Phosphate coated lithium manganese iron phosphate material, preparation method and lithium ion battery

By ALD coating using phosphate on the surface of lithium manganese iron phosphate material, a dense protective layer is formed, the problem of manganese ion dissolution is solved, the cycle life and resistivity of lithium-ion batteries are improved, and a more uniform coating effect is achieved.

CN118993011APending Publication Date: 2024-11-22BATTERO TECH CORP LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411091672.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The problem of manganese ion dissolution of lithium manganese ferrophosphate materials under high temperature conditions leads to a decrease in battery capacity and shortening of cycle life. The existing surface coating technology has problems such as high-temperature equipment demand, complex operation and insufficient cladding stability.

Method used

The coating layer is formed by using phosphate (such as titanium phosphate) on the surface of lithium manganese iron phosphate material to carry out gas solid-phase chemical adsorption reaction, and coated using atomic layer deposition (ALD) technology to form a dense protective layer to prevent manganese ions. Dissolve.

Benefits of technology

It improves the cycle life and lithium ion transmission rate of lithium manganese iron phosphate materials, reduces capacity loss during battery circulation, and improves the cycle performance and resistivity of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993011A_ABST
    Figure CN118993011A_ABST
Patent Text Reader

Abstract

The invention discloses a phosphate-coated lithium manganese iron phosphate material, a preparation method and a lithium ion battery, and relates to the technical field of lithium ion batteries. The preparation method comprises the following steps: introducing a gas-phase phosphate precursor into a reaction chamber in which a lithium manganese iron phosphate matrix is placed, and depositing the phosphate precursor on the surface of the lithium manganese iron phosphate matrix to generate a gas-solid phase chemical adsorption reaction, so as to form a phosphate-coated lithium manganese iron phosphate precursor; and sintering the phosphate-coated lithium manganese iron phosphate precursor to obtain the phosphate-coated lithium manganese iron phosphate material. A layer of phosphate can be formed on the surface of the lithium manganese iron phosphate material, and the phosphate can form a protective layer on the surface of the lithium manganese iron phosphate material to prevent manganese ions from being dissolved out, so that the capacity loss in the battery cycle process is reduced, and the cycle life of the lithium manganese iron phosphate material is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a phosphate-coated lithium manganese iron phosphate material, a preparation method thereof, and a lithium ion battery. Background Art

[0002] Lithium iron manganese phosphate (LiMn x Fe (1-x) Lithium iron manganese phosphate (LiMnPO4) is a promising cathode material that is expected to be widely used in lithium-ion batteries. However, under high temperature conditions, lithium manganese iron phosphate (LiMnPO4) materials will suffer from manganese dissolution problems, resulting in a decrease in battery capacity and a shortened cycle life during high temperature cycling.

[0003] At present, the problem of manganese dissolution in lithium manganese iron phosphate materials is often improved by coating. Commonly used coating methods include physical vapor deposition (PVD) and chemical vapor deposition (CVD). However, there are some problems and limitations in existing surface coating technologies. These existing surface coating technologies usually require high temperatures and complex equipment and are not easy to implement. Secondly, the structure and properties of the coating layer are often unable to be effectively controlled, resulting in low stability and durability of the coating layer. Some coating layers hinder the transmission of lithium ions, thereby affecting the gram capacity.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] The purpose of the present invention is to provide a phosphate-coated lithium iron manganese phosphate material, a preparation method and a lithium ion battery. In order to solve the problem of manganese dissolution in the lithium iron manganese phosphate material, the present invention coats the surface with a layer of phosphate material. Phosphate, as a stable material, can effectively prevent the dissolution of manganese ions, thereby improving the cycle life of the lithium iron manganese phosphate material. In addition, coating with titanium phosphate can also improve the lithium ion transmission rate.

[0006] The present invention is achieved in that:

[0007] In a first aspect, the present invention provides a method for preparing a phosphate-coated lithium manganese iron phosphate material, comprising:

[0008] Passing a gaseous phosphate precursor into a reaction chamber in which a lithium iron manganese phosphate substrate is placed, the phosphate precursor is deposited on the surface of the lithium iron manganese phosphate substrate to undergo a gas-solid phase chemical adsorption reaction to form a phosphate-coated lithium iron manganese phosphate precursor;

[0009] The phosphate-coated lithium manganese iron phosphate precursor is sintered to obtain a phosphate-coated lithium manganese iron phosphate material.

[0010] In an optional embodiment, the phosphate in the phosphate-coated lithium manganese iron phosphate material includes at least one of titanium phosphate and aluminum phosphate.

[0011] In an optional embodiment, when the phosphate is titanium phosphate, the phosphate precursor includes trimethyl phosphate and titanium tetrachloride, and the introduction of the phosphate precursor into the reaction chamber includes: first introducing the trimethyl phosphate into the reaction chamber to allow the trimethyl phosphate to react with the lithium manganese iron phosphate matrix for 2-4 hours; and then introducing the titanium tetrachloride to allow the titanium tetrachloride to react with the trimethyl phosphate for 8-10 hours.

[0012] In an optional embodiment, the molar ratio of the amount of trimethyl phosphate introduced to the lithium iron manganese phosphate matrix is ​​0.001-0.1:1; the molar ratio of the amount of trimethyl phosphate introduced to the amount of titanium tetrachloride introduced is 3.7-4.3:2.7-3.3.

[0013] In an optional embodiment, the phosphate precursor is introduced into the reaction chamber in a pulsed manner;

[0014] Preferably, the speed of the pulse is 0.03mol / min-0.12mol / min;

[0015] Preferably, the introduction rate of the trimethyl phosphate is greater than the introduction rate of the titanium tetrachloride;

[0016] Preferably, the introduction rate of trimethyl phosphate is 0.04 mol / min-0.12 mol / min; the introduction rate of titanium tetrachloride is 0.03 mol / min-0.09 mol / min.

[0017] In an optional embodiment, after the trimethyl phosphate is introduced, an inert gas is introduced into the reaction chamber to expel unreacted trimethyl phosphate; after the titanium tetrachloride is introduced, an inert gas is introduced into the reaction chamber to expel unreacted titanium tetrachloride.

[0018] In an optional embodiment, before placing the lithium iron manganese phosphate matrix in the reaction chamber, the method further comprises pre-treating the lithium iron manganese phosphate matrix;

[0019] Preferably, the pretreatment includes cleaning and activating the lithium manganese iron phosphate matrix;

[0020] Preferably, the cleaning comprises placing the lithium manganese iron phosphate matrix in anhydrous ethanol and using ultrasonic cleaning for 2-4 hours;

[0021] Preferably, the activation comprises drying and then grinding the cleaned lithium manganese iron phosphate matrix;

[0022] Preferably, the drying comprises drying in a vacuum drying oven at 80-120° C. for 12-24 h;

[0023] Preferably, the grinding comprises grinding in a ball mill at a rotation speed of 800-1000 rpm for 6-8 hours.

[0024] In an optional embodiment, the sintering includes placing the phosphate-coated lithium manganese iron phosphate precursor in a tube furnace under an inert atmosphere at 400-600° C. for 1-3 hours;

[0025] Preferably, before the sintering, the phosphate-coated lithium manganese iron phosphate precursor is washed with water and hydrochloric acid in sequence.

[0026] In a second aspect, the present invention provides a phosphate-coated lithium manganese iron phosphate material, which is prepared by the preparation method of the phosphate-coated lithium manganese iron phosphate material as described in any one of the aforementioned embodiments;

[0027] Preferably, the coating layer thickness of the phosphate-coated lithium manganese iron phosphate material is 0.5-1 nm;

[0028] Preferably, the average particle size of the phosphate-coated lithium manganese iron phosphate material is 200-800 nm;

[0029] Preferably, the specific surface area of ​​the phosphate-coated lithium manganese iron phosphate material is 10-30 m 2 / g.

[0030] In a third aspect, the present invention provides a lithium-ion battery comprising the phosphate-coated lithium manganese iron phosphate material as described in the aforementioned embodiment.

[0031] The present invention has the following beneficial effects:

[0032] The preparation method of the phosphate-coated lithium iron manganese phosphate material provided by the present invention is to coat the surface of the lithium iron manganese phosphate by ALD technology, deposit at the atomic level, and the coating effect is more uniform. By the above method, a layer of phosphate (such as titanium phosphate) can be formed on the surface of the lithium iron manganese phosphate, and the phosphate can form a protective layer on the surface of the lithium iron manganese phosphate material to prevent the dissolution of manganese ions, thereby reducing the capacity loss during the battery cycle and improving the cycle life of the lithium iron manganese phosphate material. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0034] Figure 1The bar graphs of powder resistivity provided for the embodiments of the present invention and comparative examples. DETAILED DESCRIPTION

[0035] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0036] The present invention provides a method for preparing a phosphate-coated lithium manganese iron phosphate material, which comprises:

[0037] A gaseous phosphate precursor is introduced into a reaction chamber in which a lithium iron manganese phosphate substrate is placed. The phosphate precursor is deposited on the surface of the lithium iron manganese phosphate substrate to undergo a gas-solid chemical adsorption reaction to form a phosphate-coated lithium iron manganese phosphate precursor. The phosphate-coated lithium iron manganese phosphate precursor is sintered to obtain a phosphate-coated lithium iron manganese phosphate material.

[0038] In the present invention, the surface of lithium manganese iron phosphate is coated by atomic layer deposition (ALD) technology to form a phosphate (such as titanium phosphate) film to improve the manganese dissolution phenomenon of the lithium manganese iron phosphate material. The phosphate can form a protective layer on the surface of the lithium manganese iron phosphate material to prevent the dissolution of manganese ions, thereby reducing the capacity loss during the battery cycle and improving the cycle life of the lithium manganese iron phosphate material.

[0039] The preparation method of the present invention specifically comprises the following steps:

[0040] S1. Preprocessing.

[0041] The lithium manganese iron phosphate substrate is cleaned and activated to improve the adhesion of the film in the subsequent gas phase reaction.

[0042] Among them, cleaning includes placing the lithium manganese iron phosphate matrix in anhydrous ethanol and using ultrasonic cleaning for 2-4 hours; activation includes drying the cleaned lithium manganese iron phosphate matrix and then grinding it; drying includes drying in a vacuum drying oven at 80-120°C for 12-24 hours; grinding includes grinding in a ball mill at a speed of 800-1000rpm for 6-8 hours.

[0043] S2. Gas phase reaction.

[0044] A gaseous phosphate precursor is introduced into a reaction chamber in which a lithium iron manganese phosphate substrate is placed. The phosphate precursor is deposited on the surface of the lithium iron manganese phosphate substrate to undergo a gas-solid phase chemical adsorption reaction to form a phosphate-coated lithium iron manganese phosphate precursor.

[0045] The phosphate in the phosphate-coated lithium manganese iron phosphate material includes at least one of titanium phosphate and aluminum phosphate.

[0046] When the phosphate is titanium phosphate, the phosphate precursor includes trimethyl phosphate and titanium tetrachloride, and the introduction of the phosphate precursor into the reaction chamber includes: firstly introducing trimethyl phosphate into the reaction chamber to react the trimethyl phosphate with the lithium manganese iron phosphate matrix for 2-4 hours; then introducing titanium tetrachloride to react the titanium tetrachloride with the trimethyl phosphate for 8-10 hours.

[0047] The molar ratio of the amount of trimethyl phosphate introduced to the lithium manganese iron phosphate matrix is ​​0.001-0.1:1;

[0048] The molar ratio of the amount of trimethyl phosphate introduced to the amount of titanium tetrachloride introduced is 3.7-4.3:2.7-3.3.

[0049] The phosphate precursor is introduced into the reaction chamber in a pulsed manner; the pulse speed is 0.03mol / min-0.12mol / min. In the present invention, the introduction speed of trimethyl phosphate is greater than the introduction speed of titanium tetrachloride; specifically, the introduction speed of trimethyl phosphate is 0.04mol / min-0.12mol / min; the introduction speed of titanium tetrachloride is 0.03mol / min-0.09mol / min. The introduction amount of trimethyl phosphate and titanium tetrachloride is determined by the required coating thickness.

[0050] Furthermore, after the trimethyl phosphate is introduced, an inert gas is introduced into the reaction chamber to discharge the unreacted trimethyl phosphate; after the titanium tetrachloride is introduced, an inert gas is introduced into the reaction chamber to discharge the unreacted titanium tetrachloride. In the present invention, the gas in the reaction chamber is replaced by introducing an inert gas into the reaction chamber, so that the remaining gas in the reaction chamber is discharged to ensure the purity of the reaction. The inert gas includes but is not limited to N2 or Ar.

[0051] S3. Cleaning.

[0052] The phosphate-coated lithium manganese iron phosphate precursor is washed with water and hydrochloric acid in sequence.

[0053] S4. Sintering.

[0054] The phosphate-coated lithium manganese iron phosphate precursor is placed in a tube furnace and sintered at 400-600° C. for 1-3 hours under an inert atmosphere to obtain a phosphate-coated lithium manganese iron phosphate material.

[0055] The phosphate-coated lithium manganese iron phosphate material prepared by the above method has a core-shell structure, wherein the phosphate is coated on the surface of the lithium manganese iron phosphate material as a coating layer, and the coating layer thickness is 0.5-1nm. It can protect the lithium manganese iron phosphate and prevent the dissolution of manganese ions, thereby reducing the capacity loss during the battery cycle and improving the cycle life of the lithium manganese iron phosphate material.

[0056] The phosphate-coated lithium manganese iron phosphate material is used as a positive electrode material to prepare a lithium ion battery. The prepared lithium ion battery has low resistivity, high cycle life, and greatly improved manganese dissolution.

[0057] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0058] Example 1

[0059] This embodiment provides a phosphate-coated lithium manganese iron phosphate material, and the preparation method thereof includes:

[0060] S1, LiMn 0.6 Fe 0.4 PO4 particles were added to anhydrous ethanol solution and cleaned by ultrasonic for 3 hours to remove uncoated free carbon; then they were baked in a vacuum drying oven at 100°C for 18 hours, and the obtained powder was ground in a ball mill for 7 hours.

[0061] S2, place lithium manganese iron phosphate in the reaction chamber, pulse 0.04 mol / min trimethyl phosphate and LiMn 0.6 Fe 0.4 PO4 was fully reacted for 3 hours, and Ar was introduced to expel the unreacted trimethyl phosphate; 0.03 mol / min titanium tetrachloride was pulsed into the reaction chamber to allow titanium tetrachloride and trimethyl phosphate to fully react for 9 hours, and Ar was introduced to expel the unreacted titanium tetrachloride, and finally titanium phosphate-coated lithium manganese iron phosphate material was obtained.

[0062] S3. Clean the obtained titanium phosphate-coated lithium manganese iron phosphate material precursor to remove unreacted precursor and other impurities.

[0063] S4. The obtained titanium phosphate-coated lithium manganese iron phosphate material precursor is transferred to a tubular furnace and sintered at 500° C. for 2 h in an inert atmosphere such as Ar or N2 to obtain a titanium phosphate-coated lithium manganese iron phosphate material with a coating thickness of about 0.5 nm.

[0064] Example 2

[0065] This embodiment is basically the same as Embodiment 1, except that, in this embodiment, the amount of trimethyl phosphate introduced is 0.08 mol / min, the amount of titanium tetrachloride introduced is 0.06 mol / min, and the coating thickness of the prepared titanium phosphate-coated lithium manganese iron phosphate material is about 1 nm.

[0066] Example 3

[0067] This embodiment is basically the same as Embodiment 1, except that, in this embodiment, the amount of trimethyl phosphate introduced is 0.12 mol / min, the amount of titanium tetrachloride introduced is 0.09 mol / min, and the coating thickness of the prepared titanium phosphate-coated lithium manganese iron phosphate material is about 2 nm.

[0068] Example 4

[0069] This embodiment provides a phosphate-coated lithium manganese iron phosphate material, and the preparation method thereof includes:

[0070] S1, LiMn 0.6 Fe 0.4 PO4 particles were added to anhydrous ethanol solution and cleaned by ultrasonic for 2 hours to remove uncoated free carbon; then they were baked in a vacuum drying oven at 80°C for 24 hours, and the obtained powder was ground in a ball mill for 6 hours.

[0071] S2, place lithium manganese iron phosphate in the reaction chamber, pulse 0.04 mol / min trimethyl phosphate and LiMn 0.6 Fe 0.4 PO4 was fully reacted for 2 hours, and Ar was introduced to expel the unreacted trimethyl phosphate; 0.03 mol / min titanium tetrachloride was pulsed into the reaction chamber to allow titanium tetrachloride and trimethyl phosphate to fully react for 8 hours, and Ar was introduced to expel the unreacted titanium tetrachloride, and finally titanium phosphate-coated lithium manganese iron phosphate material was obtained.

[0072] S3. Clean the obtained titanium phosphate-coated lithium manganese iron phosphate material precursor to remove unreacted precursor and other impurities.

[0073] S4. The obtained titanium phosphate-coated lithium manganese iron phosphate material precursor is transferred to a tubular furnace and sintered at 400° C. for 3 h in an inert atmosphere such as Ar or N2 to obtain a titanium phosphate-coated lithium manganese iron phosphate material with a coating thickness of about 0.5 nm.

[0074] Example 5

[0075] This embodiment provides a phosphate-coated lithium manganese iron phosphate material, and the preparation method thereof includes:

[0076] S1, LiMn 0.6 Fe 0.4 PO4 particles were added to anhydrous ethanol solution and ultrasonically cleaned for 4 hours to remove uncoated free carbon; then they were baked in a vacuum drying oven at 120°C for 12 hours, and the obtained powder was ground in a ball mill for 8 hours.

[0077] S2, place lithium manganese iron phosphate in the reaction chamber, pulse 0.04 mol / min trimethyl phosphate and LiMn 0.6 Fe 0.4PO4 was fully reacted for 4 hours, and Ar was introduced to expel the unreacted trimethyl phosphate; 0.03 mol / min titanium tetrachloride was pulsed into the reaction chamber to allow titanium tetrachloride and trimethyl phosphate to fully react for 10 hours, and Ar was introduced to expel the unreacted titanium tetrachloride, and finally titanium phosphate-coated lithium manganese iron phosphate material was obtained.

[0078] S3. Clean the obtained titanium phosphate-coated lithium manganese iron phosphate material precursor to remove unreacted precursor and other impurities.

[0079] S4. The obtained titanium phosphate-coated lithium manganese iron phosphate material precursor is transferred to a tubular furnace and sintered at 600° C. for 3 h in an inert atmosphere such as Ar or N2 to obtain a titanium phosphate-coated lithium manganese iron phosphate material with a coating thickness of about 0.5 nm.

[0080] Comparative Example 1

[0081] This comparative example provides an uncoated lithium manganese iron phosphate material, and the preparation method thereof comprises: 0.6 Fe 0.4 PO4 particles were added to anhydrous ethanol solution and cleaned by ultrasonic for 3 hours to remove uncoated free carbon; then they were baked in a vacuum drying oven at 100°C for 18 hours, and the obtained powder was ground in a ball mill for 7 hours.

[0082] Comparative Example 2

[0083] The present comparative example provides a phosphate-coated lithium manganese iron phosphate material, and the preparation method thereof comprises: adding phosphate (0.72 kg of barium hydrogen phosphate), 0.13 kg of lithium chloride, and 2.03 kg of a second solvent (an alcohol-water mixture, 95% ethanol) to 3.45 kg of lithium manganese iron phosphate, performing sand milling, and drying the sand milled material; performing sintering treatment (calcining at 750° C. for 12 h at a heating rate of 5° C. / min) under a nitrogen atmosphere to obtain a phosphate-coated lithium manganese iron phosphate particle material.

[0084] Comparative Example 3

[0085] The present comparative example provides a method for preparing a phosphate-coated lithium manganese iron phosphate material by physical vapor deposition (PVD), which comprises: placing an LMFP sample in a vacuum chamber of a PVD device, using a vacuum pump to reduce the air pressure in the vacuum chamber, arranging an evaporation source containing a titanium phosphate material in the vacuum chamber, evaporating the titanium phosphate into a gaseous state, and transmitting the evaporated titanium phosphate gaseous molecules in the vacuum chamber and depositing on the surface of the LMFP sample to form a coating layer.

[0086] Comparative Example 4

[0087] The present comparative example provides a method for preparing a phosphate-coated lithium manganese iron phosphate material by chemical vapor deposition (CVD), which comprises: dissolving titanium sulfate and phosphoric acid in a proper solvent in a certain proportion to form a precursor solution, placing a LMFP material in a reaction chamber of a CVD device, introducing the precursor solution into the reaction chamber in a proper manner, wherein the precursor vapor undergoes a chemical reaction in the reaction chamber to generate titanium phosphate and deposit it on the surface of the LMFP material to form a coating layer.

[0088] Comparative Example 5

[0089] This comparative example is basically the same as Example 1, except that the phosphate in this comparative example is aluminum phosphate, and its corresponding precursors are trimethyl phosphate and aluminum chloride. The preparation method of this comparative example specifically includes:

[0090] S1, LiMn 0.6 Fe 0.4 PO4 particles were added to anhydrous ethanol solution and cleaned by ultrasonic for 3 hours to remove uncoated free carbon; then they were baked in a vacuum drying oven at 100°C for 18 hours, and the obtained powder was ground in a ball mill for 7 hours.

[0091] S2, place lithium manganese iron phosphate in the reaction chamber, pulse 0.04 mol / min trimethyl phosphate, and LiMn 0.6 Fe 0.4 PO4 was fully reacted for 3 hours, and Ar was introduced to expel unreacted trimethyl phosphate; 0.03 mol / min aluminum chloride was pulsed into the reaction chamber to allow trimethyl phosphate and aluminum chloride to fully react for 9 hours, and Ar was introduced to expel unreacted aluminum chloride, finally obtaining aluminum phosphate-coated lithium manganese iron phosphate material.

[0092] S3. Clean the obtained aluminum phosphate-coated lithium manganese iron phosphate material precursor to remove unreacted precursor and other impurities.

[0093] S4. The obtained aluminum phosphate-coated lithium manganese iron phosphate material precursor is transferred to a tubular furnace and sintered at 500° C. for 2 h in an inert atmosphere such as Ar or N2 to obtain an aluminum phosphate-coated lithium manganese iron phosphate material with a coating thickness of about 0.5 nm.

[0094] Comparative Example 6

[0095] This comparative example is basically the same as Example 1, except that the order of introducing trimethyl phosphate and titanium tetrachloride in step S2 is different. In this comparative example, step S2 includes: placing lithium manganese iron phosphate in a reaction chamber, and introducing 0.03 mol / min of titanium tetrachloride and LiMn 06 Fe 04PO4 was fully reacted for 3 hours, and Ar was introduced to expel the unreacted titanium tetrachloride; 0.04 mol / min of trimethyl phosphate was pulsed into the reaction chamber to allow trimethyl phosphate and titanium tetrachloride to fully react for 9 hours, and Ar was introduced to expel the unreacted trimethyl phosphate, and finally titanium phosphate-coated lithium manganese iron phosphate material was obtained.

[0096] Experimental example

[0097] The lithium manganese iron phosphate materials prepared by Examples 1-5 and Comparative Examples 1-6 were subjected to resistivity tests and 45°C power-on cycle tests, wherein the resistivity test method includes: on a uniform sample where the probe spacing can be regarded as infinite, four probes arranged at equal intervals are inserted into the semiconductor surface, and the needle tips of the four probes are in the same straight line and are equally spaced, and a constant current source is used to provide a suitably small current I to the two outer probes, and then the voltage V between the two middle probes is measured, so that the resistivity of the sample can be accurately calculated. The test method of the 45°C power-on cycle test includes: at 45°C, charging to 4.35V with a constant current of 0.5C, charging to 0.05C with a constant voltage of 4.35V, standing for 10 minutes, discharging to 2.0V with a current of 0.5C, standing for 10 minutes, and performing a cycle test according to the above steps. The test results are as follows:

[0098]

[0099]

[0100] From the above table and Figure 1 It can be seen that the powder resistivity of Example 1 is 11.1Ω.cm lower than that of Comparative Example 1, the powder resistivity of Example 2 is 32.5Ω.cm lower than that of Comparative Example 1, and the powder resistivity of Example 3 is 21.2Ω.cm higher than that of Comparative Example 1, indicating that ALD coating below 1nm improves the powder resistivity. When the thickness of the coating layer is greater than 1nm, the thicker the coating, the higher the powder resistivity of the material. It can be seen from the number of cycles that coating with a certain thickness of Ti3(PO4)4 can reduce the manganese dissolution of lithium manganese iron phosphate at 45°C and improve the cycle performance. Changing the sintering temperature and extending the sintering time both deteriorate the performance.

[0101] Comparative Example 2 is directly coated with phosphate, and its resistivity is significantly higher than that of Example 1, and even higher than the uncoated lithium manganese iron phosphate material in Comparative Example 1. However, the number of cycles of Comparative Example 2 after coating with phosphate is better than that of Comparative Example 1, but still worse than that of Example 1.

[0102] Comparative Examples 3 and 4 use other methods to prepare titanium phosphate coatings, and the effects thereof are significantly worse than the coating methods provided in the embodiments of the present invention, which fully proves that replacing different coating methods cannot achieve significant improvement effects.

[0103] In Comparative Example 5, other phosphates (aluminum phosphate) were coated, and the effect was significantly worse than that of the titanium phosphate provided in the embodiment of the present invention, which fully proved that replacing different coating materials could not achieve significant improvement. At the same time, when other coating materials were used for coating, the conductivity became worse after coating, so the resistivity increased significantly.

[0104] In Comparative Example 6, the order of introducing trimethyl phosphate and titanium tetrachloride was changed. At this time, the reaction effect of titanium tetrachloride with the lithium iron manganese phosphate matrix was poor, resulting in poor coating effect of the final titanium phosphate on the lithium iron manganese phosphate matrix. The powder resistivity was significantly higher than that of Example 1, and the cycle performance was also significantly lower than that of Example 1.

[0105] In summary, the preparation method of the phosphate-coated lithium iron manganese phosphate material provided by the present invention is to coat the surface of the lithium iron manganese phosphate by the ALD technology, and the surface coating of the lithium iron manganese phosphate is more dense, which is beneficial to the material. By the above method, a layer of phosphate (such as titanium phosphate) can be formed on the surface of the lithium iron manganese phosphate, and the phosphate can form a protective layer on the surface of the lithium iron manganese phosphate material to prevent the dissolution of manganese ions, thereby reducing the capacity loss during the battery cycle and improving the cycle life of the lithium iron manganese phosphate material.

[0106] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a phosphate-coated lithium manganese iron phosphate material, characterized in that: It includes: Passing a gaseous phosphate precursor into a reaction chamber in which a lithium iron manganese phosphate substrate is placed, the phosphate precursor is deposited on the surface of the lithium iron manganese phosphate substrate to undergo a gas-solid phase chemical adsorption reaction to form a phosphate-coated lithium iron manganese phosphate precursor; The phosphate-coated lithium manganese iron phosphate precursor is sintered to obtain a phosphate-coated lithium manganese iron phosphate material.

2. The method for preparing the phosphate-coated lithium manganese iron phosphate material according to claim 1, characterized in that: The phosphate in the phosphate-coated lithium manganese iron phosphate material includes at least one of titanium phosphate and aluminum phosphate.

3. The method for preparing the phosphate-coated lithium manganese iron phosphate material according to claim 2, characterized in that: When the phosphate is titanium phosphate, the phosphate precursor includes trimethyl phosphate and titanium tetrachloride, and the introduction of the phosphate precursor into the reaction chamber includes: firstly introducing the trimethyl phosphate into the reaction chamber to allow the trimethyl phosphate to react with the lithium manganese iron phosphate matrix for 2-4 hours; and then introducing the titanium tetrachloride to allow the titanium tetrachloride to react with the trimethyl phosphate for 8-10 hours.

4. The method for preparing the phosphate-coated lithium manganese iron phosphate material according to claim 3, characterized in that: The molar ratio of the amount of trimethyl phosphate introduced to the lithium iron manganese phosphate matrix is ​​0.001-0.1:1; the molar ratio of the amount of trimethyl phosphate introduced to the amount of titanium tetrachloride introduced is 3.7-4.3:2.7-3.

3.

5. The method for preparing the phosphate-coated lithium manganese iron phosphate material according to claim 3, characterized in that: The phosphate precursor is introduced into the reaction chamber in a pulsed manner; Preferably, the pulse speed is 0.03mol / min-0.12mol / min, and the time is 10-20min; Preferably, the introduction rate of the trimethyl phosphate is greater than the introduction rate of the titanium tetrachloride; Preferably, the introduction rate of trimethyl phosphate is 0.04 mol / min-0.12 mol / min; the introduction rate of titanium tetrachloride is 0.03 mol / min-0.09 mol / min.

6. The method for preparing the phosphate-coated lithium manganese iron phosphate material according to claim 3, characterized in that: After the trimethyl phosphate is introduced, an inert gas is introduced into the reaction chamber to discharge unreacted trimethyl phosphate; after the titanium tetrachloride is introduced, an inert gas is introduced into the reaction chamber to discharge unreacted titanium tetrachloride.

7. The method for preparing the phosphate-coated lithium manganese iron phosphate material according to claim 1, characterized in that: Before placing the lithium iron manganese phosphate matrix in the reaction chamber, the method further includes pre-treating the lithium iron manganese phosphate matrix; Preferably, the pretreatment includes cleaning and activating the lithium manganese iron phosphate matrix; Preferably, the cleaning comprises placing the lithium manganese iron phosphate matrix in anhydrous ethanol and using ultrasonic cleaning for 2-4 hours; Preferably, the activation comprises drying and then grinding the cleaned lithium manganese iron phosphate matrix; Preferably, the drying comprises drying in a vacuum drying oven at 80-120° C. for 12-24 h; Preferably, the grinding comprises grinding in a ball mill at a rotation speed of 800-1000 rpm for 6-8 hours.

8. The method for preparing the phosphate-coated lithium manganese iron phosphate material according to claim 1, characterized in that: The sintering comprises placing the phosphate-coated lithium manganese iron phosphate precursor in a tube furnace under an inert atmosphere at 400-600° C. for 1-3 hours; Preferably, before the sintering, the phosphate-coated lithium manganese iron phosphate precursor is washed with water and hydrochloric acid in sequence.

9. A phosphate-coated lithium manganese iron phosphate material, characterized in that: It is prepared by the method for preparing the phosphate-coated lithium manganese iron phosphate material according to any one of claims 1 to 8; Preferably, the coating layer thickness of the phosphate-coated lithium manganese iron phosphate material is 0.5-1 nm; Preferably, the average particle size of the phosphate-coated lithium manganese iron phosphate material is 200-800 nm; Preferably, the specific surface area of ​​the phosphate-coated lithium manganese iron phosphate material is 10-30 m 2 / g.

10. A lithium ion battery, characterized in that: It includes the phosphate-coated lithium manganese iron phosphate material as claimed in claim 9.

Citation Information

Patent Citations

  • Composite material containing lithium manganese ferric phosphate with core-shell structure and preparation method thereof

    CN110416525A

  • Modified positive electrode material and preparation method and application thereof

    CN115432751A