Hollow fiber ceramic catalytic membrane as well as preparation method and application thereof
The preparation of hollow fiber ceramic membranes through water supply sludge by tap water plant and combined with the advanced ozone oxidation process, the problems of high cost and low retention efficiency of ceramic filter membranes are solved, and the efficient removal of small molecules is achieved and difficult to degrade organic matter, which significantly improves the performance and removal of membranes Rate.
Patent Information
- Application Number
- CN202411286348.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-11-22
AI Technical Summary
The existing ceramic filter membranes are difficult to meet the requirements of contemporary water quality purification due to high calcining temperature, high cost, large pore size, unstable membrane structure and low interception efficiency.
Sludge crystal powder was prepared by water feed sludge from tap water plant, hollow fiber ceramic membrane substrate was prepared by dry and wet spinning phase transfer method, and FeOCl catalyst was obtained through multiple impregnation and calcination, and organic matter difficult to degrade from small molecules was removed in combination with the advanced ozone oxidation process.
The resource utilization of sludge has been achieved, production costs have been reduced, the performance stability and catalytic degradation capacity of ceramic membranes have been significantly improved, and the removal rate of organic matter difficult to degrade small molecules has reached 77.6%-99.5%, and the operation and maintenance costs have been reduced.
Smart Images

Figure HDA0005043212580000011 
Figure HDA0005043212580000012
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of water treatment and membrane separation, and specifically relates to a hollow fiber ceramic catalytic membrane and a preparation method and application thereof. Background Art
[0002] With the acceleration of global urbanization, the urban population has increased dramatically, and residents' demand for safe and reliable drinking water resources has increased significantly. The flocculants used in water plants are an important means of removing suspended particles and colloidal substances in water. A large amount of water supply sludge is produced during the flocculation and sedimentation process. Its main components are flocculant residues and inorganic matter, humus and plant residues in the raw water adsorbed by flocculants. my country produces about 1.5-2.4 million tons of dry sludge every year, which is difficult to treat. It is often discharged directly into sewage pipes without any treatment, which has a great impact on the aquatic ecological environment. Traditional landfill or incineration methods are costly and easily lead to resource waste and environmental pollution. Water supply sludge is rich in inorganic components such as aluminum (Al) and silicon (Si), and has certain resource potential. It can be used to prepare lightweight ceramsite for construction or gardening, high-efficiency adsorbents for wastewater treatment, cement admixtures to improve its performance, and artificial wetland fillers to improve the ecological environment. There are also studies that use water supply sludge to directly compress and calcine to prepare inorganic filter membranes, but this method has shortcomings such as large pore size, unstable membrane structure, and low interception efficiency, which makes it difficult to meet the requirements of modern filter membrane performance for water purification. Summary of the invention
[0003] The purpose of the present invention is to provide a method for preparing a hollow fiber ceramic catalytic membrane, which can solve the cost problem of existing ceramic membranes and improve the catalytic performance of the catalytic membrane coupled with ozone advanced oxidation.
[0004] The technical solution adopted by the present invention is: a method for preparing a hollow fiber ceramic catalytic membrane, comprising the following steps:
[0005] Step 1, preparing sludge crystal powder using water supply sludge from a water plant;
[0006] Step 2, preparing a ceramic membrane suspension according to a set ratio, the ceramic membrane suspension comprising an organic solvent, a plasticizer, a dispersant and sludge crystal powder, successively adding the organic solvent, the pore-forming agent, the sludge crystal powder and the plasticizer, grinding and stirring to obtain a uniformly dispersed suspension, and performing a vacuum degassing treatment on the suspension;
[0007] Step 3, using a dry-wet spinning phase transfer method, by controlling the flow rate of the pure water condensate and the suspension, the membrane fibers are squeezed into the water tank to complete the dry-wet spinning phase transfer and obtain a membrane blank with a smooth surface;
[0008] Step 4, drying the membrane blank at room temperature and then calcining it at high temperature to obtain a hollow fiber ceramic membrane substrate, using anhydrous ethanol to prepare a ferric chloride hexahydrate solution, immersing the hollow fiber ceramic membrane substrate in the solution and ultrasonically treating it, drying it and then calcining it, repeating the above immersion and calcination process in a cycle to obtain a FeOCl hollow fiber ceramic catalytic membrane.
[0009] Furthermore, the water supply sludge from the waterworks is dried in the sun and then crushed using a grinder. The sludge powder is sieved using a sieve to obtain sludge powder with uniform particle size and calcined to obtain crystalline powder. The crystalline powder is ground in an omnidirectional ball mill to obtain crystalline powder with uniform particle size as a raw material for preparing ceramic membranes, and the powder is put into an oven for drying.
[0010] Furthermore, in step 1, the crushing time of the crusher is 50 to 120 seconds, the mesh number of the sludge screen is 70 to 150 meshes, the particle size of the inorganic powder is 106 to 212 μm, and the sludge powder is fired in a muffle furnace at a temperature of 900 to 1500°C to obtain quartz and mullite crystal powders. The grain size of the crystal powder is 30.31 to 36.16 nm, and the particle size of the inorganic powder is 53 to 90 μm.
[0011] Furthermore, in step 2, the ceramic membrane suspension includes 44% of organic solvent, 0.8% of binder, 5.5% of plasticizer, 0.8% of dispersant and 48.9% of inorganic powder in mass percentage, the grinding ball diameter is 15mm:12mm, the number ratio of the two grinding balls is 1:5, the ball mill speed is 300rpm, the suspension stirring time is 36h, the plasticizer stirring time is 36h, and the vacuum degassing time is 60min; the organic solvent is dimethylformamide, dimethylacetamide or N-methylpyrrolidone; the binder is polyvinylpyrrolidone, sodium carboxymethylcellulose or hydroxypropyl methylcellulose, the plasticizer is dibutyl phthalate, dioctyl adipate or polyether sulfone; the dispersant is polyacrylic acid or polyethylene glycol.
[0012] Furthermore, in step 3, the dry-wet spinning phase transfer uses a spinneret with an outer diameter of 2 to 4.8 mm, an inner diameter of 1 to 2.4 mm, a suspension flow rate of 10 to 15 mL / min, and an inner condensate flow rate of 10 to 20 mL / min.
[0013] Furthermore, in step 4, the calcination temperature of the membrane body is 1100-1400° C., and the calcination time is 150-240 min.
[0014] Further, in step 4, the concentration of ferric chloride hexahydrate is 0.7-1.0 g / mL -1 , ultrasonic treatment for 30-60 min, calcination temperature 210-240 ° C, FeOCl catalyst coating cycle repeated 3-5 times.
[0015] On the other hand, the present invention provides a hollow fiber ceramic catalytic membrane, which is obtained by using a preparation method based on the hollow fiber ceramic catalytic membrane.
[0016] The present invention also provides a method for treating water using the hollow fiber ceramic catalytic membrane, using the FeOCl hollow fiber ceramic catalytic membrane coupled with an ozone aeration system to remove small molecule refractory organic matter, which includes drug resistance, dyes and endocrine disruptors.
[0017] Furthermore, the air ozone generator inlet flow rate of the ozone aeration system is 100-250 mL / min, the ibuprofen removal rate is 77.6-99.5%, and the TOC removal rate is 40.2-55.6%; the methylene blue removal rate is 83.5-99.2%, and the TOC removal rate is 43.5-62.7%; the bisphenol A removal rate is 78.3-98.5%, and the TOC removal rate is 39.6-66.4%.
[0018] The beneficial effects of the present invention are as follows: water supply sludge can be calcined at high temperature to form mullite phase crystals, which have uniform particle size and stable performance and can be used as a raw material for preparing inorganic ceramic membranes. In addition, nano-catalyst particles are loaded onto the surface of a hollow fiber ceramic membrane substrate, and the prepared ceramic catalytic membrane can be coupled with an ozone advanced oxidation process, and can become a powerful tool for catalytic degradation of various organic pollutants. The ceramic membrane can catalytically degrade small molecules of difficult-to-degrade organic matter while filtering. The present invention proposes a method for preparing a hollow fiber ceramic catalytic membrane, which uses sludge generated in the flocculation process of a water plant as a raw material, realizes the resource utilization of the sludge, prepares a ceramic membrane substrate with stable performance, and further realizes the functional application of the ceramic membrane. The method first pretreats the water plant sludge to remove impurities therein, converts the pretreated sludge into mullite phase crystal powder, and prepares a hollow fiber ceramic membrane substrate. Secondly, a ceramic catalytic membrane is obtained through impregnation and roasting, and coupled with the ozone advanced oxidation process, the removal of various small molecular difficult-to-degrade organic matter can be achieved. The water sludge from the water plant is used as raw material, which significantly reduces the production cost, realizes the resource utilization of waste, and can also practice the environmental protection concept of treating waste with waste. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 Changes in crystal form and ceramic membrane substrate at different temperatures.
[0020] Figure 2 Macroscopic and microscopic morphology of hollow fiber ceramic membrane substrate. DETAILED DESCRIPTION
[0021] The present invention is described in detail below in conjunction with specific implementation modes.
[0022] The present invention provides a method for preparing a hollow fiber ceramic catalytic membrane, which is specifically implemented according to the following steps:
[0023] Step 1, pretreatment of water sludge from waterworks: dry the sludge in the sun and then crush it with a grinder for 50 to 120 seconds. Then use a sieve to screen the sludge powder. The sludge sieve has a mesh size of 70 to 150 to obtain sludge powder with uniform particle size. The inorganic powder particle size is 106 to 212 μm. The sludge powder is then fired in a muffle furnace at a temperature of 900 to 1500°C to obtain quartz phase and mullite phase crystal powders. The powder crystals are ground in an omnidirectional ball mill to obtain crystalline powder with uniform particle size as the raw material for preparing ceramic membranes. The grain size is 30.31 to 36.16 nm, and the inorganic powder particle size is 53 to 90 μm. Place in an oven for drying;
[0024] Step 2, prepare a ceramic membrane suspension of a specified proportion with an organic solvent, a binder, a plasticizer, a dispersant and sludge crystal powder, wherein the organic solvent is dimethylformamide, dimethylacetamide or N-methylpyrrolidone; the binder is polyvinylpyrrolidone, sodium carboxymethylcellulose or hydroxypropyl methylcellulose, and the plasticizer is dibutyl phthalate, dioctyl adipate or polyethersulfone; the amount of each component is calculated by mass percentage, 44% organic solvent, 0.8% binder, 5.5% plasticizer, 0.8% dispersant and 48.9% inorganic powder, and the total mass percentage of each component is 100%. NMP solvent, PVP powder, sludge crystal powder and polyethersulfone powder are added to the ball mill rotor in sequence, and the grinding ball size is 15mm:12mm with a ratio of 1:5. The ball mill speed is 300rpm, the suspension stirring time is 36h, and the polyethersulfone stirring time is 36h. Grind and stir to obtain a uniformly dispersed suspension, and finally use a vacuum pump to perform vacuum degassing for 60 minutes;
[0025] Step 3, according to the different designs of the membrane blank, the outer diameter of the single-hole spinneret used is 2-4.8 mm, the inner diameter is 1-2.4 mm, and the flow rates of the pure water condensate and the suspension are controlled, the suspension flow rate is 10-15 mL / min, and the pure water condensate flow rate is 10-20 mL / min. The membrane filaments are squeezed into the water tank to complete the dry-wet spinning phase transfer process and obtain a membrane blank with a smooth surface.
[0026] Step 4: Dry the membrane blank at room temperature, and then place it in a muffle furnace for high-temperature calcination to obtain a hollow fiber ceramic membrane substrate. The membrane blank calcination temperature is 1100-1400°C, and the calcination time is 150-240 minutes. Use anhydrous ethanol to prepare a concentration of 0.7-1.0 g / mL -1 The membrane substrate is immersed in a solution of ferric chloride hexahydrate and subjected to ultrasonic treatment for 30 to 60 minutes. After drying, it is calcined in a muffle furnace at a temperature of 210 to 240°C. The above immersion and calcination process is repeated 3 to 5 times to obtain a FeOCl hollow fiber ceramic catalytic membrane.
[0027] The hollow fiber ceramic catalytic membrane coupled with the ozone aeration system was used to remove small molecule refractory organic matter, including anti-drugs, dyes and endocrine disruptors, ibuprofen, methylene blue and bisphenol A, respectively, and the removal rate and TOC removal rate of the above three typical organic pollutants were evaluated. The air ozone generator inlet flow rate was 100-250 mL / min, the ibuprofen removal rate was 77.6-99.5%, and the TOC removal rate was 40.2-55.6%. The methylene blue removal rate was 83.5-99.2%, and the TOC removal rate was 43.5-62.7%. The bisphenol A removal rate was 78.3-98.5%, and the TOC removal rate was 39.6-66.4%.
[0028] The invention provides a method for preparing a hollow fiber ceramic catalytic membrane. First, sludge is pretreated, including drying, crushing and screening, to obtain sludge powder with uniform particle size. Secondly, the sludge powder is fired in a muffle furnace to obtain pretreated inorganic crystalline particles. A ceramic membrane suspension is prepared, and the components are fully mixed by stirring with a ball mill to obtain a uniform and stable suspension. A single-hole spinneret is used to control the flow rate of the condensate in pure water and the flow rate of the suspension, and the suspension is squeezed into a water tank to complete the phase transfer process. After drying at room temperature, a membrane blank with uniform pore size and smooth surface is obtained. Finally, the dried membrane blank is calcined at high temperature in a muffle furnace to obtain a hollow fiber ceramic membrane substrate, and a FeOCl hollow fiber ceramic catalytic membrane is obtained after impregnation and roasting.
[0029] The present invention uses water supply sludge from a waterworks as raw material, and converts the sludge into mullite phase crystal powder through high-temperature calcination, which is used as a raw material for ceramic membranes with excellent performance. Traditional ceramic membrane preparation usually requires a higher calcination temperature. The mullite phase crystal powder prepared in the present invention has
[0030] The stable crystal structure and chemical properties, and the formation of uniform crystal powder, can produce ceramic membranes with excellent performance at lower calcination temperatures, significantly reducing the calcination temperature of the ceramic membrane. This not only reduces energy consumption, but also reduces preparation costs, solves the problem of sludge treatment, and utilizes the resource utilization of water supply sludge to achieve the environmental protection concept of treating waste with waste.
[0031] The present invention controls various parameters in the dry-wet spinning process, such as the type and ratio of solvent and non-solvent, the conditions of the coagulation bath, the spinning speed, etc., so as to adjust the thickness, porosity, pore size and other structural parameters of the dense layer and the loose layer, thereby preparing a hollow fiber ceramic membrane substrate that meets different application requirements.
[0032] The hollow fiber ceramic membrane tube prepared by the present invention has a unique dense layer and loose layer structure. In the process of preparing the membrane substrate, after the suspension is extruded into the coagulation bath through the spinneret, the solvent in the suspension and the coagulation bath diffuse due to the difference in solvent polarity, the solvent near the membrane surface area is replaced by the coagulation bath, the local concentration of the suspension increases rapidly, and after reaching the saturated state, it quickly precipitates and aggregates, and the ceramic particles near the membrane surface are densely stacked, and the dense layer formed has the effect of selectivity and interception, which can provide sufficient surface area for the introduction of nano-catalytic components. In addition to the rapid phase transfer and dense layer formation in the surface area, phase separation is also occurring inside the membrane, and the exchange of the solvent and the coagulation bath is relatively slow, which leads to a relatively slow precipitation and aggregation speed of the suspension, so that the ceramic membrane substrate has more porous structures, and the formed loose layer provides a good mechanical support strength for the membrane, and also provides a large membrane flux. The synergistic effect of the dense layer and the loose layer enables the hollow fiber ceramic membrane to have a specific selective separation performance. By reasonably controlling the air gap distance, the flow rate of the pure water condensate, the concentration of the suspension, and adjusting the proportion and structure of the dense layer and the loose layer in the membrane tube section, the optimal performance of ceramic membrane selection and separation can be achieved. For example, the prepared sandwich membrane structure has a loose layer on the outer layer, a dense layer in the middle layer, and a loose layer on the inner layer. The loose layer in the membrane structure can provide a larger flux, and the dense layer has a smaller micro-nano pore size and a more tortuous pore structure than the loose layer, forming a micro-nano confinement, which can slow down the diffusion rate of pollutants in the membrane substrate and prolong their residence time in the membrane.
[0033] The present invention uses a ceramic membrane substrate impregnated with FeCl 3. 6H2O solution, FeOCl-loaded ceramic catalytic membrane was prepared, which had a large specific surface area and excellent catalytic activity. 3. In 6H2O solution, the hollow fiber ceramic substrate was repeatedly impregnated, the number of impregnations was changed, and the ceramic catalytic membrane was obtained after calcination. Nano-FeOCl catalytic active particles were loaded on the surface of the ceramic membrane, in the dense layer and loose layer structure, especially in the dense layer, which can further enhance the nano-confinement effect, slow down the diffusion rate of active species, and increase the contact degree between pollutants and active species. The nano-confinement effect can significantly improve the degradation and removal performance of the ceramic catalytic membrane for pollutants.
[0034] The hollow fiber ceramic catalytic membrane prepared by the present invention has a high packing density. The membrane area per unit volume of the hollow fiber ceramic catalytic membrane is higher than that of the traditional flat ceramic membrane and tubular ceramic membrane. The hollow fiber ceramic catalytic membrane not only promotes the mass transfer and contact efficiency of ozone, but also provides an efficient mass transfer and catalytic reaction platform for the ozone advanced oxidation coupling process, which can further improve the overall pollutant degradation efficiency.
[0035] The present invention adopts different impregnation and calcination times to load the catalyst. This preparation process can effectively regulate the nanopore size of the hollow fiber ceramic membrane, and the pore size range is 6.1 to 197.8 nm, which effectively improves the degree of reaction between the catalytic active components and pollutants, and produces a significant nano-confinement effect during the catalytic degradation process, thereby enhancing the effect of the catalytic reaction. In addition, the membrane pollution problem is effectively controlled, and the ceramic catalytic membrane has stronger self-cleaning ability and longer service life. This advantage makes the hollow fiber ceramic catalytic membrane more stable and reliable in practical applications, reducing operation and maintenance costs.
[0036] It fully contacts with O3 in water and produces a large number of free radical active species (ROS), including hydroxyl radicals, superoxide radicals and singlet oxygen non-radical species, which can fully react with pollutants in the nano-confined channels of the catalytic membrane. These free radical active species can effectively remove small molecule refractory organic matter. The catalytic synergy of nanocatalyst FeOCl and O3 shows extremely high degradation efficiency. According to experimental data, the removal rate of organic pollutants such as ibuprofen, methylene blue and bisphenol A by this catalyst can reach almost 100%, which is much higher than traditional treatment methods.
[0037] Example 1
[0038] Step 1, pretreatment of water sludge from waterworks: dry the sludge in the sun and then crush it with a grinder for 50 seconds. Then use a sieve to screen the sludge powder. The sludge sieve has a mesh size of 70 to obtain sludge powder with uniform particle size. The inorganic powder particle size is 212μm. The sludge powder is then fired in a muffle furnace at 900°C to obtain quartz phase SiO2 crystal powder. The powder crystals are ground in an omnidirectional ball mill to obtain crystalline powder with uniform particle size as the raw material for preparing ceramic membranes. The grain size is 30.31nm and the inorganic powder particle size is 90μm. Place in an oven for drying;
[0039] Step 2, prepare a ceramic membrane suspension of a specified proportion, which is composed of 44% dimethylformamide, 0.8% sodium carboxymethyl cellulose, 5.5% polyethersulfone, 0.8% polyacrylic acid and 48.9% inorganic powder by mass percentage, and the total mass percentage of each component is 100%. Add NMP solvent, PVP powder, sludge crystal powder and polyethersulfone powder to the ball mill rotor in turn, with the grinding ball size of 15mm:12mm and the ratio of 1:5; the ball mill speed is 300rpm, the suspension stirring time is 36h, and the polyethersulfone stirring time is 36h. Grind and stir to obtain a uniformly dispersed suspension, and finally use a vacuum pump for vacuum degassing, and the vacuum degassing time is 60min;
[0040] Step 3, the outer diameter of the single-hole spinneret used is 4.8 mm, the inner diameter is 2.4 mm, and the flow rates of the pure water condensate and the suspension are controlled, the suspension flow rate is 10 mL / min, and the pure water condensate flow rate is 15 mL / min. The membrane filaments are squeezed into the water tank to complete the dry-wet spinning phase transfer process and obtain a smooth surface membrane blank.
[0041] Step 4: Dry the membrane blank at room temperature, and then place it in a muffle furnace for high-temperature calcination to obtain a hollow fiber ceramic membrane substrate. The membrane blank calcination temperature is 1100°C and the calcination time is 150 min. Use anhydrous ethanol to prepare a concentration of 0.7 g mL -1 The membrane substrate was immersed in a solution of ferric chloride hexahydrate and subjected to ultrasonic treatment for 30 minutes. After drying, the membrane substrate was calcined in a muffle furnace at a temperature of 210°C. The above immersion and calcination process was repeated three times to obtain a FeOCl hollow fiber ceramic catalytic membrane.
[0042] Step 5, use hollow fiber ceramic catalytic membrane coupled ozone aeration system to remove small molecule refractory organic matter, including anti-drug, dye and endocrine disruptor, ibuprofen, methylene blue and bisphenol A, respectively, to evaluate the removal rate and TOC removal rate of the above three typical organic pollutants. The air ozone generator inlet flow rate is 100mL / min, ibuprofen removal rate is 77.6%, TOC removal rate is 40.2%. Methylene blue removal rate is 83.5%, TOC removal rate is 43.5%. Bisphenol A removal rate is 78.3%, TOC removal rate is 39.6%.
[0043] Example 2
[0044] Step 1, pretreatment of water sludge from waterworks: dry the sludge in the sun and crush it with a grinder for 70 seconds, then use a sieve to sieve the sludge powder, the sludge sieve mesh is 90 mesh, and a sludge powder with uniform particle size is obtained, and the inorganic powder particle size is 160 μm. Then the sludge powder is fired in a muffle furnace at a temperature of 1100 ° C to obtain mullite phase Al2 (Al 2.8 Si 1.2 ) 9.54 Crystal powder, use an omni-directional ball mill to grind the powder crystals to obtain a crystal powder with uniform particle size as the raw material for preparing ceramic membranes, the grain size is 34.92nm, and the inorganic powder particle size is 75μm. Put it in an oven for drying;
[0045] Step 2, prepare a ceramic membrane suspension of a specified proportion, consisting of 44% dimethylacetamide, 0.8% polyvinyl pyrrolidone, 5.5% dioctyl adipate, 0.8% polyethylene glycol and 48.9% inorganic powder, and the total mass percentage of each component is 100%. Add NMP solvent, PVP powder, sludge crystal powder and polyethersulfone powder to the ball mill rotor in turn, the grinding ball size is 15mm:12mm, and the ratio of the two grinding balls is 1:5. The ball mill speed is 300rpm, the suspension stirring time is 36h, and the polyethersulfone stirring time is 36h. Grind and stir to obtain a uniformly dispersed suspension, and finally use a vacuum pump for vacuum degassing, and the vacuum degassing time is 60min;
[0046] Step 3, the outer diameter of the single-hole spinneret used is 4.8 mm, the inner diameter is 2.4 mm, and the flow rates of the pure water condensate and the suspension are controlled, the suspension flow rate is 10 mL / min, and the pure water condensate flow rate is 15 mL / min. The membrane filaments are squeezed into the water tank to complete the dry-wet spinning phase transfer process and obtain a smooth surface membrane blank.
[0047] Step 4: Dry the membrane blank at room temperature, and then place it in a muffle furnace for high-temperature calcination to obtain a hollow fiber ceramic membrane substrate. The membrane blank calcination temperature is 1200°C and the calcination time is 180 min. Use anhydrous ethanol to prepare a concentration of 0.8 g mL -1 The membrane substrate was immersed in a solution of ferric chloride hexahydrate and subjected to ultrasonic treatment for 40 minutes. After drying, the membrane substrate was calcined in a muffle furnace at a temperature of 220°C. The above immersion and calcination process was repeated three times to obtain a FeOCl hollow fiber ceramic catalytic membrane.
[0048] Step 5, use hollow fiber ceramic catalytic membrane coupled ozone aeration system to remove small molecule refractory organic matter, including anti-drug, dye and endocrine disruptor, ibuprofen, methylene blue and bisphenol A, respectively, to evaluate the removal rate and TOC removal rate of the above three typical organic pollutants. The air ozone generator inlet flow rate is 150mL / min, ibuprofen removal rate is 96.6%, TOC removal rate is 46.7%. Methylene blue removal rate is 98.4%, TOC removal rate is 51.3%. Bisphenol A removal rate is 86.1%, TOC removal rate is 47.5%.
[0049] Example 3
[0050] Step 1: Sludge pretreatment. Dry and dehydrate the sludge to obtain a dry sludge sample. Use a pulverizer to crush the sludge for 90 seconds to obtain a relatively fine powder. Use a sieve to sieve the dried sludge. The sludge sieve has a mesh size of 120 to obtain a sludge powder with uniform powder particles. The powder particle size is 120 μm. The sludge powder is calcined in a muffle furnace at a calcination temperature of 1300°C to obtain Al2(Al 2.8 Si1.2 ) 9.54 Mullite type crystal powder, the grain size is 35.57nm. Use a 230 mesh sieve to sieve to obtain a uniform powder with a powder particle size of 63μm. The finer powder is used as the raw material for preparing ceramic membranes and is placed in an oven for drying to remove the remaining moisture;
[0051] Step 2, prepare a ceramic membrane suspension with different component proportions, which is composed of 44% N-methylpyrrolidone, 0.8% hydroxypropyl methylcellulose, 5.5% dibutyl phthalate, 0.8% polyacrylic acid and 48.9% inorganic powder by mass percentage, and the sum of the mass percentages of the above components is 100%. Add N-methylpyrrolidone solvent and polyvinylpyrrolidone (PVP) powder to the ball mill rotor, use grinding balls of 15mm:12mm in size, the ratio of the number of two grinding balls is 1:5, use zirconium oxide grinding balls, and fully stir the grinding balls at different speeds. The ball mill speed is 300rpm to obtain a uniform and stable organic solution, add the pretreated inorganic powder and continue stirring. The suspension is stirred for 36h to obtain a uniform and stable suspension. Add polyethersulfone to the suspension and continue stirring with a ball mill for 36 hours to make the polyethersulfone evenly dispersed in the suspension. Finally, use a vacuum pump to degas the suspension for 60 minutes to eliminate bubbles.
[0052] Step 3, using a single-hole spinneret with an outer diameter of 4.8 mm and an inner diameter of 2.4 mm, by controlling the flow rates of the pure water condensate and the suspension, the flow rate of the pure water condensate is 10 mL / min, and the flow rate of the suspension is 15 mL / min, the suspension is squeezed into the water tank through the single-hole spinneret to complete the phase transfer process, and after drying at room temperature, a membrane blank with uniform pore size and smooth surface is obtained.
[0053] Step 4: Dry the membrane blank at room temperature and calcine the dried membrane blank in a muffle furnace at a calcination temperature of 1300°C. The calcination time is 210 min to obtain a hollow fiber ceramic membrane substrate. The FeOCl ceramic catalytic membrane was prepared by impregnation technology combined with low-temperature calcination process. Ferric chloride hexahydrate was dissolved in anhydrous ethanol, and the concentration of ferric chloride hexahydrate was 0.9 g mL -1 The membrane substrate was immersed in the solution and then ultrasonically treated, and then stirred for 50 minutes. The membrane substrate after drying was calcined at different temperatures in a muffle furnace, and the calcination temperature was 230°C. The FeOCl catalyst coating cycle was repeated 5 times, and after naturally cooling to room temperature, it was washed with deionized water and dried to obtain a hollow fiber ceramic catalytic membrane.
[0054] Step 5, using a hollow fiber ceramic catalytic membrane coupled to an ozone aeration system to evaluate the removal of small molecule recalcitrant organic matter, the air ozone generator inlet flow rate is 200 mL / min, the small molecule recalcitrant organic matter removal rate is 99.2%, and the TOC removal rate is 62.7%.
[0055] Example 4
[0056] Step 1: Sludge pretreatment. Dry and dehydrate the sludge to obtain a dry sludge sample. Use a pulverizer to crush the sludge for 120 seconds to obtain a relatively fine powder. Use a sieve to sieve the dried sludge. The sludge sieve has a mesh size of 150 to obtain a sludge powder with uniform powder particles. The powder particle size is 106 μm. The sludge powder is calcined in a muffle furnace at a calcination temperature of 1500°C to obtain Al2(Al 2.8 Si 1.2 ) 9.6 Mullite type crystal powder, the grain size is 36.16nm. Use a 270 mesh sieve to sieve to obtain a uniform powder with a powder particle size of 53μm. The finer powder is used as the raw material for preparing ceramic membranes and is placed in an oven for drying to remove the remaining moisture;
[0057] Step 2, prepare a ceramic membrane suspension with different component proportions, which is composed of 44% dimethylformamide, 0.8% hydroxypropyl methylcellulose, 5.5% dioctyl adipate, 0.8% polyethylene glycol and 48.9% inorganic powder by mass percentage, and the sum of the mass percentages of the above components is 100%. Add N-methylpyrrolidone solvent and polyvinylpyrrolidone (PVP) powder to the ball mill rotor, use grinding balls of 15mm:12mm in size, the ratio of the two grinding balls is 1:5, use zirconium oxide grinding balls, and fully stir the grinding balls at different speeds. The ball mill speed is 300rpm to obtain a uniform and stable organic solution, add the pretreated inorganic powder and continue stirring. The suspension is stirred for 36h to obtain a uniform and stable suspension. Add polyethersulfone to the suspension and continue stirring with a ball mill for 36 hours to make the polyethersulfone evenly dispersed in the suspension. Finally, use a vacuum pump to degas the suspension for 60 minutes to eliminate bubbles.
[0058] Step 3, using a single-hole spinneret with an outer diameter of 4.8 mm and an inner diameter of 2.4 mm, by controlling the flow rates of the pure water condensate and the suspension, the flow rate of the pure water condensate is 10 mL / min, and the flow rate of the suspension is 15 mL / min, the suspension is squeezed into the water tank through the single-hole spinneret to complete the phase transfer process, and after drying at room temperature, a membrane blank with uniform pore size and smooth surface is obtained.
[0059] Step 4, drying the membrane blank at room temperature, calcining the dried membrane blank in a muffle furnace at a calcination temperature of 1400°C and a calcination time of 240 min to obtain a hollow fiber ceramic membrane substrate. The FeOCl ceramic catalytic membrane was prepared by impregnation technology combined with a low-temperature calcination process. Ferric chloride hexahydrate was dissolved in anhydrous ethanol, and the concentration of ferric chloride hexahydrate was 1.0 g mL -1 The membrane substrate was immersed in the solution and then ultrasonically treated, and then stirred for 60 minutes. The membrane substrate after drying was calcined at different temperatures in a muffle furnace, and the calcination temperature was 240°C. The FeOCl catalyst coating cycle was repeated 5 times, and after naturally cooling to room temperature, it was washed with deionized water and dried to obtain a hollow fiber ceramic catalytic membrane.
[0060] Step 5, using a hollow fiber ceramic catalytic membrane coupled to an ozone aeration system to evaluate the removal of small molecule recalcitrant organic matter, the air ozone generator inlet flow rate is 250 mL / min, the small molecule recalcitrant organic matter removal rate is 97.6%, and the TOC removal rate is 59.4%.
[0061] Figure 1 (a) shows the crystal form changes of sludge powder at different temperatures, and (b) shows the crystal form changes of ceramic membrane substrate at different temperatures. Figure 1 (a) It can be seen that after the sludge powder is fired in the muffle furnace, two types of crystal powders are obtained, namely, quartz crystal powders at 600 and 900 ° C, and mullite crystal powders at 1100-1500 ° C. As the calcination temperature increases, the grain size gradually increases. The grain size of the quartz crystal is 28.92nm at 600 ° C and 30.31 at 900 ° C, and the mullite grain size ranges from 34.92 to 36.16nm at 1100-1500 ° C. The crystal powders calcined at different temperatures above are used as raw materials for preparing hollow fiber ceramic membranes. Figure 1 (b) shows that as the calcination temperature continues to increase, the crystal form of the ceramic membrane substrate at 1100-1400℃ is all mullite-type crystal powder.
[0062] Depend on Figure 2 (a1) It can be seen that the hollow fiber ceramic membrane substrate prepared at a calcination temperature of 1300°C is dark yellow and the membrane surface is smooth and flat. Figure 2 (a2) It can be seen that the calcined grains on the surface of the hollow fiber ceramic membrane substrate are evenly dispersed, forming a relatively dense network structure, which provides a good loading platform for FeOCl nanocatalysts. After three impregnation and calcination at 220°C, Figure 2 (b1) shows that the hollow fiber ceramic catalytic membrane is reddish brown, which is consistent with the typical characteristics of FeOCl nanocatalysts. Scanning electron microscopy observation Figure 2(b2) It can be seen that the FeOCl nanocatalyst presents a petal layer structure. The larger membrane specific surface area of this structural morphology can increase the active sites of the FeOCl nanocatalyst. Figure 2 (c) is the cross-sectional morphology of the hollow fiber ceramic catalytic membrane. Most of the membrane cross-section is a dense layer structure. The active free radical species generated produce a significant nano-confined catalytic effect during the catalytic degradation process, thereby enhancing the catalytic efficiency of the catalytic membrane-coupled ozone oxidation system.
[0063] The above contents are only for explaining the technical idea of the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.
Claims
1. A method for preparing a hollow fiber ceramic catalytic membrane, characterized in that: The following steps are involved: Preparation of sludge crystal powder using water supply sludge from waterworks; A ceramic membrane suspension is prepared according to a set ratio, wherein the ceramic membrane suspension includes an organic solvent, a plasticizer, a dispersant and sludge crystal powder, and the organic solvent, the pore-forming agent, the sludge crystal powder and the plasticizer are successively added, ground and stirred to obtain a uniformly dispersed suspension, and the suspension is subjected to vacuum degassing treatment; The dry-wet spinning phase transfer method is adopted to squeeze the membrane fibers into the water tank by controlling the flow rate of the pure water condensate and suspension, completing the dry-wet spinning phase transfer and obtaining a smooth surface membrane blank. The membrane blank is dried at room temperature and then calcined at high temperature to obtain a hollow fiber ceramic membrane substrate. Anhydrous ethanol is used to prepare a ferric chloride hexahydrate solution, the hollow fiber ceramic membrane substrate is immersed in the solution and ultrasonically treated, and then dried and calcined. The above immersion and calcination process is repeated in a cycle to obtain a FeOCl hollow fiber ceramic catalytic membrane.
2. The method for preparing a hollow fiber ceramic catalytic membrane according to claim 1, characterized in that: The water supply sludge from the waterworks is dried in the sun and then crushed with a grinder. The sludge powder is sieved with a sieve to obtain sludge powder with uniform particle size and calcined to obtain crystalline powder. The crystalline powder is ground in an omnidirectional ball mill to obtain crystalline powder with uniform particle size as the raw material for preparing ceramic membranes, which is then put into an oven for drying.
3. The method for preparing a hollow fiber ceramic catalytic membrane according to claim 2, characterized in that: The crushing time of the crusher is 50 to 120 seconds, the mesh number of the sludge screen is 70 to 150 meshes, the particle size of the inorganic powder is 106 to 212 μm, and the sludge powder is sintered in a muffle furnace at a temperature of 900 to 1500°C to obtain quartz and mullite crystal powders with a grain size of 30.31 to 36.16 nm, and the particle size of the inorganic powder is 53 to 90 μm.
4. The method for preparing a hollow fiber ceramic catalytic membrane according to claim 1, characterized in that: The ceramic membrane suspension includes 44% of organic solvent, 0.8% of binder, 5.5% of plasticizer, 0.8% of dispersant and 48.9% of inorganic powder in mass percentage. The diameter of the grinding ball is 15mm:12mm, the number ratio of the two grinding balls is 1:5, the ball mill speed is 300rpm, the suspension stirring time is 36h, the plasticizer stirring time is 36h, and the vacuum degassing time is 60min. The organic solvent is dimethylformamide, dimethylacetamide or N-methylpyrrolidone; the binder is polyvinylpyrrolidone, sodium carboxymethylcellulose or hydroxypropyl methylcellulose, the plasticizer is dibutyl phthalate, dioctyl adipate or polyether sulfone; the dispersant is polyacrylic acid or polyethylene glycol.
5. The method for preparing a hollow fiber ceramic catalytic membrane according to claim 1, characterized in that: The outer diameter of the spinneret used in the dry-wet spinning phase transfer is 2 to 4.8 mm, the inner diameter is 1 to 2.4 mm, the suspension flow rate is 10 to 15 mL / min, and the inner condensate flow rate is 10 to 20 mL / min.
6. The method for preparing a hollow fiber ceramic catalytic membrane according to claim 1, characterized in that: The calcination temperature of the membrane body is 1100-1400°C, and the calcination time is 150-240 minutes.
7. The method for preparing a hollow fiber ceramic catalytic membrane according to claim 1, characterized in that: The concentration of ferric chloride hexahydrate is 0.7~1.0gmL -1 , ultrasonic treatment for 30-60 min, calcination temperature 210-240 ° C, FeOCl catalyst coating cycle repeated 3-5 times.
8. A hollow fiber ceramic catalytic membrane, characterized in that: The hollow fiber ceramic catalytic membrane is obtained by using the preparation method of any one of claims 1 to 8.
9. The use of the hollow fiber ceramic catalytic membrane as claimed in claim 8, characterized in that: FeOCl hollow fiber ceramic catalytic membrane coupled with ozone aeration system is used to remove small molecule refractory organic matter, including drug resistance, dyes and endocrine disruptors.
10. The use of the hollow fiber ceramic catalytic membrane according to claim 9, characterized in that: The air ozone generator inlet flow rate of the ozone aeration system is 100-250 mL / min, the ibuprofen removal rate is 77.6-99.5%, and the TOC removal rate is 40.2-55.6%; the methylene blue removal rate is 83.5-99.2%, and the TOC removal rate is 43.5-62.7%; the bisphenol A removal rate is 78.3-98.5%, and the TOC removal rate is 39.6-66.4%.
Citation Information
Cited By
Hollow fibers in incinerated ash and their manufacturing method
JP2026120066A
Hollow fibers in incinerated ash and their manufacturing method
JP7929536B2