Polishing processing technology of high-light-transmittance optical glass

By using fine-grained abrasives and ultrasonic cleaning technology in optical glass processing, combined with CNC polishing machines and potassium nitrate tempering, the problems of defects and unstable performance of optical glass surfaces in traditional processes are solved, and high light transmittance and high efficiency production are achieved .

CN118990135APending Publication Date: 2024-11-22日禺光学科技(苏州)有限公司
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411076292.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Traditional optical glass processing technology is difficult to achieve high-precision and high-quality polishing effects, and there are problems such as surface defects, unstable optical performance, low production efficiency and inconsistent product quality.

Method used

Grinding and polishing with coarse polishing abrasives with particle sizes of 10 to 30 μm and fine polishing abrasives of 0.5 to 5 μm, combined with ultrasonic cleaning and CNC polishing machines, use polishing agents of specific ingredients, and tempered by potassium nitrate to improve surface flatness and finish , control process parameters to ensure product quality.

Benefits of technology

It significantly improves the light transmittance and optical uniformity of optical glass, improves the imaging quality of the optical system, improves production efficiency, reduces costs, and ensures the stability and reliability of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118990135A_ABST
    Figure CN118990135A_ABST
Patent Text Reader

Abstract

The invention discloses a polishing processing technology of high-light-transmittance optical glass, which relates to the field of glass processing, and is characterized in that oil stains, attachments, impurities and flaws on the surface are removed through a chemical reagent and a mechanical mode; thirdly, rough polishing grinding materials with the particle size ranging from 10 micrometers to 30 micrometers are used for primary polishing, and the rotating speed and the pressure of polishing equipment are adjusted to reduce the surface roughness; by precisely selecting and controlling the components and concentration of the polishing agent, surface flaws and defects can be efficiently removed, the surface flatness and smoothness are greatly improved, and the light transmittance is enhanced; secondly, the optimized process effectively reduces surface scattering and absorption, the optical uniformity is improved, and the imaging quality of the optical system is remarkably improved; furthermore, the reasonable data setting ensures the quality, improves the production efficiency and reduces the cost at the same time; and finally, process parameters are strictly controlled to ensure that the product quality is stable and consistent, the reliability is enhanced, the service life is prolonged, and the optical glass has higher market competitiveness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of glass processing, in particular to a polishing process for high-transmittance optical glass. Background Art

[0002] With the rapid development of modern optical technology, optical glass, as an important optical component, has increasingly stringent performance and quality requirements. Traditional optical glass processing technology often fails to meet the needs of high precision and high quality, and there are problems such as poor polishing effect, unstable optical performance, low production efficiency and uneven product quality.

[0003] In the polishing process, due to improper selection of polishing agent ingredients, inaccurate concentration, and unreasonable control of polishing time and temperature, the optical glass surface flaws and defects are not completely removed, the surface flatness and finish are insufficient, which in turn affects the transmittance and optical uniformity of the optical glass. At the same time, traditional processes have limited effects in improving optical performance and cannot effectively reduce the scattering and absorption of the optical glass surface, which limits the improvement of the imaging quality of the optical system; in addition, production efficiency is also an important factor restricting the development of the optical glass industry. The setting of process parameters in the past failed to fully improve production efficiency while ensuring quality, resulting in high production costs. Moreover, due to the lack of strict control of process parameters, the stability and consistency of product quality are difficult to guarantee, which reduces the reliability and service life of the product.

[0004] Therefore, in order to overcome the above problems, optimize and improve the optical glass processing technology, explore more scientific and reasonable data settings and process parameters to improve polishing effects, improve optical properties, improve production efficiency and ensure product quality stability, which has become a key technical issue that needs to be urgently solved in the current optical glass processing field. Summary of the invention

[0005] Based on this, the purpose of the present invention is to provide a polishing process for high-transmittance optical glass to solve the technical problems mentioned in the above background technology.

[0006] To achieve the above-mentioned purpose, the present invention provides the following technical solution: a polishing process for high-transmittance optical glass.

[0007] The process first pre-treats the optical glass by using chemical reagents and mechanical methods to remove surface oil, attachments, impurities and defects.

[0008] Next, a rough polishing abrasive with a particle size of 10 to 30 μm is used for preliminary grinding, and the rotation speed and pressure of the grinding equipment are adjusted to reduce the surface roughness.

[0009] Then, fine polishing is performed using a fine polishing abrasive with a particle size of 0.5 to 5 μm in combination with a specific polishing pad and polishing liquid to improve the surface flatness and smoothness.

[0010] Afterwards, the polished optical glass is cleaned using an ultrasonic cleaning machine with a power of 1000 to 1500 watts and a frequency of 40 to 60 kHz, while controlling the cleaning time and temperature.

[0011] The cleaned optical glass is put into the CNC polishing machine again, and further polished with a polishing agent containing specific ingredients and proportions, and QC inspection is carried out.

[0012] After the second polishing, the qualified optical glass is cleaned again with an ultrasonic cleaner to which an appropriate amount of surfactant is added, and then dried at a drying temperature of 80 to 100°C.

[0013] The optical glass was then tempered with potassium nitrate in a tempering pot, the tempering temperature was set at 415°C, and the tempering time was maintained for 2 hours to increase its surface hardness.

[0014] During the whole processing, the particle size of the rough polishing abrasive is preferably 15 to 25 μm and the abrasive feeding speed is uniform and stable. The particle size of the fine polishing abrasive is preferably 1 to 3 μm and the ambient temperature during fine polishing is controlled at 20 to 25°C.

[0015] The polishing agent may also contain 1.15% by mass of cerium oxide and 0.08% by mass of lithium oxide, which need to be fully stirred before use.

[0016] During the tempering process, the concentration of potassium nitrate needs to be monitored and adjusted to ensure consistent tempering results. At the same time, the surface quality of the optical glass needs to be monitored and recorded in real time. After tempering, the optical glass needs to be tested for hardness and transmittance. Only products that meet the standards can enter the next process.

[0017] In summary, the present invention mainly has the following beneficial effects:

[0018] The present invention can effectively remove surface flaws and defects, greatly improve surface flatness and smoothness, and enhance light transmittance by accurately selecting and controlling the composition and concentration of the polishing agent; secondly, the optimized process effectively reduces surface scattering and absorption, improves optical uniformity, and significantly improves the imaging quality of the optical system; thirdly, reasonable data settings improve production efficiency and reduce costs while ensuring quality; finally, strict control of process parameters ensures stable and consistent product quality, enhances reliability, extends service life, and makes optical glass more competitive in the market. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 It is a flow chart of the processing technology of the present invention;

[0020] Figure 2 It is a three-dimensional structural schematic diagram of the CNC polishing machine in the present invention.

[0021] In the picture: 1. CNC polishing machine. DETAILED DESCRIPTION

[0022] The following will be combined with the accompanying drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention.

[0023] The following describes an embodiment of the present invention based on its overall structure.

[0024] Embodiment 1

[0025] like Figure 1 As shown, the polishing process of the high-transmittance optical glass in this embodiment;

[0026] Select a piece of optical glass to process;

[0027] First, it was pretreated by using acetone as a chemical reagent to remove surface oil, and then a scraper was used to mechanically remove surface impurities and defects; then a coarse polishing abrasive with a particle size of 20μm was used, the speed of the polishing equipment was set to 1000 rpm, and the pressure was adjusted to 5 Newtons for preliminary polishing;

[0028] Then, use a fine polishing abrasive with a particle size of 2μm, at an ambient temperature of 22℃, with a special polishing pad and polishing liquid for fine polishing; then use an ultrasonic cleaner with a power of 1200 watts and a frequency of 50kHz to clean at 40℃ for 15 minutes; put the cleaned optical glass into a CNC polishing machine, and use a polishing agent containing 1.08% by mass of cerium oxide and the balance of water for further polishing, and then conduct QC inspection;

[0029] The optical glass that passed the inspection was cleaned again with an ultrasonic cleaner added with a surfactant, and then dried at 90°C; finally, it was tempered with potassium nitrate in a tempering pot, and the tempering temperature was set to 415°C and maintained for 2 hours.

[0030] After testing, the hardness and transmittance of the optical glass meet the requirements.

[0031] Embodiment 2

[0032] like Figure 1 As shown, the polishing process of the high-transmittance optical glass in this embodiment;

[0033] Another piece of optical glass was selected; during pretreatment, ethanol was used to remove surface oil stains, and sandpaper was used to remove surface attachments; during rough polishing, an abrasive with a particle size of 15 μm was used, the speed was 800 rpm, and the pressure was 4 Newtons;

[0034] The fine polishing uses an abrasive with a particle size of 1μm and an ambient temperature of 20°C; it is cleaned at 35°C for 20 minutes using an ultrasonic cleaner with a power of 1000 watts and a frequency of 40kHz; the cleaned optical glass is placed in a CNC polishing machine and further polished and inspected using a polishing agent containing 1.15% by mass cerium oxide and 0.08% by mass lithium oxide, with the remainder being water; it is cleaned again after passing the test and dried at 80°C; it is tempered with potassium nitrate at 415°C for 2 hours.

[0035] The test results show that the optical glass meets the expected hardness and transmittance standards.

[0036] Embodiment 3

[0037] like Figure 1 As shown, the polishing process of the high-transmittance optical glass in this embodiment;

[0038] Prepare a piece of optical glass; in the pretreatment stage, use gasoline to remove oil stains and use a brush to remove impurities; rough polishing uses 25μm abrasive, a speed of 1200 rpm, and a pressure of 6 Newtons;

[0039] Use 3μm abrasive for fine polishing at an ambient temperature of 25℃; use a 1500-watt, 60kHz ultrasonic cleaner to clean at 45℃ for 10 minutes; put the cleaned optical glass into a CNC polishing machine, polish it with a polishing agent containing 1.08% cerium oxide and inspect it; those that pass the inspection are cleaned again and dried at 100℃; and tempered with potassium nitrate at 415℃ for 2 hours.

[0040] Finally, the hardness and light transmittance of the optical glass meet the requirements.

[0041] Embodiment 4

[0042] like Figure 1 As shown, the polishing process of the high-transmittance optical glass in this embodiment;

[0043] Take out a piece of optical glass for processing; during pretreatment, use a special cleaner to remove oil and attachments, and use a file to remove surface defects; rough polishing uses an abrasive with a particle size of 18μm, a speed of 900 rpm, and a pressure of 4.5 Newtons;

[0044] The fine polishing uses an abrasive with a particle size of 2.5μm and an ambient temperature of 23℃; it is cleaned at 40℃ for 18 minutes using an 1100-watt, 45kHz ultrasonic cleaner; the cleaned optical glass is placed in a CNC polishing machine and polished and inspected using a polishing agent containing 1.15% cerium oxide and 0.08% lithium oxide; after passing the test, it is cleaned again and dried at 95℃; it is tempered with potassium nitrate at 415℃ for 2 hours.

[0045] Tests show that the hardness and transmittance of the optical glass meet the standards.

[0046] It should be noted that if Figure 2 As shown, the polishing machine of the present invention is a numerically controlled polishing machine 1, which has the function of automatically adjusting the polishing pressure and speed.

[0047] In combination with the data settings in the above embodiments, the present invention can effectively remove flaws and defects on the surface of optical glass, improve surface flatness and smoothness, and thus improve the transmittance of optical glass by selecting appropriate polishing agent composition and concentration, and controlling parameters such as polishing time and temperature; the optimized polishing process can reduce scattering and absorption on the surface of optical glass, improve light transmittance and optical uniformity, and improve the imaging quality of the optical system; reasonable data settings can improve production efficiency and reduce production costs while ensuring polishing quality; ensure product quality stability: by strictly controlling polishing process parameters, the stability and consistency of product quality can be guaranteed, and the reliability and service life of the product can be improved.

[0048] Although an embodiment of the present invention has been shown and described, this specific embodiment is only an explanation of the present invention and is not a limitation of the invention. The specific features, structures, materials or characteristics described may be combined in a suitable manner in any one or more embodiments or examples. After reading this specification, those skilled in the art may make modifications, substitutions and variations to the embodiments without creative contribution as needed without departing from the principles and purpose of the present invention. However, as long as they are within the scope of the claims of the present invention, they are protected by patent law.

Claims

1. A polishing process for high-transmittance optical glass, characterized in that: The following steps are involved: Step 1: Pre-treat the optical glass, use chemical reagents to remove surface oil and attachments, and then use mechanical methods to remove surface impurities and defects; Step 2: Use a coarse polishing abrasive with a particle size of 10 to 30 μm for preliminary grinding, and adjust the speed and pressure of the grinding equipment to reduce the surface roughness; Step 3: Use fine polishing abrasive with a particle size of 0.5 to 5 μm for fine polishing, with a specific polishing pad and polishing liquid to improve the surface flatness and finish; Step 4: Use an ultrasonic cleaner to clean the polished optical glass, and control the cleaning time and temperature; Step 5: Put the cleaned optical glass into the polishing machine again, and further polish the optical glass using a polishing agent containing 1.08% by mass of cerium oxide and the balance of water, and perform QC inspection on the pre-polished optical glass; Step 6: Use an ultrasonic cleaning machine to clean the optical glass that has passed the secondary polishing inspection again, and add an appropriate amount of surfactant during the cleaning process to improve the cleanliness; Step 7: Use potassium nitrate to temper the optical glass in a tempering pot, set the tempering temperature to 415°C, and maintain the tempering time for 2 hours to increase the surface hardness of the optical glass.

2. The polishing process for high-transmittance optical glass according to claim 1, characterized in that: The particle size of the rough polishing abrasive is 15 to 25 μm, and the supply speed of the abrasive during the rough polishing process is uniform and stable.

3. The polishing process for high-transmittance optical glass according to claim 1, characterized in that: The particle size of the fine polishing abrasive is 1 to 3 μm, and the ambient temperature during fine polishing is controlled at 20 to 25°C.

4. The polishing process for high-transmittance optical glass according to claim 1, characterized in that: The power of the ultrasonic cleaning machine is 1000 to 1500 watts and the frequency is 40 to 60 kHz.

5. The polishing process for high-transmittance optical glass according to claim 1, characterized in that: The polishing machine is a numerically controlled polishing machine (1) and has the function of automatically adjusting polishing pressure and speed.

6. The polishing process for high-transmittance optical glass according to claim 1, characterized in that: The polishing agent contains 1.15% by mass of cerium oxide and 0.08% by mass of lithium oxide, with the remainder being water, and needs to be fully stirred before use.

7. The polishing process for high-transmittance optical glass according to claim 1, characterized in that: In step six, the optical glass after cleaning again needs to be dried at a temperature of 80 to 100°C.

8. The polishing process for high-transmittance optical glass according to claim 1, characterized in that: During the tempering process, the concentration of potassium nitrate needs to be monitored and adjusted to ensure the consistency of the tempering effect.

9. The polishing process for high-transmittance optical glass according to claim 1, characterized in that: During the entire processing process, the surface quality of the optical glass needs to be monitored and recorded in real time.

10. The polishing process for high-transmittance optical glass according to claim 1, characterized in that: After the tempering, the optical glass needs to be tested for hardness and transmittance, and only products that meet the standards can enter the next process.

Citation Information

Patent Citations

  • Manufacturing process of glass motherboard substrate

    CN104616672A

  • Chemical-mechanical polishing method of microcrystalline glass and microcrystalline glass

    CN107529477A

  • Green, cheap and environment-friendly chemical mechanical polishing method for optical quartz glass

    CN110524315A

  • Manufacturing process of three-dimensional highlight 3D glass

    CN110627350A

  • Preparation method of optical glass with high light transmittance and high stability

    CN112476072A