Preparation method of hard alloy and titanium alloy cylindrical laminated structural member

Through the thermal isostatic pressure manufacturing method, the problem of insufficient radial pressure in the manufacture of cemented carbide and titanium alloy cylindrical laminated structural parts is solved, and the good diffusion connection and wear resistance of the material is achieved, the manufacturing process is simplified, and the manufacturing process is avoided. Residual stress.

CN118989333APending Publication Date: 2024-11-22NORTHWESTERN POLYTECHNICAL UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411227947.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The prior art In the manufacturing process of cemented carbide and titanium alloy cylindrical laminated structural parts, the radial pressure is insufficient, resulting in diffusion connection difficulty and residual stress, which affects the wear resistance and ablation resistance of the material.

Method used

Using thermal isostatic pressure manufacturing method, the cemented carbide cylinder and titanium alloy powder are fixed by designing a cover structure, and the step-by-step heating and cooling pressure is applied by using a thermal isostatic pressurization furnace to achieve densification of titanium alloy powder and cemented carbide and titanium The diffusion connection of the alloy avoids residual stress caused by mechanical forces.

Benefits of technology

The good diffusion connection between cemented carbide and titanium alloy is achieved, ensuring the material's wear resistance and ablation resistance, avoiding residual stress caused by mechanical forces, and simplifying the manufacturing process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118989333A_ABST
    Figure CN118989333A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a hard alloy and titanium alloy cylindrical laminated structural member. The method comprises the following steps: preparing titanium alloy powder and a hard alloy cylinder; the sheath comprises an inner sheath, an outer sheath, an upper end cover and a lower end cover, the hard alloy cylinder is connected to the outer side of the inner sheath in a sleeving mode, and an inner cavity used for containing titanium alloy powder is formed between the outer sheath and the hard alloy cylinder; the upper end cover and the lower end cover respectively cover the upper and lower ends of the sheath, so that a sealed space is formed in the sheath; the hard alloy cylindrical part and the sheath are assembled, and a combined part is obtained; filling titanium alloy powder into the assembly, vibrating, vacuumizing and degassing; and the assembly filled with the titanium alloy powder is placed in a hot isostatic pressing furnace to be subjected to hot isostatic pressing treatment. The invention provides a titanium alloy powder and hard alloy cylinder hot isostatic pressing process, and the densification of the titanium alloy powder and the good diffusion connection of the hard alloy and the titanium alloy can be ensured at the same time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of dissimilar metal structure manufacturing, and in particular relates to a method for preparing a cemented carbide and titanium alloy cylindrical laminated structure. Background Art

[0002] At present, the materials used for artillery barrels at home and abroad are mainly PCrNi3MoV and 32CrNi3MoVE steels, which have poor wear resistance and ablation resistance, causing the artillery barrel to fail due to micro-deformation, ablation, spalling and severe wear. In order to meet the requirements of modern warfare, the current artillery barrel materials are developing in the direction of lightweight to obtain higher mobility while ensuring wear resistance and ablation resistance. Cemented carbide has high hardness, high wear resistance and good ablation resistance, and titanium alloy has excellent properties such as high specific strength, corrosion resistance and non-magnetic. Using cemented carbide as the inner lining of the barrel and titanium alloy as the outer lining of the barrel to obtain a cylindrical laminated structure barrel is expected to increase the life of the barrel and achieve lightweight artillery.

[0003] There are many methods for joining dissimilar metals between titanium alloy and cemented carbide, such as laser welding, arc welding, brazing, vacuum diffusion welding, etc. The heating and cooling speeds of laser welding, arc welding and brazing are too fast, which can easily generate large residual stress in the weld area and cause cracks inside the cemented carbide. Vacuum diffusion welding can adjust the joint composition by adding an intermediate layer to reduce the hazards of joint brittle phase and residual stress, but for diffusion joints with cylindrical structures, due to the special structure, it is difficult to generate sufficient diffusion bonding pressure on the diffusion bonding interface, which increases the difficulty of diffusion bonding.

[0004] At present, there is no report on the diffusion bonding technology of cemented carbide and titanium alloy cylindrical laminated structures. Therefore, the present invention proposes a method for hot isostatic pressing to manufacture cemented carbide and titanium alloy cylindrical laminated structures, so that the two metals can exert their respective advantages. Summary of the invention

[0005] In order to solve the problem of insufficient radial pressure during the manufacturing process of cemented carbide and titanium alloy cylindrical laminated structural parts, the present invention proposes a method for preparing cemented carbide and titanium alloy cylindrical laminated structural parts.

[0006] The specific technical solutions of the present invention are as follows: The present invention provides a method for preparing a cylindrical laminated structure of cemented carbide and titanium alloy, comprising the following steps: Step 1: Material preparation: making titanium alloy powder and cemented carbide cylinder; Step 2: Making a sheath: The sheath comprises an inner sheath, an outer sheath, an upper end cover and a lower end cover, the carbide tube is sleeved on the outer side of the inner sheath, and an inner cavity for containing the titanium alloy powder is formed between the outer sheath and the carbide tube; the upper end cover and the lower end cover respectively cover the upper and lower ends of the sheath, so that a sealed space is formed in the sheath; Step 3: Assemble the carbide cylindrical part and the sleeve to obtain an assembly; Step 4: Fill the assembly with titanium alloy powder, vibrate, evacuate, and degas; Step 5: placing the assembly filled with titanium alloy powder in a hot isostatic pressing furnace for hot isostatic pressing; Step 6: Remove the sheath component from the hot isostatically pressed assembly to obtain a cemented carbide and titanium alloy cylindrical laminated structure.

[0007] As a further illustration of the present invention, in step 1, the particle size distribution of the titanium alloy powder produced is 75-250 μm, and the tap density is 63%-67%; the inner diameter of the cemented carbide cylindrical part is 35 mm-40 mm, and the outer diameter is 43 mm-48 mm.

[0008] As a further explanation of the present invention, the inner sleeve includes two parts, a cylindrical core and a base. The base is concentric with the cylindrical core and formed integrally. A first annular groove is provided on the base. The first annular groove is located at the outer edge of the lower end of the cylindrical core. The inner diameter of the first annular groove is clearance-matched with the outer diameter of the cemented carbide tube to achieve positioning of the lower end of the cemented carbide tube.

[0009] As a further illustration of the present invention, a circular hole having a diameter the same as the outer diameter of the base is provided at the center of the lower end cover to achieve positioning of the lower end cover and the inner sleeve.

[0010] As a further explanation of the present invention, the upper end cover is provided with a powder loading port, and a second annular groove is concentrically provided at the center of the bottom surface of the upper end cover, and the inner diameter of the second annular groove is clearance-matched with the outer diameter of the cemented carbide tube to achieve positioning of the upper end of the cemented carbide tube.

[0011] As a further explanation of the present invention, steps are provided at both upper and lower ends of the outer sleeve so that the upper end cover and the lower end cover can be effectively fixed during assembly, and the outer sleeve has a clearance fit with both the upper end cover and the lower end cover.

[0012] As a further illustration of the present invention, before assembling the cemented carbide cylindrical member and the sleeve, the method further comprises: The outer surface of the obtained hard alloy cylinder is pickled, immersed in anhydrous ethanol for ultrasonic cleaning, and stored in anhydrous ethanol; the surface of the sheath component is cleaned and degreased, and a solder stopper is applied.

[0013] As a further illustration of the present invention, step 4 specifically includes: Use a funnel to load titanium alloy powder into the processed assembly, vibrate while loading the powder, and after loading, use a vacuum pump to evacuate the bag to less than 10 -2 Pa, then place the sleeve in a pit furnace and heat it to 300℃-400℃, then keep it warm and degas for 1-3h, then heat it to 600-700℃ and keep it warm and degas for 1-3h, and then use carbon dioxide gas shielded welding to seal the sleeve.

[0014] As a further illustration of the present invention, step 5 specifically includes: The assembly filled with titanium alloy powder is placed in a hot isostatic pressing furnace for hot isostatic pressing treatment; during the hot isostatic pressing process, the furnace temperature of the hot isostatic pressing furnace is raised to 890°C-970°C in a step-by-step manner, and a pressure of 100MPa-180MPa is applied to the entire furnace chamber through the pressure system of the hot isostatic pressing furnace and maintained for 2-4 hours. After the pressure holding is completed, it is cooled to room temperature with the furnace in a step-by-step manner to complete the hot isostatic pressing connection of the assembly.

[0015] As a further illustration of the present invention, the specific process of the step-by-step heating is: the furnace temperature of the hot isostatic pressing furnace is raised to 200°C-400°C and kept warm for 20min-40min; after the insulation is completed, the furnace temperature of the hot isostatic pressing furnace is raised to 500°C-650°C and kept warm for 20min-40min; then the temperature of the hot isostatic pressing furnace is raised to 890°C-970°C at a heating rate of 10°C / min; The specific process of the step cooling is: cooling to 600°C-800°C with the furnace and keeping it warm for 20min-40min; after the insulation is completed, the furnace temperature of the hot isostatic pressing furnace is cooled to 400°C-600°C with the furnace and kept warm for 20min-40min; after the insulation is completed, the furnace temperature of the hot isostatic pressing furnace is cooled to room temperature with the furnace.

[0016] Compared with the prior art, the present invention has the following beneficial technical effects: The present invention provides a method for preparing a cylindrical laminated structure of cemented carbide and titanium alloy. By designing a sheath, the cemented carbide cylinder and the sheath can be accurately fixed, and the sheath structure is simple and economical. By using titanium alloy powder and cemented carbide cylinder for hot isostatic pressing and diffusion bonding, the densification of titanium alloy powder, diffusion bonding of cemented carbide and titanium alloy, and near-net forming of the cylindrical structure can be achieved simultaneously. A connection pressure is uniformly applied by a hot isostatic pressing furnace, thereby avoiding large residual stress inside the sample and at its connection interface caused by applying mechanical force. A hot isostatic pressing process for titanium alloy powder and cemented carbide cylinder is proposed, which can simultaneously ensure the densification of titanium alloy powder and good diffusion bonding of cemented carbide and titanium alloy.

[0017] Other features and advantages of the technical solution will be described in the subsequent description, and partly become apparent from the description, or understood by implementing the technical solution. The purpose and other advantages of the technical solution can be achieved and obtained through the structures specifically pointed out in the written description and the drawings.

[0018] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] The accompanying drawings are used to provide further understanding of the present technical solution and constitute a part of the specification. Together with the embodiments of the present technical solution, they are used to explain the present technical solution and do not constitute a limitation to the present technical solution.

[0020] Figure 1 It is a schematic diagram of the package structure provided by the present invention.

[0021] Figure 2 It is a schematic diagram of the assembly of titanium alloy powder, hard alloy and packaging provided by the present invention.

[0022] Figure 3 This is the process curve for hot isostatic pressing diffusion bonding of cemented carbide and titanium alloy provided by the present invention.

[0023] Figure 4 The invention provides a cylindrical laminated structural component of hard alloy and titanium alloy connected by hot isostatic pressing and diffusion bonding.

[0024] Figure 5 It is a microstructure diagram of the interface between the YG8 cemented carbide and TA15 titanium alloy cylindrical part provided by the present invention. DETAILED DESCRIPTION

[0025] The preferred embodiments of the present technical solution are described below in conjunction with the accompanying drawings. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present technical solution, and are not used to limit the present technical solution.

[0026] There are many methods for joining dissimilar metals between titanium alloy and cemented carbide, such as laser welding, arc welding, brazing, vacuum diffusion welding, etc. The heating and cooling speeds of laser welding, arc welding and brazing are too fast, which can easily generate large residual stress in the weld area and cause cracks inside the cemented carbide. Vacuum diffusion welding can adjust the joint composition by adding an intermediate layer to reduce the hazards of joint brittle phase and residual stress, but for diffusion joints with cylindrical structures, due to the special structure, it is difficult to generate sufficient diffusion bonding pressure on the diffusion bonding interface, which increases the difficulty of diffusion bonding.

[0027] Based on the solution of the above technical problems, the present invention provides a method for preparing a cemented carbide and titanium alloy cylindrical laminated structure, comprising the following steps: Step 1: Material preparation: Make titanium alloy powder and carbide cylinder.

[0028] Specifically, in step 1, the particle size distribution of the produced titanium alloy powder is 75-250μm, for example, it can be 75μm, 125μm, 175μm, 225μm, 250μm, etc.; the tap density is 63%-67%, for example, it can be 63%, 64%, 65%, 67%, etc.; the inner diameter of the cemented carbide cylinder is 35mm-40mm, for example, it can be 35mm, 37mm, 38mm, 40mm, etc.; the outer diameter is 43mm-48mm, for example, it can be 43mm, 45mm, 46mm, 48mm, etc.

[0029] Step 2: Make the bag: Figure 1 As shown, the sleeve includes an inner sleeve 1, an outer sleeve 2, an upper end cover 3 and a lower end cover 4. The carbide tube 6 is sleeved on the outside of the inner sleeve 1, and an inner cavity for containing titanium alloy powder 7 is formed between the outer sleeve 2 and the carbide tube 6; the upper end cover 3 and the lower end cover 4 respectively cover the upper and lower ends of the sleeve to form a sealed space in the sleeve.

[0030] Specifically, the inner sleeve 1 includes two parts, a cylindrical core 101 and a base 102. The base 102 is concentric with the cylindrical core 101 and is integrally formed. A first annular groove 103 is provided on the base 102. The first annular groove 103 is located at the outer edge of the lower end of the cylindrical core 101. The inner diameter of the first annular groove 103 is clearance-matched with the outer diameter of the cemented carbide tube 6 to achieve positioning of the lower end of the cemented carbide tube 6.

[0031] Specifically, a circular hole with a diameter the same as the outer diameter of the base 102 is provided at the center of the lower end cover 4 to achieve positioning of the lower end cover 4 and the inner sleeve 1 .

[0032] Specifically, the upper end cover 3 is provided with a powder loading port 301, on which a powder loading tube 8 is installed, and a second annular groove 302 is concentrically provided at the center of the bottom surface of the upper end cover, and the inner diameter of the second annular groove 302 is clearance-matched with the outer diameter of the cemented carbide tube 6 to achieve positioning of the upper end of the cemented carbide tube 6.

[0033] Specifically, steps are provided at both upper and lower ends of the outer sleeve 2, so that the upper end cover and the lower end cover can be effectively fixed during assembly, and the outer sleeve is clearance-matched with the upper end cover and the lower end cover.

[0034] Specifically, the material of the sheath is preferably stainless steel. According to the design requirements, the required sheath is obtained by mechanical processing.

[0035] The present invention can realize accurate fixation of the hard alloy cylinder and the sleeve by designing the sleeve assembly, and the sleeve has a simple structure and good economy.

[0036] Step 3: Assemble the carbide cylindrical part and the sleeve to obtain an assembly.

[0037] Before assembling the carbide cylinder and the sleeve, the surface treatment process of each component is also included, specifically, the following processes are included: The outer surface of the obtained hard alloy cylinder is pickled, immersed in anhydrous ethanol for ultrasonic cleaning, and stored in anhydrous ethanol; the surface of the sheath component is cleaned and degreased, and a solder stopper is applied.

[0038] like Figure 2 As shown, the above assembly process is: match the carbide tube 6 with the inner sleeve 1; match the assembly of the lower end cover 4, the carbide tube 6 and the inner sleeve, and complete welding at the lower end surface; match the obtained assembly with the upper end cover 3; match the outer sleeve 2 with the obtained assembly, and complete welding at the upper and lower end surfaces that contact each other; install the powder loading pipe 8 in the powder loading port 301 of the upper end cover 3, weld to complete fixing, and obtain the final assembly.

[0039] Step 4: Fill the assembly with titanium alloy powder, vibrate, evacuate, and degas.

[0040] Specifically, the above step 4 includes: using a funnel to load the titanium alloy powder into the processed assembly, vibrating while loading the powder, and after the loading is completed, using a vacuum pump to evacuate the package to less than 10 -2 Pa, then place the sleeve in a pit furnace and heat it to 300℃-400℃, then keep it warm and degas for 1-3h, then heat it to 600-700℃ and keep it warm and degas for 1-3h, and then use carbon dioxide gas shielded welding to seal the sleeve.

[0041] The temperature of the first thermal insulation and degassing can be, for example, 300°C, 325°C, 350°C, 375°C, 400°C, etc., and the time of the first thermal insulation and degassing can be, for example, 1h, 2h, 3h, etc.; the temperature of the second thermal insulation and degassing can be, for example, 600°C, 625°C, 650°C, 675°C, 700°C, etc., and the time of the first thermal insulation and degassing can be, for example, 1h, 2h, 3h, etc.

[0042] Step 5: placing the assembly filled with titanium alloy powder in a hot isostatic pressing furnace for hot isostatic pressing treatment.

[0043] Specifically, the above step 5 specifically includes: The assembly filled with titanium alloy powder is placed in a hot isostatic pressing furnace for hot isostatic pressing treatment; during the hot isostatic pressing process, the temperature of the hot isostatic pressing furnace is increased to 890℃-970℃ in a step-by-step manner, and a pressure of 100MPa-180MPa is applied to the entire furnace chamber through the pressure system of the hot isostatic pressing furnace and maintained for 2-4 hours. After the pressure holding is completed, it is cooled to room temperature with the furnace in a step-by-step manner to complete the hot isostatic pressing connection of the assembly.

[0044] The final heating temperature of the hot isostatic pressing furnace can be, for example, 890°C, 910°C, 930°C, 950°C, 970°C, etc., the pressure of the hot isostatic pressing furnace can be, for example, 100MPa, 120MPa, 140MPa, 160MPa, 180MPa, etc., and the pressure holding time can be, for example, 2h, 2.5h, 3h, 4h, etc.

[0045] The specific process of the above-mentioned step-by-step heating is as follows: the furnace temperature of the hot isostatic pressing furnace is raised to 200°C-400°C and kept at this temperature for 20min-40min; after the heat preservation, the furnace temperature of the hot isostatic pressing furnace is raised to 500°C-650°C and kept at this temperature for 20min-40min; then the temperature of the hot isostatic pressing furnace is raised to 890°C-970°C at a heating rate of 10°C / min; In the above-mentioned step-by-step heating process, the first-stage heating temperature of the hot isostatic pressing furnace can be, for example, 200°C, 250°C, 300°C, 350°C, 400°C, etc., and the first-stage holding time can be, for example, 20min, 25min, 30min, 35min, 40min, etc. The second-stage heating temperature can be, for example, 500°C, 550°C, 600°C, 650°C, etc., and the second-stage holding time can be, for example, 20min, 25min, 30min, 35min, 40min, etc.

[0046] The specific process of step cooling is: cooling to 600℃-800℃ with the furnace and keeping it warm for 20min-40min; after the insulation is completed, the furnace temperature of the hot isostatic pressing furnace is cooled to 400℃-600℃ with the furnace and kept warm for 20min-40min; after the insulation is completed, the furnace temperature of the hot isostatic pressing furnace is cooled to room temperature with the furnace.

[0047] In the above-mentioned step cooling process, the temperature of the first stage of furnace cooling can be, for example, 600°C, 650°C, 700°C, 750°C, 800°C, etc., and the insulation time of the first stage of furnace cooling can be, for example, 20 min, 25 min, 30 min, 35 min, 40 min, etc.; the temperature of the second stage of furnace cooling can be, for example, 400°C, 450°C, 500°C, 550°C, 600°C, etc., and the insulation time of the second stage of furnace cooling can be, for example, 20 min, 25 min, 30 min, 35 min, 40 min, etc.

[0048] Step 6: Remove the sheath component from the hot isostatically pressed assembly to obtain a cemented carbide and titanium alloy cylindrical laminated structure.

[0049] By using hot isostatic pressing and diffusion bonding of titanium alloy powder and cemented carbide cylinder, the densification of titanium alloy powder, diffusion bonding of cemented carbide and titanium alloy and near-net forming of cylindrical structure can be achieved simultaneously; a connection pressure is uniformly applied through a hot isostatic pressing furnace to avoid large residual stress inside the sample and at its connection interface caused by the application of mechanical force; a hot isostatic pressing process of titanium alloy powder and cemented carbide cylinder is proposed, which can simultaneously ensure the densification of titanium alloy powder and good diffusion bonding of cemented carbide and titanium alloy.

[0050] The present invention is described in detail below in conjunction with specific embodiments and drawings. Example 1

[0051] This embodiment is a method for preparing a cylindrical laminated structure of cemented carbide and titanium alloy by hot isostatic pressing. The specific process is: Step 1, material preparation. Material preparation includes making titanium alloy powder and cemented carbide cylindrical parts.

[0052] The titanium alloy powder is TA15 titanium alloy. The particle size distribution is 75-250μm, the average particle size D(50)=190.703μm, and the tap density is 63%-67%. The cemented carbide cylindrical parts are YG8 cemented carbide, the inner diameter is 35mm, the surface is positive tolerance, the accuracy is 0~+0.025mm, the outer diameter is 43mm, the surface is negative tolerance, the accuracy is 0~-0.016mm, the height is 110mm, the surface is symmetrical tolerance, the accuracy is ±0.1mm, and the outer surface roughness is R a =0.2μm.

[0053] Step 2: Make the cover.

[0054] The material of the sheath is stainless steel. According to the design requirements, the required sheath is obtained by mechanical processing. The sheath includes an inner sheath 1, an outer sheath 2, an upper end cover 3 and a lower end cover 4. The upper and lower ends of the outer sheath 2 are designed with steps with a height of 5 mm.

[0055] Step 3, surface treatment.

[0056] The outer surface of the obtained cemented carbide cylinder is pickled, immersed in anhydrous ethanol for ultrasonic cleaning for 20 minutes, and stored in anhydrous ethanol. At the same time, the surface of the stainless steel sheath component is cleaned and degreased, and solder stop is applied.

[0057] Step 4, assembly of the carbide cylindrical part and the sleeve.

[0058] The carbide tube 6 is matched with the inner sleeve 1; the lower end cover 4 is matched with the assembly of the carbide tube and the inner sleeve, and welding is completed at the lower end face; the obtained assembly is matched with the upper end cover 3; the outer sleeve 2 is matched with the obtained assembly, and welding is completed when the upper and lower end faces are in contact with each other; the powder loading pipe 8 is installed in the powder loading port of the upper end cover 3, and is welded to complete the fixation to obtain the final assembly.

[0059] Step 5, filling the processed package with TA15 titanium alloy powder, vibrating, vacuuming and degassing.

[0060] Use a funnel to load the TA15 alloy powder into the processed bag, vibrate while loading the powder, and then the bag will be filled. Figure 2 As shown, the package is evacuated to 10-3 Pa by a vacuum pump, and then the package is placed in a pit furnace, heated to 350°C and kept for degassing for 2 hours, and then heated to 650°C and kept for degassing for 2 hours. After completion, the package is sealed by carbon dioxide gas shielded welding.

[0061] Step 6, hot isostatic pressing diffusion bonding: The obtained assembly is placed in a hot isostatic pressing furnace for hot isostatic pressing diffusion bonding treatment.

[0062] During the hot isostatic pressing diffusion bonding treatment, the temperature of the hot isostatic pressing furnace is raised to 930°C in a step-by-step manner, and a pressure of 120MPa is applied to the entire furnace chamber through the pressure system of the hot isostatic pressing furnace and maintained for 2.5 hours. After the pressure is maintained, the furnace is cooled to room temperature in a step-by-step manner to complete the hot isostatic pressing diffusion bonding of the assembly.

[0063] The specific process of step heating is: the temperature of the hot isostatic pressing furnace is increased to 300°C and kept at this temperature for 30 minutes; after the insulation, the temperature of the hot isostatic pressing furnace is increased to 600°C and kept at this temperature for 30 minutes; the hot isostatic pressing furnace continues to increase the temperature at a rate of 10°C / min to increase the temperature of the hot isostatic pressing furnace to 930°C.

[0064] The specific process of step cooling is: cooling to 800°C with the furnace and keeping it warm for 30 minutes; after the insulation is completed, the temperature of the hot isostatic pressing furnace is cooled to 600°C with the furnace and kept warm for 20 minutes; after the insulation is completed, the temperature of the hot isostatic pressing furnace is cooled to room temperature with the furnace.

[0065] Step 7, post-processing: After the hot isostatic pressing is completed, the sheath component is removed by machining. At this point, the preparation of the YG8 cemented carbide and TA15 titanium alloy cylindrical laminated structure is completed.

[0066] The density of the titanium alloy powder in the titanium alloy and cemented carbide laminated structure formed by hot isostatic pressing is greater than 98%, and the diffusion bonding interface welding rate is greater than 99.5%. Example 2

[0067] This embodiment is a method for preparing a cylindrical laminated structure of cemented carbide and titanium alloy by hot isostatic pressing. The specific process is: Step 1, material preparation. The material preparation includes making titanium alloy powder and hard alloy cylindrical parts.

[0068] The grade of titanium alloy powder produced is TC4 titanium alloy. The particle size distribution is 50-300μm, the average particle size D(50)=200.103μm, and the tap density is 63%-67%. The grade of cemented carbide cylindrical parts produced is YG20 cemented carbide, the surface of the inner diameter 40mm is positive tolerance, the accuracy is 0~+0.025mm, the surface of the outer diameter 48mm is negative tolerance, the accuracy is 0~-0.016mm, the surface of the height 120mm is symmetrical tolerance, the accuracy is ±0.1mm, and the surface roughness of the outer surface is R a =0.2μm.

[0069] Step 2: Make the cover.

[0070] The material of the jacket is stainless steel. According to the design requirements, the required jacket is obtained by mechanical processing. The upper and lower ends of the outer jacket 2 are designed with steps of 5 mm in height.

[0071] Step 3, surface treatment.

[0072] The outer surface of the obtained cemented carbide cylinder is pickled, immersed in anhydrous ethanol for ultrasonic cleaning for 20 minutes, and stored in anhydrous ethanol. At the same time, the surface of the stainless steel sheath component is cleaned and degreased, and solder stop is applied.

[0073] Step 4, assembly of the carbide cylindrical part and the sleeve.

[0074] The carbide tube 6 is matched with the inner sleeve 1; the lower end cover 4 is matched with the assembly of the carbide tube and the inner sleeve, and welding is completed at the lower end face; the obtained assembly is matched with the upper end cover 3; the outer sleeve 2 is matched with the obtained assembly, and welding is completed when the upper and lower end faces are in contact with each other; the powder loading pipe 8 is installed in the powder loading port of the upper end cover 3, and is welded to complete the fixation to obtain the final assembly.

[0075] Step 5, filling the processed package with TC4 titanium alloy powder, vibrating, vacuuming and degassing.

[0076] Use a funnel to load the TA15 alloy powder into the processed bag, vibrate while loading the powder, and then the bag will be filled. Figure 2As shown, the package is evacuated to 10-3 Pa by a vacuum pump, and then the package is placed in a pit furnace and heated to 400°C and kept for degassing for 3 hours, and then heated to 700°C and kept for degassing for 3 hours. After completion, the package is sealed by carbon dioxide gas shielded welding.

[0077] Step 6, hot isostatic pressing diffusion bonding: The obtained assembly is placed in a hot isostatic pressing furnace for hot isostatic pressing diffusion bonding treatment. During the hot isostatic pressing diffusion bonding treatment, the furnace temperature of the hot isostatic pressing furnace is raised to 970°C in a step-by-step manner, and a pressure of 180MPa is applied to the entire furnace chamber through the pressure system of the hot isostatic pressing furnace and maintained for 4 hours. After the pressure is maintained, it is cooled to room temperature with the furnace in a step-by-step manner. The hot isostatic pressing diffusion bonding of the assembly is completed.

[0078] The specific process of step heating is: the temperature of the hot isostatic pressing furnace is raised to 400°C and kept at this temperature for 40 minutes; after the insulation, the temperature of the hot isostatic pressing furnace is raised to 650°C and kept at this temperature for 40 minutes; then the temperature of the hot isostatic pressing furnace is raised to 970°C at a heating rate of 10°C / min.

[0079] The specific process of step cooling is: cooling to 600°C with the furnace and keeping it warm for 40 minutes; after the insulation is completed, the temperature of the hot isostatic pressing furnace is cooled to 400°C with the furnace and kept warm for 40 minutes; after the insulation is completed, the temperature of the hot isostatic pressing furnace is cooled to room temperature with the furnace.

[0080] Step 7, post-processing: After the hot isostatic pressing is completed, the jacket component is removed by machining. At this point, the preparation of the YG20 cemented carbide and TC4 titanium alloy cylindrical laminated structure is completed.

[0081] Obviously, those skilled in the art can make various changes and modifications to the technical solution without departing from the spirit and scope of the technical solution. Thus, if these modifications and variations of the technical solution fall within the scope of the claims of the technical solution and their equivalents, the technical solution is also intended to include these modifications and variations.

Claims

1. A method for preparing a cylindrical laminated structure of cemented carbide and titanium alloy, It is characterized in that The steps include: Step 1: Material preparation: making titanium alloy powder and cemented carbide cylinder; Step 2: Making a sheath: The sheath comprises an inner sheath, an outer sheath, an upper end cover and a lower end cover, the carbide tube is sleeved on the outer side of the inner sheath, and an inner cavity for containing the titanium alloy powder is formed between the outer sheath and the carbide tube; the upper end cover and the lower end cover respectively cover the upper and lower ends of the sheath, so that a sealed space is formed in the sheath; Step 3: Assemble the carbide cylindrical part and the sleeve to obtain an assembly; Step 4: Fill the assembly with titanium alloy powder, vibrate, evacuate, and degas; Step 5: placing the assembly filled with titanium alloy powder in a hot isostatic pressing furnace for hot isostatic pressing; Step 6: Remove the sheath component from the hot isostatically pressed assembly to obtain a cemented carbide and titanium alloy cylindrical laminated structure.

2. The method for preparing the cemented carbide and titanium alloy cylindrical laminated structure according to claim 1, It is characterized in that In step 1, the particle size distribution of the titanium alloy powder produced is 75-250 μm, and the tap density is 63%-67%; the inner diameter of the cemented carbide cylindrical part is 35 mm-40 mm, and the outer diameter is 43 mm-48 mm.

3. The method for preparing the cemented carbide and titanium alloy cylindrical laminated structure according to claim 1, It is characterized in that The inner sleeve includes two parts, a cylindrical core and a base. The base is concentric with the cylindrical core and formed integrally. A first annular groove is provided on the base. The first annular groove is located at the outer edge of the lower end of the cylindrical core. The inner diameter of the first annular groove is clearance-matched with the outer diameter of the cemented carbide tube to achieve positioning of the lower end of the cemented carbide tube.

4. The method for preparing the cemented carbide and titanium alloy cylindrical laminated structure according to claim 3, It is characterized in that A circular hole with a diameter the same as the outer diameter of the base is provided at the center of the lower end cover to achieve positioning of the lower end cover and the inner sleeve.

5. The method for preparing the cemented carbide and titanium alloy cylindrical laminated structure according to claim 1, It is characterized in that The upper end cover is provided with a powder filling port, and a second annular groove is concentrically provided at the center of the bottom surface of the upper end cover, and the inner diameter of the second annular groove is clearance-matched with the outer diameter of the cemented carbide tube to realize the positioning of the upper end of the cemented carbide tube.

6. The method for preparing the cemented carbide and titanium alloy cylindrical laminated structure according to claim 1, It is characterized in that The upper and lower ends of the outer sleeve are both provided with steps, so that the upper end cover and the lower end cover are effectively fixed during assembly, and the outer sleeve is clearance-matched with the upper end cover and the lower end cover.

7. The method for preparing the cemented carbide and titanium alloy cylindrical laminated structure according to claim 1, It is characterized in that Before assembling the carbide cylinder and the sleeve, it also includes: The outer surface of the obtained hard alloy cylinder is pickled, immersed in anhydrous ethanol for ultrasonic cleaning, and stored in anhydrous ethanol; the surface of the sheath component is cleaned and degreased, and a solder stopper is applied.

8. The method for preparing the cemented carbide and titanium alloy cylindrical laminated structure according to claim 1, It is characterized in that Step 4 specifically includes: Use a funnel to load titanium alloy powder into the processed assembly, vibrate while loading the powder, and after loading, use a vacuum pump to evacuate the bag to less than 10 -2 Pa, then place the sleeve in a pit furnace and heat it to 300℃-400℃, then keep it warm and degas for 1-3h, then heat it to 600-700℃ and keep it warm and degas for 1-3h, and then use carbon dioxide gas shielded welding to seal the sleeve.

9. The method for preparing the cemented carbide and titanium alloy cylindrical laminated structure according to claim 1, It is characterized in that Step 5 specifically includes: The assembly filled with titanium alloy powder is placed in a hot isostatic pressing furnace for hot isostatic pressing treatment; during the hot isostatic pressing process, the furnace temperature of the hot isostatic pressing furnace is raised to 890°C-970°C in a step-by-step manner, and a pressure of 100MPa-180MPa is applied to the entire furnace chamber through the pressure system of the hot isostatic pressing furnace and maintained for 2-4 hours. After the pressure holding is completed, it is cooled to room temperature with the furnace in a step-by-step manner to complete the hot isostatic pressing connection of the assembly.

10. The method for preparing the cemented carbide and titanium alloy cylindrical laminated structure according to claim 9, It is characterized in that The specific process of the step-by-step heating is as follows: the temperature of the hot isostatic pressing furnace is raised to 200°C-400°C and kept at this temperature for 20min-40min; after the heat preservation, the temperature of the hot isostatic pressing furnace is raised to 500°C-650°C and kept at this temperature for 20min-40min; then the temperature of the hot isostatic pressing furnace is raised to 890°C-970°C at a heating rate of 10°C / min; The specific process of the step cooling is: cooling to 600°C-800°C with the furnace and keeping it warm for 20min-40min; after the insulation is completed, the furnace temperature of the hot isostatic pressing furnace is cooled to 400°C-600°C with the furnace and kept warm for 20min-40min; after the insulation is completed, the furnace temperature of the hot isostatic pressing furnace is cooled to room temperature with the furnace.

Citation Information

Cited By

  • Titanium-steel cylindrical part construction method

    CN119870678A

  • A method of constructing a titanium-steel cylinder

    CN119870678B