectric and piezoelectric coupling, the problems of low efficiency and insufficient adsorption capacity of semiconductor oxide catalysts are solved, and the automobile is achieved The efficient catalytic oxidation of low concentration CO in the exhaust gas improves catalytic activity and stability.

CN118988280APending Publication Date: 2024-11-22XIAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411077842.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing semiconductor oxide catalysts are low in oxidation efficiency and high cost in catalyzing automobile exhaust, and are difficult to apply in small exhaust pipes. It is difficult to effectively adsorb the piezoelectric catalyst surface, resulting in passive adsorption of the catalyst. and high equipment complexity.

Method used

By carbonizing textile cotton thread and covering PDMS, braiding it into a mesh substrate, growing a ZnO nanorod array, and improving the adsorption and catalytic oxidation efficiency of catalytic materials to CO through triboelectric and piezoelectric coupling.

Benefits of technology

It achieves efficient adsorption and catalytic oxidation of low-concentration CO in automobile exhaust, with a catalytic activity increased by 350%, no external devices required, simple preparation method, high cycle stability and low cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118988280A_ABST
    Figure CN118988280A_ABST
Patent Text Reader

Abstract

The invention discloses a catalytic material for catalytic oxidation of CO by triboelectricity / piezoelectricity, and also discloses a preparation method of the catalytic material, and the preparation method comprises the following steps: carbonizing a textile cotton thread into a millimeter-scale carbon thread in an N2 atmosphere, placing the carbon thread in a PDMS cyclohexane solution for multiple times of dipping, then taking out the carbon thread, and drying to obtain a PDMS / C thread; metal wires and PDMS / C wires are woven into a net, and a Me-PDMS / C flexible net substrate FTEW is obtained; the method comprises the following steps: coating FTEW with a ZnO seed crystal solution for multiple times, and carrying out heat treatment on the FTEW in an N2 atmosphere to obtain textured ZnO seed crystals / FTEW; and putting the ZnO seed crystal / FTEW into an aqueous solution containing zinc nitrate, hexamethylenetetramine and polyethyleneimine, and carrying out hydrothermal treatment to obtain the ZnO nanorod array / FTEW catalytic material. The catalytic material disclosed by the invention has relatively high adsorption capacity and relatively high catalytic oxidation efficiency on CO in automobile exhaust.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of nano-catalytic materials, and relates to a catalytic material for triboelectric / piezoelectric catalytic oxidation of low-concentration CO in automobile exhaust gas. The present invention also relates to a method for preparing the catalytic material. Background Art

[0002] Local hypoxia caused by uneven mixture distribution in internal combustion engines, high-load operation of the engine, and excessive delay in ignition time are all likely to lead to an increase in the generation of CO in motor vehicle exhaust. CO is a colorless and odorless gas that is toxic to human tissue cells and threatens human health. Currently, precious metal catalysts are mostly used in three-way catalysts to accelerate the oxidation of CO, but precious metal catalysts are prone to failure and high cost. Therefore, it is urgent to develop a stable and low-cost semiconductor oxide catalyst system to replace precious metal catalysts for catalytic oxidation of CO in automobile exhaust.

[0003] However, there are two urgent problems to be solved in the catalytic oxidation of CO by oxide catalysts. First, the catalytic efficiency of semiconductor oxide catalysts is low, and ultraviolet rays are needed to excite their carriers to improve their catalytic efficiency. However, this makes it difficult for semiconductor oxide catalysts to be used in small tailpipes and increases the complexity and cost of their equipment. On the other hand, low-concentration CO in automobile exhaust is difficult to effectively adsorb on the surface of piezoelectric catalysts to participate in the reaction. To address this problem, people use porous catalyst carriers to increase the contact area between automobile exhaust and catalysts. However, this adsorption method belongs to the passive adsorption of the catalyst, and the range of adsorption of the catalyst is limited. If the flow path of the exhaust gas continues to increase or the exhaust gas flow rate continues to decrease, it will inevitably cause blockage of automobile exhaust and affect the safety of the automobile itself. Summary of the invention

[0004] The purpose of the present invention is to provide a catalytic material for triboelectric / piezoelectric catalytic oxidation of CO, which has a strong adsorption capacity and a high catalytic oxidation efficiency for CO in automobile exhaust.

[0005] Another object of the present invention is to provide a method for preparing the above catalytic material.

[0006] The technical solution adopted by the present invention is a method for preparing a catalytic material for triboelectric / piezoelectric catalytic oxidation of CO, which is specifically implemented according to the following steps:

[0007] Step 1, carbonizing the textile cotton thread into a millimeter-sized carbon thread under a N2 atmosphere, and then immersing the carbon thread in a PDMS cyclohexane solution for multiple times, and then taking out the carbon thread and drying it to obtain PDMS / C threads with different PDMS coating thicknesses;

[0008] Step 2, weaving the metal wire and the PDMS / C wire obtained in step 1 into a mesh to obtain a Me-PDMS / C flexible mesh substrate FTEW; coating the ZnO seed crystal solution on the FTEW multiple times, and then heat-treating the FTEW under a N2 atmosphere to obtain a textured ZnO seed crystal / FTEW; placing the ZnO seed crystal / FTEW in an aqueous solution containing zinc nitrate, hexamethylenetetramine and polyethyleneimine for hydrothermal treatment to obtain a ZnO nanorod array / FTEW catalytic material.

[0009] The present invention is also characterized in that:

[0010] Step 1 is implemented according to the following steps:

[0011] Step 1.1, ultrasonically clean the cotton thread in ethanol and deionized water respectively, and then dry it at 60-65°C for later use, and then carbonize the dried cotton thread at 780-800°C for 3h in a N2 atmosphere, and then cool it to room temperature to obtain a millimeter-scale carbon thread;

[0012] Step 1.2, mixing the PDMS stock solution and the curing agent in a ratio of 10:1 and adding the mixture into cyclohexane to obtain a PDMS cyclohexane solution with a concentration of 10 to 50 wt %;

[0013] Step 1.3, placing the carbon wire obtained in step 1.1 in the PDMS cyclohexane solution prepared in step 1.2, so that the PDMS completely covers the C wire, taking out the C wire after multiple immersions, hanging it in the air to dry and solidify it, and obtaining a flexible PDMS / C wire.

[0014] In step 1.3, the C line is immersed for 5 to 20 times, and the thickness of the PDMS coated around the C line in the obtained flexible PDMS / C line is 2 to 40 μm.

[0015] Step 2 is implemented as follows:

[0016] Step 2.1, weaving a metal wire with a diameter of 0.1 to 1 mm and the PDMS / C wire obtained in step 1 into a mesh to obtain a cross-woven Me-PDMS / C flexible mesh substrate FTEW with a mesh number of 16 to 200;

[0017] Step 2.2, preparing a ZnO seed crystal solution, and then coating the seed crystal solution on the FTEW for multiple times, and then heat-treating the FTEW substrate coated with the ZnO seed crystal in a N2 atmosphere to obtain a textured ZnO seed crystal / FTEW;

[0018] Step 2.3, placing the ZnO seed crystal / FTEW in an aqueous solution containing zinc nitrate, hexamethylenetetramine and polyethyleneimine for hydrothermal treatment 1 to 3 times to obtain a ZnO nanorod array / FTEW catalytic material.

[0019] In step 2.1, the metal wire is Fe, Al, Cu wire or Fe, Al, Cu alloy wire.

[0020] In step 2.2, the specific preparation process of the ZnO seed crystal solution is as follows:

[0021] Dissolve zinc acetate and sodium hydroxide in ethanol respectively to obtain 3mmol / L zinc acetate ethanol solution and 5mmol / L sodium hydroxide ethanol solution, and fully mix the two solutions under water bath conditions, wherein the water bath temperature is 60-65°C and the water bath time is 45-50min to obtain a ZnO seed crystal solution.

[0022] In step 2.2, the coating times are 50 to 200 times, the heat treatment temperature is 280-300° C., and the heat treatment time is 30-35 minutes.

[0023] In step 2.3, the concentrations of zinc nitrate, hexamethylenetetramine and polyethyleneimine are 25 mmol / L, 25 mmol / L and 1.5 mmol / L, respectively.

[0024] In step 2.3, the hydrothermal treatment temperature is 90-95°C and the time is 3-3.5h.

[0025] Another technical solution adopted by the present invention is a catalytic material for triboelectric / piezoelectric catalytic oxidation of CO, which is prepared by the above-mentioned preparation method.

[0026] The beneficial effects of the present invention are:

[0027] The method of the present invention weaves metal wires and PDMS / C wires to obtain a flexible mesh substrate (FTEW), and grows a ZnO nanorod array on the substrate. When impacted by airflow in automobile exhaust, mutual displacement friction occurs between the metal wires and the PDMS / C wires, generating a friction electric field, which can effectively adsorb CO polar molecules. At the same time, the ZnO nanorod arrays also collide with each other to generate a dynamic piezoelectric field, thereby catalytically oxidizing CO adsorbed on the surface of the catalytic material. The catalytic material of the present invention utilizes the coupling effect of the dynamic friction electric field and the dynamic piezoelectric field to enhance its adsorption and catalytic oxidation effect on CO, and realizes the purpose of utilizing the energy contained in automobile exhaust to enhance the adsorption capacity and catalytic oxidation efficiency of low-concentration CO in automobile exhaust, so that the catalytic oxidation activity of the ZnO nanorod array on low-concentration CO at a working temperature of 260° C. is increased by 350%.

[0028] The catalytic material of the present invention has the advantages of no need for external devices, simple preparation method, high cycle stability and high catalytic activity. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 is a schematic structural diagram of the catalytic material of the present invention;

[0030] Figure 2 is a SEM image of the catalytic material prepared in Example 1 of the present invention;

[0031] Figure 3 This is a comparison chart of the CO piezoelectric / triboelectric catalytic oxidation efficiency of different catalytic materials at different wind speeds. DETAILED DESCRIPTION

[0032] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0033] The method for preparing the catalytic material for triboelectric / piezoelectric catalytic oxidation of CO of the present invention is specifically implemented according to the following steps:

[0034] Step 1, Preparation of PDMS / C wire

[0035] Step 1.1, ultrasonically clean the cotton thread in ethanol and deionized water for 20 minutes, dry it at 60-65°C for later use, and then put the dried cotton thread into a tubular furnace and carbonize it at 780-800°C for 3 hours under N2 atmosphere, and then cool it to room temperature and take it out to obtain millimeter-level carbon thread;

[0036] Step 1.2, mixing the PDMS stock solution and the curing agent in a ratio of 10:1 and adding the mixture to cyclohexane to obtain a PDMS cyclohexane solution with a concentration of 10 to 50 wt %;

[0037] Step 1.3, placing the carbon wire obtained in step 1.1 in the PDMS cyclohexane solution obtained in step 1.2, so that the PDMS completely covers the C wire, and immersing the C wire multiple times, the immersion times are 5 to 20 times, to obtain PDMS / C wires with different PDMS coating thicknesses, then taking out the PDMS / C wire, and hanging it in a vacuum drying oven to dry and solidify, to obtain a flexible PDMS / C wire, wherein the thickness of the PDMS coated around the C wire is 2 to 40 μm.

[0038] Step 2, preparation of ZnO nanorod array flexible mesh catalytic material

[0039] Step 2.1, weaving a metal wire with a diameter of 0.1 to 1 mm and the PDMS / C wire obtained in step 1 into a mesh, and adjusting the spacing between the metal wire and the PDMS / C wire to obtain a cross-woven Me-PDMS / C flexible mesh substrate (FTEW) with a mesh count of 16 to 200. The metal wire can be Fe, Al, Cu wire or its alloy wire;

[0040] Step 2.2, dissolve zinc acetate and sodium hydroxide in ethanol respectively to obtain 3mmol / L zinc acetate ethanol solution and 5mmol / L sodium hydroxide ethanol solution, and fully mix the two solutions under water bath conditions to obtain ZnO seed crystal solution, wherein the water bath temperature is 60-65°C, and the water bath time is 45-50min. Afterwards, apply the seed crystal solution on the FTEW, apply 50 to 200 times, and ensure the thickness of the ZnO seed crystal layer. Transfer the FTEW substrate coated with ZnO seed crystals to a tubular furnace, and after heat treatment at 280-300°C for 30-35min under N2 atmosphere, obtain a textured ZnO seed crystal / FTEW;

[0041] Step 2.3, placing the ZnO seed crystal / FTEW in an aqueous solution containing zinc nitrate, hexamethylenetetramine and polyethyleneimine for hydrothermal treatment, wherein the concentrations of zinc nitrate, hexamethylenetetramine and polyethyleneimine are 25mmol / L, 25mmol / L and 1.5mmol / L, respectively, the hydrothermal temperature is 90-95°C, the hydrothermal time is 3-3.5h, and the hydrothermal number is 1 to 3 times, to obtain a ZnO nanorod array / FTEW catalytic material (ZnO NRs / FTEW), whose structure is as shown Figure 1 shown.

[0042] After the catalytic material of the present invention is obtained according to the above steps 1-2, it can be made into a CO catalytic oxidation device by the following method to evaluate its catalytic oxidation performance:

[0043] Take two ZnO NRs / FTEW braids prepared in step 2, stack them together to form a group of ZnO NRs / FTEW, cut and fix them in an iron pipe with a diameter of 100-200 mm, and stack multiple groups of ZnO NRs / FTEW to obtain a CO catalytic oxidation device for automobile exhaust gas; fix the CO catalytic oxidation device in a ring-shaped transparent glass tube, and introduce a CO-O2-N2 mixed gas, wherein the concentration of CO is 1-20 g / m 3 A fan was used to simulate automobile exhaust, and CO and CO2 gas sensors were used to evaluate the catalytic oxidation efficiency of the device.

[0044] The method of the present invention uses a mesh Me-PDMS / C flexible triboelectric material (FTEW) cross-woven by metal wires and PDMS / C wires as a substrate, and then grows a ZnO nanorod array on the substrate as a piezoelectric catalyst to form a mesh ZnO nanorod array / FTEW flexible catalytic material; then two ZnO nanorod arrays / FTEW meshes are assembled to form a CO catalytic oxidation device of a flexible piezoelectric catalyst / triboelectric substrate. When the gas kinetic energy contained in the automobile exhaust itself impacts the FTEW, the flexible metal wire and the PDMS / C wire are mutually displaced and rubbed to generate a triboelectric field. Due to the high intensity of the triboelectric field, CO polar molecules can be more effectively adsorbed, while non-polar CO2 is not affected by the triboelectric field, so that CO can be desorbed from the surface of the catalytic material after being catalytically oxidized to CO2. The contact position of the metal wire and the PDMS / C wire changes continuously, avoiding the adsorption saturation of the triboelectric field, and having continuous adsorption activity for CO. In addition, the ZnO NRs grown on the double-layer FTEW collide with each other under the impact of airflow, generating a dynamic piezoelectric field, thereby catalytically oxidizing CO adsorbed on the surface of ZnO nanorods. In this way, the energy in automobile exhaust can be used to adsorb and catalytically oxidize low-concentration CO through ZnO NRs / FTEW.

[0045] Example 1

[0046] Step 1, Preparation of PDMS / C wire

[0047] Step 1.1, ultrasonically clean the cotton thread in ethanol and deionized water for 20 minutes, dry it at 60°C for later use, and then put the cleaned and dried cotton thread into a tubular furnace and carbonize it at 800°C for 3 hours under N2 protection, and then cool it to room temperature and take it out to obtain millimeter-level carbon thread;

[0048] Step 1.2, mixing the PDMS stock solution and the curing agent in a ratio of 10:1 and adding the mixture into cyclohexane to obtain a 50 wt% PDMS cyclohexane solution;

[0049] Step 1.3, placing the carbon wire obtained in step 1.1 in the PDMS cyclohexane solution prepared in step 1.2, so that the PDMS completely covers the C wire, and repeatedly immersing the C wire in the PDMS for 10 times. After that, suspending the PDMS / C wire in a vacuum drying oven to dry and solidify, to obtain a flexible PDMS / C wire, wherein the thickness of the PDMS coated around the C wire is 20 μm.

[0050] Step 2, preparation of ZnO nanorod array flexible mesh catalytic material

[0051] Step 2.1, weaving Al wires with a diameter of 0.1 mm and PDMS / C wires into a mesh, and adjusting the spacing between the Al wires and the PDMS / C wires to obtain a 16-mesh cross-woven Al-PDMS / C flexible mesh substrate (FTEW);

[0052] Step 2.2, dissolve zinc acetate and sodium hydroxide in 40 mL of ethanol respectively to obtain 3 mmol / L zinc acetate ethanol solution and 5 mmol / L sodium hydroxide ethanol solution, and mix the two solutions in a 65 ° C water bath for 45 minutes to obtain a ZnO seed crystal solution. After that, the ZnO seed crystal solution is coated on the FTEW for 50 times to ensure the thickness of the ZnO seed crystal layer. The FTEW substrate coated with ZnO seed crystals is transferred to a tubular furnace and heat treated at 300 ° C for 30 minutes in a N2 atmosphere to obtain a textured ZnO seed crystal / FTEW.

[0053] Step 2.3, placing the ZnO seed crystals / FTEW in an aqueous solution containing zinc nitrate, hexamethylenetetramine and polyethyleneimine, wherein the concentrations of zinc nitrate, hexamethylenetetramine and polyethyleneimine are 25 mmol / L, 25 mmol / L and 1.5 mmol / L, respectively, and hydroheating at 90°C for 3 h, repeating the hydroheating 3 times to obtain ZnO NRs / FTEW.

[0054] Figure 2 The SEM photo of the catalytic material prepared in this embodiment shows that a ZnO nanorod array with a diameter of about 200nm and a length of about 5μm grows vertically and uniformly on the surface of the PDMS / C wire. The ZnO nanorods are single crystal nanorods in the shape of hexagonal pyramids. The vertically grown single crystal ZnO nanorods with a high aspect ratio have high strength. They can not only bend under weak external forces to generate dynamic piezoelectric fields, so that the ZnO NRs / FTEW piezoelectrically catalytically oxidizes CO, but also are not easily broken under strong external forces, so that the ZnO NRs / FTEW has a long life.

[0055] Example 2

[0056] Step 1, Preparation of PDMS / C wire

[0057] Step 1.1, same as in Example 1;

[0058] Step 1.2, mixing the PDMS stock solution and the curing agent in a ratio of 10:1 and adding the mixture into cyclohexane to obtain a 50 wt % PDMS cyclohexane solution;

[0059] Step 1.3, placing the carbon wire obtained in step 1.1 in the PDMS cyclohexane solution prepared in step 1.2, so that the PDMS completely covers the C wire, and repeatedly immersing the C wire in the PDMS 20 times. After that, suspending the PDMS / C wire in a vacuum drying oven to dry and solidify, to obtain a flexible PDMS / C wire, wherein the thickness of the PDMS coated around the C wire is about 40 μm.

[0060] Step 2, preparation of ZnO nanorod array flexible mesh catalytic material

[0061] Step 2.1, weaving Al wires with a diameter of 0.2 mm and PDMS / C wires into a mesh, and adjusting the spacing between the Al wires and the PDMS / C wires to obtain a 30-mesh cross-woven Al-PDMS / C flexible mesh substrate (FTEW);

[0062] Step 2.2, same as in Example 1;

[0063] Step 2.3, placing the ZnO seed crystals / FTEW in an aqueous solution containing zinc nitrate, hexamethylenetetramine and polyethyleneimine, wherein the concentrations of zinc nitrate, hexamethylenetetramine and polyethyleneimine are 25 mmol / L, 25 mmol / L and 1.5 mmol / L, respectively, hydroheating at 90°C for 2 h, repeating the hydroheating 3 times, to obtain ZnO NRs / FTEW.

[0064] Example 3

[0065] Step 1, Preparation of PDMS / C wire

[0066] Step 1.1, same as in Example 1;

[0067] Step 1.2, mixing the PDMS stock solution and the curing agent in a ratio of 10:1 and adding the mixture into cyclohexane to obtain a 30 wt % PDMS cyclohexane solution;

[0068] Step 1.3, placing the carbon wire obtained in step 1.1 in the PDMS cyclohexane solution prepared in step 1.2, so that the PDMS completely covers the C wire, and repeatedly immersing the C wire in the PDMS for 10 times. After that, suspending the PDMS / C wire in a vacuum drying oven to dry and solidify, to obtain a flexible PDMS / C wire, wherein the thickness of the PDMS coated around the C wire is about 10 μm.

[0069] Step 2, preparation of ZnO nanorod array flexible mesh catalytic material

[0070] Step 2.1, weaving a Cu wire with a diameter of 0.5 mm and a PDMS / C wire into a mesh, and adjusting the spacing between the Cu wire and the PDMS / C wire to obtain a 52-mesh cross-woven Cu-PDMS / C flexible mesh substrate (FTEW);

[0071] Step 2.2, same as in Example 1;

[0072] Step 2.3, placing the ZnO seed crystals / FTEW in an aqueous solution containing zinc nitrate, hexamethylenetetramine and polyethyleneimine, wherein the concentrations of zinc nitrate, hexamethylenetetramine and polyethyleneimine are 25 mmol / L, 25 mmol / L and 1.5 mmol / L, respectively, hydroheating at 90°C for 1 h, repeating the hydroheating 3 times, to obtain ZnO NRs / FTEW.

[0073] Example 4

[0074] Step 1, Preparation of PDMS / C wire

[0075] Step 1.1, same as in Example 1;

[0076] Step 1.2, mixing the PDMS stock solution and the curing agent in a ratio of 10:1 and adding the mixture into cyclohexane to obtain a 20 wt % PDMS cyclohexane solution;

[0077] Step 1.3, placing the carbon wire obtained in step 1.1 in the PDMS cyclohexane solution prepared in step 1.2, so that the PDMS completely covers the C wire, and repeatedly immersing the C wire in the PDMS for 10 times. After that, suspending the PDMS / C wire in a vacuum drying oven to dry and solidify, to obtain a flexible PDMS / C wire, wherein the thickness of the PDMS coated around the C wire is about 8 μm.

[0078] Step 2, preparation of ZnO nanorod array flexible mesh catalytic material

[0079] Step 2.1, weaving Fe wires with a diameter of 1 mm and PDMS / C wires into a mesh, and obtaining a 100-mesh cross-woven Fe-PDMS / C flexible mesh substrate (FTEW) by adjusting the spacing between the Fe wires and the PDMS / C wires;

[0080] Step 2.2, same as in Example 1;

[0081] Step 2.3, placing the ZnO seed crystals / FTEW in an aqueous solution containing zinc nitrate, hexamethylenetetramine and polyethyleneimine, wherein the concentrations of zinc nitrate, hexamethylenetetramine and polyethyleneimine are 25 mmol / L, 25 mmol / L and 1.5 mmol / L, respectively, hydroheating at 90°C for 1 h, repeating the hydroheating twice, to obtain ZnO NRs / FTEW.

[0082] Example 5

[0083] Step 1, Preparation of PDMS / C wire

[0084] Step 1.1, same as in Example 1;

[0085] Step 1.2, mixing the PDMS stock solution and the curing agent in a ratio of 10:1 and adding the mixture into cyclohexane to obtain a 10 wt % PDMS cyclohexane solution;

[0086] Step 1.3, placing the carbon wire obtained in step 1.1 in the PDMS cyclohexane solution prepared in step 1.2, so that the PDMS completely covers the C wire, and repeatedly immersing the C wire in the PDMS for 5 times. After that, suspending the PDMS / C wire in a vacuum drying oven to dry and solidify, to obtain a flexible PDMS / C wire, wherein the thickness of the PDMS coated around the C wire is about 2 μm.

[0087] Step 2, preparation of ZnO nanorod array flexible mesh catalytic material

[0088] Step 2.1, weaving Al wires and PDMS / C wires with a diameter of 1 mm into a mesh, and adjusting the spacing between the Al wires and the PDMS / C wires to obtain a 160-mesh cross-woven Al-PDMS / C flexible mesh substrate (FTEW);

[0089] Step 2.2, same as in Example 1;

[0090] Step 2.3, placing the ZnO seed crystals / FTEW in an aqueous solution containing zinc nitrate, hexamethylenetetramine and polyethyleneimine, wherein the concentrations of zinc nitrate, hexamethylenetetramine and polyethyleneimine are 25 mmol / L, 25 mmol / L and 1.5 mmol / L, respectively, hydroheating at 90°C for 2 h, repeating the hydroheating 3 times, to obtain ZnO NRs / FTEW.

[0091] Comparative Example 1

[0092] This comparative example uses only Al wire for preparation, replacing Al wire and PDMS / C wire for preparation together, and the rest is the same as Example 1, and is specifically implemented according to the following steps:

[0093] Step 1, weaving Al wires with a diameter of 0.1 mm into a mesh, and adjusting the spacing between the Al wires to obtain a 16-mesh cross-woven Al flexible mesh substrate;

[0094] Step 2, same as step 2.2 of Example 1;

[0095] Step 3 is the same as step 2.3 of Example 1.

[0096] Comparative Example 2

[0097] In this comparative example, by changing the morphology control agent (replacing polyethyleneimine with trisodium citrate), the morphology of ZnO grown by the hydrothermal method is nanoparticles (ZnO NPs), and the rest is the same as in Example 1, and is specifically implemented according to the following steps:

[0098] Step 1 is the same as step 1 of Example 1;

[0099] Step 2, preparation of ZnO nanoparticle flexible mesh catalytic material

[0100] Step 2.1 is the same as step 2.1 of Example 1;

[0101] Step 2.2 is the same as step 2.2 of Example 1;

[0102] Step 2.3, placing the ZnO seed crystal / FTEW in an aqueous solution containing zinc nitrate, hexamethylenetetramine and trisodium citrate, wherein the concentrations of zinc nitrate, hexamethylenetetramine and trisodium citrate are 25 mmol / L, 25 mmol / L and 4 mmol / L, respectively, and hydroheating at 90°C for 3 h, repeating the hydroheating 3 times to obtain ZnO NRs / FTEW.

[0103] The catalytic material prepared in Example 1 was made into a CO catalytic oxidation device, and its catalytic oxidation efficiency of CO in automobile exhaust was tested at wind speeds of 2m / s, 5m / s, 10m / s and 20m / s, respectively. The samples were marked as 2-ZnO NRs / FTEW, 5-ZnO NRs / FTEW, 10-ZnO NRs / FTEW and 20-ZnO NRs / FTEW, respectively. The catalytic material prepared in Comparative Examples 1-2 was made into a CO catalytic oxidation device, and its catalytic oxidation efficiency of CO in automobile exhaust was tested at a wind speed of 10m / s, and the samples were marked as 10-ZnO NRs / Al and 10-ZnO NPs / FTEW, respectively. The specific device manufacturing method and testing method are as follows:

[0104] Take two catalytic material fabrics, stack them together to form a double-layer fabric, cut them and fix them in an iron pipe with a diameter of 100 mm to obtain a CO catalytic oxidation device for automobile exhaust; fix the CO catalytic oxidation device in an annular transparent glass tube, and introduce a CO-O2-N2 mixed gas, in which the volume ratio of CO, O2 and N2 is 1:21:78. Use a fan to simulate automobile exhaust at different flow rates, and use CO and CO2 gas sensors to evaluate the catalytic oxidation efficiency of CO catalytic oxidation devices made of various catalytic materials.

[0105] Test results such as Figure 3As shown, it can be seen that at a mixed gas flow rate of 20 m / s, the initial catalytic oxidation temperature of ZnO NRs / FTEW for CO is 180°C, and the conversion efficiency is about 76% at a common automobile exhaust temperature of 260°C. In addition, with the increase of the mixed gas flow rate, the catalytic oxidation efficiency of ZnO NRs / FTEW for CO also increases; but when the flow rate is higher than 5 m / s, further increasing the flow rate has limited effect on the catalytic oxidation activity of ZnO NRs / FTEW. This is because the air flow rate of 5 m / s can make ZnO NRs / FTEW fully rub and collide, and although faster wind speed can increase the frequency and strength of friction and collision, thereby generating faster and larger dynamic triboelectric / piezoelectric electric fields, the excessively fast dynamic triboelectric / piezoelectric electric fields will also offset each other, so that the improvement of the catalytic activity of ZnO NRs / FTEW is limited.

[0106] By comparing Example 1 and Comparative Example 1, it can be seen that at the same flow rate of 10 m / s, compared with ZnO NRs / FTEW prepared with PDMS / C wire and Al wire, ZnO NRs / Al prepared with Al wire only requires a higher starting catalytic oxidation temperature (220°C), and the catalytic oxidation conversion efficiency of ZnO NRs / FTEW is about 350% higher than that of ZnO NRs / Al at an operating temperature of 260°C, which indicates that the friction electric field generated by the mutual friction of the flexible substrate and the dynamic piezoelectric field generated by the mutual collision between the ZnO nanorods greatly improve the catalytic oxidation efficiency of ZnO nanorods for CO.

[0107] By comparing Example 1 and Comparative Example 2, it can be seen that after the morphology of ZnO is changed from nanorods to nanoparticles, at the same flow rate of 10 m / s, the catalytic oxidation efficiency of the material for CO is significantly reduced, and the starting catalytic oxidation temperature is increased from 200°C to 280°C, indicating that the catalytic effect of using ZnO nanorods is significantly improved. This is because the kinetic energy generated by automobile exhaust can be utilized by ZnO nanorods to generate a dynamic piezoelectric field, thereby improving the catalytic oxidation efficiency.

Claims

1. A method for preparing a catalytic material for triboelectric / piezoelectric catalytic oxidation of CO, characterized in that: Follow the steps below to implement it: Step 1, carbonizing the textile cotton thread into a millimeter-sized carbon thread under a N2 atmosphere, and then immersing the carbon thread in a PDMS cyclohexane solution for multiple times, and then taking out the carbon thread and drying it to obtain PDMS / C threads with different PDMS coating thicknesses; Step 2, weaving the metal wire and the PDMS / C wire obtained in step 1 into a mesh to obtain a Me-PDMS / C flexible mesh substrate FTEW; coating the ZnO seed crystal solution on the FTEW multiple times, and then heat-treating the FTEW under a N2 atmosphere to obtain a textured ZnO seed crystal / FTEW; placing the ZnO seed crystal / FTEW in an aqueous solution containing zinc nitrate, hexamethylenetetramine and polyethyleneimine for hydrothermal treatment to obtain a ZnO nanorod array / FTEW catalytic material.

2. The method for preparing a catalytic material for triboelectric / piezoelectric catalytic oxidation of CO according to claim 1, characterized in that: Step 1 is implemented according to the following steps: Step 1.1, ultrasonically clean the cotton thread in ethanol and deionized water respectively, and then dry it at 60-65°C for later use, and then carbonize the dried cotton thread at 780-800°C for 3h in a N2 atmosphere, and then cool it to room temperature to obtain a millimeter-scale carbon thread; Step 1.2, mixing the PDMS stock solution and the curing agent in a ratio of 10:1 and adding the mixture to cyclohexane to obtain a PDMS cyclohexane solution with a concentration of 10 to 50 wt %; Step 1.3, placing the carbon wire obtained in step 1.1 in the PDMS cyclohexane solution prepared in step 1.2, so that the PDMS completely covers the C wire, taking out the C wire after multiple immersions, hanging it in the air to dry and solidify it, and obtaining a flexible PDMS / C wire.

3. The method for preparing a catalytic material for triboelectric / piezoelectric catalytic oxidation of CO according to claim 2, characterized in that: In step 1.3, the C line is immersed for 5 to 20 times, and the thickness of the PDMS coated around the C line in the obtained flexible PDMS / C line is 2 to 40 μm.

4. The method for preparing a catalytic material for triboelectric / piezoelectric catalytic oxidation of CO according to claim 1, characterized in that: Step 2 is implemented as follows: Step 2.1, weaving a metal wire with a diameter of 0.1 to 1 mm and the PDMS / C wire obtained in step 1 into a mesh to obtain a cross-woven Me-PDMS / C flexible mesh substrate FTEW with a mesh number of 16 to 200; Step 2.2, preparing a ZnO seed crystal solution, and then coating the seed crystal solution on the FTEW for multiple times, and then heat-treating the FTEW substrate coated with the ZnO seed crystal in a N2 atmosphere to obtain a textured ZnO seed crystal / FTEW; Step 2.3, placing the ZnO seed crystal / FTEW in an aqueous solution containing zinc nitrate, hexamethylenetetramine and polyethyleneimine for hydrothermal treatment 1 to 3 times to obtain a ZnO nanorod array / FTEW catalytic material.

5. The method for preparing a catalytic material for triboelectric / piezoelectric catalytic oxidation of CO according to claim 4, characterized in that: In step 2.1, the metal wire is Fe, Al, Cu wire or Fe, Al, Cu alloy wire.

6. The method for preparing a catalytic material for triboelectric / piezoelectric catalytic oxidation of CO according to claim 4, characterized in that: In step 2.2, the specific preparation process of the ZnO seed crystal solution is as follows: Dissolve zinc acetate and sodium hydroxide in ethanol respectively to obtain 3mmol / L zinc acetate ethanol solution and 5mmol / L sodium hydroxide ethanol solution, and fully mix the two solutions under water bath conditions, wherein the water bath temperature is 60-65°C and the water bath time is 45-50min to obtain a ZnO seed crystal solution.

7. The method for preparing a catalytic material for triboelectric / piezoelectric catalytic oxidation of CO according to claim 4, characterized in that: In step 2.2, the coating times are 50 to 200 times, the heat treatment temperature is 280-300° C., and the heat treatment time is 30-35 minutes.

8. The method for preparing a catalytic material for triboelectric / piezoelectric catalytic oxidation of CO according to claim 4, characterized in that: In step 2.3, the concentrations of zinc nitrate, hexamethylenetetramine and polyethyleneimine are 25 mmol / L, 25 mmol / L and 1.5 mmol / L, respectively.

9. The method for preparing a catalytic material for triboelectric / piezoelectric catalytic oxidation of CO according to claim 4, characterized in that: In step 2.3, the hydrothermal treatment temperature is 90-95°C and the time is 3-3.5h.

10. A catalytic material for triboelectric / piezoelectric catalytic oxidation of CO, characterized in that: The compound is prepared by the preparation method described in any one of claims 1 to 9.