Core nozzle with gradient structure for thin-strip continuous casting
By forming a gradient structure in the core water outlet and using silicon carbide and spinel-graphite layers, the existing core water outlet oxidation and pore problems at high temperatures are solved, the thermal conductivity and thermal shock resistance are improved, and the surface quality of the steel belt is improved .
Patent Information
- Application Number
- CN202411068900.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-22
AI Technical Summary
The existing core water outlet oxidizes and residual air in the pores at high temperatures, resulting in the formation of tiny bubbles, affecting the surface quality of the steel strip, and reducing the graphite content puts higher requirements against thermal shock.
The core water outlet with a gradient structure is adopted, the surface is a silicon carbide-based oxide layer, the intermediate transition layer is a silicon-based oxide-graphite layer, and the interior is a dense carbon-bound oxide-graphite layer, which is passed through cold isostatic molding and vacuum sintering. The furnace heat treatment is formed, and a dense silicon carbide and spinel-graphite layer is formed by osmotic reaction of metal silicon particles to reduce pore formation.
The thermal conductivity and thermal shock resistance of the core water outlet are improved, fracture failure caused by thermal stress is avoided, and graphite oxidation is prevented and air in the pores is isolated, improving the surface quality of the steel strip.
Smart Images

Figure BDA0004980231370000051 
Figure BDA0004980231370000061 
Figure BDA0004980231370000062
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of refractory materials, and relates to a core nozzle for thin strip continuous casting, and more specifically to a core nozzle with a gradient structure for thin strip continuous casting. Background Art
[0002] The steel industry has high energy consumption and carbon dioxide emissions. Exploring simple and efficient manufacturing processes is an important technical path to achieve green manufacturing and ecological development in the steel industry, and it is also an important technical route for green manufacturing and ecological development in the steel industry. At the same time, it is also the innovative development direction of the steel industry. Near-net-shape manufacturing refers to a manufacturing technology in which the size and shape of the product are closer to the final use requirements. Compared with traditional manufacturing technology, its manufacturing process is simpler and more efficient, and the energy-saving and emission-reduction effects are significant. It is a typical green manufacturing technology.
[0003] The near-net-shape manufacturing technology in the field of metallurgical process manufacturing mainly includes thin slab continuous casting and rolling and thin strip casting and rolling. Compared with thin slab continuous casting and rolling, thin strip continuous casting and rolling is a more compact hot-rolled strip steel production process. Its characteristics are that the liquid metal undergoes pressure processing and plastic deformation while crystallizing and solidifying, completing the whole process from liquid to solid thin strip in a very short time.
[0004] The uniform distribution of molten steel in the molten pool is the core key technology of thin strip continuous casting and rolling. It must be evenly distributed in the width direction of the crystallization roller and ensure the stability of the meniscus of the molten pool. The existing industrial process adopts a three-level molten steel distribution system, namely the tundish, the primary transition ladle, and the core nozzle to distribute the molten steel to the thin strip continuous casting crystallization roller. The tundish and the primary transition ladle play the role of the ladle and the tundish in the traditional continuous casting process, and maintain a stable molten steel level in the crystallizer through reasonable structure and flow control operation.
[0005] In the continuous casting and rolling of thin strips, the working layers of the tundish and primary transition ladle are made of existing mature and stable magnesium dry materials or coating materials, which can meet the erosion and scouring of high-temperature molten steel. The core nozzle plays the role of the submerged nozzle in the existing traditional continuous casting process to distribute the molten steel in the crystallizer for the second time, maintaining a reasonable and stable flow field in the crystallizer.
[0006] The core nozzle is made of alumina-graphite composite material used in traditional continuous casting. Alumina-graphite composite has excellent thermal shock resistance and resistance to molten steel erosion, but it has a high apparent porosity. During service, due to the oxidation of graphite materials and the air remaining in the pores, tiny bubbles are formed in the molten pool. However, if the tiny bubbles cannot float up in time, they will be discharged into the thin steel strip to form micro defects, thus seriously affecting the surface quality of the steel strip. On the other hand, reducing the graphite content puts higher requirements on the thermal shock resistance of the core nozzle. Summary of the invention
[0007] Therefore, the object of the present invention is to provide a core nozzle with a gradient structure, wherein the surface of the core nozzle is a silicon carbide-based oxide layer, the intermediate transition layer is a silicon-based oxide-graphite layer, and the interior is a carbon-bonded oxide-graphite layer. Alternatively, the core nozzle sequentially forms a dense silicon carbide layer, a dense metal silicon-bonded spinel-graphite layer, and a spinel-graphite layer from the surface to the interior, and finally forms a core nozzle with such a gradient structure.
[0008] The present invention specifically adopts the following technical solutions:
[0009] First, a resin-bonded core nozzle green body is prepared by cold isostatic pressing process, and the ingredient scheme (wt%) in Table 1 is used to achieve the above purpose. In the scheme in Table 1, the spinel is sintered magnesia-iron spinel or sintered ferroaluminum spinel, the critical particle size of the spinel is ≤1mm, the graphite is large flake graphite (>0.3mm) and ultrafine graphite (<0.02mm); the additive is magnesite and ferrous oxide, or ferrous oxide and aluminum hydroxide, wherein the molar ratio of magnesite to ferrous oxide is 1:1, the molar ratio of ferrous oxide to aluminum hydroxide is 1:2, the particle size of the powder is <0.047mm, and the phenolic resin is solid phenolic resin powder and liquid phenolic resin.
[0010] The blank is granulated in a high-speed mixer, dried, formed in a cold isostatic press at 80-120 MPa, and heated and solidified to obtain a core nozzle blank.
[0011] Table 1 Core nozzle green body composition materials (wt%)
[0012] Spinel 60~77 graphite 5~9 additive 10~20 Phenolic resin 6~9 Alcohol 2~4
[0013] Then, the core nozzle green body is placed in a sagger, and the green body is buried with metal silicon particles and heat treated in a vacuum sintering furnace. Below 1000°C, the resin gradually carbonizes and forms a carbon-bonded spinel-graphite green body. At this time, due to the carbonization of the resin, more organic volatiles in the green body leave channels, and magnesite and aluminum hydroxide will also decompose to release CO2 and H2O respectively, so there are more open pores inside the core nozzle green body.
[0014] When the temperature rises to 1500-1650℃, liquid silicon with suitable viscosity formed under the metal silicon particles penetrates into the interior of the blank through the open pores of the core nozzle blank. As the metal silicon penetrates into the spinel-graphite blank, the metal silicon continuously reacts with the resin carbon and graphite. Due to the size effect, a dense silicon carbide layer is formed from the surface to the inside, and the dense metal silicon is combined with the spinel-graphite layer, and the inside is the spinel-graphite layer. With the formation of the dense silicon carbide layer on the surface, the penetration reaction ends, and finally the core nozzle of this gradient structure is formed.
[0015] During the heat treatment process, the core nozzle green body will react:
[0016] MgCO3→MgO+CO2,
[0017] 2Al(OH)3→Al2O3+3H2O.
[0018] Moreover, the above reaction forms a large number of open pores, which serve as diffusion channels for liquid metal silicon to diffuse into the spinel-graphite material.
[0019] Liquid silicon reacts with graphite or resin carbon in the core nozzle:
[0020] Si(l)+C→SiC.
[0021] In the early stage, reaction and diffusion proceed simultaneously. Once the surface dense layer is formed, the metal silicon stops diffusing into the interior. At this time, the temperature is stopped, so the metal silicon in the transition layer has not fully reacted with the graphite to form a metal silicon-bonded spinel-graphite material, and the metal silicon has not yet penetrated into the interior. The main reactions are:
[0022] MgO+Fe2O3→MgAl2O4,
[0023] FeO+Al2O3→FeAl2O4.
[0024] In particular, under a vacuum atmosphere, the above reaction forms a ceramic bond, which can enhance the bonding strength of the inner layer of the core nozzle and is beneficial to the overall mechanical properties of the product.
[0025] More specifically, according to the first aspect of the present invention, a core nozzle with a gradient structure for thin strip continuous casting is proposed, and the green body of the core nozzle adopts the following ingredients in wt%: spinel: 60%~77%; graphite: 5%~9%; additives: 10%~20%; phenolic resin: 6%~9%; alcohol: 2%~4%, wherein: the spinel is sintered magnesia-iron spinel or sintered ferroaluminum spinel, and the critical particle size of the spinel is ≤1mm; the graphite is a mixture of large flake graphite and ultrafine graphite, wherein the particle size of the large flake graphite is greater than 0.3mm, and the particle size of the ultrafine graphite is less than 0.02mm; the additive is a mixture of dolomite and ferrous oxide, or the additive is a mixture of ferrous oxide and aluminum hydroxide; the phenolic resin is a mixture of solid phenolic resin powder and liquid phenolic resin.
[0026] According to the core nozzle with a gradient structure for thin strip continuous casting of the present invention, preferably, when the additive is a mixture of magnesite and ferric oxide, the molar ratio of the magnesite to the ferric oxide is 1:1.
[0027] According to the core nozzle with a gradient structure for thin strip continuous casting of the present invention, preferably, when the additive is a mixture of ferrous oxide and aluminum hydroxide, the molar ratio of the ferrous oxide to the aluminum hydroxide is 1:2.
[0028] According to the core nozzle with a gradient structure for thin strip continuous casting of the present invention, preferably, the powder particle size of the green body of the core nozzle is less than 0.047 mm.
[0029] According to the core nozzle with gradient structure for thin strip continuous casting of the present invention, preferably, the gradient structure of the core nozzle is sequentially formed from the surface to the inside: a dense silicon carbide layer; a dense metallic silicon combined spinel-graphite layer; a spinel-graphite layer.
[0030] According to a second aspect of the present invention, a method for producing a core nozzle having the aforementioned characteristics is proposed, the method comprising the following steps: granulating the raw material blank in a high-speed mixer; after drying, forming in a cold isostatic press, and heating and curing to obtain the green body of the core nozzle; placing the green body of the core nozzle in a sagger, and burying the green body with metallic silicon granules for heat treatment in a vacuum sintering furnace.
[0031] According to the method for producing a core nozzle with a gradient structure of the present invention, preferably, the drying step is carried out at 60°C.
[0032] According to the method for producing a core nozzle with a gradient structure of the present invention, preferably, the molding pressure in the cold isostatic press is controlled to be 80-120 MPa.
[0033] According to the method for producing a core nozzle with a gradient structure of the present invention, preferably, the heat treatment holding temperature is controlled to be 1500-1650°C.
[0034] According to the method for producing a core nozzle with a gradient structure of the present invention, preferably, the vacuum degree of the heat treatment is controlled to be less than 1Pa.
[0035] Beneficial technical effects
[0036] Compared with the prior art, the technical concept and corresponding technical solution of the present invention can at least achieve the following beneficial technical effects:
[0037] The surface layer and transition layer materials of the core nozzle of the present invention have high thermal conductivity. During the preheating stage of the core nozzle and the pouring process of thin strip continuous casting, a smaller temperature gradient can be quickly achieved inside and outside the material, avoiding severe thermal shock to the material caused by excessive thermal stress, thereby avoiding the problem of fracture failure of the core nozzle.
[0038] At the same time, the transition layer metal silicon of the present invention has a certain toughness under hot conditions, which can offset the thermal expansion of alumina and graphite materials, and further optimize the thermal shock resistance of the core nozzle.
[0039] In addition, the intermediate transition layer of the core nozzle of the present invention can continuously react in situ to produce a dense carbide layer during heat treatment and service. The dense carbide layer can prevent the oxidation of the graphite material on the one hand, and on the other hand, it can isolate the contact between the air in the pores of the inner layer of alumina-graphite material and the molten steel, thereby avoiding the generation of tiny bubbles in the molten pool. DETAILED DESCRIPTION
[0040] In order to make the purpose, technical solution and advantages of the embodiment of the present invention clearer, the technical solution of the embodiment of the present invention will be clearly and completely described below. Obviously, the described embodiment is a part of the embodiment of the present invention, not all of the embodiments. Based on the described embodiment of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0041] Unless otherwise defined, technical or scientific terms used in the present invention shall have the common meanings understood by one of ordinary skill in the art to which the present invention belongs.
[0042] The following are embodiments of the present invention. The described embodiments are only a part of the embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments that can be obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0043] The technical solution of the present invention is further described below through specific embodiments 1 to 3:
[0044] Example 1
[0045] The core nozzle green body was prepared according to Table 2. The mixed oil was granulated by a high-speed granulator to obtain the green body, which was dried at 60°C, formed at 80 MPa in a cold isostatic press, and treated at 180°C in a curing furnace to obtain the core nozzle green body.
[0046] Table 2 Core nozzle green body composition materials
[0047]
[0048]
[0049] Then, the core nozzle green body is placed in a sagger, and the green body is buried with metal silicon particles and heat treated in a vacuum sintering furnace with a vacuum degree of <1Pa. The treatment system is shown in Table 3, and finally a core nozzle with a gradient structure is formed.
[0050] Table 3 Firing system
[0051] temperature Heating curve Room temperature~1000℃ 5℃ / min 1000~1400℃ 3℃ / min 1400~1550℃ 1℃ / min 1550℃ Keep warm for 200 minutes
[0052] Example 2
[0053] The core nozzle green body was prepared according to Table 4. The mixed oil was granulated by a high-speed granulator to obtain the green body, which was dried at 60°C, formed at 100 MPa in a cold isostatic press, and treated at 180°C in a curing furnace to obtain the core nozzle green body.
[0054] Table 4 Core nozzle green body composition materials
[0055]
[0056] Then, the core nozzle green body is placed in a sagger, and the green body is buried with metal silicon particles and heat treated in a vacuum sintering furnace with a vacuum degree of <1Pa. The treatment system is shown in Table 5, and finally a core nozzle with a gradient structure is formed.
[0057] Table 5 Firing system
[0058] temperature Heating curve Room temperature~1000℃ 5℃ / min 1000~1400℃ 3℃ / min 1400~1550℃ 1℃ / min 1650℃ Keep warm for 120 minutes
[0059] Example 3
[0060] The core nozzle green body was prepared according to Table 6. The mixed oil was granulated by a high-speed granulator to obtain the green body, which was dried at 60°C, formed at 120 MPa in a cold isostatic press, and treated at 180°C in a curing furnace to obtain the core nozzle green body.
[0061] Table 6 Core nozzle green body composition materials
[0062]
[0063] Then, the core nozzle green body is placed in a sagger, and the green body is buried with metal silicon particles and heat treated in a vacuum sintering furnace with a vacuum degree of <1Pa. The treatment system is shown in Table 7, and finally a core nozzle with a gradient structure is formed.
[0064] Table 7 Firing system
[0065] temperature Heating curve Room temperature~1000℃ 5℃ / min 1000~1400℃ 3℃ / min 1400~1550℃ 1℃ / min 1500℃ Keep warm for 300 minutes
[0066] The above description is only a specific implementation of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A core nozzle with a gradient structure for thin strip continuous casting, characterized in that: The green body of the core nozzle adopts the following ingredients in wt%: Spinel: 60% to 77%; Graphite: 5% to 9%; Additives: 10% to 20%; Phenolic resin: 6% to 9%; Alcohol: 2% to 4%, in: The spinel is sintered magnesia-iron spinel or sintered ferroalumina spinel, and the critical particle size of the spinel is ≤1 mm; The graphite is a mixture of large flake graphite and ultrafine graphite, wherein the particle size of the large flake graphite is greater than 0.3 mm, and the particle size of the ultrafine graphite is less than 0.02 mm; The additive is a mixture of magnesite and ferric oxide, or the additive is a mixture of ferrous oxide and aluminum hydroxide; The phenolic resin is a mixture of solid phenolic resin powder and liquid phenolic resin.
2. The core nozzle with gradient structure for thin strip continuous casting according to claim 1, characterized in that: When the additive is a mixture of magnesite and ferric oxide, the molar ratio of the magnesite to the ferric oxide is 1:
1.
3. The core nozzle with gradient structure for thin strip continuous casting according to claim 1, characterized in that: When the additive is a mixture of ferrous oxide and aluminum hydroxide, the molar ratio of the ferrous oxide to the aluminum hydroxide is 1:
2.
4. The core nozzle with gradient structure for thin strip continuous casting according to claim 1, characterized in that: The powder particle size of the green body of the core nozzle is less than 0.047 mm.
5. The core nozzle with gradient structure for thin strip continuous casting according to any one of claims 1 to 4, characterized in that: The gradient structure of the core nozzle is formed in sequence from the surface to the inside: Dense silicon carbide layer; Dense metallic silicon combined with spinel-graphite layers; Spinel-graphite layers.
6. A method for producing a core nozzle according to any one of claims 1 to 5, characterized in that: The method comprises the following steps: The raw material blank is granulated in a high-speed mixer; After drying, forming in a cold isostatic press, and performing a heating and curing treatment to obtain a green body of the core nozzle; The green body of the core nozzle is placed in a sagger, and the green body is buried with metal silicon particles to perform heat treatment in a vacuum sintering furnace.
7. The method according to claim 6, characterized in that: The drying step is carried out at 60°C.
8. The method according to claim 6, characterized in that: The molding pressure in the cold isostatic press is controlled to be 80-120 MPa.
9. The method according to claim 6, characterized in that: The heat treatment is carried out at a holding temperature of 1500-1650°C.
10. The method according to claim 9, characterized in that: The vacuum degree of the heat treatment is controlled to be less than 1Pa.
Citation Information
Cited By
Magnesium aluminate spinel cover plate with compact surface and porous interior for aluminum electrolysis as well as preparation method and application of magnesium aluminate spinel cover plate
CN121850697A