Pt NPs (at) Mn3O4 composite material as well as preparation method and application thereof
Through the combination of PtNPs@Mn3O4 composite material and electrochemiluminescence technology, a high-sensitivity detection method for Salmonella typhimurium was designed, which solved the problem of insufficient detection speed and sensitivity in the prior art, and realized the food safety field Quickly detect requirements.
Patent Information
- Application Number
- CN202411100752.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-12
AI Technical Summary
Existing bacterial detection methods such as microbial culture, PCR and ELISA have shortcomings in sensitivity and speed, and are difficult to meet the immediate detection needs of Salmonella typhimurium, especially in the field of food safety.
Using PtNPs@Mn3O4 composite material as the sensing substrate, it is prepared by high-temperature carbonization and impregnation reduction, combined with electrochemiluminescence technology, an electrochemiluminescence sensor was designed, and a specific nucleic acid aptamer regulation strategy was used to achieve high levels of Salmonella typhimurium. Sensitivity detection.
It has achieved rapid, sensitive and specific detection of Salmonella typhimurium, which has stable and broad application value, and can effectively prevent disease outbreaks in food safety testing.
Smart Images

Figure CN118988307A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of food safety detection, and specifically relates to a PtNPs@Mn3O4 composite material and a preparation method and application thereof. Background Art
[0002] Foodborne diseases caused by pathogens can cause fever, diarrhea, and even death within 12-72 hours, and have become a focus of global public health attention. Among them, Salmonella typhimurium (S.typhimurium) is one of the most common foodborne pathogens. In addition, S.typhimurium can invade the food production chain through various pathways, and has a lot of opportunities to reproduce and grow in every link from farmland to cooking, causing a variety of health problems. Therefore, early identification and timely diagnosis are crucial to prevent large-scale contamination and spread of S.typhimurium.
[0003] Currently, the main strategies for bacterial detection include microbial culture, polymerase chain reaction (PCR), and enzyme-linked immunosorbent assay (ELISA). Microbial culture, as the gold standard detection method, is accurate but takes at least 24-36 hours and is not suitable for rapid screening or on-site testing. Although PCR-based nucleic acid analysis has high sensitivity and specificity, it is complex to operate and requires professionals or expensive equipment. ELISA is widely used due to its advantages such as high specificity, low cost, and automated operation, but its sensitivity is relatively low.
[0004] Electrochemiluminescence (ECL), as a product of the combination of electrochemistry and chemiluminescence, has the characteristics of high sensitivity and efficiency, and can meet the needs of actual sample monitoring. Therefore, it is favored by many scholars in the field of food safety analysis and detection. To this end, an efficient detection method based on electrochemiluminescence sensor is developed for S. typhimurium to prevent the outbreak of foodborne diseases caused by it, thereby ensuring food safety. Summary of the invention
[0005] The purpose of the present invention is to provide a PtNPs@Mn3O4 composite material and its preparation method and application to meet the needs of real-time detection of S.typhimurium and ensure the sensitivity of detection. The PtNPs@Mn3O4 composite material is modified as a sensing substrate and is designed into a sensor based on a specific nucleic acid aptamer regulation strategy.
[0006] The present invention solves the above technical problems through the following technical solutions.
[0007] The first object of the present invention is to provide a PtNPs@Mn3O4 composite material, wherein the composite material is prepared by reducing a platinum source into nano-platinum PtNPs under the action of a reducing agent and dispersively loading the platinum source onto Mn3O4 having a nanoflower surface structure, thereby obtaining a Pt NPs@Mn3O4 composite material having a hollow nanostructure. The particle size of the Pt NPs@Mn3O4 composite material is 100nm to 250nm, and the particle size of the nano-platinum PtNPs is 2nm to 5nm.
[0008] The second object of the present invention is to provide a method for preparing the above-mentioned PtNPs@Mn3O4 composite material, comprising the following steps:
[0009] Mix KMnO4 and oleic acid, and calcine at 80℃~300℃ in air atmosphere to obtain Mn3O4;
[0010] Mn3O4 is dissolved in a solvent, a platinum source and a reducing agent are added in sequence, and then impregnation reduction is performed at room temperature to obtain a PtNPs@Mn3O4 composite material.
[0011] Furthermore, the mass molar ratio of Mn3O4 and Pt NPs in the Pt NPs@Mn3O4 composite material is 20mg~50mg:1.2×10 -3 mmol~1.6×10 -3 mmol.
[0012] Furthermore, the molar ratio of the reducing agent to the platinum source is 3:0.1-0.3, the platinum source is chloroplatinic acid, the reducing agent is sodium borohydride or ascorbic acid, and the immersion reduction time is 10 min-60 min.
[0013] Furthermore, the mass volume ratio of KMnO4 to oleic acid is 0.1 g to 0.3 g: 1 mL, and the calcination time is 200 min to 400 min.
[0014] The third object of the present invention is to provide an application of the above-mentioned Pt NPs@Mn3O4 composite material in the preparation of a sensor for detecting Salmonella typhimurium, wherein the sensor is an electrochemiluminescent sensor.
[0015] Furthermore, the sensor includes: a substrate, and an electrode layer attached to the substrate, the electrode layer includes a working electrode layer, and the surface of the working electrode layer is coated with a Pt NPs@Mn3O4 composite material, cDNA and Apt-DA in sequence.
[0016] Furthermore, the nucleotide sequence of the cDNA is: 5'-SH-(CH2)6-CTGTCATAATGTCAA-3'; the nucleotide sequence of the Apt-DA is: 5'-COOH-(CH2)6-TATGGCGGCGTCACCCGACGGGGACTTGACATTATGACAG-3'.
[0017] Furthermore, the method for using the sensor to detect Salmonella typhimurium comprises the following steps:
[0018] The sample to be tested is dropped onto the surface of the working electrode layer of the sensor and reacted at room temperature for 40 to 60 minutes. The quantitative detection of Salmonella typhimurium is achieved by measuring the ECL response.
[0019] Furthermore, the detection range of the sensor is 10 1 CFU / mL~10 5 CFU / mL.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] (1) The present invention prepares the PtNCs@Mn3O4 composite material by high-temperature carbonization and impregnation reduction. Since the platinum nanoparticles have excellent catalytic performance on H2O2 and the hollow nanoflower structure of Mn3O4 can provide more reaction active sites, PtNPs@Mn3O4 can be used as a co-reaction catalyst to effectively catalyze the luminescence system of the luminescent reagent Luminol and the co-reactant H2O2, enhance the electrochemiluminescence signal, and be used to modify the sensing interface, increase the electron transfer rate on the electrode surface and catalyze the electrochemiluminescence system, thereby improving the sensitivity of the sensor and enhancing the ECL response.
[0022] (2) The PtNPs@Mn3O4 composite material prepared by the present invention exhibits stable behavior in an electrochemical environment and can maintain its chemical and physical properties during long-term operation, thereby ensuring the stability and reliability of the sensor; the specific recognition of the target and the aptamer causes a change in the distance between the electroactive molecules at the sensing interface, thereby causing a significant change in the electrochemiluminescence signal. At the same time, the sensor provided by the present invention using PtNPs@Mn3O4 as a co-reaction catalyst also exhibits good selectivity and stability, and has broad application value.
[0023] (3) The electrochemiluminescent sensor prepared by the present invention is used for the detection of Salmonella typhimurium. The electrochemiluminescent sensor has good stability, high sensitivity, and a wide linear range, and can achieve simple, rapid, highly sensitive, and specific detection. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a schematic diagram of the principle of detecting S. typhimurium using the electrochemiluminescence sensor provided by the present invention.
[0025] Figure 2 This is a transmission electron microscope image of Mn3O4 prepared in Example 1 of the present invention.
[0026] Figure 3 This is a transmission electron microscope image of the PtNPs@Mn3O4 composite material prepared in Example 1 of the present invention.
[0027] Figure 4 This is the X-ray photoelectron spectrum of the PtNPs@Mn3O4 composite material prepared in Example 1 of the present invention.
[0028] Figure 5 The ECL test chart of the catalytic performance of the PtNPs@Mn3O4 composite material prepared in Example 1 of the present invention.
[0029] Figure 6 This is the AC impedance spectrum of the sensor construction process of the present invention.
[0030] Figure 7 It is the time-current curve diagram of the sensor corresponding to different concentrations of S. typhimurium of the present invention.
[0031] Figure 8 It is a linear fitting curve diagram of the logarithmic value of S. typhimurium at different concentrations and the current of the present invention.
[0032] Fig. 9 This is a diagram showing the selectivity test results of the sensor provided by the present invention.
[0033] Fig.10 This is a graph showing the stability test results of the sensor provided by the present invention. DETAILED DESCRIPTION
[0034] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] It should be noted that the professional terms used in the present invention are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention. Unless otherwise specifically stated, the various raw materials, reagents, instruments and equipment used in the following embodiments of the present invention can be purchased from the market or prepared by existing methods.
[0036] On the one hand, the present invention provides a PtNPs@Mn3O4 composite material, wherein the composite material is prepared by reducing a platinum source into nano-platinum Pt NPs under the action of a reducing agent and dispersing the platinum source into Mn3O4 having a nanoflower surface structure to obtain a PtNPs@Mn3O4 composite material having a hollow nanostructure. The particle size of the PtNPs@Mn3O4 composite material is 100nm to 250nm, and the particle size of the nano-platinum PtNPs is 2nm to 5nm.
[0037] In some specific embodiments, the mass molar ratio of Mn3O4 to Pt NPs in the Pt NPs@Mn3O4 composite material is 20 mg to 50 mg: 1.2×10 -3 mmol~1.6×10 -3 The composite material is prepared by a reaction ratio of 40 mg: 1.5×10 -3 The obtained composite material has an average particle size of about 150 nm.
[0038] It should be noted that in the present invention, PtNPs@Mn3O4 is solid powder, and the source of PtNPs is not limited, and can be prepared using platinum acid or salt solution as a raw material. In some specific embodiments, the platinum source is chloroplatinic acid.
[0039] In the present invention, the PtNPs@Mn3O4 composite material provided by the present invention has the following advantages compared with other sensing substrates: (1) PtNPs@Mn3O4 has excellent catalytic performance, can effectively catalyze the reaction of luminescent reagent luminol (Luminol) and hydrogen peroxide (H2O2), and significantly enhance the electrochemiluminescence signal. This catalytic action reduces the time required for detection and improves the efficiency of the detection process; (2) PtNPs@Mn3O4 has a hollow nanostructure, which provides a large surface area and more active sites. Nanoscale platinum particles are evenly distributed on the Mn3O4 nanoflowers, which can significantly increase the electron transfer rate at the electrode interface; (3) The PtNPs@Mn3O4 composite material exhibits stable behavior in an electrochemical environment and can maintain its chemical and physical properties during long-term operation, thereby ensuring the stability and reliability of the sensor. Therefore, the new co-reaction catalyst PtNPs@Mn3O4 provided by the present invention can significantly improve the sensitivity of the sensor as a sensing substrate.
[0040] On the other hand, the present invention provides a method for preparing a PtNPs@Mn3O4 composite material, comprising the following steps:
[0041] Mix KMnO4 and oleic acid, and calcine at 80°C to 300°C for 200min to 400min in an air atmosphere to obtain Mn3O4;
[0042] Mn3O4 is dissolved in a solvent, a platinum source and a reducing agent are added in sequence, and the mixture is impregnated and reduced at room temperature. The reaction is performed for 10 min to 60 min, and the PtNPs@Mn3O4 composite material is obtained by centrifugation.
[0043] The present invention prepares a PtNCs@Mn3O4 composite material by high-temperature carbonization and impregnation reduction, which is used to modify the sensing interface, increase the electron transfer rate on the electrode surface and catalyze the electrochemiluminescence system, and enhance the ECL response.
[0044] In some specific embodiments, the molar ratio of the reducing agent to the platinum source is 3:0.1-0.3, the platinum source is chloroplatinic acid, the reducing agent is sodium borohydride or ascorbic acid, the platinum source is a chloroplatinic acid solution with a molar concentration of 20mM, and the reducing agent is a sodium borohydride solution with a molar concentration of 0.1M; the solvent is water, more preferably ultrapure water. In the present invention, the purpose of the solvent is to dissolve Mn3O4, and the platinum source is impregnated and reduced under the action of the reducing agent.
[0045] In some specific embodiments, the mass volume ratio of KMnO4 to oleic acid is 0.1 g to 0.3 g: 1 mL.
[0046] In addition, the present invention provides the use of the above-mentioned PtNPs@Mn3O4 composite material in preparing a sensor for detecting Salmonella typhimurium, wherein the sensor is an electrochemiluminescent sensor.
[0047] In some specific embodiments, the sensor includes: a substrate, and an electrode layer attached to the substrate, the electrode layer includes a working electrode layer, and the surface of the working electrode layer is coated with a Pt NPs@Mn3O4 composite material, cDNA and Apt-DA in sequence. As a preferred embodiment of the present invention, the working electrode layer is a glassy carbon electrode, and the PtNPs@Mn3O4 composite material, cDNA and Apt-DA are coated on the surface of the glassy carbon electrode in sequence. The electrode layer also includes a counter electrode and a reference electrode. The counter electrode can be a platinum wire electrode, and the reference electrode can be Ag / AgCl.
[0048] In some specific embodiments, the nucleotide sequence of the cDNA is: 5'-SH-(CH2)6-CTGTCATAATGTCAA-3'; the nucleotide sequence of the Apt-DA is: 5'-COOH-(CH2)6-TATGGCGGCGTCACCCGACGGGGACTTGACATTATGACAG-3'.
[0049] In addition, the present invention also provides a method for quantitatively detecting Salmonella typhimurium, using the sensor for detection. In some specific embodiments, the method for using the sensor to detect Salmonella typhimurium comprises the following steps:
[0050] The sample to be detected is dripped onto the surface of the working electrode layer of the sensor, and reacted at room temperature for 40 to 60 minutes. The quantitative detection of Salmonella typhimurium is achieved by measuring the ECL response. In some specific embodiments, the detection range of the sensor is 10 1 ~10 5 CFU / mL.
[0051] The electrochemiluminescent sensor provided by the present invention has the following mechanism for detecting S.typhimurium: Figure 1 As shown, the details are as follows:
[0052] When S.typhimurium is not present, Apt-DA binds to the cDNA fixed on the electrode surface through DNA hybridization to form a double-stranded structure. Due to the inhibitory effect of DA molecules on the luminescence system, the ECL response is quenched, showing a "signal off" state. When S.typhimurium is present, based on the specific binding of the target and the aptamer, the DA molecule detaches from the electrode interface, the ECL response increases significantly, and the "signal on" state is presented. Therefore, the quantitative determination of S.typhimurium can be achieved through the difference in ECL signals, and the reliability of the detection is improved based on the recognition of specific aptamers.
[0053] The PtNPs@Mn3O4 composite material prepared by the present invention can show good catalytic performance and can be used as a sensing substrate of the sensor, which is beneficial to improve the detection sensitivity. When the analyte S.typhimurium is present, S.typhimurium binds to the aptamer modified with DA, causing DA to detach from the electrode surface, causing a change in the electrochemiluminescence signal. Based on the specific recognition between the target and the nucleic acid aptamer and the dopamine quenching regulation strategy, the quantitative detection of S.typhimurium is achieved by comparing the relationship between the change in the electrochemiluminescence signal and the concentration of the target.
[0054] The sensor made of the PtNPs@Mn3O4 composite material of the present invention has excellent catalytic performance for the electrochemiluminescence system, which can effectively enhance the ECL intensity and shorten the detection time. The PtNPs@Mn3O4 electrochemiluminescence sensor for detecting S.typhimurium constructed by the present invention has a detection range of 10 1 ~10 5CFU / mL, showing a low detection limit and has good application prospects in food safety testing.
[0055] The invention is further described below through specific examples.
[0056] Example 1
[0057] A method for preparing a PtNPs@Mn3O4 composite material comprises the following steps:
[0058] S1. Preparation of Mn3O4: 0.5 g of KMnO4 was dissolved in 250 mL of ultrapure water and stirred vigorously for 30 min to form a reaction mixture, 5 mL of oleic acid was added to the reaction mixture, and then stirring was continued at 28 ° C for 5 h to obtain a brown-black precipitate, which was washed with ultrapure water and ethanol in turn to remove unreacted starting raw materials, and dried at 80 ° C for 10 h to obtain precursor particles, and the precursor particles were calcined at 200 ° C for 200 min in an air atmosphere to obtain monodispersed Mn3O4 nanoparticles;
[0059] S2. Preparation of Pt NPs@Mn3O4: A simple impregnation chemical reduction method was used. 100 mg of Mn3O4 sample was dispersed in 30 mL of deionized water, and then 0.5 mL of 20 mM HPtCl4 solution was added and ultrasonically treated for 30 min. After the ultrasonic treatment, 3 mL of a mixed solution containing 0.1 M NaBH4 and 0.2 M NaOH was quickly injected into the above solution and stirred for 10 min. Finally, the precipitate was separated by centrifugation and washed with deionized water and ethanol, and dried under vacuum at 60 °C for 24 h to obtain Pt NPs@Mn3O4.
[0060] Example 2
[0061] A method for preparing a PtNPs@Mn3O4 composite material comprises the following steps:
[0062] S1. Preparation of Mn3O4: 1.0 g of KMnO4 was dissolved in 250 mL of ultrapure water and stirred vigorously for 30 min to form a reaction mixture, 5 mL of oleic acid was added to the reaction mixture, and then stirring was continued at 28°C for 5 h to obtain a brown-black precipitate, which was washed with ultrapure water and ethanol in turn to remove unreacted starting raw materials, and dried at 80°C for 10 h to obtain precursor particles, and the precursor particles were calcined at 200°C for 300 min in an air atmosphere to obtain monodispersed Mn3O4 nanoparticles;
[0063] S2. Preparation of Pt NPs@Mn3O4: A simple impregnation chemical reduction method was used. 100 mg of Mn3O4 sample was dispersed in 30 mL of deionized water, and then 0.5 mL of 40 mM HPtCl4 solution was added and ultrasonically treated for 30 min. After the ultrasonic treatment, 3 mL of a mixed solution containing 0.1 M NaBH4 and 0.2 M NaOH was quickly injected into the above solution and stirred for 40 min. Finally, the precipitate was separated by centrifugation and washed with deionized water and ethanol, and dried under vacuum at 60 °C for 24 h to obtain Pt NPs@Mn3O4.
[0064] Example 3
[0065] A method for preparing a PtNPs@Mn3O4 composite material comprises the following steps:
[0066] S1. Preparation of Mn3O4: 1.5 g of KMnO4 was dissolved in 250 mL of ultrapure water and stirred vigorously for 30 min to form a reaction mixture, 5 mL of oleic acid was added to the reaction mixture, and then stirring was continued at 28°C for 5 h to obtain a brown-black precipitate, which was washed with ultrapure water and ethanol in turn to remove unreacted starting raw materials, and dried at 80°C for 10 h to obtain precursor particles, which were calcined at 200°C for 400 min in an air atmosphere to obtain monodispersed Mn3O4 nanoparticles;
[0067] S2. Preparation of Pt NPs@Mn3O4: A simple impregnation chemical reduction method was used. 100 mg of Mn3O4 sample was dispersed in 30 mL of deionized water, and then 0.5 mL of 60 mM HPtCl4 solution was added and ultrasonically treated for 30 min. After the ultrasonic treatment, 3 mL of a mixed solution containing 0.1 M NaBH4 and 0.2 M NaOH was quickly injected into the above solution and stirred for 60 min. Finally, the precipitate was separated by centrifugation and washed with deionized water and ethanol, and dried under vacuum at 60 °C for 24 h to obtain Pt NPs@Mn3O4.
[0068] The structures of the PtNPs@Mn3O4 composite materials prepared in Examples 1-3 are similar, and the effects are parallel. The PtNPs@Mn3O4 composite material prepared in Example 1 is taken as an example to illustrate the structure and performance of the PtNPs@Mn3O4 composite material prepared in Example 1, as follows:
[0069] The Mn3O4 nanoflowers and PtNPs@Mn3O4 composite materials prepared in Example 1 were observed by transmission electron microscopy. Figure 2 and Figure 3 shown.
[0070] Figure 2 This is a transmission electron microscope image of Mn3O4 prepared in Example 1 of the present invention. Figure 2 As shown in the figure, the Mn3O4 nanoparticles are uniform in size, with a particle size of about 150nm. There is a clear contrast difference between the inside and outside of the nanoparticles, which shows that the Mn3O4 particles are hollow structures and have good dispersibility.
[0071] Figure 3 This is a transmission electron microscope image of the PtNPs@Mn3O4 composite material prepared in Example 1 of the present invention. Figure 3 As shown in the figure, the particle size of PtNPs is about 2nm, and they are evenly distributed on the surface of Mn3O4 nanoflowers without obvious agglomeration. The prepared Mn3O4 nanoflower structure provides a good loading for Pt nanoparticles, which can effectively improve the overall catalytic performance of the composite material.
[0072] Furthermore, X-ray photoelectron spectroscopy was used to investigate whether the Pt NPs@Mn3O4 composite material was successfully constructed. Figure 4 shown.
[0073] Figure 4 This is the X-ray photoelectron spectrum of the Pt NPs@Mn3O4 composite material prepared in Example 1 of the present invention. Figure 4 As shown, the full spectrum of XPS shows several characteristic peaks: 71.55, 284.85, 531.45, and 641.85 eV, corresponding to Pt4f, C1s, O1s, and Mn 2p, respectively, indicating the presence of Pt, C, O, and Mn, thus proving the successful synthesis of the PtNPs@Mn3O4 composite material.
[0074] Figure 5 The ECL test graph is for the catalytic performance of the PtNPs@Mn3O4 composite material prepared in Example 1 of the present invention. Figure 5 As shown, the catalytic performance of the composite material prepared in Example 1 on the Luminol-H2O2 luminescence system under ECL test conditions was studied. First, the good hollow structure of Mn3O4 can expose more active sites for the catalysis of H2O2, thereby improving the ECL response. The ECL response of the PtNPs@Mn3O4 composite material is significantly enhanced relative to the bare electrode, indicating that the PtNPs@Mn3O4 composite material can effectively promote the generation efficiency of hydroxyl radicals when modifying the electrode, and has good ECL performance in the luminol system. This is consistent with the predicted mechanism and qualitative analysis results.
[0075] Application Examples
[0076] Example 1 was composed of Mn3O4 and PtNPs at 40 mg: 1.5×10 -3The electrochemiluminescent sensor of the Pt NPs@Mn3O4 composite material was prepared with a reaction ratio of mmol. The preparation method of the sensor is as follows:
[0077] Electrode construction:
[0078] Step 1: polish the bare electrode to a mirror surface using 0.3 nm and 0.05 nm Al2O3 polishing powders in sequence, and clean the electrode surface with ultrapure water and dry it;
[0079] Step 2: Add 6 μL of 2.0 mg / mL Pt NPs@Mn3O4 nanoparticle solution onto the surface of the glassy carbon electrode (GCE) to form a uniform nanofilm.
[0080] Step 3: Next, 6 μL of 1.0 μg / mL cDNA sequence was fixed on the electrode interface via Pt-S bonds;
[0081] Step 4: Subsequently, 6 μL of 6-mercaptohexanol (MCH) solution was added and incubated for 40 min to block the unreacted active sites;
[0082] Step 5, add 6 μL of 1.0 μg / mL Apt-DA to the electrode surface where cDNA is fixed, and incubate at 37°C for 1 h to form double-stranded DNA;
[0083] Step 6: Finally, the electrode surface is modified with Salmonella typhimurium solutions of different concentrations and incubated for 40 minutes to obtain an electrochemiluminescent sensor for detecting S. typhimurium.
[0084] The detection effect of the electrochemiluminescent sensor prepared by the above method on S. typhimurium was tested as follows:
[0085] Electrochemical impedance spectroscopy (EIS) was used to study the electrode assembly process. Figure 6 The AC impedance spectrum of the sensor construction process of the present invention is as follows: Figure 6 As shown in Figure 2, the semicircle diameter represents the charge transfer resistance (Ret), which is related to the modification of the electrode surface. Figure 6 As shown in the figure, after PtNPs@Mn3O4 is deposited (curve b), the poor conductivity of PtNPs@Mn3O4 hinders electron transfer and the charge transfer resistance increases (curve b). cDNA is modified on the electrode surface through Pt-S bonds, and Ret increases (curve c). Then MCH is added to block the nonspecific active sites on the sensor interface. Because MCH forms an insulating layer that increases steric hindrance, Ret further increases (curve d). After Apt-DA is added, the non-conductive material will seriously hinder [Fe(CN)6] 3- / [Fe(CN)6]4- The diffusion of the modified electrode and the Ret value are much larger than those of the unmodified electrode. The EIS results show that the electrochemiluminescence sensor was successfully constructed.
[0086] Take 1 mL of S. typhimurium in the late logarithmic culture stage and centrifuge at 8000 rpm for 5 minutes in a 2 mL sterilized centrifuge tube to collect the bacteria. Wash with an equal volume of 2× PBS and dilute the bacteria tenfold. Spread on a plate to determine the bacterial count range of 10 1 CFU / mL~10 5 CFU / mL. The test conditions of the ECL response curve of the ECL sensor to targets with different colony counts are to measure the signal response of the experiment in 15mL PBS (pH=7.0) solution and record the electrochemiluminescence curve (the solution contains 1mM Luminol and 2mM H2O2) under the conditions of potential range of 0V~0.8V and scan rate of 50mV / s. The results are shown in Figure 7 and Figure 8 shown.
[0087] Figure 7 The time-current curve diagram of the sensor corresponding to different concentrations of S. typhimurium of the present invention; Figure 8 : is a linear fitting curve diagram of the logarithmic value of S.typhimurium at different concentrations and the current of the present invention. Figure 7 and Figure 8 As shown, the concentration of Salmonella typhimurium was 10 1 CFU / mL~10 5 There is a good linear correlation in the CFU / mL range. As the concentration of Salmonella typhimurium increases, the ECL signal continues to increase. The linear regression equation is ECL = 2279.16LogC-736.64, and the correlation coefficient R 2 is 0.997; where ECL is the change in ECL intensity, C is the target concentration, and the LOD obtained by calculation is 6 CFU / mL (where S / N=3).
[0088] Fig. 9 The selectivity test result diagram of the sensor provided by the present invention. Fig. 9 The results show that the four interfering strains are similar to the negative control group, because non-target bacteria will not be recognized by Apt and no obvious signal changes will be produced. Only when the sample contains Salmonella typhimurium, Apt can recognize the target bacteria, Apt-DA falls off the electrode surface, the ECL signal is restored, and both the target sample and the mixed sample produce obvious ECL signal changes. These phenomena show that Apt can only specifically bind to the target without interference, and can well distinguish mixed strain samples containing Salmonella typhimurium.
[0089] In addition, the ECL sensor was scanned continuously for 10 cycles under the same conditions to test the stability of the sensor. The results are shown in Fig.10 shown.
[0090] Fig.10 This is a graph showing the stability test results of the sensor provided by the present invention. Fig.10 It can be seen that the relative standard deviation of the ECL signal response is 3.30%, indicating that the sensor has good stability.
[0091] It should be noted that when the present invention involves a numerical range, it should be understood that the two endpoints of each numerical range and any value between the two endpoints can be selected. Since the steps and methods used are the same as those in the embodiments, in order to avoid redundancy, the present invention describes a preferred embodiment. Although the preferred embodiments of the present invention have been described, those skilled in the art may make additional changes and modifications to these embodiments once they know the basic creative concept. Therefore, the attached claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.
[0092] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. A PtNPs@Mn3O4 composite material, characterized in that: The composite material is prepared by reducing a platinum source into nano-platinum Pt NPs under the action of a reducing agent and dispersing and loading the nano-platinum on Mn3O4 with a nano-flower surface structure to obtain a PtNPs@Mn3O4 composite material with a hollow nano-structure. The particle size of the PtNPs@Mn3O4 composite material is 100nm-250nm.
2. A method for preparing the PtNPs@Mn3O4 composite material according to claim 1, characterized in that: The following steps are involved: Mix KMnO4 and oleic acid, and calcine at 80℃~300℃ in air atmosphere to obtain Mn3O4; Mn3O4 is dissolved in a solvent, a platinum source and a reducing agent are added in sequence, and then impregnation reduction is performed at room temperature to obtain a Pt NPs@Mn3O4 composite material.
3. The method for preparing the PtNPs@Mn3O4 composite material according to claim 2, characterized in that: The mass molar ratio of M3O4 and PtNPs in the PtNPs@Mn3O4 composite material is 20mg~50mg:1.2×10 -3 mmol~1.6×10 -3 mmol.
4. The method for preparing the PtNPs@Mn3O4 composite material according to claim 2, characterized in that: The molar ratio of the reducing agent to the platinum source is 3:0.1-0.3, the platinum source is chloroplatinic acid, the reducing agent is sodium borohydride or ascorbic acid, and the immersion reduction time is 10 minutes to 60 minutes.
5. The method for preparing the PtNPs@Mn3O4 composite material according to claim 2, characterized in that: The mass volume ratio of KMnO4 to oleic acid is 0.1g-0.3g:1mL, and the calcination time is 200min-400min.
6. Use of the PtNPs@Mn3O4 composite material according to claim 1 in preparing a sensor for detecting Salmonella typhimurium, characterized in that: The sensor is an electrochemiluminescent sensor.
7. The use according to claim 6, characterized in that: The sensor comprises: a substrate, and an electrode layer attached to the substrate, wherein the electrode layer comprises a working electrode layer, and a PtNPs@Mn3O4 composite material, cDNA and Apt-DA are sequentially coated on the surface of the working electrode layer.
8. The use according to claim 7, characterized in that: The nucleotide sequence of the cDNA is: 5'-SH-(CH2)6-CTGTCATAATGTCAA-3'; the nucleotide sequence of the Apt-DA is: 5'-COOH-(CH2)6-TATGGCGGCGTCACCCGACGGGGACTTGACATTATGACAG-3'.
9. The use according to claim 6, characterized in that: The method for using the sensor to detect Salmonella typhimurium comprises the following steps: The sample to be detected is dropped onto the surface of the working electrode layer of the sensor, and reacted at room temperature for 40 to 60 minutes. The detection of Salmonella typhimurium is achieved by measuring the ECL response.
10. The use according to claim 9, characterized in that: The detection range of the sensor is 10 1 CFU / mL~10 5 CFU / mL.
Citation Information
Patent Citations
Noble metal-Mn3O4-carbon nanotube composite material, and preparation method and application thereof
CN103111294A
MnO2 hybrid nanoflower, and preparation method and application thereof
CN108918864A
Simple preparation method of glycerol biosensor chip
CN112240901A
ECL-based electrode, manufacturing method for ECL-based electrode, ECL sensor, manufacturing method for ECL sensor, method for ECL detection of nucleic acid-specific site modification, and kit for nucleic acid modification detection used for method for ECL detection of nucleic acid-specific site modification
US20240044803A1
Cited By
Pt-modified Mn3O4 composite material, preparation method thereof, gas sensitive element and application of gas sensitive element
CN120334304A